Polarizing plate with adhesive layer

By using a highly heat-resistant (meth)acrylic resin adhesive layer on the polarizing plate, the problem of warping of the polarizing plate at high temperatures is solved, and the heat-resistant durability and operability of the laminated optical member are improved.

CN114456723BActive Publication Date: 2024-10-29SUMITOMO CHEM CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210119590.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-05-23
Publication Date
2024-10-29
Estimated Expiration
2038-05-23

AI Technical Summary

Technical Problem

The existing polarizing plate with an adhesive layer is prone to warping due to thermal influence when assembled into an image display device, affecting operability and durability, and the heat-resistant durability of the laminated optical components is insufficient.

Method used

Use a polarizing plate with a maximum curling force of 500mN or more at 80°C, and use the adhesive layer in which the difference between the gel fraction after heating at 80°C for 24 hours and the gel fraction at 23°C is greater than 5 percentage points ( A meth)acrylic resin adhesive composition that forms a laminated optical member with high warpage resistance and heat resistance durability.

Benefits of technology

It has significantly improved the warpage resistance and heat resistance durability of the laminated optical components, ensuring stability under high temperature conditions and long-term reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114456723B_ABST
    Figure CN114456723B_ABST
Patent Text Reader

Abstract

The present invention provides a polarizing plate with an adhesive layer, which can impart good warping resistance and heat resistance durability to a laminated optical component. The present invention provides a polarizing plate with an adhesive layer, which comprises a polarizing plate having a maximum curling force of 500 mN or more at 80°C and an adhesive layer laminated on the polarizing plate, wherein the absolute value of the difference between the gel fraction (G80) [%] of the adhesive layer after heating at 80°C for 24 hours and the gel fraction (G23) [%] at 23°C is greater than 5 percentage points.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present application is a divisional application of an application filed on May 23, 2018, with application number 201880035314.1 and invention name “Polarizing plate with adhesive layer”. Technical Field

[0002] The present invention relates to a polarizing plate with an adhesive layer, comprising a polarizing plate and an adhesive layer laminated thereon. Background Art

[0003] Polarizing plates formed by laminating protective films on one or both sides of a polarizer are optical components widely used in image display devices such as liquid crystal display devices, organic electroluminescent (organic EL) display devices, etc., including mobile phones / televisions, and especially in various mobile devices such as mobile phones, smartphones, and tablet terminals in recent years.

[0004] Polarizing plates are often used by being attached to image display elements (liquid crystal cells, organic EL display elements, etc.) via an adhesive layer (see, for example, Japanese Patent Publication No. 2010-229321 (Patent Document 1)). Therefore, polarizing plates are sometimes marketed in the form of polarizing plates with an adhesive layer having an adhesive layer pre-applied on one surface.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2010-229321 Summary of the invention

[0008] Problems to be solved by the invention

[0009] When a laminated optical component formed by laminating a polarizing plate with an adhesive layer to an optical component such as an image display element is assembled in the manufacturing process of an image display device or assembled in an image display device for use, warping may occur due to the influence of heat, etc. In recent years, with the thinning of image display elements and polarizing plates, the warping problem of laminated optical components has become increasingly prominent.

[0010] The warping of the laminated optical member may reduce the workability of the above-mentioned manufacturing process, or cause a part of the laminated optical member to be pressed against the frame when the laminated optical member is stored in the frame for transportation, thereby applying stress and causing failures such as damage to the laminated optical member.

[0011] Furthermore, the laminated optical member is required to have excellent heat resistance durability even when it is affected by heat or the like during the manufacturing process of being incorporated into an image display device or when being incorporated into an image display device for use.

[0012] The present invention provides a polarizing plate with a pressure-sensitive adhesive layer that can impart resistance to the above-mentioned warping (hereinafter also referred to as “warping resistance”) and excellent heat-resistant durability to a laminated optical member.

[0013] Means for solving problems

[0014] The present invention provides the pressure-sensitive adhesive layer-attached polarizing plate and laminated optical member described below.

[0015] [1] A polarizing plate with an adhesive layer, comprising a polarizing plate having a maximum curling force of 500 mN or more at 80° C. and an adhesive layer laminated on the polarizing plate,

[0016] The absolute value of the difference between the gel fraction (G80) [%] of the adhesive layer after heating at 80°C for 24 hours and the gel fraction (G23) [%] at 23°C is greater than 5 percentage points.

[0017] [2] The polarizing plate with an adhesive layer according to [1], wherein the adhesive layer has a gel fraction (G80) of 60% or more after being heated at 80° C. for 24 hours.

[0018] [3] The polarizing plate with an adhesive layer according to [1] or [2], wherein the adhesive layer has a gel fraction (G80) of 95% or less after being heated at 80° C. for 24 hours.

[0019] [4] The pressure-sensitive adhesive layer-attached polarizing plate according to any one of [1] to [3], wherein the polarizing plate includes a polarizer having a thickness of 10 μm or more.

[0020] [5] The pressure-sensitive adhesive layer-attached polarizing plate according to any one of [1] to [4], wherein the pressure-sensitive adhesive layer is formed from a pressure-sensitive adhesive composition containing a (meth)acrylic resin.

[0021] [6] The pressure-sensitive adhesive layer-attached polarizing plate according to [5], wherein the (meth)acrylic resin contains a structural unit derived from a (meth)acrylic monomer having a carboxyl group and a structural unit derived from an alkoxyalkyl (meth)acrylamide monomer.

[0022] [7] The polarizing plate with an adhesive layer according to [5] or [6], wherein the content of the crosslinking agent in the adhesive composition is 0 parts by mass or more and 2 parts by mass or less based on 100 parts by mass of the (meth)acrylic resin.

[0023] [8] A laminated optical member comprising a laminate of the pressure-sensitive adhesive layer-attached polarizing plate according to any one of [1] to [7] and an optical member other than the pressure-sensitive adhesive layer-attached polarizing plate.

[0024] Effects of the Invention

[0025] The present invention can provide a polarizing plate with a pressure-sensitive adhesive layer that can provide a laminated optical member having excellent warpage resistance and heat resistance durability. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a schematic cross-sectional view showing an example of the pressure-sensitive adhesive layer-attached polarizing plate and the laminated optical member according to the present invention.

[0027] Figure 2 This is a schematic cross-sectional view showing another example of the pressure-sensitive adhesive layer-attached polarizing plate and the laminated optical member according to the present invention.

[0028] Figure 3 This is a schematic cross-sectional view showing another example of the pressure-sensitive adhesive layer-attached polarizing plate and the laminated optical member according to the present invention.

[0029] Figure 4 This is a schematic cross-sectional view showing another example of the pressure-sensitive adhesive layer-attached polarizing plate and the laminated optical member according to the present invention. DETAILED DESCRIPTION

[0030] <Polarizing plate with adhesive layer>

[0031] [1] Structure of polarizing plate with adhesive layer

[0032] The polarizing plate with an adhesive layer includes a polarizing plate and an adhesive layer laminated thereon. Figure 1 to Figure 4 An example of the layer structure of the polarizing plate with an adhesive layer is shown in FIG.

[0033] Figure 1 The polarizing plate 25 with adhesive layer shown includes a polarizing plate 10 and a first adhesive layer 20 laminated thereon. The polarizing plate 10 has a polarizer 1 and a first protective film 3 attached to one side thereof. The first protective film 3 is attached to the surface of the polarizer 1 opposite to the first adhesive layer 20. Figure 1 As shown in the example, the first protective film 3 may have a surface treatment layer 2 formed on its outer surface (the surface opposite to the polarizer 1). The first adhesive layer 20 may be used, for example, for bonding to an optical member 30. The optical member 30 will be described later.

[0034] Figure 2 The polarizing plate 25 with an adhesive layer shown in the figure includes, in addition to the polarizing plate 10, a second protective film 4 bonded to the other side of the polarizing plate 1. Figure 1 The first adhesive layer 20 is laminated on the outer surface of the second protective film 4 .

[0035] Figure 3 The polarizing plate 25 with an adhesive layer shown in the figure includes, in addition to the polarizing plate 10, a retardation film 7 bonded to the other surface of the polarizing plate 1 via a second adhesive layer 8. Figure 1 same.

[0036] Figure 4 The polarizing plate 25 with an adhesive layer shown in the figure includes, in addition to the polarizing plate 10, a retardation film 7 bonded to the outer surface of the second protective film 4 via a second adhesive layer 8. Figure 2 Same. Figure 3 and Figure 4 In the example shown, the first adhesive layer 20 is bonded to the retardation film 7 .

[0037] The pressure-sensitive adhesive layer-attached polarizing plate 25 may include a separator laminated on the outer surface of the first pressure-sensitive adhesive layer 20 .

[0038] 〔2〕Polarizing plate

[0039] The polarizing plate 10 constituting the pressure-sensitive adhesive layer-attached polarizing plate 25 includes at least a polarizer 1 , and generally includes the polarizer 1 and a thermoplastic resin film as a protective film or the like laminated and bonded to at least one surface thereof.

[0040] 〔2-1〕Polarizing plate

[0041] The polarizer 1 is a film having the function of selectively transmitting linear polarized light in a certain direction from natural light. Examples thereof include: an iodine-based polarizer in which iodine as a dichroic pigment is adsorbed and oriented on a polyvinyl alcohol-based resin film; a dye-based polarizer in which a dichroic dye as a dichroic pigment is adsorbed and oriented on a polyvinyl alcohol-based resin film; and a coating-type polarizer in which a dichroic dye in a lyotropic liquid crystal state is coated, oriented, and fixed. These polarizers selectively transmit linear polarized light in a certain direction from natural light and absorb linear polarized light in another direction, and are therefore called absorption-type polarizers.

[0042] The polarizer 1 is not limited to an absorption-type polarizer, and may be a reflection-type polarizer that selectively transmits linear polarized light in a certain direction from natural light and reflects linear polarized light in another direction, or a scattering-type polarizer that scatters linear polarized light in another direction. From the perspective of excellent visual recognition, an absorption-type polarizer is preferred. Among them, a polyvinyl alcohol-based polarizer composed of a polyvinyl alcohol-based resin is more preferred, a polyvinyl alcohol-based polarizer in which a dichroic pigment such as iodine or a dichroic dye is adsorbed and oriented on a polyvinyl alcohol-based resin film is further preferred, and a polyvinyl alcohol-based polarizer in which iodine is adsorbed and oriented on a polyvinyl alcohol-based resin film is particularly preferred.

[0043] As the polyvinyl alcohol resin constituting the polyvinyl alcohol polarizer, a polyvinyl alcohol resin obtained by saponifying a polyvinyl acetate resin can be used. As the polyvinyl acetate resin, in addition to polyvinyl acetate which is a homopolymer of vinyl acetate, copolymers of vinyl acetate and other copolymerizable monomers can be listed. As other monomers copolymerizable with vinyl acetate, unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and (meth) acrylamides having an ammonium group can be listed.

[0044] The saponification degree of the polyvinyl alcohol resin is usually 85 mol% or more and 100 mol% or less, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, and polyvinyl formal or polyvinyl acetal modified by aldehydes may be used. The average degree of polymerization of the polyvinyl alcohol resin is usually 1000 or more and 10000 or less, preferably 1500 or more and 5000 or less. The average degree of polymerization of the polyvinyl alcohol resin can be obtained according to JIS K 6726.

[0045] Such a film made of polyvinyl alcohol resin is used as the original film of polarizer 1. The method of forming the polyvinyl alcohol resin film is not particularly limited, and a known method can be used. The thickness of the polyvinyl alcohol original film is, for example, 150 μm or less, preferably 100 μm or less (for example, 50 μm or less), and 5 μm or more.

[0046] The polarizer 1 can be manufactured by a method including the following steps, namely, a step of uniaxially stretching a polyvinyl alcohol resin film; a step of adsorbing a dichroic pigment by dyeing the polyvinyl alcohol resin film with a dichroic pigment; a step of treating the polyvinyl alcohol resin film adsorbed with the dichroic pigment with an aqueous boric acid solution (cross-linking treatment); and a step of washing the film with water after the treatment with the aqueous boric acid solution.

[0047] The uniaxial stretching of the polyvinyl alcohol-based resin film can be carried out before, during or after the dyeing of the dichroic pigment. When the uniaxial stretching is carried out after dyeing, the uniaxial stretching can be carried out before or after the boric acid treatment. In addition, the uniaxial stretching can also be carried out in these stages.

[0048] When uniaxial stretching is performed, the uniaxial stretching can be performed between rollers having different peripheral speeds, or a hot roller can be used for uniaxial stretching. In addition, the uniaxial stretching can be dry stretching performed in the atmosphere, or wet stretching performed in a state where the polyvinyl alcohol-based resin film is swollen using a solvent such as water. The stretching ratio is usually 3 times or more and 8 times or less.

[0049] As the method of dyeing the polyvinyl alcohol resin film with a dichroic pigment, for example, a method of immersing the film in an aqueous solution containing a dichroic pigment, etc. can be cited. As the dichroic pigment, iodine and dichroic organic dyes are used. It should be noted that the polyvinyl alcohol resin film is preferably immersed in water before the dyeing process.

[0050] As a dyeing treatment method based on iodine, a method of immersing a polyvinyl alcohol-based resin film in an aqueous solution containing iodine and potassium iodide can be cited. The content of iodine in the aqueous solution can be 0.01 mass parts or more and 1 mass parts or less relative to 100 mass parts of water. The content of potassium iodide can be 0.5 mass parts or more and 20 mass parts or less relative to 100 mass parts of water. In addition, the temperature of the aqueous solution can be 20° C. or more and 40° C. or less.

[0051] On the other hand, as a dyeing treatment method using a dichroic organic dye, there can be cited a method of immersing a polyvinyl alcohol-based resin film in an aqueous solution containing a dichroic organic dye. The aqueous solution containing a dichroic organic dye may contain an inorganic salt such as sodium sulfate as a dyeing auxiliary. The content of the dichroic organic dye in the aqueous solution may be 1×10 -4 The temperature of the aqueous solution may be 20° C. to 80° C.

[0052] As a boric acid treatment method after dyeing based on a dichroic pigment, a method of immersing the dyed polyvinyl alcohol-based resin film in an aqueous solution containing boric acid, etc. can be cited. In the case of using iodine as a dichroic pigment, the aqueous solution containing boric acid preferably contains potassium iodide. The amount of boric acid in the aqueous solution containing boric acid can be more than 2 parts by mass and less than 15 parts by mass relative to 100 parts by mass of water. The amount of potassium iodide in the aqueous solution can be more than 0.1 parts by mass and less than 20 parts by mass relative to 100 parts by mass of water. The temperature of the aqueous solution can be more than 50°C, for example, more than 50°C and less than 85°C.

[0053] The polyvinyl alcohol resin film treated with boric acid is usually washed with water. The washing treatment can be performed, for example, by immersing the polyvinyl alcohol resin film treated with boric acid in water. The temperature of water in the washing treatment is usually 5° C. to 40° C. After washing with water, a drying treatment is performed to obtain the polarizer 1 .

[0054] The drying process can be performed using a hot air dryer or a far-infrared heater. The polarizing plate 10 can be obtained by bonding a thermoplastic resin film as a protective film or the like to one or both surfaces of the polarizer 1 using an adhesive.

[0055] In addition, as another example of the method for manufacturing the polarizer 1, for example, the method described in Japanese Patent Publication No. 2000-338329 or Japanese Patent Publication No. 2012-159778 can be cited. In this method, after a solution containing a polyvinyl alcohol-based resin is applied to the surface of a substrate film to provide a resin layer, a laminated film comprising a substrate film and a resin layer is stretched, and then a dyeing treatment, a cross-linking treatment, etc. are performed to form a polarizer layer (polarizer) comprising a resin layer. The polarizing laminated film comprising a substrate film and a polarizer layer can be prepared by laminating a thermoplastic resin film as a protective film or the like on the polarizer layer, and then peeling off and removing the substrate film to form a polarizing plate 10 having a thermoplastic resin film on one side of the polarizer. If a thermoplastic resin film is further laminated on the polarizer layer exposed by peeling off the substrate film, a polarizing plate 10 having a thermoplastic resin film on both sides of the polarizer is obtained.

[0056] The thickness of the polarizer 1 can be set to 40 μm or less, preferably 30 μm or less. According to the method described in Japanese Patent Publication No. 2000-338329 or Japanese Patent Publication No. 2012-159778, the polarizer 1 of the film can be manufactured more easily, and it is easier to make the thickness of the polarizer 1 be, for example, 20 μm or less, further 15 μm or less, further 10 μm or less or 8 μm or less. The thickness of the polarizer 1 is usually 2 μm or more, preferably 5 μm or more, and more preferably 10 μm or more. Reducing the thickness of the polarizer 1 is beneficial to the thinning of the polarizer 10, the polarizer 25 with an adhesive layer, the laminated optical component, and the image display device.

[0057] 〔2-2〕Thermoplastic resin film

[0058] The thermoplastic resin film attached to one or both sides of the polarizer 1 can be a film containing a light-transmitting (preferably optically transparent) thermoplastic resin, for example, a polyolefin resin such as a chain polyolefin resin (polypropylene resin, etc.), a cyclic polyolefin resin (norbornene resin, etc.); a cellulose ester resin such as triacetyl cellulose and diacetyl cellulose; a polyester resin such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate; a polycarbonate resin; a (meth) acrylic resin; or a mixture, copolymer, or the like thereof.

[0059] The thermoplastic resin film on one or both sides of the polarizer 1 may be an unstretched film, or a film that has been uniaxially stretched or biaxially stretched. The biaxial stretching may be a simultaneous biaxial stretching in which the film is stretched in two stretching directions at the same time, or a sequential biaxial stretching in which the film is stretched in a first direction and then in a second direction different from the first direction.

[0060] The thermoplastic resin film attached to one or both sides of the polarizing plate 1 may be Figure 1 to Figure 4The protective film having the role of protecting the polarizing plate 1 such as the first protective film 3 and the second protective film 4 shown may also be a protective film having an optical function such as a retardation film.

[0061] Phase difference film is an optical functional film used for the purpose of phase difference compensation of a liquid crystal unit as an image display element, etc. For example, a phase difference film having an arbitrary phase difference value can be prepared by stretching a film containing the above-mentioned thermoplastic resin (uniaxial stretching or biaxial stretching, etc.) or forming a liquid crystal layer on the thermoplastic resin film.

[0062] Examples of the chain polyolefin-based resin include homopolymers of chain olefins such as polyethylene resins and polypropylene resins, and copolymers containing two or more chain olefins.

[0063] Cyclic polyolefin resins are a general term for resins containing cyclic olefins represented by norbornene, tetracyclododecene (also known as dimethyl octahydronaphthalene) or their derivatives as polymerized units. Examples of cyclic polyolefin resins include ring-opening (co)polymers of cyclic olefins and hydrogenated products thereof, addition polymers of cyclic olefins, copolymers of cyclic olefins with chain olefins such as ethylene and propylene or aromatic compounds having a vinyl group, and modified (co)polymers thereof modified with unsaturated carboxylic acids or their derivatives.

[0064] Among them, a norbornene-based resin using a norbornene-based monomer such as norbornene or a polycyclic norbornene-based monomer as a cyclic olefin is preferably used.

[0065] The cellulose ester resin is a resin in which at least a part of the hydroxyl groups in cellulose is esterified with acetic acid, and may be a mixed ester in which a part is esterified with acetic acid and another part is esterified with another acid. The cellulose ester resin is preferably an acetyl cellulose resin.

[0066] Examples of the acetyl cellulose-based resin include triacetyl cellulose, diacetyl cellulose, cellulose acetate propionate, and cellulose acetate butyrate.

[0067] The polyester resin is a resin other than the above-mentioned cellulose ester resin having an ester bond, and is generally a resin containing a polycondensate of a polycarboxylic acid or a derivative thereof and a polyol.

[0068] Examples of the polyester resin include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polytrimethylene terephthalate, polytrimethylene naphthalate, polycyclohexanedimethylene terephthalate, and polycyclohexanedimethylene naphthalate.

[0069] Among them, polyethylene terephthalate is preferably used from the viewpoints of mechanical properties, solvent resistance, scratch resistance, cost, etc. Polyethylene terephthalate refers to a resin in which 80 mol% or more of repeating units are composed of ethylene terephthalate, and may contain structural units derived from other copolymer components.

[0070] As other copolymerization components, a dicarboxylic acid component and a diol component are mentioned.

[0071] Examples of the dicarboxylic acid component include isophthalic acid, 4,4'-dicarboxybiphenyl, 4,4'-dicarboxybenzophenone, bis(4-carboxyphenyl)ethane, adipic acid, sebacic acid, 5-sodium sulfoisophthalate, and 1,4-dicarboxycyclohexane.

[0072] Examples of the diol component include propylene glycol, butylene glycol, neopentyl glycol, diethylene glycol, cyclohexanediol, ethylene oxide adducts of bisphenol A, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.

[0073] If necessary, two or more dicarboxylic acid components or diol components may be used in combination.

[0074] Furthermore, hydroxycarboxylic acids such as p-hydroxybenzoic acid, p-hydroxyethoxybenzoic acid, and β-hydroxyethoxybenzoic acid can also be used in combination with the above-mentioned dicarboxylic acid components or diol components.

[0075] As other copolymerization components, a small amount of a dicarboxylic acid component and / or a diol component having an amide bond, a urethane bond, an ether bond, a carbonate bond or the like can be used.

[0076] Polycarbonate resins are polyesters formed from carbonic acid and diols or bisphenols. Among them, aromatic polycarbonates having diphenylalkane in the molecular chain are preferably used from the viewpoints of heat resistance, weather resistance, and acid resistance.

[0077] Examples of the polycarbonate include polycarbonates derived from bisphenols such as 2,2-bis(4-hydroxyphenyl)propane (also known as bisphenol A), 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)isobutane, and 1,1-bis(4-hydroxyphenyl)ethane.

[0078] The (meth)acrylic resin may be, for example, a polymer containing methacrylate as a main monomer (containing 50% by mass or more), and is preferably a copolymer obtained by copolymerizing methacrylate with other copolymerization components.

[0079] In one preferred embodiment, the (meth)acrylic resin contains methyl methacrylate as a copolymerization component, or contains methyl methacrylate and methyl acrylate as copolymerization components.

[0080] Examples of other copolymerization components other than methyl acrylate include:

[0081] Methacrylates other than methyl methacrylate such as ethyl methacrylate, n-butyl methacrylate, isobutyl methacrylate or tert-butyl methacrylate, cyclohexyl methacrylate, phenyl methacrylate, benzyl methacrylate, 2-ethylhexyl methacrylate and 2-hydroxyethyl methacrylate;

[0082] Acrylates such as ethyl acrylate, n-butyl acrylate, isobutyl acrylate or tert-butyl acrylate, cyclohexyl acrylate, phenyl acrylate, benzyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, etc.;

[0083] Hydroxyalkyl acrylates such as methyl 2-(hydroxymethyl)acrylate, methyl 2-(1-hydroxyethyl)acrylate, ethyl 2-(hydroxymethyl)acrylate, n-butyl 2-(hydroxymethyl)acrylate, isobutyl 2-(hydroxymethyl)acrylate or tert-butyl 2-(hydroxymethyl)acrylate;

[0084] Unsaturated acids such as methacrylic acid and acrylic acid;

[0085] Halogenated styrenes such as chlorostyrene and bromostyrene;

[0086] Substituted styrenes such as vinyltoluene and α-methylstyrene;

[0087] Unsaturated nitriles such as acrylonitrile and methacrylonitrile;

[0088] Unsaturated anhydrides such as maleic anhydride and citraconic anhydride;

[0089] Monofunctional monomers such as unsaturated imides such as phenylmaleimide and cyclohexylmaleimide.

[0090] The above other monofunctional monomers may be used alone or in combination of two or more.

[0091] As the other copolymerization components, a polyfunctional monomer can be used.

[0092] Examples of the polyfunctional monomer include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, nonaethylene glycol di(meth)acrylate, tetradecaethylene glycol di(meth)acrylate, and the like, which are obtained by esterifying both terminal hydroxyl groups of ethylene glycol or its oligomers with (meth)acrylic acid;

[0093] The product obtained by esterifying both terminal hydroxyl groups of propylene glycol or its oligomers with (meth)acrylic acid;

[0094] Those obtained by esterifying the hydroxyl group of a diol with (meth)acrylic acid, such as neopentyl glycol di(meth)acrylate, hexanediol di(meth)acrylate, and butanediol di(meth)acrylate;

[0095] The product obtained by esterifying both terminal hydroxyl groups of bisphenol A, alkylene oxide adducts of bisphenol A or halogen-substituted products thereof with (meth) acrylic acid;

[0096] Those obtained by esterifying a polyol such as trimethylolpropane or pentaerythritol with (meth)acrylic acid, and those obtained by ring-opening addition of epoxy groups of glycidyl (meth)acrylate to terminal hydroxyl groups thereof;

[0097] Those obtained by ring-opening addition of the epoxy group of glycidyl (meth)acrylate to dibasic acids such as succinic acid, adipic acid, terephthalic acid, phthalic acid, halogen-substituted dibasic acids thereof, or alkylene oxide adducts thereof;

[0098] Aryl (meth) acrylate; aromatic divinyl compounds such as divinylbenzene, etc.

[0099] Among them, ethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, and neopentyl glycol dimethacrylate are preferably used.

[0100] The (meth)acrylic resin may be a resin modified by a reaction between functional groups of the copolymer. Examples of such reactions include a polymer chain decarbinolation condensation reaction between the methyl group of methyl (meth)acrylate and the hydroxyl group of methyl 2-(hydroxymethyl)acrylate; a polymer chain dehydration condensation reaction between the carboxyl group of (meth)acrylic acid and the hydroxyl group of methyl 2-(hydroxymethyl)acrylate, and the like.

[0101] The glass transition temperature of the (meth)acrylic resin is preferably 80° C. to 160° C. The glass transition temperature can be controlled by adjusting the polymerization ratio of the methacrylate monomer to the acrylate monomer, the carbon chain length of each ester group and the type of functional group they have, and the polymerization ratio of the multifunctional monomer to the entire monomer.

[0102] As a means for increasing the glass transition temperature of the (meth) acrylic resin, it is also effective to introduce a ring structure into the main chain of the polymer. The ring structure is preferably a heterocyclic structure such as a cyclic anhydride structure, a cyclic imide structure, and a lactone structure. Specifically, examples include: cyclic anhydride structures such as glutaric anhydride structure and succinic anhydride structure; cyclic imide structures such as glutarimide structure and succinimide structure; lactone ring structures such as butyrolactone and valerolactone.

[0103] There is a tendency that the glass transition temperature of the (meth)acrylic resin can be increased as the content of the ring structure in the main chain increases.

[0104] The cyclic anhydride structure and the cyclic imide structure can be introduced by the following methods, namely, a method of introducing by copolymerizing monomers having a cyclic structure such as maleic anhydride and maleimide; a method of introducing a cyclic anhydride structure by a dehydration-demethanolation condensation reaction after polymerization; a method of introducing a cyclic imide structure by reacting an amino compound, etc.

[0105] A resin (polymer) having a lactone ring structure can be obtained by the following method, i.e., after preparing a polymer having a hydroxyl group and an ester group in the polymer chain, the hydroxyl group and the ester group in the obtained polymer are subjected to cyclization condensation by heating in the presence of a catalyst such as an organic phosphorus compound as required to form a lactone ring structure.

[0106] The (meth)acrylic resin and the thermoplastic resin film formed therefrom may contain additives as required, such as lubricants, anti-blocking agents, heat stabilizers, antioxidants, antistatic agents, light stabilizers, impact resistance improvers, surfactants, and the like.

[0107] These additives may also be used when other thermoplastic resins other than the (meth)acrylic resin are used as the thermoplastic resin constituting the thermoplastic resin film.

[0108] From the viewpoint of film forming properties or impact resistance of the film, the (meth)acrylic resin may contain acrylic rubber particles as an impact modifier. Acrylic rubber particles are particles containing an elastic polymer mainly composed of acrylic ester as an essential component, and examples thereof include particles of a single-layer structure substantially containing only the elastic polymer and particles of a multi-layer structure containing the elastic polymer as one layer.

[0109] Examples of the elastic polymer include cross-linked elastic copolymers obtained by copolymerizing an alkyl acrylate as a main component with other vinyl monomers and cross-linking monomers copolymerizable therewith.

[0110] Examples of the alkyl acrylate constituting the main component of the elastic polymer include alkyl acrylates having an alkyl group with 1 to 8 carbon atoms, such as methyl acrylate, ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate. Alkyl acrylates having an alkyl group with 4 or more carbon atoms are preferably used.

[0111] Examples of other vinyl monomers copolymerizable with the alkyl acrylate include compounds having one polymerizable carbon-carbon double bond in the molecule, more specifically, methacrylates such as methyl methacrylate; aromatic vinyl compounds such as styrene; and vinyl cyanide compounds such as acrylonitrile.

[0112] Examples of the crosslinkable monomers include crosslinkable compounds having at least two polymerizable carbon-carbon double bonds in the molecule, and more specifically, (meth)acrylates of polyols such as ethylene glycol di(meth)acrylate and butanediol di(meth)acrylate; alkenyl (meth)acrylates such as allyl (meth)acrylate; and divinylbenzene.

[0113] A laminate of a film formed of a (meth) acrylic resin containing no rubber particles and a film formed of a (meth) acrylic resin containing rubber particles may be used as the thermoplastic resin film to be bonded to the polarizer 1. In addition, a product obtained by forming a (meth) acrylic resin layer on one or both sides of a phase difference display layer formed of a resin different from the (meth) acrylic resin to display a phase difference may be used as the thermoplastic resin film to be bonded to the polarizer 1.

[0114] The thermoplastic resin film may contain an ultraviolet absorber. When the polarizing plate 10 is applied to an image display device such as a liquid crystal display device, the thermoplastic resin film containing an ultraviolet absorber is arranged on the visible side of the image display element (such as a liquid crystal cell), thereby suppressing the degradation of the image display element due to ultraviolet rays.

[0115] Examples of the ultraviolet absorber include salicylate compounds, benzophenone compounds, benzotriazole compounds, cyanoacrylate compounds, and nickel complex salt compounds.

[0116] When thermoplastic resin films are laminated on both sides of polarizer 1, these thermoplastic resin films can be films made of the same thermoplastic resin or films made of different thermoplastic resins. In addition, these thermoplastic resin films can be the same or different in terms of thickness, the presence or absence of additives or their types, phase difference characteristics, etc.

[0117] The thermoplastic resin film may have a surface treatment layer 2 (coating layer) such as a hard coat layer, an antiglare layer, an antireflection layer, a light diffusion layer, an antistatic layer, an antifouling layer, or a conductive layer on its outer surface (the surface opposite to the polarizer 1 ).

[0118] The thickness of the thermoplastic resin film is usually 5 μm or more and 200 μm or less, preferably 10 μm or more and 120 μm or less, more preferably 10 μm or more and 85 μm or less, and further preferably 15 μm or more and 60 μm or less. The thickness of the thermoplastic resin film may be 50 μm or less, or 40 μm or less. Reducing the thickness of the thermoplastic resin film is beneficial for thinning the polarizing plate 10, and further the polarizing plate 25 with an adhesive layer, the laminated optical component, and the image display device.

[0119] The surface of the thermoplastic resin film to be coated with the adhesive may be subjected to a surface modification treatment such as saponification, plasma treatment, corona treatment, or primer treatment from the viewpoint of improving adhesion, or may not be subjected to a surface modification treatment from the viewpoint of simplifying the process.

[0120] When the thermoplastic resin film is a cellulose acetate resin film, it is preferably subjected to a saponification treatment from the viewpoint of improving adhesion. Examples of the saponification treatment include a method of immersing the film in an aqueous solution of an alkali such as sodium hydroxide or potassium hydroxide.

[0121] 〔2-3〕Manufacturing of polarizing plates

[0122] Examples of the adhesive for bonding the thermoplastic resin film to the polarizer 1 include a water-based adhesive and an active energy ray-curable adhesive.

[0123] Examples of the water-based adhesive include conventionally known adhesive compositions using a polyvinyl alcohol-based resin or a polyurethane resin as a main component.

[0124] When a polyvinyl alcohol-based resin is used as the main component of the adhesive, the polyvinyl alcohol-based resin may be a polyvinyl alcohol resin such as partially saponified polyvinyl alcohol, completely saponified polyvinyl alcohol, or a modified polyvinyl alcohol-based resin.

[0125] The polyvinyl alcohol-based resin may be a polyvinyl alcohol-based copolymer obtained by saponifying a copolymer of vinyl acetate and other monomers copolymerizable therewith, in addition to a vinyl alcohol homopolymer obtained by saponifying polyvinyl acetate which is a homopolymer of vinyl acetate.

[0126] The aqueous adhesive containing the polyvinyl alcohol resin may contain a curing component or a crosslinking agent such as a polyaldehyde, a melamine compound, a zirconium oxide compound, a zinc compound, glyoxal, a glyoxal derivative, or a water-soluble epoxy resin in order to improve adhesiveness.

[0127] Examples of aqueous adhesives containing a polyurethane resin as a main component include a polyester ionomer polyurethane resin and a compound having a glycidyl group. The polyester ionomer polyurethane resin is a polyurethane resin having a polyester skeleton into which a small amount of ionic components (hydrophilic components) are introduced.

[0128] The active energy ray-curable adhesive is an adhesive that is cured by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays. When an active energy ray-curable adhesive is used, the adhesive layer of the polarizing plate 10 is a cured layer of the adhesive.

[0129] The active energy ray-curable adhesive may be an adhesive containing an epoxy compound cured by cationic polymerization as a curable component, and is preferably an ultraviolet curable adhesive containing the epoxy compound as a curable component. The epoxy compound refers to a compound having an average of one or more, preferably two or more epoxy groups in the molecule. Only one epoxy compound may be used, or two or more epoxy compounds may be used in combination.

[0130] Examples of epoxy compounds include hydrogenated epoxy compounds (glycidyl ethers of polyols having alicyclic rings) obtained by reacting epichlorohydrin with alicyclic polyols obtained by hydrogenating aromatic rings of aromatic polyols; aliphatic epoxy compounds such as polyglycidyl ethers of aliphatic polyols or alkylene oxide adducts thereof; and epoxy compounds having one or more epoxy groups bonded to an alicyclic ring in the molecule, i.e., alicyclic epoxy compounds.

[0131] The active energy ray-curable adhesive may contain a radically polymerizable (meth)acrylic compound as a curable component instead of or together with the epoxy compound. Examples of the (meth)acrylic compound include (meth)acrylic acid ester monomers having one or more (meth)acrylic acid ester groups in the molecule; (meth)acrylic acid ester oligomers having at least two (meth)acrylic acid ester groups in the molecule obtained by reacting two or more functional group-containing compounds; and other (meth)acrylic acid ester oligomers having at least two (meth)acrylic acid ester groups in the molecule.

[0132] When an epoxy compound that cures by cationic polymerization is included as a curing component, the active energy ray-curable adhesive preferably contains a photocationic polymerization initiator. Examples of the photocationic polymerization initiator include aromatic diazonium salts, aromatic iodonium salts, aromatic sulfonium salts, and onium salts, and iron-arene complexes.

[0133] In the case of containing a radical polymerizable component such as a (meth) acrylic acid compound, the active energy ray-curable adhesive preferably contains a photoradical polymerization initiator. Examples of the photoradical polymerization initiator include acetophenone-based initiators, benzophenone-based initiators, benzoin ether-based initiators, thioxanthone-based initiators, xanthone, fluorenone, camphorquinone, benzaldehyde, anthraquinone, and the like.

[0134] The bonding of the polarizer 1 and the thermoplastic resin film may include the following steps: applying an adhesive to the bonding surface of the polarizer 1 and / or the bonding surface of the thermoplastic resin film, or injecting an adhesive between the polarizer 1 and the thermoplastic resin film, overlapping the two films with a layer of adhesive between them, and bonding them from top and bottom using, for example, a bonding roller.

[0135] In the formation of the adhesive layer, various coating methods such as scraper, winding rod, die coater, comma coater, gravure coater, etc. can be utilized. In addition, it is also possible to continuously supply the polarizer 1 and the thermoplastic resin film in such a way that the bonding surfaces of the two become the inner side while casting the adhesive therebetween.

[0136] Before applying the adhesive, one or both of the bonding surfaces of the polarizer 1 and the thermoplastic resin film may be subjected to an adhesion-facilitating treatment (surface activation treatment) such as saponification treatment, corona discharge treatment, plasma treatment, flame treatment, primer treatment, anchor coating treatment, etc.

[0137] When an active energy ray-curable adhesive is used, the adhesive layer is dried as necessary and then irradiated with active energy rays to cure the adhesive layer.

[0138] The light source used for irradiating active energy rays can be any light source that can generate ultraviolet rays, electron rays, X-rays, etc. In particular, it is suitable to use a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a chemical lamp, a black light lamp, a microwave-excited mercury lamp, a metal halide lamp, etc., which have a light emission distribution at a wavelength of less than 400 nm.

[0139] In the obtained polarizing plate 10 , the thickness of the adhesive layer formed of the aqueous adhesive is, for example, 10 nm to 10 μm, preferably 20 nm to 5 μm, more preferably 30 nm to 1 μm, and further preferably 40 nm to 500 nm.

[0140] The thickness of the adhesive layer formed of the active energy ray-curable adhesive is, for example, 10 nm to 20 μm, preferably 100 nm to 10 μm, and more preferably 500 nm to 5 μm.

[0141] When the thermoplastic resin films are bonded to both surfaces of the polarizing plate 1 , the thicknesses of the two adhesive layers may be the same or different.

[0142] 〔2-4〕Other components of polarizing plate

[0143] The polarizing plate 10 may include other optically functional films in addition to the polarizing plate 30 for imparting desired optical functions, and a suitable example thereof is as follows: Figure 3 and Figure 4 A retardation film such as the retardation film 7 shown.

[0144] As described above, the thermoplastic resin film as a protective film may also serve as a phase difference film, or a phase difference film separate from the thermoplastic resin film may be laminated. In the latter case, the phase difference film may be laminated on the outer surface of the thermoplastic resin film via a pressure-sensitive adhesive layer or an adhesive layer.

[0145] Alternatively, a phase difference film may be laminated instead of the thermoplastic resin film (see Figure 3 In this case, the phase difference film may be laminated on the surface of the polarizing plate 1 via a pressure-sensitive adhesive layer or an adhesive layer.

[0146] Examples of the retardation film include a birefringent film composed of a stretched film of a light-transmitting thermoplastic resin; a film in which discotic liquid crystal or nematic liquid crystal is oriented and fixed; and a retardation film in which the liquid crystal layer is formed on a substrate film.

[0147] The base film is usually a film made of a thermoplastic resin, and an example of the thermoplastic resin is a cellulose ester resin such as triacetyl cellulose.

[0148] As the thermoplastic resin for forming the birefringent film, the thermoplastic resins described above for the thermoplastic resin film can be used.

[0149] Examples of other optically functional films (optical members) that may be included in the polarizing plate 10 include a light-collecting plate, a brightness enhancement film, a reflective layer (reflective film), a semi-transmissive reflective layer (semi-transmissive reflective film), a light diffusion layer (light diffusion film), etc. These are generally provided when the polarizing plate 10 is a polarizing plate disposed on the back side (backlight side) of the liquid crystal unit.

[0150] The focusing plate is used for the purpose of controlling the light path, and may be a prism array plate, a lens array plate, a plate with dots, or the like.

[0151] The brightness enhancement film is used for the purpose of improving the brightness of the liquid crystal display device using the polarizing plate 10. Specifically, there can be cited a reflective polarization separator designed to produce anisotropy in reflectivity by stacking a plurality of thin films having different refractive index anisotropies, a circular polarization separator obtained by supporting an oriented film of a cholesteric liquid crystal polymer or an oriented liquid crystal layer thereof on a base film, and the like.

[0152] In order to make the polarizing plate 10 a reflective, semi-transmissive, or diffuse optical component, a reflective layer, a semi-transmissive reflective layer, and a light diffusion layer are provided respectively. A reflective polarizing plate is used for a liquid crystal display device that reflects incident light from the visible side and displays, and a light source such as a backlight source can be omitted, so it is easy to thin the liquid crystal display device. A semi-transmissive polarizing plate is used for a liquid crystal display device that is reflective in a bright place and displays with light from a backlight source in a dark place. In addition, a diffuse polarizing plate is used for a liquid crystal display device that imparts light diffusivity and suppresses poor display such as moire. The reflective layer, the semi-transmissive reflective layer, and the light diffusion layer can be formed using a known method.

[0153] The polarizing plate 10 may include a protective film for protecting the surface (typically the surface of the thermoplastic resin film) on the side opposite to the side to be laminated with the first adhesive layer 20. The protective film is peeled off together with the adhesive layer it has, for example, after the polarizing plate 25 with an adhesive layer is attached to an optical member such as an image display element.

[0154] The protective film is composed of, for example, a base film and an adhesive layer laminated thereon.

[0155] The resin constituting the substrate film may be a thermoplastic resin such as polyethylene resin such as polyethylene, polypropylene resin such as polypropylene, polyester resin such as polyethylene terephthalate or polyethylene naphthalate, or polycarbonate resin, and preferably a polyester resin such as polyethylene terephthalate.

[0156] 〔2-5〕Curling force of polarizing plate

[0157] The present invention is advantageous for improving the curl resistance of a laminated optical member and is therefore particularly effective when the polarizing plate 10 is prone to curling.

[0158] The curling ease of the polarizing plate 10 can be evaluated, for example, by the maximum curling force at 80° C. The maximum curling force at 80° C. is measured by the method described in the section [Examples] described later.

[0159] The polarizing plate 10 of the pressure-sensitive adhesive layer-attached polarizing plate 25 may have a maximum curling force of 500 mN or more at 80° C. Even in this case, according to the present invention, a laminated optical member having excellent warpage resistance can be provided.

[0160] The maximum curling force of the polarizing plate 10 of the polarizing plate 25 with an adhesive layer at 80°C may be 700 mN or more, 1000 mN or more, 1200 mN or more, or 1500 mN or more. The maximum curling force of the polarizing plate 10 of the polarizing plate 25 with an adhesive layer at 80°C is usually 10000 mN or less, 5000 mN or less, 3000 mN or less, or 2000 mN or less.

[0161] As an example of the structure of the polarizing plate 10 which easily curls, any of the following structures (a) to (h) can be mentioned, for example.

[0162] (a) The thickness of the polarizing plate 1 is

[0163] (b) Thermoplastic resin film thin structure,

[0164] (c) the adhesive layer interposed between the polarizer 1 and the thermoplastic resin film is a cured layer of an active energy ray-curable adhesive,

[0165] (d) A configuration in which a thermoplastic resin film is bonded to only one side of the polarizing plate 1,

[0166] (e) the thermoplastic resin films bonded to both sides of the polarizing plate 1 have different structures (resin type, thickness, presence or absence of a surface treatment layer, etc.),

[0167] (f) the adhesive layers for bonding the thermoplastic resin film to both sides of the polarizing plate 1 are composed of adhesives of different types;

[0168] (g) a structure in which thermoplastic resin films are laminated to both surfaces of the polarizing plate 1, and another optically functional film is laminated to one of the thermoplastic resin films;

[0169] (h) In addition, the total number of films and layers on one side is different from the total number of films and layers on the other side based on the polarizing plate 1.

[0170] In addition, the larger the size of the polarizing plate 10, the easier it is to curl. From the viewpoint of the maximum curling force at 80°C, the polarizing plate 10 is preferably a single piece of a square or substantially square polarizing plate and has a size of 100 mm × 40 mm or more, and more preferably has a size of 150 mm × 40 mm or more. The size of the polarizing plate 10 is, for example, 1650 mm × 930 mm or less, and preferably 1430 mm × 810 mm or less.

[0171] [3] Adhesive layer

[0172] The pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer 20 ) constituting the pressure-sensitive adhesive layer-attached polarizing plate 25 is formed from a pressure-sensitive adhesive composition.

[0173] [3-1] (Meth) acrylic resin

[0174] The adhesive composition preferably includes a (meth) acrylic resin from the viewpoints of the optical properties (transparency, polarization properties, etc.) of the polarizing plate with an adhesive layer, the warping resistance or heat resistance durability of the laminated body of the polarizing plate with an adhesive layer and other optical components, i.e., the laminated optical components, and the adhesion between the adhesive layer (first adhesive layer 20) in the laminated optical components and other optical components. The adhesive composition may include one or more (meth) acrylic resins.

[0175] In the present specification, "(meth)acrylic" means acrylic and / or methacrylic, and the same applies to "(meth)" when referring to (meth)acrylate or the like.

[0176] The heat resistance durability refers to resistance to problems such as lifting or peeling at the interface between the pressure-sensitive adhesive layer and other optical members, and foaming of the pressure-sensitive adhesive layer, which may occur when the laminated optical member is placed at high temperature or in an environment with repeated high and low temperatures.

[0177] From the viewpoints of the optical properties (transparency, polarization properties, etc.) of the polarizing plate with an adhesive layer, the warping resistance or heat resistance durability of the laminated optical components, and / or the adhesion between the adhesive layer of the laminated optical components and other optical components, the (meth)acrylic resin is preferably a polymer containing a structural unit derived from a (meth)acrylate represented by the following formula (I) as a main component.

[0178]

[0179] The main component means that the content of the main component in all the structural units constituting the (meth)acrylic resin is 50% by mass or more.

[0180] In the above formula (I), R 1 represents a hydrogen atom or a methyl group, R 2 It represents an alkyl group having 1 to 14 carbon atoms which may be substituted with an alkoxy group having 1 to 10 carbon atoms, or an aralkyl group having 7 to 21 carbon atoms which may be substituted with an alkoxy group having 1 to 10 carbon atoms. When the aralkyl group is substituted with an alkoxy group, the carbon number of the aralkyl group is the number of carbon atoms excluding the carbon atoms of the alkoxy group.

[0181] R2 is preferably an alkyl group having 1 to 14 carbon atoms which may be substituted with an alkoxy group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 14 carbon atoms which is not substituted with the alkoxy group.

[0182] Examples of the (meth)acrylate represented by formula (I) include alkyl (meth)acrylates having a linear alkyl ester portion such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-octyl (meth)acrylate, and lauryl (meth)acrylate; and alkyl (meth)acrylates having a branched alkyl ester portion such as isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isooctyl (meth)acrylate.

[0183] When R2 is an alkyl group substituted with an alkoxy group, that is, as the (meth)acrylate represented by formula (I) when R2 is an alkoxyalkyl group, for example, 2-methoxyethyl (meth)acrylate, ethoxymethyl (meth)acrylate, etc. can be mentioned.

[0184] Examples of the (meth)acrylate represented by formula (I) when R2 is an aralkyl group having 7 to 21 carbon atoms include benzyl (meth)acrylate and the like.

[0185] The (meth)acrylate represented by formula (I) may be used alone or in combination of two or more. Among them, the (meth)acrylate preferably contains n-butyl acrylate.

[0186] The (meth)acrylic resin contains preferably 50% by mass or more, more preferably 55% by mass or more of structural units derived from n-butyl acrylate in all structural units constituting the (meth)acrylic resin. The content of the structural units derived from n-butyl acrylate is usually 90% by mass or less, preferably 85% by mass or less, more preferably 80% by mass or less, and further preferably 75% by mass or less in all structural units constituting the (meth)acrylic resin.

[0187] On the basis of n-butyl acrylate, (meth)acrylates shown in formula (I) other than n-butyl acrylate may also be used in combination. For example, the (meth) acrylic resin preferably comprises a structural unit derived from n-butyl acrylate and a structural unit derived from methyl acrylate. In the case where the (meth) acrylic resin comprises a structural unit derived from n-butyl acrylate and a structural unit derived from methyl acrylate, the content of the structural unit derived from n-butyl acrylate is as shown above, and the content of the structural unit derived from methyl acrylate is generally 1% by mass or more and 50% by mass or less in all structural units constituting the (meth) acrylic resin, preferably 5% by mass or more and 45% by mass or less, and more preferably 10% by mass or more and 40% by mass or less.

[0188] From the viewpoints of the optical properties (transparency, polarization properties, etc.) of the polarizing plate with an adhesive layer, the warping resistance or heat resistance durability of the laminated optical components, and / or the adhesion between the adhesive layer of the laminated optical components and other optical components, the content of the structural unit derived from the (meth)acrylate represented by formula (I) is preferably 60% by mass or more and less than 100% by mass, more preferably 70% by mass or more and 99.9% by mass or less, and further preferably 80% by mass or more and 99.6% by mass or less in all the structural units constituting the (meth)acrylic resin.

[0189] The (meth)acrylic resin may contain a structural unit derived from a (meth)acrylic monomer having a hydroxyl group. The inclusion of such a structural unit may be advantageous in improving the warpage resistance or heat resistance durability of the laminated optical component and / or the adhesion between the adhesive layer of the laminated optical component and other optical components.

[0190] As the (meth)acrylic monomer having a hydroxyl group, a (meth)acrylate having a hydroxyl group can be mentioned.

[0191] Examples of the (meth)acrylate having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-(2-hydroxyethoxy)ethyl (meth)acrylate, 2- or 3-chloro-2-hydroxypropyl (meth)acrylate, and diethylene glycol mono(meth)acrylate.

[0192] From the viewpoints of the warping resistance or heat resistance durability of the laminated optical components, and / or the processability of the adhesive layer of the laminated optical components, and the adhesion with other optical components, the content of the structural unit derived from the (meth)acrylic monomer having a hydroxyl group is preferably 0.1 mass % to 5 mass %, and more preferably 0.5 mass % to 4 mass % in all the structural units constituting the (meth)acrylic resin.

[0193] The (meth)acrylic resin may contain a structural unit derived from a monomer having other polar functional groups other than the (meth)acrylic monomer having a hydroxyl group. The monomer having other polar functional groups is preferably a (meth)acrylic monomer having other polar functional groups.

[0194] Examples of the polar functional group possessed by the monomer having other polar functional groups include a carboxyl group (free carboxyl group), an amino group, a heterocyclic group (for example, an epoxy group), and an amide group.

[0195] Examples of monomers having other polar functional groups include:

[0196] Monomers having a carboxyl group such as (meth)acrylic acid and β-carboxyethyl (meth)acrylate ((meth)acrylic acid-based monomers having a carboxyl group);

[0197] Monomers having a heterocyclic group such as (meth)acryloylmorpholine, vinylcaprolactam, N-vinyl-2-pyrrolidone, vinylpyridine, tetrahydrofurfuryl (meth)acrylate, caprolactone-modified tetrahydrofurfuryl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, glycidyl (meth)acrylate, and 2,5-dihydrofuran;

[0198] Monomers having an amino group other than a heterocyclic ring, such as aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and dimethylaminopropyl (meth)acrylate, etc.

[0199] The monomers having other polar functional groups may be used alone or in combination of two or more.

[0200] From the viewpoint of the warping resistance or heat resistance durability of the laminated optical components, and / or the adhesion between the adhesive layer of the laminated optical components and other optical components, the content of the structural units derived from monomers having other polar functional groups in all the structural units constituting the (meth)acrylic resin is preferably from 0.1 mass % to 5 mass %, and more preferably from 0.5 mass % to 3 mass %.

[0201] The (meth)acrylic resin may further include a structural unit derived from a monomer having one ethylenic double bond and at least one aromatic ring in the molecule (but excluding monomers belonging to the above formula (I) or having the above polar functional group).

[0202] Containing a structural unit derived from a monomer having one ethylenic double bond and at least one aromatic ring in the molecule may be advantageous from the viewpoint of effectively suppressing whitening or color unevenness of the laminated optical member.

[0203] Examples of the monomer having one ethylenic double bond and at least one aromatic ring in the molecule include a (meth)acrylic monomer having an aromatic ring.

[0204] Examples of the (meth)acrylic monomer having an aromatic ring include neopentyl glycol benzoate (meth)acrylate and (meth)acrylates having an aryloxyalkyl group such as a phenoxyethyl group-containing (meth)acrylate represented by the following formula (II). (Meth)acrylates having an aryloxyalkyl group are preferred.

[0205]

[0206] In formula (II), R 3 represents a hydrogen atom or a methyl group, i represents an integer from 1 to 8, R 4 represents a hydrogen atom, an alkyl group, an aralkyl group or an aryl group. 4 In the case of an alkyl group, the number of carbon atoms may be about 1 to about 9, in the case of an aralkyl group, the number of carbon atoms may be about 7 to about 11, and in the case of an aryl group, the number of carbon atoms may be about 6 to about 10.

[0207] Respectively, as the constituent R in formula (II) 4 Examples of the alkyl group having 1 to 9 carbon atoms include methyl, butyl, nonyl, etc. Examples of the aralkyl group having 7 to 11 carbon atoms include benzyl, phenethyl, naphthylmethyl, etc. Examples of the aryl group having 6 to 10 carbon atoms include phenyl, tolyl, naphthyl, etc.

[0208] Specific examples of the phenoxyethyl-containing (meth)acrylate represented by formula (II) include 2-phenoxyethyl (meth)acrylate, 2-(2-phenoxyethoxy)ethyl (meth)acrylate, ethylene oxide-modified nonylphenol (meth)acrylate, and 2-(o-phenylphenoxy)ethyl (meth)acrylate.

[0209] The phenoxyethyl group-containing (meth)acrylate may be used alone or in combination of two or more.

[0210] Among them, the (meth)acrylate containing a phenoxyethyl group preferably includes one or more selected from 2-phenoxyethyl (meth)acrylate, 2-(o-phenylphenoxy)ethyl (meth)acrylate, and 2-(2-phenoxyethoxy)ethyl (meth)acrylate, and more preferably includes one or two selected from 2-(o-phenylphenoxy)ethyl (meth)acrylate and 2-(2-phenoxyethoxy)ethyl (meth)acrylate.

[0211] From the viewpoint of effectively suppressing whitening or color unevenness in laminated optical components, the content of structural units derived from monomers having one olefinic double bond and at least one aromatic ring in the molecule is preferably from 1 mass % to 20 mass % in all structural units constituting the (meth)acrylic resin, and more preferably from 5 mass % to 15 mass % in all structural units constituting the (meth)acrylic resin.

[0212] The (meth)acrylic resin may contain structural units derived from monomers other than the (meth)acrylate of formula (I) described above, the monomer having a polar functional group, and the monomer having one ethylenic double bond and at least one aromatic ring in the molecule (hereinafter also referred to as "other monomers").

[0213] Examples of other monomers include structural units derived from (meth)acrylates having an alicyclic structure in the molecule, structural units derived from styrene-based monomers, structural units derived from vinyl-based monomers, structural units derived from monomers having a plurality of (meth)acryloyl groups in the molecule, and structural units derived from (meth)acrylamide monomers.

[0214] The other monomers may be used alone or in combination of two or more.

[0215] Containing a structural unit derived from other monomers, particularly a structural unit derived from a (meth)acrylamide monomer, may be advantageous in improving the warpage resistance or heat resistance durability of the laminated optical member and / or the adhesion between the pressure-sensitive adhesive layer of the laminated optical member and other optical members.

[0216] The alicyclic structure in the (meth)acrylate having an alicyclic structure in the molecule refers to a cycloalkane structure having generally 5 or more, preferably 5 or more and 7 or less carbon atoms.

[0217] Examples of the (meth)acrylate having an alicyclic structure include isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, cyclododecyl (meth)acrylate, methylcyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, cyclohexylphenyl (meth)acrylate, and α-ethoxycyclohexyl acrylate.

[0218] Examples of the styrene monomer include styrene; alkyl styrenes such as methyl styrene, dimethyl styrene, trimethyl styrene, ethyl styrene, diethyl styrene, triethyl styrene, propyl styrene, butyl styrene, hexyl styrene, heptyl styrene, and octyl styrene; halogenated styrenes such as fluorostyrene, chlorostyrene, bromostyrene, dibromostyrene, and iodostyrene; nitrostyrene, acetyl styrene, methoxy styrene, and divinylbenzene.

[0219] Examples of the vinyl monomers include: fatty acid vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, vinyl 2-ethylhexanoate, and vinyl laurate; vinyl halides such as vinyl chloride and vinyl bromide; vinylidene halides such as vinylidene chloride; nitrogen-containing aromatic vinyls such as vinyl pyridine, vinyl pyrrolidone, and vinyl carbazole; conjugated diene monomers such as butadiene, isoprene, and chloroprene; acrylonitrile, methacrylonitrile, and the like.

[0220] Examples of monomers having multiple (meth)acryloyl groups in the molecule include monomers having two (meth)acryloyl groups in the molecule, such as 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, and tripropylene glycol di(meth)acrylate; and monomers having three (meth)acryloyl groups in the molecule, such as trimethylolpropane tri(meth)acrylate.

[0221] The (meth)acrylamide monomers include N-hydroxymethyl (meth)acrylamide, N-(2-hydroxyethyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(4-hydroxybutyl) (meth)acrylamide, N-(5-hydroxypentyl) (meth)acrylamide, N-(6-hydroxyhexyl) (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N-isopropyl ... acrylamide, N-(3-dimethylaminopropyl)(meth)acrylamide, N-(1,1-dimethyl-3-oxobutyl)(meth)acrylamide, N-[2-(2-oxo-1-imidazolidinyl)ethyl](meth)acrylamide, 2-acryloylamino-2-methyl-1-propanesulfonic acid, N-(methoxymethyl)acrylamide, N-(ethoxymethyl)(meth)acrylamide, N-(propyloxymethyl)(meth)acrylamide, N-(1-methylethoxymethyl) (Meth)acrylamide, N-(1-methylpropoxymethyl) (meth)acrylamide, N-(2-methylpropoxymethyl) (meth)acrylamide [alias: N-(isobutoxymethyl) (meth)acrylamide], N-(butoxymethyl) (meth)acrylamide, N-(1,1-dimethylethoxymethyl) (meth)acrylamide, N-(2-methoxyethyl) (meth)acrylamide, N-(2-ethoxyethyl) (meth)acrylamide, N-(2-propoxyethyl) (meth)acrylamide, N-〔2-(1-methylethoxy)ethyl〕 (meth)acrylamide, N-〔2-(1-methylpropoxy)ethyl〕 (meth)acrylamide, N-〔2-(2-methylpropoxy)ethyl〕 (meth)acrylamide [alias: N-(2-isobutoxyethyl) (meth)acrylamide], N-(2-butoxyethyl) (meth)acrylamide, N-〔2-(1,1-dimethylethoxy)ethyl〕 (meth)acrylamide, etc. Among them, N-(methoxymethyl)acrylamide, N-(ethoxymethyl)acrylamide, N-(propoxymethyl)acrylamide, N-(butoxymethyl)acrylamide, and N-(2-methylpropoxymethyl)acrylamide are preferably used.

[0222] From the viewpoint of the warpage resistance and heat resistance durability of the laminated optical member, the adhesion between the pressure-sensitive adhesive layer of the laminated optical member and other optical members, etc., the (meth)acrylamide monomer is preferably an alkyl(meth)acrylamide monomer which may be substituted with an alkoxy group.

[0223] In the alkyl(meth)acrylamide monomer which may be substituted with an alkoxy group, the number of carbon atoms of the alkoxy group is preferably 1 to 10, and the number of carbon atoms of the alkyl group is preferably 1 to 14. When an alkyl group is substituted with an alkoxy group, the number of carbon atoms of the alkyl group is the number of carbon atoms excluding the carbon atoms of the alkoxy group.

[0224] Examples of the alkyl (meth) acrylamide monomer which may be substituted with an alkoxy group include an alkoxyalkyl (meth) acrylamide monomer represented by the following formula (III).

[0225]

[0226] In formula (III), R 5 represents a hydrogen atom or a methyl group, R 6 represents an alkyl group having 1 to 14 carbon atoms. n represents an integer of 1 to 8.

[0227] Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, an n-hexyl group, an n-heptyl group, and an n-octyl group.

[0228] n is preferably 1 or more and 6 or less.

[0229] From the viewpoint of the warping resistance or heat resistance durability of the laminated optical component, and / or the adhesion between the adhesive layer of the laminated optical component and other optical components, the content of the structural units derived from other monomers (especially the (meth)acrylamide monomer) in all the structural units constituting the (meth)acrylic resin is preferably from 0.1 mass % to 20 mass %, more preferably from 0.2 mass % to 10 mass %, and further preferably from 0.3 mass % to 5 mass %.

[0230] From the viewpoint of the warping resistance or heat resistance durability of the laminated optical component and / or the adhesion between the adhesive layer of the laminated optical component and other optical components, the (meth)acrylic resin preferably contains a structural unit derived from a (meth)acrylic monomer having a carboxyl group and a structural unit derived from an alkoxyalkyl (meth)acrylamide monomer.

[0231] From the viewpoint of the warping resistance or heat resistance durability of the laminated optical component and / or the adhesion between the adhesive layer of the laminated optical component and other optical components, the total content of the structural units derived from the (meth)acrylic monomer having a carboxyl group and the structural units derived from the alkoxyalkyl (meth)acrylamide monomer is preferably 0.1 mass % or more and 15 mass % or less, more preferably 0.2 mass % or more and 10 mass % or less, and further preferably 0.3 mass % or more and 4 mass % or less in all the structural units constituting the (meth)acrylic resin.

[0232] The weight average molecular weight (Mw) of the (meth)acrylic resin based on standard polystyrene conversion by gel permeation chromatography (GPC) is preferably in the range of 500,000 to 2,000,000, and more preferably in the range of 600,000 to 1,800,000. An adhesive composition containing a (meth)acrylic resin having an Mw within the above range may be advantageous from the viewpoint of ensuring the warpage resistance or heat resistance durability of the laminated optical component and / or the operability of the (meth)acrylic resin during the preparation of the adhesive composition.

[0233] The molecular weight distribution represented by the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is generally about 2 or more and 10 or less, and preferably 3 or more and 8 or less.

[0234] (Meth) acrylic resin can be produced by known methods such as solution polymerization, bulk polymerization, suspension polymerization, emulsion polymerization, etc. A polymerization initiator is generally used in the production of (meth) acrylic resin. The polymerization initiator can be used in an amount of 0.001 parts by mass or more and 5 parts by mass or less relative to a total of 100 parts by mass of all monomers used in the production of (meth) acrylic resin. In addition, (meth) acrylic resin can be produced by a method of polymerization using active energy rays such as ultraviolet rays.

[0235] As the polymerization initiator, a thermal polymerization initiator, a photopolymerization initiator, or the like is used.

[0236] Examples of the photopolymerization initiator include 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone.

[0237] Examples of the thermal polymerization initiator include azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), dimethyl-2,2'-azobis(2-methylpropionate), and 2,2'-azobis(2-hydroxymethylpropionitrile); organic peroxides such as lauryl peroxide, tert-butyl hydroperoxide, benzoyl peroxide, tert-butyl perbenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, dipropyl peroxydicarbonate, tert-butyl peroxyneodecanoate, tert-butyl peroxypivalate, and (3,5,5-trimethylhexanoyl) peroxide; and inorganic peroxides such as potassium persulfate, ammonium persulfate, and hydrogen peroxide.

[0238] Furthermore, a redox initiator using a peroxide and a reducing agent in combination can also be used as the polymerization initiator.

[0239] As a method for producing a (meth)acrylic resin, among the methods shown above, a solution polymerization method is preferred. An example of the solution polymerization method is as follows: the monomers and organic solvents used are mixed, a thermal polymerization initiator is added under a nitrogen atmosphere, and the mixture is stirred at a temperature of about 40° C. to about 90° C., preferably about 50° C. to about 80° C. for about 3 hours to about 15 hours. In order to control the reaction, the monomers and the thermal polymerization initiator may be added continuously or intermittently during the polymerization, or may be added in a state of being dissolved in an organic solvent.

[0240] Examples of the organic solvent include aromatic hydrocarbons such as toluene and xylene; esters such as ethyl acetate and butyl acetate; aliphatic alcohols such as propanol and isopropanol; and ketones such as acetone, methyl ethyl ketone and methyl isobutyl ketone.

[0241] 〔3-2〕Crosslinking agent

[0242] The pressure-sensitive adhesive composition may further contain a crosslinking agent. The crosslinking agent is a compound that reacts with a polar functional group or the like in the (meth)acrylic resin to crosslink the (meth)acrylic resin.

[0243] Examples of the crosslinking agent include crosslinking agents selected from isocyanate compounds, epoxy compounds, aziridine compounds, metal chelate compounds, and the like.

[0244] Among them, the isocyanate compound, the epoxy compound, and the aziridine compound have at least two functional groups in the molecule that can react with the polar functional group or the like in the (meth)acrylic resin.

[0245] The cross-linking agent may be used alone or in combination of two or more.

[0246] The isocyanate compound is a compound having at least two isocyanate groups (—NCO) in the molecule.

[0247] Examples of the isocyanate compounds include tolylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, naphthalene diisocyanate, triphenylmethane triisocyanate, etc. In addition, adducts obtained by reacting polyols such as glycerin or trimethylolpropane with these isocyanate compounds, and products obtained by converting isocyanate compounds into dimers, trimers, etc. can also serve as crosslinking agents.

[0248] Two or more isocyanate compounds may be used in combination.

[0249] The epoxy compound is a compound having at least two epoxy groups in the molecule.

[0250] Examples of epoxy compounds include bisphenol A type epoxy resins, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerol diglycidyl ether, glycerol triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, N,N-diglycidyl aniline, N,N,N',N'-tetraglycidyl meta-xylylenediamine, and 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane.

[0251] Two or more epoxy compounds may be used in combination.

[0252] The aziridine compound is a compound also called aziridine, which has at least two three-membered ring skeletons containing one nitrogen atom and two carbon atoms in the molecule.

[0253] Examples of aziridine compounds include diphenylmethane-4,4'-bis(1-aziridinecarboxamide), toluene-2,4-bis(1-aziridinecarboxamide), triethylene melamine, isophthaloylbis-1-(2-methylaziridine), tri-1-aziridinylphosphine oxide, hexamethylene-1,6-bis(1-aziridinecarboxamide), trimethylolpropane-tri-β-aziridine propionate, and tetramethylolmethane-tri-β-aziridine propionate.

[0254] Two or more aziridine compounds may be used in combination.

[0255] Examples of the metal chelate compound include compounds in which acetylacetone or ethyl acetoacetate is coordinated to a polyvalent metal such as aluminum, iron, copper, zinc, tin, titanium, nickel, antimony, magnesium, vanadium, chromium, and zirconium.

[0256] Two or more metal chelate compounds may be used in combination.

[0257] Among them, isocyanate compounds may be advantageous in improving the warpage resistance or heat resistance durability of a laminated optical member and / or the adhesion between the pressure-sensitive adhesive layer of the laminated optical member and other optical members.

[0258] Among the isocyanate compounds, preferably used are: xylene diisocyanate, toluene diisocyanate or hexamethylene diisocyanate; adducts obtained by reacting polyols such as glycerol or trimethylolpropane with these isocyanate compounds; products obtained by making these isocyanate compounds into dimers, trimers, etc. or mixtures thereof; mixtures of two or more of the isocyanate compounds listed above, etc.

[0259] Suitable isocyanate compounds include toluene diisocyanate, an adduct obtained by reacting a polyol with toluene diisocyanate, a dimer of toluene diisocyanate, and a trimer of toluene diisocyanate; or hexamethylene diisocyanate, an adduct obtained by reacting a polyol with hexamethylene diisocyanate, a dimer of hexamethylene diisocyanate, and a trimer of hexamethylene diisocyanate.

[0260] The content of the crosslinking agent in the adhesive composition is usually 0 to 5 parts by mass, preferably 0 to 2 parts by mass, relative to 100 parts by mass of the (meth)acrylic resin. When the adhesive composition contains a crosslinking agent, the lower limit of the content is, for example, 0.05 parts by mass relative to 100 parts by mass of the (meth)acrylic resin.

[0261] 〔3-3〕Ionic compounds

[0262] The adhesive composition may further contain an ionic compound as an antistatic agent for imparting antistatic properties to the adhesive layer (first adhesive layer 20). The ionic compound is a compound having an inorganic cation or an organic cation and an inorganic anion or an organic anion.

[0263] Two or more ionic compounds may be used.

[0264] Examples of inorganic cations include lithium cations (Li + 〕、Sodium cation〔Na + 〕、Potassium cation〔K + 〕Alkali metal ions such as beryllium cation〔Be 2+ 〕、Magnesium cation〔Mg 2+ 〕、Calcium cation〔Ca 2+ 〕and other alkaline earth metal ions, etc.

[0265] Examples of the organic cation include an imidazolium cation, a pyridinium cation, a pyrrolidinium cation, an ammonium cation, a sulfonium cation, and a phosphonium cation.

[0266] Among the above-mentioned cationic components, organic cationic components are preferably used from the aspect of excellent compatibility with the adhesive composition. Among the organic cationic components, pyridinium cations and imidazolium cations are particularly preferably used from the viewpoint that they are not easily charged when peeling off the separation membrane provided on the adhesive layer (first adhesive layer 20).

[0267] Examples of inorganic anions include chloride anions [Cl - 〕、bromide anion〔Br - 〕、iodide anion〔I - 〕、Tetrachloroaluminate anion〔AlCl4- 〕、heptachlorodialuminate anion〔Al2Cl7 - 〕、Tetrafluoroborate anion〔BF4 - 〕、Hexafluorophosphate anion〔PF6 - 〕、Perchlorate anion〔ClO4 - 〕、nitrate anion〔NO3 - 〕、Hexafluoroarsenate anion〔AsF6 - 〕、Hexafluoroantimonate anion〔SbF6 - 〕、Hexafluoroniobate anion〔NbF6 - 〕、Hexafluorotantalate anion〔TaF6 - 〕、Dicyanamide anion〔(CN)2N - 〕wait.

[0268] Examples of organic anions include acetate anions [CH3COO - 〕、Trifluoroacetate anion〔CF3COO - 〕、Methanesulfonate anion 〔CH3SO3 - 〕、Trifluoromethanesulfonate anion〔CF3SO3 - 〕、p-toluenesulfonate anion〔p-CH3C6H4SO3 - 〕、Bis(fluorosulfonyl)imide anion〔(FSO2)2N - 〕、Bis(trifluoromethanesulfonyl)imide anion〔(CF3SO2)2N - 〕、Tris(trifluoromethanesulfonyl)methanide anion〔(CF3SO2)3C - 〕、Dimethylphosphinate anion〔(CH3)2POO - 〕、(Poly)hydrofluoride fluoride anion〔F(HF) n - 〕(n is about 1 or more and 3 or less), thiocyanate anion〔SCN - 〕、Perfluorobutanesulfonate anion〔C4F9SO3 - 〕、Bis(pentafluoroethanesulfonyl)imide anion〔(C2F5SO2)2N - 〕、Perfluorobutyrate anion〔C3F7COO - 〕、(trifluoromethanesulfonyl)(trifluoromethanecarbonyl)imide anion〔(CF3SO2)(CF3CO)N - 〕、Perfluoropropane-1,3-disulfonate anion〔 - O3S(CF2)3SO3 - 〕、Carbonate anion 〔CO3 2- 〕wait.

[0269] Among the above-mentioned anionic components, from the aspect of imparting an ionic compound with excellent antistatic performance, it is particularly preferred to use anionic components containing fluorine atoms. As anionic components containing fluorine atoms, bis(fluorosulfonyl)imide anions, hexafluorophosphate anions or bis(trifluoromethanesulfonyl)imide anions can be cited.

[0270] Specific examples of the ionic compound can be selected from the combination of the above-mentioned cationic component and anionic component. Examples of the ionic compound having an organic cation are shown below, classified according to the structure of the organic cation.

[0271] Pyridinium salts:

[0272] N-Hexylpyridinium hexafluorophosphate,

[0273] N-octylpyridinium hexafluorophosphate,

[0274] N-octyl-4-methylpyridinium hexafluorophosphate,

[0275] N-butyl-4-methylpyridinium hexafluorophosphate,

[0276] N-decylpyridinium bis(fluorosulfonyl)imide,

[0277] N-dodecylpyridinium bis(fluorosulfonyl)imide,

[0278] N-Tetradecylpyridinium bis(fluorosulfonyl)imide,

[0279] N-hexadecylpyridinium bis(fluorosulfonyl)imide,

[0280] N-dodecyl-4-methylpyridinium bis(fluorosulfonyl)imide,

[0281] N-Tetradecyl-4-methylpyridinium bis(fluorosulfonyl)imide,

[0282] N-hexadecyl-4-methylpyridinium bis(fluorosulfonyl)imide,

[0283] N-Benzyl-2-methylpyridinium bis(fluorosulfonyl)imide,

[0284] N-Benzyl-4-methylpyridinium bis(fluorosulfonyl)imide,

[0285] N-hexylpyridinium bis(trifluoromethanesulfonyl)imide,

[0286] N-octylpyridinium bis(trifluoromethanesulfonyl)imide,

[0287] N-octyl-4-methylpyridinium bis(trifluoromethanesulfonyl)imide,

[0288] N-Butyl-4-methylpyridinium bis(trifluoromethanesulfonyl)imide.

[0289] Imidazolium salts:

[0290] 1-Ethyl-3-methylimidazolium hexafluorophosphate,

[0291] 1-Ethyl-3-methylimidazolium p-toluenesulfonate,

[0292] 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide,

[0293] 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide,

[0294] 1-Butyl-3-methylimidazolium methanesulfonate,

[0295] 1-Butyl-3-methylimidazolium bis(fluorosulfonyl)imide.

[0296] Pyrrolidinium salts:

[0297] N-butyl-N-methylpyrrolidinium hexafluorophosphate,

[0298] N-butyl-N-methylpyrrolidinium bis(fluorosulfonyl)imide, N-butyl-N-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide.

[0299] Quaternary ammonium salts:

[0300] Tetrabutylammonium hexafluorophosphate,

[0301] Tetrabutylammonium p-toluenesulfonate,

[0302] (2-Hydroxyethyl)trimethylammonium bis(trifluoromethanesulfonyl)imide,

[0303] (2-Hydroxyethyl)trimethylammonium dimethylphosphinate.

[0304] Examples of the ionic compound having an inorganic cation are shown below.

[0305] Lithium bromide,

[0306] Lithium iodide,

[0307] Lithium tetrafluoroborate,

[0308] Lithium hexafluorophosphate,

[0309] Lithium thiocyanate,

[0310] Lithium perchlorate,

[0311] Lithium trifluoromethanesulfonate,

[0312] Lithium bis(fluorosulfonyl)imide,

[0313] Lithium bis(trifluoromethanesulfonyl)imide,

[0314] Lithium bis(pentafluoroethanesulfonyl)imide,

[0315] Lithium tris(trifluoromethanesulfonyl)methanide,

[0316] Lithium p-toluenesulfonate,

[0317] Sodium hexafluorophosphate,

[0318] Sodium bis(fluorosulfonyl)imide,

[0319] Sodium bis(trifluoromethanesulfonyl)imide,

[0320] Sodium p-toluenesulfonate,

[0321] Potassium hexafluorophosphate,

[0322] Potassium bis(fluorosulfonyl)imide,

[0323] Potassium bis(trifluoromethanesulfonyl)imide,

[0324] Potassium p-toluenesulfonate.

[0325] The ionic compound is preferably solid at room temperature. Compared with the case of using an ionic compound that is liquid at room temperature, the antistatic performance can be maintained for a long time by using an ionic compound that is solid at room temperature. From the viewpoint of long-term stability of antistatic properties, the ionic compound preferably has a melting point of 30°C or more, and further 35°C or more. On the other hand, if its melting point is too high, the compatibility with the (meth) acrylic resin deteriorates, and therefore, the melting point of the ionic compound is preferably 90°C or less, more preferably 70°C or less, and further preferably less than 50°C.

[0326] The content of the ionic compound in the adhesive composition is preferably 0.2 mass parts or more and 8 mass parts or less relative to 100 mass parts of (meth) acrylic resin, more preferably 0.2 mass parts or more and 6 mass parts or less, further preferably 0.5 mass parts or more and 5 mass parts or less, and particularly preferably 1 mass part or more and 5 mass parts or less. The content of the ionic compound of 0.2 mass parts or more is beneficial for improving the antistatic performance, and 8 mass parts or less is beneficial for maintaining the heat resistance and durability of the adhesive layer (first adhesive layer 20).

[0327] 〔3-4〕Silane compounds

[0328] The adhesive composition may further contain a silane compound, thereby improving the adhesion between the adhesive layer (first adhesive layer 20) and an optical member such as a glass substrate.

[0329] Examples of the silane compound include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(2-methoxyethoxy)silane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyldimethoxymethylsilane, and 3-glycidoxypropylethoxydimethylsilane.

[0330] Two or more silane compounds may be used.

[0331] The silane compound may be a silicone oligomer type silane compound. When the silicone oligomer is represented as a (monomer) oligomer, for example, the following silane compounds can be mentioned.

[0332] 3-Mercaptopropyltrimethoxysilane-tetramethoxysilane copolymer,

[0333] 3-Mercaptopropyltrimethoxysilane-tetraethoxysilane copolymer,

[0334] 3-Mercaptopropyltriethoxysilane-tetramethoxysilane copolymer,

[0335] Copolymers containing mercaptopropyl groups, such as 3-mercaptopropyltriethoxysilane-tetraethoxysilane copolymer;

[0336] Mercaptomethyltrimethoxysilane-tetramethoxysilane copolymer,

[0337] Mercaptomethyltrimethoxysilane-tetraethoxysilane copolymer,

[0338] Mercaptomethyltriethoxysilane-tetramethoxysilane copolymer,

[0339] Copolymers containing mercaptomethyl such as mercaptomethyltriethoxysilane-tetraethoxysilane copolymer;

[0340] 3-Glycidoxypropyltrimethoxysilane-tetramethoxysilane copolymer,

[0341] 3-Glycidoxypropyltrimethoxysilane-tetraethoxysilane copolymer,

[0342] 3-Glycidoxypropyltriethoxysilane-tetramethoxysilane copolymer,

[0343] 3-Glycidoxypropyltriethoxysilane-tetraethoxysilane copolymer,

[0344] 3-Glycidoxypropylmethyldimethoxysilane-tetramethoxysilane copolymer,

[0345] 3-Glycidoxypropylmethyldimethoxysilane-tetraethoxysilane copolymer,

[0346] 3-Glycidoxypropylmethyldiethoxysilane-tetramethoxysilane copolymer,

[0347] 3-glycidoxypropylmethyldiethoxysilane-tetraethoxysilane copolymer and other copolymers containing 3-glycidoxypropyl;

[0348] 3-methacryloxypropyltrimethoxysilane-tetramethoxysilane copolymer,

[0349] 3-methacryloxypropyltrimethoxysilane-tetraethoxysilane copolymer,

[0350] 3-methacryloxypropyltriethoxysilane-tetramethoxysilane copolymer,

[0351] 3-methacryloxypropyltriethoxysilane-tetraethoxysilane copolymer,

[0352] 3-methacryloxypropylmethyldimethoxysilane-tetramethoxysilane copolymer,

[0353] 3-methacryloxypropylmethyldimethoxysilane-tetraethoxysilane copolymer,

[0354] 3-methacryloxypropylmethyldiethoxysilane-tetramethoxysilane copolymer,

[0355] 3-methacryloxypropylmethyldiethoxysilane-tetraethoxysilane copolymer and other methacryloxypropyl-containing copolymers;

[0356] 3-Acryloxypropyltrimethoxysilane-tetramethoxysilane copolymer,

[0357] 3-Acryloxypropyltrimethoxysilane-tetraethoxysilane copolymer,

[0358] 3-Acryloxypropyltriethoxysilane-tetramethoxysilane copolymer,

[0359] 3-Acryloxypropyltriethoxysilane-tetraethoxysilane copolymer,

[0360] 3-Acryloxypropylmethyldimethoxysilane-tetramethoxysilane copolymer,

[0361] 3-Acryloxypropylmethyldimethoxysilane-tetraethoxysilane copolymer,

[0362] 3-Acryloxypropylmethyldiethoxysilane-tetramethoxysilane copolymer,

[0363] 3-acryloxypropylmethyldiethoxysilane-tetraethoxysilane copolymer and other copolymers containing acryloxypropyl;

[0364] Vinyltrimethoxysilane-tetramethoxysilane copolymer,

[0365] Vinyltrimethoxysilane-tetraethoxysilane copolymer,

[0366] Vinyltriethoxysilane-tetramethoxysilane copolymer,

[0367] Vinyltriethoxysilane-tetraethoxysilane copolymer,

[0368] Vinylmethyldimethoxysilane-tetramethoxysilane copolymer,

[0369] Vinylmethyldimethoxysilane-tetraethoxysilane copolymer,

[0370] Vinylmethyldiethoxysilane-tetramethoxysilane copolymer,

[0371] Vinyl-containing copolymers such as vinylmethyldiethoxysilane-tetraethoxysilane copolymer;

[0372] 3-aminopropyltrimethoxysilane-tetramethoxysilane copolymer,

[0373] 3-aminopropyltrimethoxysilane-tetraethoxysilane copolymer,

[0374] 3-aminopropyltriethoxysilane-tetramethoxysilane copolymer,

[0375] 3-aminopropyltriethoxysilane-tetraethoxysilane copolymer,

[0376] 3-aminopropylmethyldimethoxysilane-tetramethoxysilane copolymer,

[0377] 3-aminopropylmethyldimethoxysilane-tetraethoxysilane copolymer,

[0378] 3-aminopropylmethyldiethoxysilane-tetramethoxysilane copolymer,

[0379] Amino group-containing copolymers such as 3-aminopropylmethyldiethoxysilane-tetraethoxysilane copolymer, and the like.

[0380] The silane compounds illustrated above are mostly liquid. The content of the silane compound in the adhesive composition is generally 0.01 mass parts or more and 10 mass parts or less relative to 100 mass parts of (meth) acrylic resin, preferably 0.05 mass parts or more and 5 mass parts or less, more preferably 0.2 mass parts or more and 0.4 mass parts or less. If the content of the silane compound is more than 0.01 mass parts, it is easy to obtain the effect of improving the adhesion of the adhesive layer (first adhesive layer 20) and the optical components such as the glass substrate. In addition, if the content of the silane compound is less than 10 mass parts, it is possible to suppress the silane compound from seeping out of the adhesive layer.

[0381] 〔3-5〕Other ingredients

[0382] The adhesive composition may contain additives such as a crosslinking catalyst, a weathering stabilizer, a tackifier, a plasticizer, a softener, a dye, a pigment, an inorganic filler, light scattering particles, and resins other than (meth) acrylic resins. In addition, an ultraviolet curable compound may be added to the adhesive composition, and after forming the adhesive layer, ultraviolet rays may be irradiated to cure it, thereby forming a harder adhesive layer.

[0383] Examples of the crosslinking catalyst include amine compounds such as hexamethylenediamine, ethylenediamine, polyethyleneimine, hexamethylenetetramine, diethylenetriamine, triethylenetetramine, isophoronediamine, trimethylenediamine, polyamino resins, and melamine resins.

[0384] 〔3-6〕Gel fraction of adhesive layer

[0385] In the polarizing plate with an adhesive layer involved in the present invention, from the viewpoint of achieving both good warping resistance and good heat resistance durability of the laminated optical components, the absolute value of the difference between the gel fraction (hereinafter sometimes referred to as "G80") [%] of the adhesive layer (first adhesive layer 20) after heating at 80°C for 24 hours and the gel fraction (hereinafter sometimes referred to as "G23") [%] at 23°C is greater than 5 percentage points.

[0386] In particular, from the viewpoint of improving the warpage resistance, the absolute value of the difference between G80 [%] and G23 [%] is preferably 10 percentage points or more, more preferably 15 percentage points or more, further preferably 20 percentage points or more, and particularly preferably 50 percentage points or more.

[0387] In order to improve the warpage resistance of the laminated optical component, the heat resistance durability of the laminated optical component, the adhesion between the adhesive layer (first adhesive layer 20) of the laminated optical component and other optical components, etc., the adhesive layer preferably satisfies one or more of the above (A) and (B).

[0388] (A) G23 is 80% or less.

[0389] (B) G80 is 60% or more.

[0390] From the viewpoint of the warpage resistance of the laminated optical member, G80 is preferably 60% or more, more preferably 65% ​​or more, further preferably 70% or more, and is preferably 95% or less, more preferably 90% or less, further preferably 88% or less.

[0391] In addition, from the viewpoint of the warpage resistance of the laminated optical member, G23 is preferably 80% or less. The lower limit of G23 is not particularly limited, but is preferably 5% or more.

[0392] Generally, G80 is larger than G23. G23 and G80 are measured by the method described in the section [Examples] described later.

[0393] For example, there is a tendency that G23 can be reduced by making the adhesive composition forming the adhesive layer contain no crosslinking agent or reducing its content. In addition, there is a tendency that G23 can be reduced by reducing the content of polar functional groups that can react with the crosslinking agent in the (meth) acrylic resin contained in the adhesive composition.

[0394] In addition, the pressure-sensitive adhesive composition containing a (meth)acrylic resin containing a structural unit derived from a (meth)acrylic monomer having a carboxyl group and a structural unit derived from an alkoxyalkyl (meth)acrylamide monomer such as the alkoxyalkyl (meth)acrylamide monomer represented by the above formula (III) is advantageous in terms of improving G80.

[0395] From the viewpoint of improving G80, the (meth)acrylic resin preferably contains a structural unit derived from a (meth)acrylic ester represented by the above formula (I), a structural unit derived from a (meth)acrylic monomer having a hydroxyl group, a structural unit derived from a (meth)acrylic monomer having a carboxyl group, a structural unit derived from a phenoxyethyl-containing (meth)acrylic ester represented by the above formula (II), and a structural unit derived from an alkoxyalkyl (meth)acrylamide monomer such as an alkoxyalkyl (meth)acrylamide monomer represented by the above formula (III).

[0396] [3-7] Formation of adhesive layer

[0397] The adhesive layer (first adhesive layer 20 ) can be obtained by dissolving or dispersing the components constituting the adhesive composition in a solvent to prepare a solvent-containing adhesive composition, applying the solvent-containing adhesive composition on a substrate film or polarizing plate 10 , and drying the solvent.

[0398] The substrate film is generally a thermoplastic resin film, and a typical example thereof is a release film subjected to a release treatment. The release film can be, for example, a release film obtained by subjecting the surface of a film containing a resin such as polyethylene terephthalate, polybutylene terephthalate, polycarbonate, or polyarylate to be formed with a silicone treatment or the like to a release treatment.

[0399] For example, the adhesive composition may be directly applied to the release-treated surface of a separator to form an adhesive layer, and the adhesive layer with the separator may be laminated on the polarizing plate 10 to obtain a polarizing plate with an adhesive layer.

[0400] Alternatively, the adhesive composition may be directly applied to the surface of the polarizing plate 10 to form an adhesive layer, and a separator may be laminated on the outer surface of the adhesive layer as necessary to produce a polarizing plate with an adhesive layer.

[0401] When a pressure-sensitive adhesive layer is provided on the surface of the polarizing plate 10 , the bonding surface of the polarizing plate 10 and / or the bonding surface of the pressure-sensitive adhesive layer is preferably subjected to surface activation treatment such as plasma treatment or corona treatment, and more preferably corona treatment.

[0402] The thickness of the adhesive layer (first adhesive layer 20) is preferably 10 μm to 45 μm, more preferably 10 μm to 30 μm, and further preferably 10 μm to 25 μm. The thickness of the adhesive layer within this range may be advantageous in improving the warpage resistance or heat resistance durability of the laminated optical component, and / or the adhesion between the adhesive layer of the laminated optical component and other optical components.

[0403] <Laminated optical components>

[0404] like Figure 1 to Figure 4 As shown, the laminated optical member is a laminate of the polarizing plate 25 with an adhesive layer and an optical member 30 other than the polarizing plate 25 with an adhesive layer. Generally, the laminated optical member includes the optical member 30 and the polarizing plate 25 with an adhesive layer laminated thereon with the first adhesive layer 20 interposed therebetween.

[0405] According to the pressure-sensitive adhesive layer-attached polarizing plate 25 of the present invention, a laminated optical member having excellent warpage resistance and heat resistance durability can be provided.

[0406] Examples of the optical member 30 include image display elements such as a liquid crystal cell and an organic EL display element.

[0407] The optical member 30 may be a member constituting the above-mentioned image display element, for example, a substrate.

[0408] Examples of the substrate include thermoplastic resin films and glass substrates.

[0409] Example

[0410] The present invention will be described in more detail below with reference to Examples, but the present invention is not limited to these Examples. Hereinafter, parts and % indicating the amount or content are by mass unless otherwise specified.

[0411] <Production Examples 1 to 9: Production of (meth)acrylic resin for adhesive layer>

[0412] A monomer mixture having the monomer composition shown in Table 1 (mass % when the total amount of monomers is 100 mass %) and diluted with ethyl acetate was added to a reaction vessel equipped with a condenser, a nitrogen inlet pipe, a thermometer and a stirrer, and the internal temperature was raised to 55°C while replacing the air in the device with nitrogen to make it oxygen-free. Then, the entire amount of a solution prepared by dissolving azobisisobutyronitrile (polymerization initiator) in ethyl acetate was added. After adding the polymerization initiator, the temperature was maintained for 1 hour, and then, while the internal temperature was maintained at 54-56°C, ethyl acetate was continuously added to the reaction vessel, and the addition of ethyl acetate was stopped at the moment when the concentration of the (meth) acrylic resin reached 35 mass %, and then, the temperature was kept at the same temperature from the start of the addition of ethyl acetate until 12 hours had passed. Finally, ethyl acetate was added and adjusted so that the concentration of the (meth) acrylic resin reached 20 mass %, to prepare an ethyl acetate solution of the (meth) acrylic resin.

[0413] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the obtained (meth)acrylic resin were measured.

[0414] Regarding Mw and Mn, a total of five columns, namely, four "TSKgelXL" columns manufactured by Tosoh Corporation and one "Shodex GPC KF-802" column manufactured by Showa Denko K.K. and sold by Shoko Tsusho Co., Ltd., were connected in series in a GPC apparatus, and tetrahydrofuran was used as an eluent. The measurements were performed in accordance with standard polystyrene conversion under the conditions of a sample concentration of 5 mg / mL, a sample introduction volume of 100 μL, a temperature of 40°C, and a flow rate of 1 mL / min.

[0415] Table 1 summarizes the monomer composition (mass %) of the monomer mixture used, and the Mw and molecular weight distribution (Mw / Mn) of the obtained (meth)acrylic resin.

[0416] [Table 1]

[0417]

[0418] The abbreviations in the column "Monomer composition" in Table 1 refer to the following monomers.

[0419] BA: Butyl acrylate

[0420] MA: Methyl acrylate

[0421] PEA: 2-Phenoxyethyl acrylate

[0422] PEA2: 2-(2-phenoxyethoxy)ethyl acrylate

[0423] HEA: 2-Hydroxyethyl Acrylate

[0424] BMAA: N-Butoxymethylacrylamide

[0425] MEA: Methoxyethyl acrylate

[0426] AA: Acrylic acid

[0427] <Examples 1 to 9, Comparative Examples 1 to 2>

[0428] (1) Preparation of adhesive composition

[0429] A crosslinking agent and a silane compound were mixed in the amounts (parts by mass) shown in Table 2 (there is an example where the crosslinking agent was not mixed) with respect to 100 parts by mass of the solid content of the (meth) acrylic resin obtained in the above production example, and ethyl acetate was added so that the solid content concentration became 28% by mass to prepare a solution of an adhesive composition. In Table 2, the amounts (parts by mass) of the crosslinking agent and the silane compound are expressed in terms of solid content.

[0430] [Table 2]

[0431]

[0432] The crosslinking agent used in the examples and comparative examples was "Coronate L" (trimethylolpropane adduct of toluene diisocyanate in ethyl acetate solution: solid content concentration of 75% by mass) obtained from Tosoh Corporation. In addition, the silane compound used in the examples and comparative examples was "KBM-403" (3-glycidoxypropyltrimethoxysilane) obtained from Shin-Etsu Chemical Co., Ltd.

[0433] (2) Preparation of Adhesive Layer and Measurement of Gel Fraction

[0434] The adhesive composition prepared in the above (1) was applied onto the release-treated surface of a release membrane comprising a polyethylene terephthalate film ["PLR-382190" obtained from LINTEC Co., Ltd.] using a coater in such a manner that the thickness after drying was 20 μm, and dried at 100° C. for 1 minute to prepare an adhesive layer (adhesive sheet).

[0435] The gel fraction [gel fraction at 23°C (G23)] of the adhesive layer (adhesive sheet) left to stand at 23°C for 5 days immediately after it was obtained was measured. The gel fraction was measured according to the following [a] to [d]. The results are shown in Table 3.

[0436] [a] An adhesive layer having an area of ​​about 8 cm×about 8 cm and a metal mesh (the mass thereof is denoted as Wm) formed of SUS304 having an area of ​​about 10 cm×about 10 cm are bonded together.

[0437] [b] The laminate obtained in [a] is weighed and its mass is defined as Ws. Then, it is folded four times so as to enclose the adhesive layer, fixed with a stapler, and weighed. Its mass is defined as Wb.

[0438] [c] The net fixed by the stapler in [b] above was placed in a glass container, 60 mL of ethyl acetate was added and immersed, and the glass container was stored at room temperature for 3 days.

[0439] [d] The web was taken out from the glass container, dried at 120° C. for 4 hours and then weighed. The mass was designated as Wa, and the gel fraction was calculated based on the following formula.

[0440] Gel fraction (mass %) = [{Wa-(Wb-Ws)-Wm} / (Ws-Wm)] × 100

[0441] The gel fraction [gel fraction after heating at 80°C for 24 hours (G80)] was measured in the same manner as above except that the gel fraction was measured for the adhesive layer (adhesive sheet) immediately after being left at 23°C for 5 days and then left in a dry atmosphere at 80°C for 24 hours. The results are shown in Table 3. The difference between G80 and G23 (G80-G23) is also shown in Table 3.

[0442] (3) Preparation of polarizing plate and measurement of maximum curling force at 80°C

[0443] A polarizing plate was prepared by bonding a protective film of 75 μm thick containing a (meth)acrylic resin to one side of a polarizer of 23 μm thick obtained by iodine adsorption orientation on a uniaxially stretched polyvinyl alcohol film via an active energy ray-curable adhesive, and bonding a phase difference film of 50 μm thick containing a cyclic polyolefin resin to the other side via an active energy ray-curable adhesive.

[0444] The maximum curling force of the obtained polarizing plate at 80° C. was measured in the following manner.

[0445] A sample of 40 mm × 40 mm in size was cut from the polarizing plate so that a pair of opposing sides were parallel to the absorption axis of the polarizer. The sample was placed on the main plate of a viscoelasticity measuring device ["Physica MCR301" manufactured by Anton Paar] with the phase difference film side facing up without fixing the sides, and a measuring fixture (PP25) was arranged in the center. The spacing of the measuring fixtures was adjusted so that the stress applied to the measuring fixtures reached about 3 N, and the position raised 0.02 mm from this point was set as the reference height.

[0446] Next, while monitoring the stress applied to the measuring jig, the temperature of the main body plate was raised from 23°C to 80°C at 2°C / min, maintained at 80°C for 240 minutes, and then cooled to 23°C at 2°C / min. The maximum value of the stress applied to the measuring jig accompanying the thermal shrinkage of the sample recorded at this time was defined as the maximum curling force [mN] at 80°C. The maximum curling force at 80°C was 1716mN.

[0447] (4) Preparation of polarizing plate with adhesive layer

[0448] The surface of the adhesive layer prepared in (2) above opposite to the separator (adhesive layer surface) was bonded to the outer surface of the phase difference film of the polarizing plate using a laminator and then cured for 5 days at 23° C. and 65% relative humidity to obtain a polarizing plate with an adhesive layer.

[0449] (5) Evaluation of warpage resistance of laminated optical members

[0450] The polarizing plate with adhesive obtained in the above (4) is cut into a size of 150 mm × 40 mm in such a way that the absorption axis of the polarizer becomes the long side. The separation film is peeled off from the cut polarizing plate with adhesive, and the exposed adhesive layer is bonded to the central part of an alkali-free glass substrate ("Eagle XG" manufactured by Corning) with a length of 160 mm, a width of 50 mm, and a thickness of 0.5 mm, and it is used as a sample. The sample is placed in a dry atmosphere at 80°C for 24 hours. Thereafter, it is taken out in an environment with a temperature of 23°C and a relative humidity of 55%. Within 30 minutes after taking it out, a two-dimensional dimension measuring device ("NEXIV Model: VMZ-R4540" manufactured by Nikon) is used to measure the difference in height from the base between the central part of the polarizing plate of the sample and each corner (4 points) of the polarizing plate. The average value of the obtained 4 values ​​is set as the warping amount [mm] of the sample. The results are shown in Table 3. If the warping amount is less than 2.0 mm, the warping resistance can be evaluated as good.

[0451] (6) Evaluation of heat resistance and durability of laminated optical components

[0452] (6-1) Presence of floating / peeling and foaming at the interface

[0453] After the separator was peeled off from the polarizing plate with adhesive layer prepared in (4), the adhesive layer was bonded to both sides of an alkali-free glass substrate ("Eagle XG" manufactured by Corning Incorporated) to form a crossed Nicol prism to prepare an evaluation sample. The following two heat resistance durability tests were performed using the sample.

[0454] [Heat resistance durability test]

[0455] Heat resistance test at 80°C in dry conditions for 500 hours

[0456] Heat shock resistance (HS) test: 1 cycle is to keep the temperature at 70°C for 30 minutes, then keep the temperature at -40°C for 30 minutes, and repeat this for 200 cycles.

[0457] The samples after each test were visually observed for floating and peeling at the interface between the adhesive layer and the glass substrate, and for foaming of the adhesive layer, and heat resistance durability was evaluated according to the following evaluation criteria. The results are shown in Table 3 (heat resistance durability X in Table 3).

[0458] A: No appearance changes such as floating, peeling, or foaming were observed

[0459] B: Slight changes in appearance such as floating, peeling, and foaming were observed

[0460] C: Clearly observed changes in appearance such as floating, peeling, and foaming

[0461] (6-2) Is there any foaming at the interface end?

[0462] After the separator was peeled off from the polarizing plate with adhesive layer prepared in (4), the adhesive layer was bonded to both sides of an alkali-free glass substrate ("Eagle XG" manufactured by Corning Incorporated) to form a crossed Nicol prism to prepare an evaluation sample. The following two heat resistance durability tests were performed using the sample.

[0463] [Heat resistance durability test]

[0464] Heat resistance test at 80°C in dry conditions for 500 hours

[0465] Heat shock resistance (HS) test: 1 cycle is to keep the temperature at 70°C for 30 minutes, then keep the temperature at -40°C for 30 minutes, and repeat this for 200 cycles.

[0466] The samples after each test were visually observed for the presence of stripe-like bubbles generated at the edge of the interface between the adhesive layer and the glass substrate at the edge of the evaluation sample, and the heat resistance durability was evaluated according to the following evaluation criteria. The results are shown in Table 3 (Heat Resistance Durability Y in Table 3).

[0467] A: No streak-like foaming was observed

[0468] B: Slight streak-like foaming was observed

[0469] C: Stripe-like foaming was clearly observed

[0470] (7) Evaluation of adhesion of laminated optical components

[0471] The polarizing plate with adhesive obtained in the above (4) was cut into a size of 150 mm × 25 mm in such a way that the absorption axis of the polarizer became the long side. The separation film was peeled off from the cut polarizing plate with adhesive, and the exposed adhesive layer was attached to the central part of an alkali-free glass substrate ("Eagle XG" manufactured by Corning) with a length of 160 mm, a width of 50 mm, and a thickness of 0.7 mm. Then, the obtained test piece attached to the glass substrate (polarizing plate with adhesive attached to the glass substrate) was placed in an autoclave at a temperature of 50°C and a pressure of 5 kgf / cm 2 The sample was pressurized at 490.3 kPa for 20 minutes and then stored at 23°C and 55% relative humidity for 24 hours.

[0472] Next, the blade of the cutter was placed between the glass substrate and the adhesive layer, and 30 mm was peeled off from the end in the length direction. The peeled portion was clamped by the clamping part of a universal tensile testing machine [trade name "AGS-50NX" manufactured by Shimadzu Corporation]. The test piece in this state was subjected to a 180-degree peeling test at a clamping moving speed of 300 mm / min in an atmosphere of temperature 23°C and relative humidity 55% according to JIS K 6854-2:1999 "Adhesives - Peel Adhesion Strength Test Method - Part 2: 180-degree peeling", and the average peeling force over a length of 120 mm excluding 30 mm of the clamping part was obtained, and it was set as the adhesion force at a temperature of 23°C. The results are shown in Table 3.

[0473] The adhesion was measured in the same manner as above except that the sample was left in a dry atmosphere at 50° C. for 48 hours and then measured in an atmosphere at a temperature of 23° C. and a relative humidity of 55%, and the result was defined as the adhesion at 50° C. The results are shown in Table 3.

[0474] [Table 3]

[0475]

[0476] Description of Reference Numerals

[0477] 1 polarizing plate, 2 surface treatment layer, 3 first protective film, 4 second protective film, 7 phase difference film, 8 second adhesive layer, 10 polarizing plate, 20 first adhesive layer, 25 polarizing plate with adhesive layer, 30 optical member.

Claims

1. A polarizing plate with an adhesive layer, comprising a polarizing plate having a maximum curling force of 500 mN or more at 80° C. and an adhesive layer laminated on the polarizing plate, The adhesive layer is formed on the entire surface of the polarizing plate and is formed of an adhesive composition containing a (meth)acrylic resin. The (meth)acrylic resin comprises a structural unit derived from a (meth)acrylic monomer having a carboxyl group and a structural unit derived from an alkoxyalkyl (meth)acrylamide monomer. The polarizing plate includes a polarizer and two thermoplastic resin films bonded to both sides of the polarizer. The two thermoplastic resin films are different from each other in the type, thickness, or presence or absence of surface treatment of the thermoplastic resin constituting the films, The absolute value of the difference between the gel fraction G80 of the adhesive layer after heating at 80° C. for 24 hours and the gel fraction G23 at 23° C. is greater than 5 percentage points, The G80 and the G23 are expressed in %.

2. The polarizing plate with an adhesive layer according to claim 1, wherein The adhesive layer has a gel fraction G80 of 60% or more after being heated at 80° C. for 24 hours.

3. The polarizing plate with an adhesive layer according to claim 1 or 2, wherein The adhesive layer has a gel fraction G80 of 95% or less after being heated at 80° C. for 24 hours.

4. The polarizing plate with an adhesive layer according to claim 1 or 2, wherein The polarizing plate includes a polarizer having a thickness of 10 μm or more.

5. The polarizing plate with an adhesive layer according to claim 1, wherein The content of the crosslinking agent in the pressure-sensitive adhesive composition is 0 parts by mass or more and 2 parts by mass or less relative to 100 parts by mass of the (meth)acrylic resin.

Citation Information

Patent Citations

  • Polarizing plate and its production

    JP2000338329A

  • Adhesive composition for optical use

    JP2010229321A

  • Polarizing laminate film, method for manufacturing polarizing plate or polarizing plate with base film, double-sided laminate film, double-sided polarizing laminate film, double-sided bonding film, and single-sided bonding film

    JP2012159778A

  • Adhesive composition for optical components, adhesive for optical components, optical component with adhesive layer, and image display device

    CN103168083A

  • Double-sided pressure-sensitive adhesive sheet, module for touch panel and its manufacturing method