Coated wires and wiring harnesses
By using a specific resin composition in insulated wires and adjusting the water content, the problem of surface roughness of the insulation coating caused by zinc oxide and imidazole compounds has been solved, and the heat resistance, appearance and water-stopping properties have been improved, ensuring the coating High-quality performance for wires and harnesses.
Patent Information
- Application Number
- CN202111227802.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-10-30
- Filing Date
- 2021-10-21
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-10-21
AI Technical Summary
When zinc oxide and imidazole-based compounds are used in existing insulated wires with excellent heat resistance, the surface of the insulation coating is rough, which affects the water-stopping properties and appearance. When installing the water-stopping parts, small gaps may be generated, reducing the waterproof performance.
A resin composition containing silane-grafted polyolefin, unmodified polyolefin, modified polyolefin, flame retardant, cross-linking catalyst, zinc oxide and imidazole compound is used as the material of the insulating coating, and the water content is adjusted to Improve the fluidity of the resin mixture, ensure that the surface roughness Ra of the insulating coating part is 4.0 μm or less, and enhance fluidity and surface smoothness.
It realizes coated wires and wire harnesses with excellent heat resistance and excellent appearance, improves water-stopping properties and manufacturability, reduces the generation of cutting chips, and improves the waterproof performance and production efficiency of wire harnesses.
Smart Images

Figure CN114446525B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to coated electric wires and wire harnesses. Background Art
[0002] Patent Document 1 discloses, as an insulated wire having excellent heat resistance, an insulated wire in which an insulating coating is formed by crosslinking a specific polyolefin composition.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2019-163406 Summary of the invention
[0006] [Problems to be Solved by the Invention]
[0007] There is a demand for a covered electric wire that is excellent in heat resistance and appearance.
[0008] Patent Document 1 discloses zinc oxide and imidazole compounds as additives for improving heat resistance in the above-mentioned composition. The present inventors have found that zinc oxide and imidazole compounds affect the appearance of the insulating coating. Specifically, the surface of the insulating coating is rough.
[0009] In addition, in applications where water-stopping properties are required in the coated wire, a cylindrical water-stopping member is installed on the outer periphery of the coated wire. When the surface of the insulating coating is rough, the water-stopping member will not fit closely with the outer peripheral surface of the insulating coating. Therefore, a small gap may be generated between the insulating coating and the water-stopping member. The above-mentioned small gap will reduce the water-stopping properties between the insulating coating and the water-stopping member.
[0010] In view of the above circumstances, one object of the present disclosure is to provide a covered electric wire having excellent heat resistance and excellent appearance. In addition, another object of the present disclosure is to provide a wiring harness including a covered electric wire having excellent heat resistance and excellent appearance.
[0011] [Means for solving the problem]
[0012] The covered electric wire disclosed in the present invention is a covered electric wire having a conductor and an insulating covering portion, wherein:
[0013] The insulating coating is composed of a resin composition.
[0014] The resin composition comprises:
[0015] Silane grafted polyolefin;
[0016] Unmodified polyolefins;
[0017] A modified polyolefin having one or more functional groups selected from the group consisting of a carboxyl group, an ester group, an acid anhydride group, an amino group, and an epoxy group;
[0018] Flame retardants;
[0019] a cross-linking catalyst; and
[0020] Zinc oxide and imidazole compounds,
[0021] The insulating coating has a surface roughness Ra of 4.0 μm or less.
[0022] The wiring harness disclosed herein comprises the insulated electric wire disclosed herein, a terminal, and a waterproof member.
[0023] The terminal is mounted on at least one of the two ends of the covered electric wire.
[0024] The waterproof member is mounted on the outer periphery of the insulating coating.
[0025] [Effects of the Invention]
[0026] The covered electric wire of the present disclosure and the covered electric wire included in the wire harness of the present disclosure are excellent in heat resistance and appearance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a perspective view showing an example of a covered electric wire according to the embodiment.
[0028] Figure 2 This is a side view showing an example of a wire harness according to the embodiment. DETAILED DESCRIPTION
[0029] [Description of Embodiments of the Present Disclosure]
[0030] The covered electric wire of the present disclosure is based on the following findings.
[0031] When the resin mixture used in the raw material of the insulating sheath is a polyolefin composition containing the above-mentioned zinc oxide and imidazole compounds, the surface of the insulating sheath may be rough. As one of the reasons, it is known that when the above-mentioned resin mixture is extruded to form the insulating sheath, the zinc oxide and imidazole compounds will reduce the fluidity of the above-mentioned resin mixture. The inventors have studied how to improve the fluidity of the above-mentioned resin mixture, and found that the water content of the above-mentioned resin mixture is related to the surface roughness of the insulating sheath. If the above-mentioned water content is high, there may be a difference in the distribution state of bubbles generated by the vaporization of water inside the above-mentioned resin mixture and on the outer surface of the above-mentioned resin mixture. It is known that the fluidity of the above-mentioned resin mixture may be reduced due to the difference in the above-mentioned bubble distribution state. Due to the reduction in the fluidity of the above-mentioned resin mixture, undesirable phenomena such as melt fracture are easily generated during extrusion. It is known that an insulating sheath with a rough surface will be molded due to melt fracture, etc. The inventors have found that when the water content in the above-mentioned resin mixture is appropriately adjusted, especially when the above-mentioned water content is reduced to a certain extent, an insulating sheath with a smooth surface can be manufactured.
[0032] Initially, the contents of the embodiments of the present disclosure are listed for description.
[0033] (1) A covered electric wire according to one embodiment of the present disclosure is a covered electric wire including a conductor and an insulating covering portion, wherein:
[0034] The insulating coating is composed of a resin composition.
[0035] The resin composition comprises:
[0036] Silane grafted polyolefin;
[0037] Unmodified polyolefins;
[0038] A modified polyolefin having one or more functional groups selected from the group consisting of a carboxyl group, an ester group, an acid anhydride group, an amino group, and an epoxy group;
[0039] Flame retardants;
[0040] a cross-linking catalyst; and
[0041] Zinc oxide and imidazole compounds,
[0042] The insulating coating has a surface roughness Ra of 4.0 μm or less.
[0043] The covered electric wire of the present disclosure contains zinc oxide and an imidazole compound, and thus has excellent heat resistance. Since the insulating coating containing a crosslinking catalyst is usually crosslinked, the covered electric wire of the present disclosure also has excellent heat resistance.
[0044] As described above, the surface roughness Ra of the insulating coating is small, so that the surface of the insulating coating is smooth. The appearance of the covered electric wire disclosed in this way is also excellent. In the case where a water-stopping component is installed on the periphery of the covered electric wire disclosed in this way, the insulating coating and the water-stopping component are in close contact. Therefore, the water-stopping property of the covered electric wire disclosed in this way is also excellent. It should be noted that the surface roughness Ra is the arithmetic mean roughness. In addition, by making the surface of the insulating coating smooth, the installation of the water-stopping component is easy. From this aspect, when the covered electric wire disclosed in this way is used in a wiring harness for waterproofing purposes, the manufacturability of the above-mentioned wiring harness is excellent.
[0045] Furthermore, by making the surface of the insulating coating smooth, when the covered electric wire of the present disclosure is cut, it is not easy to generate cuttings from the insulating coating. Therefore, in the operation of installing the terminal at the end of the cut covered electric wire as described below, the reduction in workability due to cuttings can be suppressed. From this aspect, when the covered electric wire of the present disclosure is used in a wire harness, the manufacturability of the wire harness is excellent.
[0046] (2) As an example of the covered electric wire of the present disclosure, there is an embodiment in which the unmodified polyolefin includes a block polypropylene.
[0047] In the above embodiment, the resin mixture as the raw material of the insulating coating has excellent fluidity during the manufacturing process. Therefore, it is easy to manufacture a coated electric wire with excellent appearance. From this point of view, the above embodiment has excellent manufacturability.
[0048] (3) As an example of the covered electric wire of the present disclosure, there is a mode in which the surface roughness Ra is 3.0 μm or less.
[0049] In the above-mentioned embodiment, the appearance, waterproofing property, and workability during terminal installation are more excellent.
[0050] (4) As an example of the covered electric wire of the present disclosure, there is a mode in which the surface roughness Ra is 2.0 μm or less.
[0051] In the above aspect, the appearance, the waterproof property, and the workability during the terminal installation are further excellent.
[0052] (5) As an example of the covered electric wire of the present disclosure, there is a mode in which the surface roughness Ra is 0.6 μm or more.
[0053] In the production process according to the above method, the water content can be easily adjusted, thereby achieving excellent manufacturability.
[0054] (6) As an example of the covered electric wire of the present disclosure, there can be mentioned:
[0055] The above conductors consist of stranded wires,
[0056] An embodiment in which two or more metal wires constituting the stranded wire are each aluminum alloy wire.
[0057] The above method is lighter than the case where the metal wire is a copper wire or a copper alloy wire. In addition, the above method is easier to bend than the case where the conductor is a single aluminum alloy wire with the same cross-sectional area. From this point of view, the above method has excellent flexibility.
[0058] (7) A wire harness according to one aspect of the present disclosure includes the covered electric wire, the terminal, and the waterproof member according to any one of (1) to (6).
[0059] The terminal is mounted on at least one of the two ends of the covered electric wire.
[0060] The waterproof member is mounted on the outer periphery of the insulating coating.
[0061] The covered electric wire of the present disclosure included in the wire harness of the present disclosure is excellent in heat resistance and appearance. For the above reasons, the wire harness of the present disclosure is also excellent in water stopping property and manufacturability.
[0062] [Details of the embodiments of the present disclosure]
[0063] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings as appropriate. The same reference numerals in the drawings represent the same names.
[0064] [Covered wire]
[0065] The following reference Figure 1 The covered electric wire according to the embodiment will be described.
[0066] The covered electric wire 1 of the embodiment includes a conductor 2 and an insulating coating 3. The conductor 2 includes a single metal wire 22 or a plurality of metal wires 22. Figure 1 The case where the conductor 2 is a stranded wire 20 having a plurality of metal wires 22 is exemplified. The insulating coating 3 is a molded body made of a resin composition. The insulating coating 3 covers the outer periphery of the conductor 2. Typically, a resin mixture as a raw material of the insulating coating 3 is extruded onto the outer periphery of the conductor 2, thereby molding into a predetermined shape, and then cross-linking is performed to manufacture the insulating coating 3. The insulating coating 3 constitutes the outer surface of the coated electric wire 1. Therefore, the appearance of the insulating coating 3 is also the appearance of the coated electric wire 1.
[0067] In the covered electric wire 1 of the embodiment, the insulating coating 3 is made of a specific resin composition. In the covered electric wire 1 of the embodiment, the surface roughness Ra of the insulating coating 3 is 4.0 μm or less. Such an insulating coating 3 has a smooth surface.
[0068] The following describes the use of the insulating coating 3, the conductor 2, and the covered electric wire 1 in order.
[0069] 〈Insulation coating〉
[0070] "composition"
[0071] The resin composition constituting the insulating coating 3 comprises (A) silane-grafted polyolefin, (B) unmodified polyolefin, (C) modified polyolefin, (D) flame retardant, (E) crosslinking catalyst, and (F) zinc oxide and imidazole compound. The resin composition may further comprise one or more additives selected from the group consisting of (G) antioxidant, (H) metal deactivator and (I) lubricant.
[0072] The components of the above-mentioned resin combination are described below. In the following description, about the content of each component (A), (B) and (C) as the resin component in the above-mentioned resin combination, the ratio contained in 125 mass parts of the total of these three components is expressed in mass parts. The content of each component other than the above-mentioned three components in the above-mentioned resin combination is expressed in mass parts relative to 125 mass parts of the total of the above-mentioned three components. It should be noted that the total mass parts of the above-mentioned resin combination as a whole including the above-mentioned resin component can, for example, be 195 mass parts or more and 250 mass parts or less. In the determination of each component, representatively, the use of nuclear magnetic resonance spectroscopy (NMR) can be cited.
[0073] (A) Silane-grafted polyolefin
[0074] The silane-grafted polyolefin is a component obtained by graft-polymerizing a silane coupling agent onto a polyolefin as a main chain, that is, a component into which a silane grafted chain is introduced. The content of the silane-grafted polyolefin may be, for example, 50 parts by mass or more and 80 parts by mass or less.
[0075] As the polyolefin in the silane grafted polyolefin, for example, one or more polymers selected from the group consisting of polyethylene (PE), polypropylene (PP), and copolymers of ethylene or propylene and α-olefins can be cited. PE is a homopolymer of ethylene. PP is a homopolymer of propylene. For example, the above copolymers can include ethylene-butene copolymers and ethylene-octene copolymers.
[0076] (B) Unmodified polyolefin
[0077] The unmodified polyolefin is a polyolefin composed of hydrocarbons, and a modification group has not been introduced by graft polymerization, copolymerization, etc. The content of the unmodified polyolefin may be, for example, 30 parts by mass or more and 55 parts by mass or less.
[0078] As the unmodified polyolefin, for example, one or more polymers listed as polyolefins in (A) silane grafted polyolefin can be cited. In particular, when the unmodified polyolefin and the polyolefin in (A) silane grafted polyolefin include the same polymer, the compatibility is excellent. Therefore, the resin mixture is easily kneaded uniformly during the manufacturing process. By using the resin mixture that has been uniformly kneaded, it is easy to manufacture a coated wire 1 with excellent heat resistance and appearance.
[0079] Alternatively, as the unmodified polyolefin, there can be mentioned polyolefin elastomers based on olefins. The polyolefin elastomer imparts flexibility to the insulating coating 3. Examples of polyolefin elastomers include polyolefin-based thermoplastic elastomers (TPO), ethylene-propylene rubber (EPM, EPR), ethylene-propylene-diene copolymers (EPDM, EPT), etc. Examples of TPO include polyethylene-based elastomers and polypropylene-based elastomers.
[0080] Alternatively, as unmodified polyolefin, polymers containing one or more of the above-mentioned polymers and polyolefin elastomers can be cited. As a specific example, elastomers containing PE and PP can be cited. It is known that in this method, the polyolefin elastomer can improve the fluidity of the resin mixture during the manufacturing process. In this method, the total content of the above-mentioned one or more polymers can be cited, for example, from 25 parts by mass to 45 parts by mass. The content of the polyolefin elastomer can be cited, for example, from 3 parts by mass to 10 parts by mass.
[0081] Alternatively, as an unmodified polyolefin, a block polypropylene can be cited. Hereinafter, the block polypropylene will be referred to as block PP. It is known that block PP can improve the fluidity of the resin mixture during the manufacturing process. It is known that the effect of improving the fluidity in block PP is higher than the effect of improving the fluidity in the above-mentioned polyolefin elastomer. By making the fluidity of the resin mixture containing block PP excellent, it is easy to produce an insulating sheath 3 with a smooth surface. In addition, when a resin mixture containing block PP is used as shown in the test example described later, compared with the case where block PP is not included, even if the water content in the above-mentioned resin mixture increases to a certain extent, it is easy to produce an insulating sheath 3 with a smooth surface. From this aspect, in the resin mixture containing block PP, the range of the above-mentioned water content that can produce the insulating sheath 3 with a smooth surface can be said to be wider. Such a resin mixture is easy to adjust the above-mentioned water content. For example, the drying time can be shortened. Or, for example, the drying operation can be carried out using simple equipment. Preferably, no drying is required. Since excessive moisture adjustment is not necessary, the covered electric wire 1 including the insulating coating 3 including the block PP has excellent appearance and also excellent manufacturability.
[0082] Alternatively, as unmodified polyolefin, a polymer including one or more of the above-mentioned polymers and block PP can be cited. As a specific example, a polymer including PE and block PP can be cited. By including block PP, as described above, the fluidity of the resin mixture during the manufacturing process is excellent. In this embodiment, the total content of the above-mentioned one or more polymers can be cited, for example, from 25 parts by mass to 45 parts by mass. The content of block PP can be cited, for example, from 3 parts by mass to 10 parts by mass.
[0083] (C) Modified polyolefin
[0084] The modified polyolefin herein has one or more functional groups selected from the group consisting of a carboxyl group, an ester group, an anhydride group, an amino group, and an epoxy group. The content of the modified polyolefin may be, for example, 3 parts by weight or more and 15 parts by weight or less. It should be noted that the modified polyolefin introduced with a silanol derivative is classified as (A) silane-grafted polyolefin, and therefore is not classified as (C) modified polyolefin.
[0085] The modified polyolefin functions as a compatibilizer for the resin components (A) and (B) and the inorganic component zinc oxide. This function can improve the dispersibility of the inorganic component, thereby making it easy to manufacture the insulating coating 3 in which the inorganic component is uniformly dispersed. As a result, it is easy to manufacture the coated wire 1 with excellent heat resistance. The polyolefin in the modified polyolefin can include, for example, one or more polymers included in the polyolefin listed in the (A) silane grafted polyolefin.
[0086] Examples of polymerizable compounds having a carboxyl group include acrylic acid, methacrylic acid, crotonic acid, α-chloroacrylic acid, itaconic acid, butenetricarboxylic acid, maleic acid, fumaric acid, and derivatives containing these components in a part of the molecular structure. When the acids listed above form anhydrides, the anhydride groups can be introduced using the anhydrides.
[0087] Examples of the polymerizable compound having an ester group include vinyl acetate and vinyl propionate.
[0088] Examples of the polymerizable compound having an amino group include esters, vinylamine, allylamine, and derivatives containing these components in a part of the molecular structure.
[0089] Examples of the polymerizable compound having an epoxy group include glycidyl ethers, p-glycidyl styrene, and derivatives containing these components in a part of the molecular structure.
[0090] The polymerizable monomer copolymerizable with the polymerizable compound having the functional group may include at least one of an olefin monomer having no functional group and a polymerizable monomer having a functional group other than a carboxyl group and an epoxy group. Examples of the olefin monomer include PE and PP.
[0091] (D) Flame retardant
[0092] Examples of the flame retardant include at least one of a metal hydroxide and a bromine-based flame retardant.
[0093] Metal hydroxides can provide flame retardancy, excellent heat deformation resistance, and low cost. Examples of metal hydroxides include magnesium hydroxide, aluminum hydroxide, and zirconium hydroxide. When the flame retardant only includes metal hydroxide, the content of the metal hydroxide can be, for example, 10 parts by weight or more and 100 parts by weight or less.
[0094] Bromine flame retardants can be included together with inorganic flame retardants. Bromine flame retardants can include, for example, one or more selected from the group consisting of phthalimide flame retardants, ethylene bispentabromobenzene, and derivatives of ethylene bispentabromobenzene. The above-mentioned bromine flame retardants have a high melting point, thereby making the heat resistance of the insulating coating 3 excellent. Antimony trioxide can be cited as an inorganic flame retardant. The content of only bromine flame retardants can be cited, for example, more than 10 parts by mass and less than 40 parts by mass. The content of only inorganic flame retardants can be cited, for example, more than 5 parts by mass and less than 20 parts by mass.
[0095] When the flame retardant includes a metal hydroxide and a bromine-based flame retardant, the content of the metal hydroxide and the content of the bromine-based flame retardant may be less than the above range. For example, the content of the metal hydroxide is 10 to 50 parts by mass, the content of the bromine-based flame retardant is 5 to 20 parts by mass, and the content of the inorganic flame retardant additive is 5 to 20 parts by mass.
[0096] (E) Cross-linking catalyst
[0097] The crosslinking catalyst is a silanol condensation catalyst for silane crosslinking the (A) silane-grafted polyolefin. The content of the crosslinking catalyst may be, for example, 0.01 parts by mass or more and 10 parts by mass or less.
[0098] Examples of the crosslinking catalyst include metal carboxylates, titanates, organic bases, inorganic acids, organic acids, etc. More specifically, tin compounds such as dibutyltin dilaurate, dibutyltin dimaleate, dibutyltin diisooctylthioglycolate, and dibutyltin β-mercaptopropionate are included.
[0099] (F) Zinc oxide and imidazole compounds
[0100] Zinc oxide and imidazole compounds contribute to the improvement of heat resistance and resistance to long-term heating. The content of zinc oxide and the content of imidazole compounds can be, for example, 1 part by mass or more and 15 parts by mass or less, respectively. When the above content is within the above range, the heat resistance and resistance to long-term heating of the insulating coating 3 are excellent, and the zinc oxide and imidazole compounds are easily dispersed in the resin component during the manufacturing process. Therefore, it is easy to manufacture the insulating coating 3 in which zinc oxide and imidazole compounds are uniformly dispersed. As a result, it is easy to manufacture the coated wire 1 with excellent heat resistance.
[0101] Examples of imidazole compounds include mercaptobenzimidazole (MBI). In particular, when the imidazole compound is 2-mercaptobenzimidazole or its zinc salt, the stability at high temperatures is excellent, thereby obtaining an insulating sheath 3 having excellent heat resistance. It should be noted that imidazole compounds are not used to prevent oxidative degradation but to prevent degradation due to peroxide decomposition of rubber hydrocarbons, and are therefore called antioxidants.
[0102] (G) Antioxidants
[0103] The antioxidant may be, for example, a hindered phenol antioxidant. Hindered phenols having a melting point of 200° C. or higher are particularly preferred. The content of the antioxidant may be, for example, 1 part by mass or more and 10 parts by mass or less. When the content is within the above range, blooming due to the antioxidant may be suppressed. When the content is 2 parts by mass or more, an effect of improving heat resistance may also be expected.
[0104] (H) Metal passivator
[0105] The metal passivator may include a component that has the function of preventing the oxidation of the conductor 2 caused by the contact between the metal constituting the conductor 2 and the insulating coating 3. For example, copper passivators, chelating agents, etc. may be mentioned. As specific examples, hydrazide derivatives, salicylic acid derivatives, etc. may be mentioned. The content of the metal passivator may be, for example, 0.5 parts by mass or more and 10 parts by mass or less. When the above content is within the above range, blooming and cross-linking obstacles caused by the metal passivator may be suppressed. In addition, when the metal constituting the conductor 2 is copper or a copper alloy, a good effect of preventing copper poisoning may be obtained.
[0106] (I) Lubricant
[0107] The lubricant improves the lubricity of the insulating coating 3. From the perspective of compatibility with the resin component, the lubricant is preferably a fatty acid derivative such as erucic acid, oleic acid, or stearic acid, or a polyethylene wax. The content of the lubricant is, for example, 0.1 parts by mass to 10 parts by mass.
[0108] (Other additives)
[0109] The resin composition constituting the insulating coating 3 may contain additives other than the above components within a range that does not hinder the purpose of having excellent heat resistance and a smooth surface. Examples of additives other than the above components include inorganic fillers, pigments, silicone oils, and the like.
[0110] Examples of inorganic fillers include magnesium oxide and calcium carbonate. Inorganic fillers can be used to adjust the hardness of the resin. By properly adjusting the hardness of the resin, the insulating coating 3 has excellent thermal viscosity and heat deformation resistance. From the perspective of resin strength, the content of the inorganic filler can be, for example, 30 parts by mass or less. Pigments can color the insulating coating 3.
[0111] Surface roughness
[0112] The insulating coating 3 of the covered electric wire 1 of the embodiment has a smooth surface. Quantitatively speaking, the surface roughness Ra of the insulating coating 3 is 4.0 μm or less. The covered electric wire 1 of such an embodiment has a smooth appearance. From this point of view, the covered electric wire 1 of the embodiment has an excellent appearance. In addition, a cylindrical water stop member 7 ( Figure 2 ), the inner circumferential surface of the water stop component 7 is in close contact with the outer surface of the insulating coating 3. Due to this close contact, no small gap is generated between the outer surface of the insulating coating 3 and the inner circumferential surface of the water stop component 7. Therefore, water does not penetrate into the small gap through the capillary phenomenon. The covered wire 1 of such an embodiment has excellent water stopping properties. Furthermore, by making the insulating coating 3 have a smooth surface, it is not easy for the operator to generate cutting chips from the insulating coating 3 when cutting the covered wire 1. Therefore, in the equipment for cutting the covered wire 1, the terminal 6 ( Figure 2 ) is installed at the end of the cut covered electric wire 1, and the above-mentioned cutting chips are not easily accumulated in the processing equipment. As a result, the number of maintenance operations for removing the above-mentioned cutting chips from the above-mentioned processing equipment is reduced. From this point of view, the covered electric wire 1 of the embodiment also contributes to improving the wiring harness 5 ( Figure 2 )’s manufacturability.
[0113] The smaller the surface roughness Ra, the better the appearance, waterproofness, and workability of the covered wire 1 when attaching the terminal 6. In view of these effects, the surface roughness Ra is preferably 3.0 μm or less. More preferably, the surface roughness Ra is 2.0 μm or less.
[0114] The lower limit of the surface roughness Ra is not limited. However, in order to reduce the surface roughness Ra as much as possible, the water content of the resin mixture needs to be reduced as much as possible during the manufacturing process. For example, excessive water content adjustment such as extending the drying time is required. From the perspective of manufacturability, the surface roughness Ra can be above 0.6 μm. When the surface roughness Ra is above 0.8 μm, it is easy to shorten the drying time.
[0115] When the surface roughness Ra is 0.6 μm to 4.0 μm, further 0.8 μm to 3.0 μm, or 1.0 μm to 2.0 μm, the covered electric wire 1 having an excellent appearance can be manufactured with good productivity.
[0116] "thickness"
[0117] The insulating coating 3 covers the outer circumference of the conductor 2. The insulating coating 3 is typically provided in such a manner that the outer diameter of the coated wire 1 is substantially the same at any position in the axial direction of the coated wire 1. The thickness of the insulating coating 3 is equivalent to the distance between the outer circumferential surface of the conductor 2 and the outer circumferential surface of the coated wire 1. The above thickness can be appropriately selected within a range having a specific insulation strength relative to the operating voltage. For example, in automotive applications, the above thickness can be 0.5 mm or more and 2.0 mm or less. It should be noted that the "high voltage" in the operating voltage for automotive applications is specified by JASO D624 (JP) 2015 edition. "Low voltage" is specified by JASO D611 (JP) 2014 edition.
[0118] "shape"
[0119] The outer shape of the insulating coating 3 is typically circular in a cross section when the coated electric wire 1 is cut along a plane perpendicular to the axial direction of the coated electric wire 1. The outer surface of the insulating coating 3 is a cylindrical surface.
[0120] <conductor>
[0121] Examples of the metal constituting the conductor 2 include pure aluminum, aluminum alloys, pure copper, and copper alloys. The conductor 2 composed of pure aluminum or aluminum alloys is lighter than the conductor 2 composed of pure copper or copper alloys, and exhibits the effect of not generating copper poisoning. In particular, the mechanical properties such as strength and impact resistance of the conductor 2 composed of aluminum alloys are superior to those of the conductor 2 composed of pure aluminum. The electrical conductivity of the conductor 2 composed of pure copper or copper alloys is superior to that of the conductor 2 composed of pure aluminum or aluminum alloys. The composition of the aluminum alloy and the composition of the copper alloy can utilize known compositions.
[0122] Conductor 2 can be exemplified by Figure 1The conductor 2 may be a stranded wire 20 shown in the figure, a single-wire metal wire 22 not shown, or a stranded wire assembly not shown. The stranded wire 20 is formed by twisting a plurality of metal wires 22. The stranded wire assembly is formed by twisting a plurality of stranded wires 20. The conductor 2 may be either a single stranded wire 20 or a plurality of stranded wires 20. The stranded wire 20 is easier to bend than a single-wire metal wire having the same cross-sectional area, and thus has excellent flexibility. The stranded wire assembly has excellent flexibility and can ensure a larger conductor cross-sectional area.
[0123] The conductor 2 of this example is a stranded wire 20. The plurality of metal wires 22 constituting the stranded wire 20 are each an aluminum alloy wire. Therefore, as described above, the conductor 2 of this example has the effects of being light in weight, not causing copper poisoning, and having excellent flexibility.
[0124] The outer diameter and cross-sectional area of the conductor 2 can be appropriately selected according to the application of the covered wire 1. For example, in automotive applications, the cross-sectional area of the conductor 2 can be 3 mm. 2 Above 200mm 2 the following.
[0125] <use>
[0126] As an example of the use of the covered electric wire 1 of the embodiment, power lines, information communication lines, etc. in transmission equipment such as automobiles, ships, and aircraft, and other equipment including robots can be cited. The power line is, for example, an electric wire that connects a battery and an electric motor provided in the above-mentioned transmission equipment such as automobiles. Power lines are generally electric wires for high voltage use. Information communication lines are generally electric wires for low voltage use. In electric wires for high voltage use, as electricity is applied, the conductor 2 releases heat through Joule heat. If the current used is further increased, the heat release of the conductor 2 also increases. Therefore, high heat resistance is required in the insulating coating. As described above, the covered electric wire 1 of the embodiment has an insulating coating 3 with excellent heat resistance, and is therefore suitable for electric wires for high voltage use such as the above-mentioned power line.
[0127] Automobile electric wires are classified into grades A to E according to the allowable heat resistance temperature in the international standard ISO 6722. As described above, the covered electric wire 1 of the embodiment has excellent heat resistance, and thus has a D-class property with a heat resistance temperature of 150°C, for example.
[0128] [Wire Harness]
[0129] The covered electric wire 1 of the embodiment is typically provided with a terminal 6 ( Figure 2) is utilized in a state where it is installed on at least one of the two end portions of the covered electric wire 1. Usually, terminals 6 are installed at both ends of the covered electric wire 1, respectively. The covered electric wire 1 of the embodiment in which the terminals 6 are installed is used in a wiring harness. As an example of a wiring harness, there can be cited a method in which a single electric wire is provided and the electric wire is the covered electric wire 1 of the embodiment. As another example of a wiring harness, there can be cited a method in which a plurality of electric wires are provided and at least one of the plurality of electric wires is the covered electric wire 1 of the embodiment. The method in which a plurality of electric wires are provided may also include a component for bundling the plurality of electric wires. For example, the bundling component may include a tubular protective component such as a corrugated tube, a bundling component such as a tape, and the like.
[0130] Refer to the following Figure 2 A wire harness according to the embodiment will be described.
[0131] The wire harness 5 of the embodiment includes the insulated wire 1 of the embodiment, a terminal 6, and a waterproof member 7. The terminal 6 is attached to at least one of the two ends of the insulated wire 1. The waterproof member 7 is attached to the outer periphery of the insulating coating 3. The terminal 6 and the waterproof member 7 can use known members. Figure 2 A crimp terminal having a hole 63 is illustrated.
[0132] The terminal 6 is typically a part including a wire barrel portion 60 and a connecting portion 62. The wire barrel portion 60 is a portion electrically connected to the conductor 2 of the insulated wire 1. The wire barrel portion 60 of this example is crimped to the conductor 2, thereby being electrically and mechanically connected to the conductor 2. The connecting portion 62 is a portion electrically connected to a connection object of the insulated wire 1. The illustration of the connection object of the insulated wire 1 is omitted. The connecting portion 62 of this example is flat. In addition, the connecting portion 62 includes a hole 63 that passes through the front and back of the connecting portion 62. A bolt not shown in the figure is inserted into the hole 63. The connecting portion 62 of the terminal 6 is electrically and mechanically connected to the above-mentioned connection object by means of a bolt.
[0133] The water stop member 7 is typically a cylindrical rubber member having an inner diameter smaller than the outer diameter of the coated wire 1 and an outer diameter larger than the outer diameter of the coated wire 1. By utilizing elastic deformation to make the inner diameter of the water stop member 7 wider than the outer diameter of the coated wire 1, the coated wire 1 can be inserted through the inner periphery of the water stop member 7. In addition, by utilizing elastic contraction to reduce the inner diameter of the water stop member 7, the inner peripheral surface of the water stop member 7 can be made to fit closely with the outer surface of the coated wire 1. By this close fit, the state in which the water stop member 7 is mounted on the outer periphery of the coated wire 1 can be maintained.
[0134] The wiring harness 5 of the embodiment is typically used in a state where the terminal 6 and its vicinity are arranged in the housing of a connector not shown. The water stop member 7 is arranged between the inner peripheral surface of the housing and the outer surface of the covered wire 1 and is compressed by both. The water stop member 7 is elastically deformed by the compression, thereby fitting closely with both. Due to this close fitting, the wiring harness 5 of the embodiment has excellent water stop properties, and can be appropriately used for waterproof purposes.
[0135] [Manufacturing method of covered electric wire]
[0136] The covered electric wire 1 of the embodiment can be representatively manufactured by the following covered electric wire manufacturing method. The covered electric wire manufacturing method comprises the following steps: a step of forming a covering layer by extruding a resin mixture containing the above-mentioned components (A) to (F) onto the outer periphery of the conductor 2; and a step of cross-linking the above-mentioned covering layer. The above-mentioned resin mixture may also contain (G) to (I) and other additives as appropriate in addition to the above-mentioned components. The components constituting the above-mentioned resin mixture may be commercially available products.
[0137] The resin mixture is obtained by kneading the above components before extrusion. A known kneading machine can be used for kneading. As described above, if the components have excellent compatibility, a resin mixture with a uniform composition can be easily obtained.
[0138] When manufacturing the above-mentioned resin mixture, a batch containing at least one of the above-mentioned components and a binder resin can be used. The binder resin can be, for example, one or more polymers listed as polyolefins in the above-mentioned (A) silane-grafted polyolefin. For example, when a batch containing a crosslinking catalyst is used, it is expected to prevent the silane crosslinking reaction in the silane-grafted polyolefin from being carried out due to moisture in the atmosphere. When a batch is used, the content of the binder resin can be adjusted in such a way that the content of each component meets the above-mentioned range.
[0139] The batch material may also be manufactured in multiple stages. As a specific example, a method for manufacturing a covered electric wire includes a step of manufacturing a first batch material, a step of manufacturing a second batch material including the first batch material, and a step of manufacturing a third batch material including the second batch material, wherein the third batch material is extruded.
[0140] In the crosslinking step of the coating layer, the crosslinking conditions may be adjusted so that the degree of crosslinking of the insulating coating 3 after crosslinking reaches 50% or more in terms of gel fraction. The higher the gel fraction, the better the heat resistance of the insulating coating 3. From the perspective of heat resistance, the gel fraction may be 60% or more. The gel fraction is generally used as an indicator of the crosslinking state of the crosslinked wire. The gel fraction may be measured, for example, in accordance with JASO D608 2013 edition.
[0141] In order to manufacture the covered wire 1 of the embodiment, the water content contained in the resin mixture before extrusion can be adjusted. In particular, the water content can be reduced by drying the resin mixture compared to before drying. Although it varies depending on the composition of the resin mixture before extrusion, for example, the resin mixture is set to 100% by mass, and the water content in the resin mixture satisfies 700 mass ppm or less. By making the water content satisfy the above range, it is easy to manufacture an insulating coating 3 with a smooth surface. The water content can be 500 mass ppm or less, 300 mass ppm or less. The adjustment conditions of the water content can be set in a manner that the water content (mass ppm) in the batch material finally extruded is reduced. In addition, the adjustment conditions of the water content can be set, for example, using the surface roughness Ra of the insulating coating 3 as an indicator.
[0142] In the case of manufacturing batches in multiple stages as described above, it is possible to dry each batch, dry only one batch, or dry any multiple batches. The more drying steps are performed and the longer the drying time is, the easier it is to reduce the moisture content. However, the increase in the number of steps and the extension of the drying time will lead to a decrease in the manufacturability of the coated wire 1. From the perspective of manufacturability, for example, the water content can be adjusted in such a way that the surface roughness Ra of the insulating coating 3 satisfies 0.6 μm or more.
[0143] In addition, kneading conditions, extrusion conditions, cross-linking conditions, etc. can refer to known conditions.
[0144] (Main effect)
[0145] The coated electric wire 1 of the embodiment has excellent heat resistance. In addition, in the coated electric wire 1 of the embodiment, the surface roughness Ra of the insulating coating 3 is small, thereby having a smooth surface. The coated electric wire 1 of such an embodiment has excellent appearance and excellent water stopping properties. The above effects can be specifically described using the test examples described below.
[0146] [Test Example 1]
[0147] A covered electric wire was produced using a mixture of two or more resins having different compositions, and the appearance and water stopping properties of each covered electric wire were examined.
[0148] In this test, a coating layer is formed by extruding a resin mixture onto the outer periphery of a conductor, and then the coating layer is cross-linked to form an insulating coating. Thus, the coated wires manufactured in this test all have an insulating coating obtained by cross-linking. The conductor here is a stranded wire assembly consisting of a plurality of aluminum alloy wires.
[0149] (composition)
[0150] The composition of each resin mixture is shown in Table 1. In Table 1, the unit of the content of each component constituting each resin mixture is part by mass. Four resin mixtures of compositions No. 1 to No. 3 and No. 101 were prepared.
[0151] The resin mixtures of compositions No. 1 to No. 3 all contain (A) silane-grafted polyolefin, (B) unmodified polyolefin, (C) modified polyolefin, (D) flame retardant, (E) cross-linking catalyst, (F) zinc oxide and imidazole compound, (G) antioxidant, (H) metal deactivator, (I) lubricant, and (J) pigment composition.
[0152] The resin mixtures of compositions No. 1 to No. 3 have different components of (B).
[0153] The resin mixtures of compositions No. 1, No. 2 and composition No. 101 described below contain polyethylene (PE) and polypropylene elastomer (PP elastomer) as component (B). The resin mixtures of compositions No. 1, No. 2 and No. 101 do not contain block polypropylene (block PP).
[0154] The resin mixture of composition No. 3 contains PE and block PP as component (B). The resin mixture of composition No. 3 does not contain PP elastomer.
[0155] The resin mixture of composition No. 101 contains components (A) to (E) and components (G) to (J). The resin mixture of composition No. 101 does not contain component (F).
[0156] The following commercially available products were used as the raw materials of the above-mentioned components.
[0157] (A) A batch containing silane-grafted polyethylene and polyethylene as a binder resin was used as the raw material of the silane-grafted polyolefin. The batch was SH700N manufactured by Mitsubishi Chemical Corporation and is indicated as "silane-grafted polyethylene batch" in Table 1.
[0158] (B) PE is Engage ENR7256.02 manufactured by Dow Elastomers Co. PE here is a base polymer and is indicated as "base PE" in Table 1.
[0159] The PP elastomer used in composition No. 1 is Q200F manufactured by Sun Allomer Co., Ltd.
[0160] The PP elastomer used in compositions No. 2 and No. 101 is Newcon NAR6 manufactured by Japan Polypropylene Co., Ltd.
[0161] The block PP used in composition No. 3 was EG7F manufactured by Japan Polypropylene Co., Ltd.
[0162] (C) The modified polyolefin is maleic acid-modified polyethylene, Modic M512 manufactured by Mitsubishi Chemical Corporation.
[0163] (D) The flame retardant is a metal hydroxide. A specific flame retardant is magnesium hydroxide, which is Kisuma 5 manufactured by Kyowa Chemical Industry Co., Ltd.
[0164] (E) A raw material of a crosslinking catalyst used was a batch material containing less than 1 part by mass of a tin compound and the balance being a binder resin. The binder resin was polyethylene. The batch material was LZ015H manufactured by Mitsubishi Chemical Corporation.
[0165] (F) Zinc oxide was zinc white type 1 manufactured by Hakusui Tech Co., Ltd. The imidazole compound was 2-mercaptobenzimidazole, ANTAGE MB manufactured by Kawaguchi Chemical Industry Co., Ltd.
[0166] (G) The antioxidant was a hindered phenol-based antioxidant, and was Irganox 1010 manufactured by BASF Japan Co., Ltd.
[0167] (H) The metal deactivator is a hydrazide derivative, CDA-1 manufactured by ADEKA Corporation.
[0168] (I) The lubricant was erucamide, Alflo P10 manufactured by NOF Corporation.
[0169] (J) Pigment composition A batch containing 1 part by mass of a pigment and the balance being a binder resin was used. The binder resin was polyethylene. This batch was a commercially available color batch.
[0170] In this test, batches are manufactured in multiple stages. For resin mixtures of composition No. 1 to No. 3, the first batch, the second batch, and the third batch are manufactured in sequence. The first batch contains component (B), component (C), and component (F), and does not contain the remaining components listed in Table 1. The second batch contains the above-mentioned first batch, component (D), component (G), component (H), and component (I), and does not contain the remaining components listed in Table 1. The third batch contains the above-mentioned second batch, component (A), component (E), and component (J). That is, the third batch contains all the components listed in Table 1.
[0171] In the resin mixture of composition No. 1 to No. 3, the water content contained in the above-mentioned second batch of materials is adjusted. Here, the above-mentioned water content is changed by changing the time for drying the second batch of materials after measuring the water content (mass ppm) of the second batch of materials. The longer the drying time, the lower the above-mentioned water content is compared with the state before the drying operation. In the determination of the above-mentioned water content, for example, the use of the Karl Fischer method can be cited. In addition, in the determination of the above-mentioned water content, a commercially available water content measuring device can be used. It should be noted that the water contained in the above-mentioned second batch of materials is caused by the moisture absorption of the above-mentioned second batch of materials. Therefore, depending on the surrounding environment, etc., there may be a situation where the above-mentioned water content is low in the state before the drying operation. In this case, the drying time can be shortened. Or sometimes the drying operation is not required.
[0172] In the resin mixture of composition No. 101, the following fourth batch and fifth batch were manufactured in sequence. The fourth batch contained component (B), component (C), component (D), component (G), component (H) and component (I), and did not contain the residual components listed in Table 1. That is, the components of the fourth batch were obtained by removing component (F) from the above-mentioned second batch. The fifth batch contained the fourth batch, component (A), component (E) and component (J). That is, the fifth batch contained all the components listed in Table 1 except component (F).
[0173] [Table 1]
[0174]
[0175] (Appearance)
[0176] 〈Surface roughness〉
[0177] The surface roughness Ra (μm) of the insulating coating of each sample of the coated wire produced using each of the above resin mixtures was measured. The measurement results are shown in Tables 2 to 4. The surface roughness Ra is the arithmetic mean roughness. The surface roughness Ra was measured using a commercially available surface roughness measuring instrument in accordance with JIS B 0601:2013.
[0178] 〈Gloss, matte feeling〉
[0179] For each sample of the coated wire, the appearance is evaluated by whether the insulating coating has gloss / concave and convex parts and whether the insulating coating has a rough feeling. The above-mentioned gloss / concave and convex parts are confirmed by visually checking the insulating coating. The above-mentioned rough feeling is confirmed by the operator touching the insulating coating with the index finger of the bare hand. The evaluation is performed by comparing the insulating coating of each sample with a predetermined reference product as follows. The evaluation results are shown in Tables 2 to 4.
[0180] The reference product is one covered electric wire selected from a plurality of covered electric wires produced using the resin mixture of composition No. 3. The surface roughness Ra of the insulating coating of the reference product is 3.5 μm.
[0181] 《Evaluation of gloss / concavity》
[0182] The evaluation of Very Good means that the gloss of the insulating coating portion of each sample is better than that of the reference product, and that irregularities are difficult to be visually confirmed.
[0183] The evaluation of "Good" means that the gloss of the insulating coating portion of each sample is equivalent to that of the reference product and that it is difficult to visually confirm unevenness.
[0184] The evaluation of "bad" means that the gloss of the insulating coating portion of each sample is inferior to that of the reference product, and the unevenness is difficult to be confirmed by visual observation.
[0185] The evaluation of Very Bad means that the gloss of the insulating coating portion of each sample is inferior to that of the reference product and the unevenness can be confirmed visually.
[0186] Evaluation of the rough feeling
[0187] The evaluation of "very good" means that the roughness of the insulating coating portion of each sample is less than that of the reference product and is better than that of the reference product.
[0188] The evaluation of "Good" means that the roughness of the insulating coating of each sample is equivalent to that of the reference product.
[0189] The evaluation of "bad" means that the roughness of the insulating coating portion of each sample is greater than that of the reference product and is inferior to the reference product.
[0190] The evaluation of Very Bad means that the roughness of the insulating coating of each sample is significantly worse than that of the reference product. The roughness is such that the tester feels pain when touching the insulating coating.
[0191] (water-stopping property)
[0192] For each sample of the covered wire, whether water penetrates from the boundary between the insulating coating and the rubber plug as a waterproof member is evaluated to see whether the waterproof performance is good or not. Here, the test is conducted based on IEC 60529:2001 to evaluate whether the waterproof performance meets IP level 3. The evaluation results are shown in Tables 2 to 4.
[0193] The evaluation of "good" means that there is no intrusion from the above boundary, that is, the waterproof performance satisfies IP level 3.
[0194] The evaluation of "bad" means that the device is infiltrated from the above boundary, that is, the device does not satisfy the waterproof performance of IP level 3.
[0195] [Table 2]
[0196]
[0197] [Table 3]
[0198]
[0199] [Table 4]
[0200]
[0201] Hereinafter, the covered electric wires of samples No. 1 to No. 8 are referred to as a specific electric wire group, and the covered electric wires of samples No. 51 to No. 56 are referred to as a comparative electric wire group.
[0202] As shown in Tables 2 to 4, the specific electric wire group has a glossy appearance and is excellent. In addition, the specific electric wire group is also excellent in water stopping property. In addition, the specific electric wire group does not have unevenness that would cause a rough feeling. From this aspect, it is easy for the operator to handle the specific electric wire group.
[0203] The comparison wire group has no gloss and poor appearance. In addition, the waterproofing property of the comparison wire group is also poor. In addition, the comparison wire group includes a coated wire with unevenness that produces a rough feeling. From this point of view, the operator needs to be careful when handling the comparison wire group.
[0204] As one of the reasons for obtaining the above results, the difference in the surface roughness Ra of the insulating coating is considered. In a specific wire group, the surface roughness Ra of the insulating coating is 4.0 μm or less. The smaller the surface roughness Ra, the more glossy it is, and it does not have a rough feeling. From the aspects of appearance and water stopping, it is preferred that the surface roughness Ra is 3.5 μm or less, and further 3.0 μm or less, 2.5 μm or less. In addition, when (B) the unmodified polyolefin contains block PP, it is easier to reduce the surface roughness Ra than when it contains PP elastomer. From this aspect, it is believed that the effect of improving the fluidity of the resin mixture in the manufacturing process of block PP is greater than that of PP elastomer. It can also be seen that by using a resin mixture containing block PP, it is easy to form an insulating coating with a smooth surface.
[0205] In the covered wire of sample No. 111, the surface roughness Ra of the insulating coating is small, thereby making the appearance and water-stopping property excellent. However, the heat resistance of the covered wire of sample No. 111 is inferior to that of the specific wire group. The heat resistance of the covered wire of sample No. 111 is Class C with a heat resistance temperature of 120°C specified in ISO 6722. In contrast, the heat resistance of the specific wire group is Class D with a heat resistance temperature of 150°C specified in ISO6722. As one of the reasons for the excellent heat resistance of the specific wire group, the resin composition constituting the insulating coating contains component (F). As one of the other reasons, the above-mentioned resin composition contains more component (G) than sample No. 111.
[0206] Next, the results of a study on the cause of the difference in the surface roughness Ra of the insulating coating portion will be described.
[0207] First, from the comparison between the specific wire group and the covered wire of sample No. 111, it can be seen that the presence or absence of component (F) affects the surface roughness Ra. The imidazole compound and zinc oxide contained in the excellent resin mixture are powders, so it is easy to reduce the fluidity of the resin mixture. The reduction in fluidity in the resin mixture is considered to be the main cause of melt fracture, etc.
[0208] Next, the specific wire group and the comparative wire group are compared. Both are the same in that they contain component (F). However, the surface roughness Ra of the insulating coating of the two is different. As one of the reasons for this difference, the difference in the moisture content (mass ppm) contained in the resin mixture during the manufacturing process is considered. The moisture content (mass ppm) shown in Tables 2 to 4 is the mass ratio of the moisture contained in the second batch of materials relative to the second batch of materials. Here, the smaller the moisture content (mass ppm) of the second batch of materials, the smaller the surface roughness Ra. It should be noted that before the third batch of materials is about to be extruded, the absolute value (gram) of the water content in the second batch of materials may not actually change. Or there is a situation where the absolute value (gram) of the water content increases less. In the above case, the moisture content (mass ppm) of the third batch of materials is less than the moisture content (mass ppm) of the second batch of materials. By further reducing the moisture content (mass ppm) of the third batch of materials as the resin mixture just before extrusion, it can be expected that it is easy to further reduce the influence of moisture on the surface roughness. It is thus easy to manufacture a coated wire with a smaller surface roughness Ra.
[0209] As shown in Table 2 and Table 3, in the resin mixtures of compositions No. 1 to No. 4, if the water content of the second batch material is 400 mass ppm or less, the surface roughness Ra is 4.0 μm or less.
[0210] As shown in Table 4, in the resin mixture of composition No. 3, if the moisture content of the second batch of materials is less than 750 mass ppm, the surface roughness Ra is less than 4.0 μm. If the moisture content is less than 700 mass ppm, the surface roughness Ra more reliably satisfies less than 4.0 μm. Compared with the resin mixtures of compositions No. 1 to No. 4, in the resin mixture of composition No. 3, even if the moisture content of the second batch of materials is high, an insulating sheath with a small surface roughness Ra can be manufactured. From this aspect, the drying time of the second batch of materials in composition No. 3 can be shorter than the drying time in compositions No. 1 to No. 4. Alternatively, in composition No. 3, drying can sometimes be omitted. Based on this result, it can be said that the drying time in the case where the resin mixture contains block polyolefins is easy to be shorter than the drying time in the case where it contains polyolefin elastomers.
[0211] It should be noted that, according to Table 4, it can be inferred that the water content of the second batch material used in the production of the above-mentioned reference product is about 600 mass ppm.
[0212] For each sample of the coated wire, a cross section cut by a plane orthogonal to the axial direction of the coated wire was obtained, and the cross section was observed. In the comparison wire group, bubbles were confirmed in the insulating coating. In addition, there were more bubbles in the area close to the outer surface of the insulating coating than in the inner part of the insulating coating close to the conductor. Thus, in the comparison wire group, there was a significant difference in the distribution state of bubbles between the inner and outer surface areas of the insulating coating. In contrast, in the specific wire group, substantially no bubbles were confirmed, or substantially no difference in the distribution state of bubbles was confirmed. As described above, it can be seen that in the specific wire group, by reducing the water content, the bubbles on the outer surface side of the insulating coating are reduced or substantially absent, so it is also easy to make the insulating coating have a smooth surface.
[0213] As shown above, the coated electric wire whose insulating coating is composed of a specific resin composition and whose surface roughness Ra is 4.0 μm or less has excellent heat resistance and appearance. It is also shown that the above-mentioned coated electric wire has excellent water-stopping property. It is further shown that such a coated electric wire can be manufactured by applying a resin mixture of a specific composition to the raw material and reducing the water content of the resin mixture.
[0214] The present invention is not limited to these examples but is indicated by the claims, and is intended to include all modifications within the meaning and scope equivalent to the claims.
[0215] For example, in Test Example 1, the types and contents of the components of the resin mixture used as the raw material of the insulating coating may be appropriately changed. For example, the resin mixture of Test Example 1 may not contain a pigment.
[0216] Explanation of symbols
[0217] 1 Coated wire
[0218] 2 conductors, 20 strands, 22 wires
[0219] 3 Insulation coating
[0220] 5. Wiring Harness
[0221] 6 terminals, 60 wire barrel, 62 connection, 63 holes
[0222] 7 Waterstop components
Claims
1. A covered electric wire comprising a conductor and an insulating covering, wherein: The insulating coating is composed of a resin composition, The resin composition comprises: Silane grafted polyolefin; Unmodified polyolefins; A modified polyolefin having one or more functional groups selected from the group consisting of a carboxyl group, an ester group, an acid anhydride group, an amino group, and an epoxy group; Flame retardants; Cross-linking catalyst; as well as Zinc oxide and imidazole compounds, The unmodified polyolefin comprises: one or more polymers selected from the group consisting of polyethylene, polypropylene, and copolymers of ethylene or propylene and α-olefin; and block polypropylene, When the total amount of the silane-grafted polyolefin, the unmodified polyolefin and the modified polyolefin is 125 parts by mass, the content of the one or more polymers is 25 parts by mass to 45 parts by mass, and the content of the block polypropylene is 3 parts by mass to 10 parts by mass, The surface roughness Ra of the insulating coating is less than or equal to 2.0 μm.
2. The covered electric wire according to claim 1, wherein The surface roughness Ra is greater than or equal to 0.6 μm.
3. The covered electric wire according to claim 1 or 2, wherein: The conductor comprises a stranded wire, The two or more metal wires constituting the stranded wire are each an aluminum alloy wire.
4. A wiring harness, wherein: The wire harness comprises the covered electric wire according to any one of claims 1 to 3, a terminal, and a waterproof member. The terminal is mounted on at least one of the two ends of the covered electric wire. The waterproof member is mounted on the outer periphery of the insulating coating.