Boron-doped nano-polycrystalline diamond using nano-graphite as carbon source and preparation method thereof

By using nanographite and nanoboron as raw materials to synthesize boron-doped nanopolycrystalline diamond in a domestic hinged six-sided top press, the problems of insufficient performance and high reaction conditions of traditional polycrystalline diamond were solved, and high hardness and The preparation of nano-polycrystalline diamond with impact resistance and toughness is suitable for industrial production and retains the excellent characteristics of diamond.

CN114471365BActive Publication Date: 2024-10-15HENAN LIUMIANDING NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210212132.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-06
Publication Date
2024-10-15
Estimated Expiration
2042-03-06

AI Technical Summary

Technical Problem

Traditional polycrystalline diamond shows insufficient performance in the field of high-precision machining, especially in the fields of aerospace, medical equipment and automobile manufacturing. Moreover, the reaction conditions in the preparation process of boron-doped nano-polycrystalline diamond are high, making it difficult to use domestic equipment. realize industrialized production.

Method used

Using nano-graphite as the carbon source and nano-boron as the boron source, the boron-doped nano-polycrystalline diamond was synthesized in a domestic hinged six-sided top press by the infiltration method, using steps such as chemical purification, ball milling and vacuum heat treatment to avoid Add a sintering agent and use secondary pressure to achieve high-temperature and high-pressure synthesis.

Benefits of technology

The preparation of nano-polycrystalline diamond with high hardness and impact resistance is achieved, which reduces production conditions, is suitable for industrial production, retains the excellent characteristics of diamond to the maximum extent, and provides excellent cutting materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 220306104940
    Figure 220306104940
  • Figure 220306104944
    Figure 220306104944
Patent Text Reader

Abstract

The invention discloses a method for preparing boron-doped nano-polycrystalline diamond using nano-graphite as a carbon source, wherein nano-graphite and nano-boron are used as raw materials to synthesize boron-doped nano-polycrystalline diamond by melt infiltration in a domestic hinged six-sided top press. Compared with conventional nano-polycrystalline diamond prepared from nano-diamond, the boron-doped nano-polycrystalline diamond obtained by the invention has the advantages of high hardness and strong impact toughness, reduced production cost and more in line with industrialized production mode, and can be used as a new generation of high-precision cutting tools.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The patent of this invention relates to the field of high-precision cutting abrasives and grinding tools, specifically a preparation method for synthesizing boron-doped nano-polycrystalline diamond by melt infiltration using nano-graphite and nano-boron as raw materials in a domestic hinged six-sided top press. It is mainly used in the fields of high-precision machining and cutting. Background Art

[0002] Diamond is currently the most ideal cutting tool, but natural diamond is difficult to mine and its reserves are scarce. Therefore, the commonly used diamond is artificially synthesized. Since artificial diamond particles are small and cannot be used directly as cutting tools, they need to be sintered to form larger blocks before they can be used to make tools. People generally sinter diamond micropowders by powder sintering to prepare isotropic diamond polycrystals. However, the preparation of polycrystalline diamond requires the addition of sintering aids such as Fe, Co, Ni and ceramics to ensure that the sintering conditions are within the phase stability region of diamond. This will greatly reduce the performance of the polycrystalline diamond produced by sintering. With the further emergence of emerging materials and the increasing requirements for cutting tools in industrial production, traditional polycrystalline diamond can no longer meet the high-precision machining and cutting requirements in some fields such as aerospace, medical equipment, automobile manufacturing, and military equipment manufacturing. At present, the main research direction is to develop diamond tool materials with excellent performance, so as to promote the development of industrialization.

[0003] The main way to dope polycrystalline diamond with boron is to fully mix a certain proportion of carbon source and boron source, in order to change some physical and chemical properties of polycrystalline diamond and reduce its reaction conditions. Common carbon sources include graphite, carbon nano-onion, C60, amorphous carbon, etc. When the two are fully mixed in the HTHP environment to prepare boron-doped nano-polycrystalline diamond, a higher toughness and stable cutting performance are obtained.

[0004] In the research of various boron-doped nano-polycrystalline diamonds, the preparation of boron-doped nano-polycrystalline diamonds using carbon nano-onions as a carbon source has solved the density problem of most of the internal structures of the polycrystalline, but the actual result of boron doping is not uniform, and the reaction temperature and required pressure are still too high (12-14Gpa), which cannot be carried out in a domestic large-cavity press and is not suitable for industrial production. There are areas with high boron content around the nano-polycrystalline diamond, which greatly reduces the hardness of the nano-polycrystalline diamond. Nanographite as a carbon source has good density and uniformity that other carbon sources do not have, does not require graphitization, and has a simple process flow. Using nano-boron as a doping boron source, which is compatible with nano-graphite, ensures the density of the reaction raw materials and greatly reduces the temperature and pressure conditions required for the nano-polycrystalline diamond reaction. Using nano-graphite as a carbon source to synthesize nano-polycrystalline diamond is a very promising approach, but in fact its reaction mechanism has not been fully explained, and whether the raw materials have an effect on the assembly of the synthetic block needs further discussion. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing boron-doped nano-polycrystalline diamond using nano-graphite as a carbon source.

[0006] The present invention is a method for preparing boron-doped nano-polycrystalline diamond using nano-graphite as a carbon source, which specifically comprises the following steps:

[0007] 1) The nanographite is subjected to surface purification treatment and then sintered at high temperature and high pressure. The obtained material has high strength and wear resistance. The purification treatment method adopted is a chemical method. The nanographite is placed in a solution prepared with dilute hydrochloric acid and dilute sulfuric acid in a certain proportion, stirred, left to stand for a period of time, rinsed with deionized water until neutral, dried and placed in a drying container for use;

[0008] 2) Weigh nanographite and nanoboron, add polyvinyl pyrrolidone dispersant to nanographite and nanoboron respectively, disperse them in ethanol by ultrasound, remove the solvent, and fully dry to obtain dispersed nanographite and nanoboron. Evenly mix the treated nanographite and nanoboron in a high-energy ball mill, with a ball-to-material ratio of 1:1, a mixed material mass of 1.5-2.0g, 10ml of anhydrous ethanol, a rotation speed of 600r / min, and a ball diameter of 2mm; add alcohol every 10min during the ball milling process, and stop the ball milling after 30min; open the ball mill, wait for the alcohol to evaporate, put the mixture of nanographite powder and nanoboron powder into a graphite cup, and then place the loaded graphite cup in a vacuum furnace for vacuum heat treatment to remove oxygen and water vapor adsorbed on the surface of the powder and make its surface have better reaction activity; during the heating period, the maximum temperature in the vacuum furnace is 350℃, and the vacuum degree is 3×10-3Pa;

[0009] 3) The mixed powder obtained in step 2) is first cold pressed and then hot pressed and sintered, and the mixed powder material obtained in step 2) is pressed into tablets in a press machine, and the tablets are placed in a magnesium oxide hexahedral block;

[0010] 4) Assembly process of domestic hinged six-sided top press: The six-sided top press experiment selected is 10-3 assembly, and the sealing edge is made by MDX-540 model engraving machine; the heating tube is made of metal rhenium; the samples are loaded in sequence; after the samples are loaded, the sealing edge and the magnesium oxide hexahedral block assembly block are first assembled into eight cubic tungsten carbide blocks in sequence; the cube composed of eight cubic blocks is placed in a cubic cavity composed of six hard steel wedge blocks, and the temperature is raised to 400bar in 20 hours, and then heated. The heating method is to heat according to the power percentage input, and then use the secondary pressurization method to synthesize diamond at high temperature and high pressure, and slowly release the pressure after heating is completed;

[0011] In step 1), the mixing ratio of dilute hydrochloric acid and dilute sulfuric acid is 1:3;

[0012] In step 1), the concentration of dilute sulfuric acid is 3 mol / L, and the concentration of dilute hydrochloric acid is 1.4 mol / L;

[0013] In step 2), the mass fraction of nano-graphite is 80-90wt%, and the mass fraction of nano-boron is 15-20wt%;

[0014] In step 4), the specific process conditions for synthesizing boron-doped nano-polycrystalline diamond at high temperature and high pressure are: first, pressurize to 2.5-2.8 GPa, and heat to 432-460 K, then unload the pressure to 0.9-1.1 GPa, and keep the temperature at 432-460 K for 500-520 s, then increase the pressure to 6.5-7.5 GPa, and heat to 1600-1700 K, and keep the pressure for 15 hours to synthesize boron-doped nano-polycrystalline diamond;

[0015] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0016] 1) The present invention is the first to synthesize boron-doped nano-polycrystalline diamond in one step in a hinged six-sided top press by melt infiltration method using nano-graphite as a carbon source and nano-boron as a boron source. The reaction materials are weighed and processed and mixed according to the designed mass ratio of carbon content and boron content without introducing other side reactions. The reaction is more stable under high temperature and high pressure through secondary pressurization, and the time required to generate the required substances is constant, thereby realizing the controllable preparation of boron-doped nano-polycrystalline diamond.

[0017] 2) Compared with the traditional synthesis of diamond polycrystals using sintering agents, the boron-doped nano-polycrystalline diamond prepared by the present invention does not add any sintering agent during the sintering process, thereby retaining the excellent properties of diamond as a cutting tool to the greatest extent.

[0018] 3) The boron-doped nano-polycrystalline diamond prepared by the present invention uses a large hinged six-sided top press chamber, which is conducive to industrial production. While improving the toughness of the nano-polycrystalline diamond, the hardness of the nano-polycrystalline diamond is better retained, the production conditions of the boron-doped nano-polycrystalline diamond are greatly reduced, and the surface activity of the nano-polycrystalline diamond is changed, thereby obtaining a better cutting material. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a schematic diagram of the magnesium oxide assembly block structure in the prior art.

[0020] Figure 2 This is an electron microscope image of boron-doped nano-polycrystalline diamond.

[0021] Among them: 1-conductive ring; 2-titanium sheet; 3-molybdenum cup; 4-carbon tube; 5-dolomite core;

[0022] 6-dolomite tube; 7-nano carbon-boron mixture; 8-composite material; 9-pyrophyllite block. DETAILED DESCRIPTION

[0023] The present invention is further described below by way of examples, but the embodiments of the present invention are not limited thereto.

[0024] The nano-graphite and nano-boron involved in the following embodiments are all commercially available products.

[0025] Embodiment 1:

[0026] A method for preparing boron-doped nano-polycrystalline diamond using nano-graphite as a carbon source comprises the following steps:

[0027] 1) The nanographite is subjected to surface purification treatment and then sintered at high temperature and high pressure. The obtained material has high strength and wear resistance. The purification method adopted is a chemical method. The nanographite is placed in a solution of 1.4 mol / L dilute hydrochloric acid and 3 mol / L dilute sulfuric acid in a ratio of 1:3, stirred, left to stand for a period of time, rinsed with deionized water until neutral, dried and placed in a drying container for use;

[0028] 2) Weigh the nanographite and nanoboron with a mass fraction of 80-90wt% and 15-20wt% respectively obtained in step 1, wherein polyvinyl pyrrolidone dispersant is added to the nanographite and nanoboron respectively, dispersed in ethanol by ultrasound, the solvent is removed, and the dispersed nanographite and nanoboron are obtained by drying. The treated nanographite and nanoboron are uniformly mixed in a high-energy ball mill, the ball milling adopts a ball-to-material ratio of 1:1, the mass of the mixed material is 1.5-2.0g, anhydrous ethanol is 10ml, the speed is 600r / min, and the ball diameter is 2mm; alcohol is added every 10min during the ball milling process, and the ball milling is stopped after 30min of ball milling; after opening the ball milling jar, wait for the alcohol to evaporate, and put the mixture of nanographite powder and nanoboron powder into a graphite cup, and then place the loaded graphite cup in a vacuum furnace for vacuum heat treatment to remove oxygen and water vapor adsorbed on the surface of the powder and make its surface have better reaction activity; during the heating period, the maximum temperature in the vacuum furnace is 350℃, and the vacuum degree is 3×10 -3 Pa;

[0029] 3) The mixed powder obtained in step 2) is first cold pressed and then hot pressed and sintered, and the mixed powder material obtained in step 2) is pressed into tablets in a press machine, and the tablets are placed in a magnesium oxide hexahedral block;

[0030] 4) Assembly process of domestic hinged six-sided top press: The six-sided top press experiment selected is 10-3 assembly, the sealing edge is made by MDX-540 model engraving machine; the heating tube is made of metal rhenium; the samples are loaded in sequence; after the samples are loaded, the sealing edge and the magnesium oxide hexahedron block assembly block are first assembled into eight cubic tungsten carbide blocks in sequence; the cube composed of eight cubic blocks is placed in a cubic cavity composed of six hard steel wedge blocks, raised to 400 bar in 20 hours, and then heated, and the heating method is based on the power percentage The input is heated, and then the high temperature and high pressure diamond synthesis is carried out by secondary pressurization. First, the pressure is increased to 2.5-2.8GPa, and the temperature is increased to 432-460K, and then the pressure is reduced to 0.9-1.1GPa, and the temperature is maintained at 432-460K for 500-520s, and then the pressure is increased to 6.5-7.5GPa, and the temperature is increased to 1600-1700K at the same time, and the pressure is maintained for 15h. After the heating is completed, the pressure is slowly reduced and cooled. After the temperature in the chamber drops to 430K, the assembly block is taken out and the synthesis rod is taken out;

[0031] After testing, the Vickers hardness of boron-doped nano-polycrystalline diamond reached 64.53Gpa and the impact toughness reached 91.7Mpa.

[0032] The purpose of the present invention is to obtain boron-doped nano-polycrystalline diamond which has the advantages of high hardness and strong impact toughness, reduces production costs and is more in line with industrial production models. Therefore, in the preparation process of boron-doped nano-polycrystalline diamond, it is very meaningful to use nano-graphite as a carbon source compared with nano-diamond as a carbon source.

Claims

1. A method for preparing boron-doped nano-polycrystalline diamond using nano-graphite as a carbon source, characterized in that: The preparation method comprises the following steps: 1) The surface of the nanographite is purified by a chemical method, in which the nanographite is placed in a solution prepared with dilute hydrochloric acid and dilute sulfuric acid in a certain proportion, stirred, allowed to stand for a period of time, rinsed with deionized water until neutral, dried, and placed in a drying container for standby use; 2) weighing nano graphite and nano boron, the mass fraction of nano graphite is 80wt%, and the mass fraction of nano boron is 20wt%; wherein polyvinyl pyrrolidone dispersant is added to nano graphite and nano boron respectively, dispersed in ethanol by ultrasonic, the solvent is removed, and the dispersed nano graphite and nano boron are fully dried; the treated nano graphite and nano boron are uniformly mixed in a high energy ball mill, the ball milling adopts a ball-to-material ratio of 1:1, the mass of the mixed material is 1.5-2.0g, 10ml of anhydrous ethanol, a speed of 600r / min, and a ball diameter of 2mm; alcohol is added every 10min during the ball milling process, and the ball milling is stopped after 30min of ball milling; after opening the ball milling jar, the alcohol is evaporated, and the mixture of nano graphite powder and nano boron powder is loaded into a graphite cup, and then the loaded graphite cup is placed in a vacuum furnace for vacuum heat treatment to remove oxygen and water vapor adsorbed on the surface of the powder and make the surface have better reaction activity; during the heating period, the maximum temperature in the vacuum furnace is 350°C, and the vacuum degree is 3×10 -3 Pa; 3) The mixed powder obtained in step 2) is first cold pressed and then hot pressed and sintered, and the mixed powder material obtained in step 2) is tableted in a press machine, and the tablets are placed in a magnesium oxide hexahedral block; 4) Assembly process of domestic hinged six-sided top press: The six-sided top press experiment selected is 10-3 assembly, and the sealing edge is made by MDX-540 model engraving machine; the heating tube is made of metal rhenium; the samples are loaded in sequence; after the samples are loaded, the sealing edge and the magnesium oxide hexahedral block assembly block are first assembled into eight cubic tungsten carbide blocks in sequence; the cube composed of eight cubic blocks is placed in a cubic cavity composed of six hard steel wedge blocks, and the pressure is raised to 400bar in 20 hours, and then heated. The heating method is to heat according to the power percentage input, and then use the secondary pressurization method to synthesize diamond at high temperature and high pressure, and slowly release the pressure after heating is completed; In step 4), the specific high temperature and high pressure process conditions for synthesizing boron-doped nano-polycrystalline diamond are: first, pressurize to 2.5-2.8GPa, and heat to 432-460K, then unload the pressure to 0.9-1.1GPa, keep the temperature at 432-460K for 500-520s, then increase the pressure to 6.5-7.5GPa, and heat to 1600-1700K at the same time, and maintain the pressure for 15h to synthesize boron-doped nano-polycrystalline diamond.

2. The preparation method according to claim 1, characterized in that: In step 1), the mixing ratio of dilute hydrochloric acid and dilute sulfuric acid is 1:

3.

3. The preparation method according to claim 1, characterized in that: In step 1), the concentration of dilute sulfuric acid is 3 mol / L, and the concentration of dilute hydrochloric acid is 1.4 mol / L.