Liquid crystal polymer powder and method for producing the same
Through the processes of fine pulverization and wet high-pressure crushing in the liquid nitrogen state, the problem of fine fibrillation of liquid crystal polymer was solved, and a liquid crystal polymer powder with an average fiber diameter of less than 1 μm and a low lump content was achieved, which is suitable for electronics. Material.
Patent Information
- Application Number
- CN202080066956.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-25
- Filing Date
- 2020-09-23
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-09-23
AI Technical Summary
With the existing technology, it is difficult to microfiberize liquid crystal polymers through electric field spinning or melt-blown methods, and the use of fibrous raw materials can easily lead to nozzle clogging, making it impossible to achieve microfibrillation with fiber diameters less than 3 μm.
The liquid crystal polymer is pulverized in a liquid nitrogen state using a fine pulverization step, and then fiberized using a wet high-pressure crushing device to obtain a fine fibrous liquid crystal polymer powder with an average fiber portion diameter of 1 μm or less and a low lump portion content.
It achieves fine fiberization without using fibrous raw materials, reduces the risk of nozzle clogging, improves the tensile elastic modulus and heat resistance of liquid crystal polymer powder, and is suitable as a filler for electronic materials.
Smart Images

Figure CN114450328B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to liquid crystal polymer powder and a method for producing the same. Background Art
[0002] As prior art documents disclosed about liquid crystal polymers, there are Japanese Patent Application Publication No. 2003-193387 (Patent Document 1), Japanese National Publication No. 2005-501760 (Patent Document 2), Japanese Patent Application Publication No. 2008-50715 (Patent Document 3), and Japanese Patent No. 5904307 (Patent Document 4).
[0003] Patent Document 1 describes a method for producing a microfibrillated product of a rigid straight-chain aromatic synthetic polymer, characterized in that a granular rigid straight-chain aromatic synthetic polymer is subjected to mechanical treatment in a water suspension state to perform pre-pulping until the weight-average fiber length of the rigid straight-chain aromatic synthetic polymer is 1.6 mm or less, and then subjected to a homogenizer treatment. It is described that as rigid straight-chain aromatic synthetic polymers, aromatic polyamides represented by poly(p-phenylene terephthalamide) and aromatic polyesters of liquid crystal polymers represented by poly(p-hydroxybenzoic acid) can be cited.
[0004] Patent document 2 describes a pulverization method for forming small particles of anisotropic thermotropic liquid crystal polymer from larger particles. It is described that the pulverization method includes the following: (a) a first pulverization stage of pulverizing the anisotropic thermotropic liquid crystal polymer using a first pulverizing device; (b) taking out the anisotropic thermotropic liquid crystal polymer from the first pulverizing device; (c) a second pulverization stage of pulverizing the anisotropic thermotropic liquid crystal polymer from (b) using a second pulverizing device; and (d) taking out the anisotropic thermotropic liquid crystal polymer from the second pulverizing device. It is described that if LCP (Liquid Crystal Polymer) is anisotropic, when enough small particles are generated, they are fibrous. It is described that at least about 90 weight percent of the product of (d) passes through a 60-mesh screen. It should be noted that the mesh of the 60-mesh screen is about 0.27 mm.
[0005] Patent document 3 describes a method for producing microfibers, wherein the fiber contains a solvent in a ratio of 0.1 to 20% by weight relative to the entire fiber, (1) the average fiber length (L) is 0.01 to 1 mm, (2) the average fiber diameter (D) is 0.001 to 1 μm, and (3) the ratio (L / D) of the average fiber length (L) to the average fiber diameter (D) is 1000 to 10000. The method for producing microfibers comprises dispersing the fiber in a solvent, microfibrillating the fiber by mechanical shearing force, and then drying the fiber. The method describes that the fiber is selected from aromatic polyamide fibers and polyarylate fibers.
[0006] Patent document 4 describes a method for producing a fibrillated liquid crystal polymer powder containing fibrillated liquid crystal polymer particles. The production method includes a crushing step and a fibrillating step in sequence. In the crushing step, a biaxially oriented liquid crystal polymer film is crushed to obtain a liquid crystal polymer powder. In the fibrillating step, the liquid crystal polymer powder is crushed by using a wet high-pressure crushing device to obtain a fibrillated liquid crystal polymer powder. In the crushing step, crushing using a freeze-crystallization method is implemented. It is described that crushing using a freeze-crystallization method refers to crushing in a state where a film of LCP, etc. is frozen. It is described that in order to crush the liquid crystal polymer in a frozen state, it can be considered, for example, to inject liquid nitrogen into the crushed material obtained by coarsely crushing a strip-shaped film composed of a liquid crystal polymer while sequentially feeding it into a crushing device.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2003-193387
[0010] Patent Document 2: Japanese Patent Application No. 2005-501760
[0011] Patent Document 3: Japanese Patent Application Publication No. 2008-50715
[0012] Patent document 4: Japanese Patent No. 5904307. Summary of the invention
[0013] In recent years, research and development of microfibers have been actively carried out. Microfibers are, for example, fibers with a fiber diameter of 3 μm to 5 μm. As materials constituting microfibers, cellulose can be mainly cited. Cellulose, for example, forms the cell wall of plants in the form of aggregates. Microfibers composed of cellulose can be relatively easily obtained by physically or chemically destroying the aggregates of cellulose for defibration.
[0014] However, cellulose is a polysaccharide and contains a large number of hydroxyl groups, so it has extremely high hygroscopicity. Therefore, it becomes a problem when using fine fibers composed of cellulose as electronic materials such as materials constituting a part of a circuit board. Specifically, there arises a problem that the electrical properties change due to moisture absorption of the fine fibers, and a problem that the dimensions of components composed of the fine fibers change due to moisture absorption or drying of the fine fibers.
[0015] Therefore, the inventors of the present application have studied liquid crystal polymers as materials for forming fine fibers that can be used as electronic materials. This is because liquid crystal polymers have low hygroscopicity. In addition, the inventors of the present application have studied the use of liquid crystal polymers that are not fibrous materials as raw materials for fine fiberization from the perspective of manufacturing costs.
[0016] In the electrospinning method, which is one of the methods for producing fine fibers, it is necessary to dissolve the raw material to be finely fiberized in a solvent. However, it is difficult to finely fiberize a liquid crystal polymer by the electrospinning method, and the practicability is low from the viewpoint of mass production.
[0017] In the melt-blowing method, which is one of the methods for producing fine fibers, the material for fine fiberization is melted and the molten material is ejected from a nozzle. The material is stretched by blowing hot air on the molten material ejected from the nozzle. However, liquid crystal polymers have low melt tension. Therefore, if a liquid crystal polymer is to be finely fiberized by the melt-blowing method, the liquid crystal polymer is cut before being fully stretched. Therefore, in the melt-blowing method, the average diameter of the fiber portion cannot be reduced to about 3 μm or less.
[0018] In addition, for example, in Patent Document 1, a granular liquid crystal polymer is used as a raw material. The granular liquid crystal polymer is uniaxially oriented and has very strong anisotropy. If the granular liquid crystal polymer with strong anisotropy is mechanically treated in a water suspension state and pre-pulped, crushing based on a pattern divided along the orientation axis of the molecule is preferentially produced. As a result, a fibrous raw material powder with a large aspect ratio is obtained. Even if a homogenizer (wet high-pressure crushing device) is used to crush the fibrous raw material powder with a large aspect ratio into a fibrous liquid crystal polymer with an average diameter of 1 μm, the nozzle will frequently be clogged and crushing will not be possible. In addition, Patent Document 1 does not record the fiber diameter of the fibril of the obtained liquid crystal polymer.
[0019] For example, Patent Document 2 does not describe that the obtained LCP is fine fibers having an average diameter of 1 μm or less.
[0020] For example, in order to obtain fine fibers, it is necessary to use a fibrous raw material. It should be noted that Patent Document 3 does not clearly describe the content of bulk liquid crystal polymer in the entire fiber.
[0021] For example, in Patent Document 4, since the obtained liquid crystal polymer powder has a fibrillated surface, most of the particles constituting the liquid crystal polymer powder are in a bulk form.
[0022] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to obtain a fine fibrous liquid crystal polymer powder having a low content of bulk portions without using a fibrous raw material.
[0023] The liquid crystal polymer powder according to the present invention includes a fiber portion. The fiber portion is composed of fibrous particles whose ratio of the length in the long side direction to the fiber diameter, i.e., the aspect ratio, is 10 times or more. In the liquid crystal polymer powder, the average diameter of the fiber portion is 1 μm or less. In the liquid crystal polymer powder, the content of the block portion that is substantially not fiberized is 20% or less.
[0024] The method for producing a liquid crystal polymer powder according to the present invention comprises a fine grinding step and a fiberizing step. In the fine grinding step, the liquid crystal polymer is dispersed in liquid nitrogen and then crushed to obtain a granular finely ground liquid crystal polymer. In the fiberizing step, the granular finely ground liquid crystal polymer is crushed by a wet high-pressure crushing device to obtain a liquid crystal polymer powder.
[0025] According to the present invention, a fine fibrous liquid crystal polymer powder having a low content of bulk parts can be obtained without using a fibrous raw material. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a photograph of the finely pulverized liquid crystal polymer after being pulverized in the finely pulverizing step of Example 1.
[0027] Figure 2 This is a photograph of the liquid crystal polymer powder after it was repeatedly crushed five times through the fiberization step of Example 1.
[0028] Figure 3 This is a photograph of the finely pulverized liquid crystal polymer after being pulverized in the finely pulverizing step of Example 2.
[0029] Figure 4 This is a photograph of the internal cross section of the finely pulverized liquid crystal polymer pulverized in the finely pulverizing step of Example 2.
[0030] Figure 5 This is a photograph of the liquid crystal polymer powder after it was repeatedly crushed five times through the fiberization step of Example 2.
[0031] Figure 6 This is a photograph of the finely pulverized liquid crystal polymer after finely pulverized in the finely pulverizing step of Example 3.
[0032] Figure 7 This is a photograph of the liquid crystal polymer powder after it was repeatedly crushed five times through the fiberization step of Example 3.
[0033] Figure 8 This is a photograph of the finely pulverized liquid crystal polymer after being pulverized in the finely pulverizing step of Comparative Example 1.
[0034] Fig. 9This is a photograph of the internal cross section of the finely pulverized liquid crystal polymer pulverized in the finely pulverizing step of Comparative Example 1.
[0035] Fig.10 This is a photograph of the finely pulverized liquid crystal polymer after being pulverized in the finely pulverizing step of Comparative Example 2.
[0036] Fig.11 This is a photograph of the liquid crystal polymer powder after it was repeatedly crushed 7 times through the fiberization step of Comparative Example 2.
[0037] Fig.12 This is an image showing an example of particles of a liquid crystal polymer powder photographed in order to measure the average diameter of the fiber portion in this example.
[0038] Fig.13 This is an example of a 3D analysis image of the aggregation part of the liquid crystal polymer powder of Example 1.
[0039] Fig.14 This is an example of a 3D analysis image of the aggregation part of the liquid crystal polymer powder of Comparative Example 2.
[0040] Fig.15 This is a graph showing changes in D50 of the liquid crystal polymer powder in the fiberizing step of Examples 1 to 3 and Comparative Example 2 with respect to the number of crushings. DETAILED DESCRIPTION
[0041] <Liquid crystal polymer powder>
[0042] Hereinafter, an embodiment of the present invention will be described. First, a liquid crystal polymer powder according to an embodiment of the present invention will be described. The liquid crystal polymer powder according to an embodiment of the present invention includes a fiber portion and a block portion. The fiber portion may be included in the liquid crystal polymer powder as a coagulation portion formed by agglomeration of fibrous particles, and the block portion may be included in the liquid crystal polymer as a coagulation portion formed by agglomeration of blocky particles. It should be noted that the liquid crystal polymer powder according to this embodiment may not include a block portion.
[0043] The fiber portion is composed of fibrous particles. In the present embodiment, the fibrous particles are liquid crystal polymer particles having a ratio of the length in the long side direction to the fiber diameter, i.e., an aspect ratio of 10 times or more. The length in the long side direction and the fiber diameter of the fibrous particles can be measured based on image data of the fibrous particles obtained when observing the fibrous particles using a scanning electron microscope.
[0044] In the liquid crystal polymer powder of this embodiment, the average diameter of the fiber portion is 1 μm or less. The value of the average diameter of the fiber portion is the average value of the fiber diameters of the plurality of fibrous particles constituting the fiber portion. Thus, the liquid crystal polymer powder of this embodiment includes fine fibrous particles.
[0045] The block portion is a liquid crystal polymer powder that is not substantially fiberized. The block portion may have a flat shape. In the liquid crystal polymer powder of the present embodiment, the content of the block portion is 20% or less. That is, in the liquid crystal polymer powder of the present embodiment, the content of the block portion becomes relatively low. The content of the block portion is evaluated by the number of block portions contained in the liquid crystal polymer powder relative to the number of condensed portions. In the present embodiment, when the liquid crystal polymer powder is placed on a plane, the condensed portion whose maximum height is greater than 10 μm is the block portion, and the condensed portion whose maximum height is less than 10 μm is the fiber portion.
[0046] As described above, in this embodiment, the average diameter of the fiber portion of the liquid crystal polymer powder is 1 μm or less, the content of the block portion is 20% or less, and the fine fibrous liquid crystal polymer powder is obtained without using a fibrous raw material and the content of the block portion is low. In addition, the liquid crystal polymer powder having an average diameter of the fiber portion of 1 μm or less and a content of the block portion of 20% or less has a high tensile elastic modulus and a large surface area. Therefore, the liquid crystal polymer powder of this embodiment is easy to obtain close adhesion with other components and is suitable as a filler added to the coating for reinforcement.
[0047] In addition, the liquid crystal polymer powder of the present embodiment is composed of a thermotropic liquid crystal polymer. The liquid crystal polymer powder of the present embodiment is heated to 400°C in an inert atmosphere, cooled to room temperature at a temperature drop rate of 40°C / min or more, and heated again at a temperature rise rate of 40°C / min. The endothermic peak temperature measured by a differential scanning calorimeter exceeds 330°C. Therefore, the liquid crystal polymer powder of the present embodiment has high heat resistance and can be used as an electronic material. It should be noted that in this specification, the endothermic peak temperature measured as above is sometimes referred to as the "melting point".
[0048] The liquid crystal polymer powder of the present embodiment preferably has a D50 value of 13 μm or less as measured by particle size measurement using a particle size distribution measuring apparatus based on a laser diffraction scattering method.
[0049] <Method for producing liquid crystal polymer powder>
[0050] The following describes a method for producing a liquid crystal polymer powder according to an embodiment of the present invention. The method for producing a liquid crystal polymer powder according to an embodiment of the present invention includes a coarse pulverization step, a fine pulverization step, a coarse particle removal step, and a fibrillation step in this order.
[0051] In the coarse pulverization process, first, as a raw material, a molded product of a liquid crystal polymer is prepared. As the molded product of the liquid crystal polymer, uniaxially oriented granular, biaxially oriented film-like or powdery liquid crystal polymers can be cited. As the molded product of the liquid crystal polymer, from the viewpoint of manufacturing cost, etc., preferably a granular or powdery liquid crystal polymer, more preferably a granular liquid crystal polymer. In this embodiment, the molded product of the liquid crystal polymer does not contain a fibrous liquid crystal polymer directly molded by an electrolytic spinning method or a melt-blowing method. Among them, the molded product of the liquid crystal polymer may include a fibrous liquid crystal polymer processed by crushing a granular liquid crystal polymer or a powdery liquid crystal polymer.
[0052] The melting point of the molded product of the liquid crystal polymer is preferably higher than 330° C., more preferably higher than 350° C. Thus, a liquid crystal polymer powder having high heat resistance and suitable as a material for electronic components can be obtained.
[0053] It should be noted that among the molded products of liquid crystal polymers, film-like liquid crystal polymers are usually molded by melt extrusion. However, for liquid crystal polymers having a melting point greater than 330°C, when attempting to mold a film-like liquid crystal polymer by melt extrusion, a large number of fish eyes of the liquid crystal polymer are generated, or degradation due to decomposition occurs. This is because for liquid crystal polymers having a melting point greater than 330°C, if you want to mold a film-like liquid crystal polymer by melt extrusion, you need to heat the liquid crystal polymer to near the decomposition temperature and continuously knead it. Therefore, as a molded product of a liquid crystal polymer, a film-like liquid crystal polymer with a melting point greater than 330°C cannot be used.
[0054] Next, the liquid crystal polymer is coarsely pulverized to obtain a coarsely pulverized liquid crystal polymer. For example, the liquid crystal polymer is coarsely pulverized by using a cutting and grinding device to obtain a coarsely pulverized liquid crystal polymer. The size of the coarsely pulverized liquid crystal polymer particles is not particularly limited as long as they can be used as a raw material for the fine pulverization step described later. The maximum particle size of the coarsely pulverized liquid crystal polymer is, for example, less than 3 mm.
[0055] The method for producing the liquid crystal polymer powder of the present embodiment does not necessarily need to include a coarse pulverization step. For example, if the liquid crystal polymer molded product can be used as a raw material for the fine pulverization step, the liquid crystal polymer molded product can be directly used as a raw material for the fine pulverization step.
[0056] In the fine pulverizing step, as a liquid crystal polymer, the coarsely pulverized liquid crystal polymer is dispersed in liquid nitrogen and pulverized to obtain a granular finely pulverized liquid crystal polymer. In the fine pulverizing step, the coarsely pulverized liquid crystal polymer dispersed in liquid nitrogen is pulverized using a medium. The medium is, for example, beads. In the fine pulverizing step of the present embodiment, from the perspective of handling liquid nitrogen, it is preferred to use a bead mill with fewer technical problems. As an apparatus that can be used in the fine pulverizing step, for example, "LNM-08", a liquid nitrogen bead mill manufactured by IMEX, can be cited.
[0057] In the fine pulverizing step of the present embodiment, the pulverizing method of pulverizing the liquid crystal polymer in a state of being dispersed in liquid nitrogen is different from the conventional freezing pulverizing method. The conventional freezing pulverizing method is a method of pulverizing the pulverized raw material while injecting liquid nitrogen into the pulverizing raw material and the pulverizing device body, but the liquid nitrogen is gasified at the moment when the pulverized raw material is pulverized. That is, in the conventional freezing pulverizing method, the pulverized raw material is not dispersed in the liquid nitrogen at the moment when the pulverized raw material is pulverized.
[0058] In the conventional freezing and pulverizing method, the heat of the pulverized raw material itself, the heat generated from the pulverizing device, and the heat generated by the pulverization of the pulverized raw material cause the liquid nitrogen to vaporize in a very short time. Therefore, in the conventional freezing and pulverizing method, the raw material being pulverized inside the pulverizing device reaches a temperature of -196°C, which is much higher than the boiling point of liquid nitrogen. That is, in the conventional freezing and pulverizing method, the pulverization is usually carried out under the condition of the temperature inside the pulverizing device being around 0°C to 100°C. In the conventional freezing and pulverizing method, even when liquid nitrogen is supplied as much as possible, the temperature inside the pulverizing device is about -150°C at the lowest.
[0059] Therefore, in the conventional freeze-crushing method, for example, when a uniaxially oriented granular liquid crystal polymer or a coarsely pulverized product of a granular liquid crystal polymer is pulverized along a plane substantially parallel to the axial direction of the molecular axis of the liquid crystal polymer, a fibrous liquid crystal polymer having a large aspect ratio and a fiber diameter much larger than 1 μm can be obtained. That is, in the conventional freeze-crushing direction, even if a uniaxially oriented granular liquid crystal polymer or a coarsely pulverized product of a granular liquid crystal polymer is pulverized, a granular finely pulverized liquid crystal polymer cannot be obtained.
[0060] In the present embodiment, the pulverization is performed in a state where the pulverized raw material is dispersed in liquid nitrogen, so that compared with the conventional freezing pulverization method, the raw material in a further cooled state can be pulverized. Specifically, the pulverized raw material at a temperature lower than -196°C, which is the boiling point of liquid nitrogen, can be pulverized. If the pulverized raw material at a temperature lower than -196°C is pulverized, the raw material is pulverized by repeatedly performing brittle destruction of the pulverized raw material. Thus, for example, even in the case of pulverizing a uniaxially oriented liquid crystal polymer, not only the destruction of the surface roughly parallel to the axial direction of the molecular axis of the liquid crystal polymer is performed, but also brittle destruction is performed along the surface intersecting the above-mentioned axial direction, so that a granular finely pulverized liquid crystal polymer can be obtained.
[0061] In the fine pulverization step of the present embodiment, the liquid crystal polymer that has become granular by brittle fracture is continuously impacted by a medium, etc., while maintaining the brittle state in liquid nitrogen. As a result, a plurality of fine cracks are formed from the outer surface to the inside of the liquid crystal polymer obtained in the fine pulverization step of the present embodiment.
[0062] The finely pulverized liquid crystal polymer particles obtained in the fine pulverization step preferably have a D50 of 50 μm or less as measured by a particle size distribution measuring device using a laser diffraction scattering method. This can prevent the finely pulverized liquid crystal polymer particles from clogging the nozzle in the fiberizing step described below.
[0063] In this embodiment, in the coarse particle removal step, coarse particles are removed from the granular finely pulverized liquid crystal polymer obtained in the above-mentioned finely pulverized step. For example, the granular finely pulverized liquid crystal polymer is sieved on a sieve to obtain a granular finely pulverized liquid crystal polymer under the sieve, and the coarse particles contained in the granular finely pulverized liquid crystal polymer can be removed by removing the granular liquid crystal polymer on the sieve. The type of the sieve can be appropriately selected, and as the sieve, for example, a sieve with a mesh size of 53 μm can be cited. It should be noted that the method for producing the liquid crystal polymer powder of this embodiment may not necessarily include a coarse particle removal step.
[0064] In the fiberizing step, the granular liquid crystal polymer is crushed by a wet high-pressure crushing device to obtain a liquid crystal polymer powder. In the fiberizing step, the finely pulverized liquid crystal polymer is first dispersed in a dispersion medium. The dispersed finely pulverized liquid crystal polymer may not be subjected to coarse particles, but preferably, coarse particles are removed. Examples of the dispersion medium include water, ethanol, methanol, isopropanol, toluene, benzene, xylene, phenol, acetone, methyl ethyl ketone, diethyl ether, dimethyl ether, hexane, or mixtures thereof.
[0065] Next, the finely pulverized liquid crystal polymer in the state of being dispersed in the dispersion medium, that is, the finely pulverized liquid crystal polymer in the form of a slurry, is passed through a nozzle under a state of being pressurized at high pressure. By passing the nozzle at high pressure, the shear force or collision energy brought by the high-speed flow in the nozzle acts on the liquid crystal polymer, and the granular finely pulverized liquid crystal polymer is crushed, thereby performing fiberization of the liquid crystal polymer, and the liquid crystal polymer powder of the present embodiment can be obtained. From the viewpoint of applying high shear force or high collision energy, it is preferred to reduce the nozzle diameter of the above-mentioned nozzle as much as possible within a range that does not cause clogging of the finely pulverized liquid crystal polymer in the above-mentioned nozzle. The particle size of the granular finely pulverized liquid crystal polymer in the present embodiment is relatively small, so the nozzle diameter of the wet high-pressure crushing device used in the fiberization process can be reduced. The nozzle diameter is, for example, less than 0.2 mm.
[0066] In the present embodiment, as described above, a plurality of fine cracks are formed in the granular finely pulverized liquid crystal polymer powder. Therefore, by pressurizing the wet high-pressure disperser, the dispersion medium invades the inside of the finely pulverized liquid crystal polymer from the fine cracks. Then, when the slurry-like finely pulverized liquid crystal polymer passes through the nozzle and is located at normal pressure, the dispersion medium invading the inside of the finely pulverized liquid crystal polymer expands in a short time. The dispersion medium invading the inside of the finely pulverized liquid crystal polymer expands, thereby destroying the inside of the finely pulverized liquid crystal polymer. Therefore, the fiberization proceeds to the inside of the finely pulverized liquid crystal polymer, and the molecules of the liquid crystal polymer are separated into domain units arranged in a unidirectional manner. In this way, in the fiberization process of the present embodiment, by defibrillating the granular finely pulverized liquid crystal polymer obtained in the finely pulverized process of the present embodiment, it is possible to obtain a liquid crystal polymer powder of the present embodiment that has a low content of block portions and is in the form of fine fibers compared to the liquid crystal polymer powder obtained by pulverizing the granular liquid crystal polymer obtained in the previous freeze-pulverization method.
[0067] In the fiberizing step of the present embodiment, the liquid crystal polymer powder can be obtained by repeatedly crushing the finely pulverized liquid crystal polymer using a wet high-pressure crushing device. The number of crushings performed by the wet high-pressure crushing device is preferably small. The number of crushings performed by the wet high-pressure crushing device can be, for example, less than 5 times.
[0068] As described above, the method for producing a liquid crystal polymer powder according to one embodiment of the present invention comprises a fine grinding step and a fiberizing step. In the fine grinding step, the liquid crystal polymer is dispersed in liquid nitrogen and then crushed to obtain a granular finely ground liquid crystal polymer. In the fiberizing step, the finely ground liquid crystal polymer is crushed by a wet high-pressure crushing device to obtain a liquid crystal polymer powder. Thus, when a liquid crystal polymer other than a fibrous liquid crystal polymer is used as a raw material, a fine fibrous liquid crystal polymer powder with a low content of a block portion can be obtained.
[0069] In the method for producing a liquid crystal polymer powder according to one embodiment of the present invention, the liquid crystal polymer dispersed in liquid nitrogen is pulverized using a medium in the fine pulverization step. Thus, the raw material dispersed in liquid nitrogen can be pulverized with a simple configuration.
[0070] Example
[0071] Hereinafter, the present invention will be described in more detail with reference to the accompanying drawings and by giving examples, but the present invention is not limited to these.
[0072] (Example 1)
[0073] In Example 1, first, a film-shaped liquid crystal polymer having a thickness of 250 μm and having biaxially oriented molecules in the plane direction is put into a cutting and grinding device for coarse grinding. The melting point of the liquid crystal polymer used in Example 1 is 315° C. The coarsely ground liquid crystal polymer is discharged from a discharge hole having a diameter of 3 mm provided in the cutting and grinding device, thereby obtaining a coarsely ground liquid crystal polymer.
[0074] Next, the coarsely pulverized liquid crystal polymer was finely pulverized using a liquid nitrogen bead mill (IMEX, LNM-08). In the pulverization using the liquid nitrogen bead mill, the container capacity was set to 0.8 L, Zirconia beads with a diameter of 5 mm were used as the medium, the input amount of the medium was set to 500 mL, 30 g of the coarsely pulverized liquid crystal polymer was added, and the pulverization process was performed at a rotation speed of 2000 rpm for 120 minutes. In the liquid nitrogen bead mill, the coarsely pulverized liquid crystal polymer was dispersed in liquid nitrogen and subjected to wet pulverization.
[0075] Figure 1 This is a photograph of the finely pulverized liquid crystal polymer after being pulverized by the finely pulverizing step of Example 1. Figure 1 As shown, the coarsely pulverized liquid crystal polymer is pulverized by a liquid nitrogen bead mill to obtain a granular finely pulverized liquid crystal polymer. Figure 1 and the following Figure 2 to Figure 12 The photo in the figure was taken using a scanning electron microscope.
[0076] Next, the finely pulverized liquid crystal polymer was sieved with a sieve having a mesh size of 53 μm to remove coarse particles contained in the finely pulverized liquid crystal polymer, and the finely pulverized liquid crystal polymer that passed through the sieve was recovered. The yield of the finely pulverized liquid crystal polymer based on the removal of the coarse particles was 85% by mass.
[0077] Next, the finely pulverized liquid crystal polymer from which the coarse particles were removed was dispersed in a 20 wt% ethanol aqueous solution. The ethanol slurry in which the finely pulverized liquid crystal polymer was dispersed was repeatedly pulverized several times using a wet high-pressure crushing device under the conditions of a nozzle diameter of 0.2 mm and a pressure of 200 MPa to perform fiberization. As the wet high-pressure crushing device, Nanovater (registered trademark) C-ES008 manufactured by Yoshida Machinery Industry Co., Ltd. was used.
[0078] Figure 2 This is a photograph of the liquid crystal polymer powder after repeated crushing 5 times through the fiberization process of Example 1. Figure 2 As shown, fine fibrous liquid crystal polymer powder is obtained by crushing the finely pulverized liquid crystal polymer.
[0079] (Example 2)
[0080] In Example 2, a uniaxially oriented granular liquid crystal polymer was put into the cutting and grinding device instead of the film-like liquid crystal polymer put into the cutting and grinding device in Example 1, thereby obtaining a roughly pulverized liquid crystal polymer. It should be noted that a liquid crystal polymer with a melting point of 315° C. was used in Example 2. Then, fine pulverization using a liquid nitrogen bead mill was performed in the same manner as in Example 1.
[0081] Figure 3 This is a photograph of the finely pulverized liquid crystal polymer after being pulverized by the finely pulverizing step of Example 2. Figure 3 As shown, in Example 2, the coarsely pulverized liquid crystal polymer was also pulverized by a liquid nitrogen bead mill to obtain a finely pulverized liquid crystal polymer.
[0082] Figure 4 This is a photograph of the internal cross section of the finely pulverized liquid crystal polymer after being pulverized by the finely pulverizing step of Example 2. Figure 4 As shown, it can be confirmed that a large number of cracks are formed inside the finely pulverized liquid crystal polymer of Example 2.
[0083] Then, the coarse particles contained in the finely pulverized liquid crystal polymer were removed in the same manner as in Example 1, and the finely pulverized liquid crystal polymer from which the coarse particles were removed was crushed several times by a wet high-pressure crushing device to be fiberized.
[0084] Figure 5 This is a photograph of the liquid crystal polymer powder after repeated crushing 5 times through the fiberization process of Example 2. Figure 5 As shown, in Example 2, by crushing the finely pulverized liquid crystal polymer, a fine fibrous liquid crystal polymer powder was obtained without clogging the nozzle of the wet high-pressure crushing device with the liquid crystal polymer.
[0085] (Example 3)
[0086] In Example 3, a uniaxially oriented granular liquid crystal polymer was put into the cutting and grinding device instead of the film-like liquid crystal polymer put into the cutting and grinding device in Example 1, thereby obtaining a roughly pulverized liquid crystal polymer. In Example 3, unlike Examples 1 and 2, a liquid crystal polymer with a melting point of 350° C. was used. Then, fine pulverization was performed using a liquid nitrogen bead mill in the same manner as in Examples 1 and 2.
[0087] Figure 6 This is a photograph of the finely pulverized liquid crystal polymer after finely pulverizing in the finely pulverizing step of Example 3. Figure 6 As shown, in Example 3, the coarsely pulverized liquid crystal polymer was also pulverized by a liquid nitrogen bead mill to obtain a granular finely pulverized liquid crystal polymer.
[0088] Then, coarse particles contained in the finely pulverized liquid crystal polymer were removed in the same manner as in Examples 1 and 2, and the finely pulverized liquid crystal polymer from which the coarse particles were removed was crushed by a wet high-pressure crushing device to be fiberized.
[0089] Figure 7 This is a photograph of the liquid crystal polymer powder after it was repeatedly crushed 5 times in the fiberization process in Example 3. Figure 7 As shown, in Example 3, a fine fibrous liquid crystal polymer powder was obtained by crushing the finely pulverized liquid crystal polymer without clogging the nozzle of the wet high-pressure crushing device with the liquid crystal polymer. Furthermore, in Example 3, a granular liquid crystal polymer powder was used as a raw material instead of a film-like liquid crystal polymer, so that a polymer with a relatively high melting point could be used as the liquid crystal polymer, and a fine fibrous liquid crystal polymer powder with a high melting point could be obtained.
[0090] (Comparative Example 1)
[0091] In Comparative Example 1, first, a uniaxially oriented particulate liquid crystal polymer was coarsely pulverized using a cutting mill in the same manner as in Example 2 to obtain a coarsely pulverized liquid crystal polymer.
[0092] Next, the roughly pulverized liquid crystal polymer is finely pulverized using a dry freeze pulverizing device (manufactured by HOSOK AWA MICRON, Linrex Mill (registered trademark)). In the dry freeze pulverizing device, liquid nitrogen is supplied to the inside of the device together with the roughly pulverized liquid crystal polymer. However, the liquid nitrogen supplied to the inside of the device is instantly vaporized, so that nitrogen exists in the form of gas inside the device.
[0093] Figure 8 This is a photograph of the finely pulverized liquid crystal polymer after being pulverized by the finely pulverizing step of Comparative Example 1. Figure 8As shown, the finely pulverized liquid crystal polymer obtained by pulverizing the coarsely pulverized liquid crystal polymer using a dry freeze pulverization device is a fibrous liquid crystal polymer having a fiber diameter of several tens to several hundreds of μm.
[0094] In this comparative example, the reason why the finely pulverized liquid crystal polymer becomes a fibrous liquid crystal polymer is considered as follows. When manufacturing the granular liquid crystal polymer used in this comparative example, first, the liquid crystal polymer in a molten state is extruded from a die to form a strand. The strand is strongly uniaxially oriented in a direction parallel to the extrusion direction by the strong shear force accompanying the extrusion from the die. Then, the granular liquid crystal polymer is obtained by cutting the strand into a specified length. As a result, the molecules of the granular liquid crystal polymer and the coarsely pulverized liquid crystal polymer obtained by coarsely pulverizing it are also uniaxially oriented, and therefore have strong anisotropy. Therefore, in the conventional dry freezing pulverizing device, it is believed that the above-mentioned coarsely pulverized liquid crystal polymer is pulverized along this uniaxial orientation to obtain a fibrous liquid crystal polymer.
[0095] Next, the fibrous finely pulverized liquid crystal polymer of several tens μm to several hundreds μm was sieved with a 53 μm sieve to remove the coarse particles, and the finely pulverized liquid crystal polymer that passed through the sieve was recovered. The yield of the finely pulverized liquid crystal polymer based on the removal of the coarse particles was 3% by mass. In addition, the finely pulverized liquid crystal polymer after the coarse particles were removed was also fibrous.
[0096] Fig. 9 This is a photograph of the internal cross section of the finely pulverized liquid crystal polymer after being pulverized by the finely pulverizing step of Comparative Example 1. Fig. 9 As shown, it can be confirmed that the number of cracks inside the finely pulverized liquid crystal polymer of Comparative Example 1 is extremely smaller than the number of cracks inside the finely pulverized liquid crystal polymer of Example 2.
[0097] Next, the fibrous finely pulverized liquid crystal polymer from which the coarse particles were removed was subjected to further fiberization by crushing with a wet high-pressure crushing device under the same conditions as in Example 2, i.e., the same conditions as in Example 1. However, the nozzle of the wet high-pressure crushing device was clogged with the fibrous finely pulverized liquid crystal polymer, so that no liquid crystal polymer powder could be obtained in Comparative Example 1.
[0098] (Comparative Example 2)
[0099] In Comparative Example 2, a biaxially oriented film-like liquid crystal polymer was first roughly pulverized by a cutting mill in the same manner as in Example 1 to obtain a roughly pulverized liquid crystal polymer. Then, the roughly pulverized liquid crystal polymer was finely pulverized using the dry freeze pulverizing device used in Comparative Example 1.
[0100] Fig.10This is a photograph of the finely pulverized liquid crystal polymer after being pulverized by the finely pulverizing step of Comparative Example 2. Fig.10 As shown, in Comparative Example 2, a finely pulverized liquid crystal polymer was obtained by finely pulverizing a coarsely pulverized liquid crystal polymer using a dry freeze pulverizing device.
[0101] Next, coarse particles contained in the finely pulverized liquid crystal polymer were removed in the same manner as in Examples 1 to 3, and then the finely pulverized liquid crystal polymer from which the coarse particles were removed was crushed by a wet high-pressure crusher under the same conditions as in Examples 1 to 3 to attempt to fiberize the polymer.
[0102] Fig.11 This is a photograph of the liquid crystal polymer powder after it was repeatedly crushed by the fiberization process of Comparative Example 2. Fig.11 As shown, in Comparative Example 2, the liquid crystal polymer powder was obtained by crushing the finely pulverized liquid crystal polymer. It should be noted that in Comparative Example 2, although the surface of the finely pulverized liquid crystal polymer could be fibrillated only once or twice, the entire finely pulverized liquid crystal polymer could not be finely fibrillated.
[0103] [Measurement of average diameter of fiber portion]
[0104] In Examples 1 to 3 and Comparative Example 2, the average diameter of the fiber portion contained in the liquid crystal polymer powder obtained by fibrillation using a wet high-pressure crushing device was measured.
[0105] In the determination of the above average diameter, first, the liquid crystal polymer powder to be measured is dispersed in ethanol to prepare a slurry containing 0.01wt% of the liquid crystal polymer powder. At this time, the slurry is prepared in such a way that the water content in the slurry is less than 1wt%. Then, 5μL to 10μL of the slurry is dripped on a glass slide, and the slurry on the glass slide is naturally dried. By allowing the slurry to dry naturally, the liquid crystal polymer powder is arranged on the glass slide.
[0106] Next, a predetermined region of the liquid crystal polymer powder disposed on the slide glass is observed using a scanning electron microscope to collect image data of 100 or more particles constituting the liquid crystal polymer powder. Fig.12 FIG. 1 is an image showing an example of particles of a liquid crystal polymer powder photographed in order to measure the average diameter of the fiber portion in this embodiment. Fig.12 As shown, particles of the liquid crystal polymer powder are shown in white.
[0107] In the acquisition of image data, the above-mentioned area is set according to the size of each particle of the liquid crystal polymer so that the number of image data becomes more than 100. In addition, for each particle of the liquid crystal polymer, in order to suppress the leakage of the acquisition of image data and the generation of measurement errors, the magnification of the scanning electron microscope is appropriately changed to 500 times, 3000 times or 10000 times, and the above-mentioned image data is acquired.
[0108] Next, using the above-mentioned image data, the long-side dimensions and width-direction dimensions of each particle of the liquid crystal polymer powder are measured. The direction of the longest path that can be taken on a particle of the liquid crystal polymer powder captured along each of the above-mentioned image data, that is, the path from one end of the particle through the approximate center of the particle to the end on the opposite side of the one end, is defined as the long-side direction. Then, the length of the longest path is measured as the long-side dimension. Furthermore, the dimensions of the particles in the direction orthogonal to the long-side direction are measured at three locations of a particle of the liquid crystal polymer powder where the above-mentioned long-side directions are different from each other. The average value of the dimensions measured at the three locations is taken as the width-direction dimension of each particle of the liquid crystal polymer powder.
[0109] Then, a particle of the liquid crystal polymer powder whose long side dimension is 10 times or more than the width direction dimension is defined as a fibrous particle constituting the fiber portion. That is, the fiber diameter of the particle of the liquid crystal polymer powder constituting the fiber portion is the width direction dimension of the liquid crystal polymer powder. Then, the fiber diameters of 100 fibrous particles constituting the fiber portion are measured. The value obtained by averaging the measurement results of these fiber diameters is taken as the average diameter of the fiber portion.
[0110] At least in Examples 1 to 3, it was confirmed that the average diameter of the fiber portion was 1 μm or less.
[0111] [Evaluation of the content of lump parts]
[0112] In Examples 1 to 3, the content of blocky parts contained in the liquid crystal polymer powder was evaluated for the liquid crystal polymer powder obtained by 5 times of crushing using a wet high-pressure crushing device, and in Comparative Example 2, the liquid crystal polymer powder obtained by 15 times of crushing using a wet high-pressure crushing device was evaluated.
[0113] In the evaluation of the content of the block portion, first, the liquid crystal polymer powder to be evaluated is taken in the state of a slurry just after being crushed by a wet high-pressure crushing device. The slurry-like liquid crystal polymer powder is further diluted by adding mixed ethanol to the taken slurry-like liquid crystal polymer powder. The mixed ethanol is added until the content of the liquid crystal polymer powder in the slurry is diluted to less than 0.01wt%. After the diluted slurry is dropped onto a glass slide, it is placed at room temperature to vaporize the ethanol as the dispersion medium of the slurry. The liquid crystal polymer powder is arranged on the glass slide in this way.
[0114] Next, the liquid crystal polymer powder disposed on the slide glass was observed using a laser microscope (manufactured by KEYENCE, VK-8700) at a magnification of 100 times. Through this observation, it was confirmed that the liquid crystal polymer powder contained a plurality of agglomerates in Examples 1 to 3 and Comparative Example 2. It should be noted that the agglomerates can also be confirmed by, for example, a scanning electron microscope, such as Figure 5 and Fig.11 As shown, in Examples 1 to 3 and Comparative Example 2, the liquid crystal polymer powder includes an aggregation part.
[0115] Furthermore, the maximum heights of the plurality of condensed portions are measured for the liquid crystal polymer powder to be measured. The method for measuring the maximum height of the condensed portion is described below. First, a contour map of the height of the condensed portion arranged on the above-mentioned slide is prepared using a data analysis application attached to the above-mentioned laser microscope, with the surface of the slide as the reference height. The contour map is prepared by correcting the inclination of the slide so that the surface of the liquid crystal polymer powder side of the slide becomes horizontal. Furthermore, a 3D analysis image showing the contour map in 3D is output. Fig.13 This is an example of a 3D analysis image of the aggregation part of the liquid crystal polymer powder of Example 1. Fig.14 This is an example of a 3D analysis image of the agglomeration part of the liquid crystal polymer powder of Comparative Example 2. Fig.13 and Fig.14 As shown in FIG. 1 , the overall height of the aggregation part of Example 1 and the overall height of the aggregation part of Comparative Example 2 are greatly different.
[0116] 30 agglomerates were selected from the liquid crystal polymer powder to be measured by the above-mentioned microscope observation, and the maximum height of each of these agglomerates was measured. In Examples 1 to 3, it was confirmed that the average diameter of the fiber part was 1 μm, so the agglomerate with a maximum height of 10 μm was determined to be a block part of the liquid crystal polymer that was not fibrous. Then, in the liquid crystal polymer powder, the ratio of the number of block parts to the number of 30 agglomerates with the maximum height measured was evaluated as the content rate of the block parts contained in the liquid crystal polymer powder.
[0117] The details of the evaluation results of the content of the block portion of Example 1 and Comparative Example 2 are shown in the following Table 1. In the following Table 1, 30 selected aggregation portions are numbered for each of Example 1 and Comparative Example 2, and the results of measuring the maximum height of the aggregation portion with each number are shown.
[0118] [Table 1]
[0119] Assay number Example 1 Comparative Example 2 1 0.8 15.6 2 1.3 5.1 3 1.8 8.3 4 1.4 7.9 5 1.9 22.2 6 6.0 3.7 7 3.9 19.5 8 1.1 25.9 9 1.1 11.8 10 1.7 12.1 11 1.9 22.9 12 1.1 26.8 13 0.8 10.5 14 2.6 15.1 15 2.0 6.1 16 10.3 8.9 17 1.6 13.4 18 1.7 39.5 19 1.8 14.6 20 2.2 31.1 21 5.2 11.7 22 4.5 21.5 23 2.7 35.5 24 5.4 7.7 25 2.8 9.3 26 2.5 7.7 27 0.5 5.6 28 0.7 12.6 29 3.5 16.6 30 2.5 14.2 Average value of maximum height of coagulation part (μm) 2.6 15.4 Number of blocks 1 20 Content of block part (%) 3.3 66.7
[0120] In Examples 2 and 3, the content of the lump portion was evaluated in the same manner as in Example 1 and Comparative Example 2. The evaluation results of the content of the lump portion in Examples 1 to 3 and Comparative Example 2 are shown in Table 2 below.
[0121] [Table 2]
[0122] Example 1 Example 2 Example 3 Comparative Example 2 3.3% 3.3% 6.7% 66.7%
[0123] As shown in Tables 1 and 2, the content of the block portion of the liquid crystal polymer powder in Examples 1, 2, and 3 was 3.3%, 3.3%, and 6.7%, respectively, all of which were less than 20%. On the other hand, in Comparative Example 2, the content of the block portion of the liquid crystal polymer powder was 66.7%, which was greater than 20%. That is, in Comparative Example 2, a large amount of finely pulverized liquid crystal polymer that was not finely fibrous but remained in a granular state was contained.
[0124] [Particle size determination]
[0125] In Examples 1 to 3 and Comparative Example 2, the D50 value was investigated by measuring the particle size of the finely pulverized liquid crystal polymer just after the coarse particles were removed by the fine pulverization process and the fine fibrous liquid crystal polymer powder obtained by crushing a predetermined number of times by the fibrillation process. In Examples 1 to 3 and Comparative Example 2, the D50 value was investigated for the liquid crystal polymer just after the 1st to 5th, 10th and 15th crushing by the fibrillation process.
[0126] In the particle size determination, a particle size distribution measuring device based on the laser diffraction scattering method (manufactured by Horiba, LA-950) was used. As a dispersion medium, an Ekinen was used to disperse the liquid crystal polymer to be measured. After ultrasonic treatment for 10 seconds was applied to the liquid crystal polymer to be measured dispersed in the dispersion medium, the liquid crystal polymer was placed in a particle size distribution measuring device to perform particle size determination.
[0127] Fig.15 This is a graph showing the change in D50 of the liquid crystal polymer powder relative to the number of crushing times in the fiberizing step of Examples 1 to 3 and Comparative Example 2. Fig.15In the figure, the liquid crystal polymer having a pulverization frequency of 0 refers to the liquid crystal polymer before pulverization in the fiberizing step, that is, the finely pulverized liquid crystal polymer immediately after the coarse particles are removed.
[0128] like Fig.15 As shown, in Example 1, the D50 value of the finely pulverized liquid crystal polymer just after the coarse particles were removed was 23 μm. In addition, in Examples 1 to 3, at the time of the first crushing, D50 was significantly reduced compared with Comparative Example 2. For example, in Example 1, at the time of the first crushing, the D50 of the liquid crystal polymer was 9.3 μm. In Examples 1 to 3, since the finely pulverized liquid crystal polymer was obtained using a liquid nitrogen bead mill, the finely pulverized liquid crystal polymer became a fully brittle state. Therefore, it is believed that the fine fiberization in the fiberization process is rapidly carried out, and the entire powdered liquid crystal polymer is finely fiberized by one crushing, and D50 is significantly reduced.
[0129] On the other hand, the D50 value of the liquid crystal polymer of Comparative Example 2 was larger even after 15 crushings than the D50 value of 9.3 μm obtained by one crushing in Example 1. It is considered that the liquid crystal polymer of Comparative Example 2 was not sufficiently embrittled in the fine pulverizing step, and therefore, it was not easy to be finely fiberized in the fiberizing step performed after the fine pulverizing step.
[0130] In the description of the above embodiments, combinable configurations may be combined with each other.
[0131] The embodiments and examples of the present disclosure should be considered to be illustrative in all respects and not restrictive. The scope of the present invention is not indicated by the above description but by the scope of claims, and is intended to include all changes within the meaning and scope equivalent to the scope of claims.
Claims
1. A liquid crystal polymer powder comprising a fiber portion consisting of fibrous particles having a ratio of a length in a long side direction to a fiber diameter, i.e., an aspect ratio, of 10 or more, and a bulk portion having a content of 20% or less that has not been fiberized, The block portion is a condensed portion having a maximum height greater than 10 μm when placed on a plane. The fiber portion has an average diameter of 1 μm or less.
2. The liquid crystal polymer powder according to claim 1, wherein After heating to 400°C in an inert atmosphere, cooling to room temperature at a temperature drop rate of 40°C / min or more, and heating again at a temperature rise rate of 40°C / min, the endothermic peak temperature measured using a differential scanning calorimeter exceeded 330°C.
3. A method for producing a liquid crystal polymer powder, comprising the following steps: a fine pulverizing step of pulverizing the uniaxially or biaxially oriented liquid crystal polymer dispersed in liquid nitrogen using a medium to obtain a granular finely pulverized liquid crystal polymer; and In the fiberizing step, the finely pulverized liquid crystal polymer is crushed multiple times using a wet high-pressure crushing device to obtain a liquid crystal polymer powder.