A polyglycolic acid graft copolymer with high thermal stability and its preparation method and application

By modifying polyglycolic acid through graft copolymerization, a polyglycolic acid graft copolymer with high thermal stability is formed, which solves the problem of poor thermal stability of polyglycolic acid and improves its thermal stability and melt processing performance.

CN114478932BActive Publication Date: 2024-11-05CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111148082.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-10-28
Filing Date
2021-09-29
Publication Date
2024-11-05
Estimated Expiration
2041-09-29

AI Technical Summary

Technical Problem

Polyglycolic acid has poor thermal stability and is prone to thermal degradation during processing, especially in the high temperature and high humidity environment of summer, which affects its performance and storage and transportation conditions.

Method used

By graft copolymerization, monomers or oligomers with α- and β-unsaturated groups are grafted onto the polyglycolic acid backbone to form polyglycolic acid graft copolymers with high thermal stability, thereby improving their thermal stability.

Benefits of technology

It effectively improves the thermal stability of polyglycolic acid, increasing its 5% thermal weight loss temperature by at least 10°C, and improves its melt processing performance, making it suitable for processing a variety of polymer materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114478932B_ABST
    Figure CN114478932B_ABST
Patent Text Reader

Abstract

The present invention relates to a polyglycolic acid graft copolymer with high thermal stability in the field of polymer materials, and a preparation method and application thereof. The polyglycolic acid graft copolymer with high thermal stability has a main chain of a polyglycolic acid homopolymer or a copolymer of glycolide and other cyclic monomers, and a side chain of at least one of a monomer derivative, an oligomer or a polymer generated by graft polymerization. The main chain of the polyglycolic acid graft copolymer accounts for 80 to 99% of the total mass of the polyglycolic acid graft copolymer, and the side chain accounts for 1 to 20% of the total mass of the polyglycolic acid graft copolymer. The polyglycolic acid resin of the present invention is excellent in melt processability and the like, and is suitable for use as polymer materials such as sheets, films, fibers, blow-molded products, composite materials, and other molded products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polymer materials, and more particularly to a polyglycolic acid graft copolymer with high thermal stability and a preparation method and application thereof. Background Art

[0002] Polyglycolic acid (PGA), also known as polyglycolic acid and polyhydroxyacetic acid, is the simplest linear aliphatic polyester. The polyglycolic acid (PGA) can be obtained by melt polycondensation of glycolic acid, dealcoholization polycondensation of glycolic acid alkyl esters, desalination polycondensation of glycolates, direct condensation polymerization of glycolic acid / esters, or by glycolide ring-opening polymerization. Polyglycolic acid is a typical high-crystallinity polymer with a stable lattice and a high melting point. However, its thermal degradation temperature is close to its melting point, and it is prone to degradation during molding and processing. The processing temperature range is much narrower than other biodegradable materials, which affects its performance. PGA is very easy to absorb water and degrade, has poor stability, and has harsh storage and transportation conditions, which increases costs, especially in high temperature and high humidity environments in summer.

[0003] Polyglycolic acid has excellent biodegradability. It can enter the human circulatory system to be degraded in the body and excreted from the body. It can also be degraded in the in vitro environment. It is mainly used in medical sutures, drug controlled release carriers, fracture fixation materials, tissue engineering scaffolds, reinforcement materials, etc. Through solution spinning and melt spinning, polyglycolic acid can be processed into surgical sutures with strong tensile strength and can maintain sufficient time, which is suitable for suturing deep tissue wounds.

[0004] Japanese patent JP2012040688A discloses a laminated multilayer film having an outer layer made of polylactic acid, an adhesive layer made of aliphatic-aromatic polyester and a layer made of polyglycolide. CN105793040A discloses a biodegradable polyester mixture composed of 55-90% by weight of polyglycolide and 10-45% by weight of a degradable polyester (formed by aliphatic or aliphatic and aromatic dicarboxylic acids and aliphatic diols) to prepare a barrier film for food or beverage packaging. CN1160584A discloses a blend containing polyglycolide for preparing a coating containing animal growth hormone. CN107556536A discloses a low-cost bio-based fully degradable film of polyglycolide / thermoplastic starch / polybutylene adipate terephthalate. However, there is currently no method for improving its thermal stability. Summary of the invention

[0005] In order to solve the problem that polyglycolic acid in the prior art has poor thermal stability and is prone to thermal degradation during processing, the present invention proposes a polyglycolic acid graft copolymer with high thermal stability. Specifically, it relates to a polyglycolic acid graft copolymer with high thermal stability and its preparation method and application. The polyglycolic acid graft copolymer is modified by grafting a monomer, oligomer or polymer having at least one α, β-unsaturated group, and the reactive group is grafted onto the polyglycolic acid main chain. The thermal stability of the polyglycolic acid graft copolymer can be effectively improved, and its 5% thermal weight loss temperature can be increased by at least about 10°C, and the performance is better than the existing similar polyglycolic acid.

[0006] One of the purposes of the present invention is to provide a polyglycolic acid graft copolymer with high thermal stability, wherein the main chain is a polyglycolic acid homopolymer or a copolymer of glycolide and other cyclic monomers, and the side chain is at least one of a monomer derivative, an oligomer or a polymer generated by graft polymerization.

[0007] In the above technical solution, the main chain of the polyglycolic acid graft copolymer accounts for 80 to 99% of the total mass of the polyglycolic acid graft copolymer, and the side chain accounts for 1 to 20% of the total mass of the polyglycolic acid graft copolymer.

[0008] In some specific technical solutions of the present invention, the main chain of the polyglycolic acid graft copolymer is a polyglycolic acid homopolymer.

[0009] In some specific technical solutions of the present invention, the main chain of the polyglycolic acid graft copolymer is a copolymer of glycolide and other cyclic monomers. The cyclic monomers include at least one of lactide, butyrolactone, valerolactone, caprolactone, caprolactam, enantholactone, capryllactone, capryllactam, etc.

[0010] In the above technical solution, the side chain of the polyglycolic acid graft copolymer is a graft-polymerized monomer derivative, oligomer or polymer having at least one α, β-unsaturated group.

[0011] In the above technical solution, the α, β-unsaturated groups in the side chains of the polyglycolic acid graft copolymer are at least one of vinyl groups, acrylate groups, methacrylate groups, allyl groups, acetylene groups, and the like.

[0012] in,

[0013] The monomer derivative, oligomer or polymer of the side chain of the polyglycolic acid graft copolymer carries at least one polar group, and the polar group is selected from at least one of hydroxyl, carboxyl, carbonyl, ester, amino, thiol, sulfonic acid, ether bond, halogen, peptide bond, anhydride bond, etc.

[0014] The α, β-unsaturated groups of the monomer derivatives, oligomers or polymers of the side chains of the polyglycolic acid graft copolymer can be at least one of maleic anhydride, acrylic acid, methacrylic acid, acrylates, methacrylates, acrylamides and methacrylamides. The side chain monomer can react with polyglycolic acid under certain conditions by free radicals, and then be covalently grafted onto the main chain of the polyglycolic acid molecule to generate a new chemical composition and a polyglycolic acid graft copolymer with a side chain, which has a special modification effect. More preferably, the side chain monomer is at least one of glycidyl methacrylate (GMA), diethyl maleate, etc.

[0015] In the technical solution of the present invention,

[0016] The polyglycolic acid graft copolymer with high thermal stability can be obtained by graft polymerization reaction of the following components in percentage by mass:

[0017] (1) 80-99% polyglycolic acid homopolymer or copolymer of glycolide and other cyclic monomers;

[0018] (2) 1 to 20% of at least one of a monomer, oligomer or polymer having at least one α, β-unsaturated group;

[0019] (3) 0.05-2% free radical initiator;

[0020] The mass ratio of the (3) free radical initiator to the (2) monomer, oligomer or polymer having at least one α, β-unsaturated group is ≤0.3:1, preferably (0.01-0.3):1, and more preferably (0.02-0.2):1.

[0021] Wherein, the amount of the polyglycolic acid homopolymer or the copolymer of glycolide and other cyclic monomers may be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 98.5%, 98.6%, 98.7%, 98.8%, 98.9% or any value in between the above values;

[0022] The amount of the monomer, oligomer or polymer having at least one α, β-unsaturated group may be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 19.5%, 19.6%, 19.7%, 19.8%, 19.9% ​​or any value between the above values;

[0023] The amount of the free radical initiator may be 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0% or any value therebetween;

[0024] Preferably, the polyglycolic acid graft copolymer with high thermal stability can be obtained by graft polymerization reaction of the following components in percentage by mass:

[0025] (1) 90-97% polyglycolic acid homopolymer or copolymer of glycolide and other cyclic monomers;

[0026] (2) 2 to 10% of at least one of a monomer, oligomer or polymer having at least one α, β-unsaturated group;

[0027] (3) 0.1-1% free radical initiator.

[0028] The amount of the polyglycolic acid homopolymer or the copolymer of glycolide and other cyclic monomers may be 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97% or any value between the above values;

[0029] The amount of the monomer, oligomer or polymer having at least one α, β-unsaturated group can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 9.5%, 9.6%, 9.7%, 9.8%, 9.9% or any value in between.

[0030] The amount of the free radical initiator can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0% or any value in between.

[0031] In the above technical solution, the polyglycolic acid graft copolymer with high thermal stability has a thermal decomposition temperature increased by at least 10°C compared with the polyglycolic acid without reaction grafting, thereby improving its melt stability and thus improving the melt processing of polyglycolic acid.

[0032] The 5% thermal weight loss temperature of the polyglycolic acid graft copolymer can be at least 10° C. higher than that of the ungrafted polyglycolic acid.

[0033] In the above technical solution, the initiator may be a free radical initiator, which is an organic compound that can decompose to generate free radicals under certain conditions, including but not limited to: at least one of acyl peroxide, alkyl peroxide, aromatic substituted alkyl peroxide, perester, alkyl hydroperoxide, ketone peroxide, azo compounds, etc. The alkyl peroxide is preferably a dialkyl peroxide; the aromatic substituted alkyl peroxide is preferably an aromatic substituted dialkyl peroxide.

[0034] The free radicals generated by the decomposition of the initiator attack the methylene group on the main chain of polyglycolic acid, making the main chain carbon as a grafting site, forming a polyglycolic acid main chain free radical initiator monomer grafting, and forming a polymer of the grafted monomer to form a polyglycolic acid resin containing a grafted chain segment. At the same time, the free radicals formed by the decomposition will annihilate the catalyst remaining in the synthesis process of polyglycolic acid and the free radicals decomposed by the end group, thereby preventing the degradation of polyglycolic acid and improving its stability.

[0035] Preferably,

[0036] The acyl peroxide may be selected from benzoyl peroxide (BPO); and / or,

[0037] The alkyl peroxide or aromatic hydrocarbon-substituted alkyl peroxide may be selected from at least one of di-tert-butyl peroxide, diisopropylphenyl peroxide, isopropylphenyl peroxide butyl, 3,3,5-trimethylcyclohexane-1,1-diperoxy-tert-butyl, 2,5-di-tert-butyl peroxyhexane, etc.; and / or,

[0038] The perester may be selected from at least one of tert-butyl perpivalate, tert-butyl per-2-ethylhexanoate, tert-butyl perbenzoate, dodecanoic acid peroxide, etc.; and / or,

[0039] The alkyl hydroperoxide may be selected from at least one of tert-butyl hydroperoxide, cumene hydroperoxide, etc.; the ketone peroxide may be selected from methyl ethyl ketone peroxide; and / or,

[0040] The azo compound can be selected from azobisisobutyronitrile (AIBN) and the like.

[0041] In the above technical solution, the initiator is preferably at least one of benzoyl peroxide, azobisisobutyronitrile, diisopropylbenzene peroxide, di-tert-butyl peroxide, tert-butyl hydroperoxide, benzoic acid peroxide, 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane, etc. More preferably, the initiator is at least one of diisopropylbenzene peroxide, benzoic acid peroxide, 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane, etc.

[0042] In some specific embodiments of the present invention, the polyglycolic acid resin may further contain a functional additive accounting for 0.1 to 2% of the total mass of the polyglycolic acid resin.

[0043] In the above technical solution, the functional additives can be selected from the common functional additives in the field of plastic modification and processing, preferably at least one of a compatibilizer, an antioxidant, a light stabilizer, an anti-blocking agent, a release agent, a pigment, an inorganic filler, etc.

[0044] The second object of the present invention is to provide a method for preparing the polyglycolic acid graft copolymer with high thermal stability. The polyglycolic acid resin obtained by this method can effectively improve its thermal stability and increase its 5% thermal weight loss temperature by at least about 10°C, and its performance is better than that of existing similar polyglycolic acids.

[0045] The preparation method may include the following steps:

[0046] The components including the polyglycolic acid homopolymer or copolymer of glycolide and other cyclic monomers, monomers, oligomers or polymers having at least one α, β-unsaturated group, and a free radical initiator are melt-blended and reacted and extruded to obtain the polyglycolic acid graft copolymer with high thermal stability.

[0047] Specifically, melt blending reaction extrusion can be used to uniformly mix the required amounts of the components in a molten state to obtain the polyglycolic acid resin with high thermal stability.

[0048] in,

[0049] The method is preferably a twin-screw continuous extrusion method.

[0050] The method preferably comprises mixing the components including the polyglycolic acid homopolymer or copolymer of glycolide and other cyclic monomers, monomers, oligomers or polymers having at least one α, β-unsaturated group, and a free radical initiator in a desired proportion and then adding the mixture to a twin-screw extruder for extrusion granulation.

[0051] The method preferably comprises metering the components including the polyglycolic acid homopolymer or copolymer of glycolide and other cyclic monomers, monomers, oligomers or polymers having at least one α, β-unsaturated group, and free radical initiators into a twin-screw extruder according to a certain feeding ratio for extrusion granulation.

[0052] The temperature of the reactive extrusion may be 160°C-280°C, more preferably 180-260°C; and / or,

[0053] The screw speed may be 50 rpm-1200 rpm, more preferably 100 rpm-500 rpm.

[0054] The continuous twin-screw extruder equipment suitable for the present invention includes twin-screw extruders of different designs, such as ZSKMcc18 or ZSK40 co-rotating parallel twin-screw extruders produced by Coperion of Germany.

[0055] The third object of the present invention is to provide a polyglycolic acid graft copolymer resin with high thermal stability obtained by the preparation method.

[0056] A fourth object of the present invention is to provide the application of the polyglycolic acid graft copolymer with high thermal stability in applications with higher thermal stability, such as specific applications in melt processing, such as specific applications in blown film, cast film, multilayer film, sheet, fiber, and injection molded products.

[0057] Polyglycolic acid is prone to degradation and gas generation during melt processing, so its melt stability is insufficient, and the temperature difference between the decomposition temperature and the melting temperature (T d -T m ) is small, which is not conducive to melt processing and affects the quality of the product. The polyglycolic acid resin of the present invention has excellent melt processability and is suitable for use as polymer materials such as sheets, films, fibers, blow molded products, composite materials, and other molded products. In the above technical solution, the application is not particularly limited, for example, but not limited to, it has a wide range of applications in medicine, daily necessities, packaging, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 Thermogravimetric analysis curves of the particles prepared in Examples 1 to 4 and Comparative Examples 1 to 2;

[0059] Figure 2 The first cooling curve of the particles prepared in Examples 1 to 4 and Comparative Examples 1 to 2;

[0060] Figure 3 The second heating curve of the particles prepared in Examples 1 to 4 and Comparative Examples 1 to 2;

[0061] Figure 4 The first temperature rise curve of the thin film prepared by hot pressing into film and then immersing in liquid nitrogen and rapidly cooling the film in Examples 3 and 4 and Comparative Example 1;

[0062] Figure 5 IR spectra of the graft copolymer prepared in Example 4 and the unmodified PGA in Comparative Example 1. DETAILED DESCRIPTION

[0063] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0064] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0065] Source of raw materials

[0066] The raw materials used in the present invention are all commercially available.

[0067] Polyglycolic acid (PGA), Corbin Purac.

[0068] Glycidyl methacrylate, Chinese medicine reagent grade.

[0069] 2,5-Dimethyl-2,5-bis(tert-butylperoxy)hexane, Chinese medicine reagent grade.

[0070] Dicumyl peroxide, Jiangsu Daoming Chemical Co., Ltd.

[0071] Styrene, Chinese medicine reagent grade.

[0072] Polyethylene glycol methyl acrylate (PEGMA), relative molecular weight about 500 g / mol, Sigma-Aldrich Company.

[0073] The present invention performs performance measurement according to the following method:

[0074] Thermal performance analysis (DSC): The test was conducted on a Discovery series differential scanning calorimeter (DSC) produced by TA Instruments, and the processing software was TA Instruments Trios version 3.1.5. The DSC instrument was equipped with a Refrigerated Cooling System 90 mechanical refrigeration accessory. The test atmosphere was 50mL / min of nitrogen, and the sample amount required for the test was 5-10mg. The test procedure was as follows: first stabilize the temperature at 40°C, then increase the temperature to 260°C at 10°C / min and keep the temperature constant for 2min, then cool down to -60°C at 10°C / min and keep the temperature constant for 2min, examine the crystallization performance of the particles or films, and then increase the temperature to 260°C at 10°C / min. Record the first heating and cooling process and the second heating process.

[0075] Thermogravimetric analysis (TGA): The test was conducted on a Discovery series thermogravimetric analyzer from THERMAL ANALYSIS, using TA Instruments Trios 3.1.4 software. Before the test, the machine was preheated until the temperature of the balance cavity was stable at 40°C. During the test, 5 to 10 mg of sample was weighed and placed in a ceramic crucible. The test was conducted in an air atmosphere with a flow rate of 20 mL / min. The temperature rise range was 30 to 600°C, and the heating rate was 10°C / min. The weight loss curve of the sample was recorded.

[0076] Melt Flow Rate (MFR): According to ISO 1133 standard, using Lloyd DAVENPORT TM The measurement was performed using an MFI-10 / 230 melt indexer with a barrel temperature of 230°C, a weight load of 1.05kg, a die diameter of 2.095mm, a length of 8mm, a preheating time of 300s, and automatic sample cutting at set intervals. The average value was taken 5 times and the measurement results were expressed in grams per 10 minutes (g / 10min).

[0077] [Example 1]

[0078] The polyglycolic acid (PGA) used in the present invention is from Corbin Purac. The monomer glycidyl methacrylate is of Chinese medicine reagent grade. The initiator is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, of Chinese medicine reagent grade. The three are pre-blended in a mass ratio of 97.9:2:0.1, and the blend is prepared using PolyLab HAAKE from Thermo Fisher Scientific, USA. TMRheomex OS PTW16 co-rotating twin-screw extruder (screw diameter 16mm, L / D=40) was used for extrusion granulation. The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. After calibration, the feeder is used to feed the PGA blend into the twin screws at a feed rate of 2000g / hr. The temperatures of sections 2-11 of the extruder are 200°C, 220°C, 230°C, 230°C, 240°C, 250°C, 250°C, 240°C, 230°C and 220°C, respectively. The screw speed is set at 200rpm and the torque is 7.5-8.5Nm. The extruder is equipped with a circular die with a diameter of 3 mm. After the sample strip is extruded from the die and air-cooled, it is cut into cylindrical yellow particles with a length of about 3 mm by a pelletizer, namely PGA modified particles A. The melt index thereof is measured to be 14.6 g / 10 min. The particles are collected and packaged for later use.

[0079] [Example 2]

[0080] The polyglycolic acid (PGA) used in the present invention is from Corbin Purac. The monomer diethyl maleate is of Chinese medicine reagent grade. The initiator is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, of Chinese medicine reagent grade. The three are pre-blended in a mass fraction of 97.8:2:0.2, and the blend is prepared using PolyLabHAAKE from Thermo Fisher Scientific, USA. TM Rheomex OS PTW16 co-rotating twin-screw extruder (screw diameter 16mm, L / D=40) was used for extrusion granulation. The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. After calibration, the feeder is used to feed the PGA blend into the twin screws at a feed rate of 2000g / hr. The temperatures of sections 2-11 of the extruder are 200°C, 220°C, 230°C, 230°C, 240°C, 250°C, 250°C, 240°C, 230°C and 220°C, respectively. The screw speed is set at 200rpm and the torque is 6-7Nm. The extruder is equipped with a circular die with a diameter of 3 mm. After the sample strip is extruded from the die and air-cooled, it is cut into cylindrical yellow particles with a length of about 3 mm by a pelletizer, namely PGA modified particles B. The melt index is measured to be 134 g / 10 min. The particles are collected and packaged for later use.

[0081] [Example 3]

[0082] The polyglycolic acid (PGA) used in the present invention is from Corbin Purac. The monomer diethyl maleate is of Chinese medicine reagent grade. The initiator is dicumyl peroxide (DCP). The three are pre-blended in a mass ratio of 97.8:2:0.2, and the blend is prepared using PolyLab HAAKE from Thermo Fisher Scientific, USA. TM Rheomex OS PTW16 co-rotating twin-screw extruder (screw diameter 16mm, L / D=40) was used for extrusion granulation. The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. After calibration, the feeder is used to feed the PGA blend into the twin screws at a feed rate of 2000g / hr. The temperatures of sections 2-11 of the extruder are 200°C, 220°C, 230°C, 230°C, 240°C, 250°C, 250°C, 240°C, 230°C and 220°C, respectively. The screw speed is set at 200rpm and the torque is 6-7Nm. The extruder is equipped with a circular die with a diameter of 3 mm. After the sample strip is extruded from the die and air-cooled, it is cut into cylindrical yellow particles with a length of about 3 mm by a pelletizer, namely PGA modified particles C. The melt index is measured to be 30 g / 10 min. The particles are collected and packaged for later use.

[0083] [Example 4]

[0084] The polyglycolic acid (PGA) used in the present invention is from Corbin Purac. The monomer glycidyl methacrylate is of Chinese medicine reagent grade. The initiator is dicumyl peroxide (DCP). The three are pre-blended in a mass ratio of 95.6:4:0.4, and the blend is prepared using PolyLab HAAKE from Thermo Fisher Scientific, USA. TM Rheomex OSPTW16 co-rotating twin-screw extruder (screw diameter 16mm, L / D=40) was used for extrusion granulation. The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. After calibration, the feeder is used to feed the PGA blend into the twin screws at a feed rate of 2000g / hr. The temperatures of sections 2-11 of the extruder are 200°C, 220°C, 230°C, 230°C, 240°C, 250°C, 250°C, 240°C, 230°C and 220°C, respectively. The screw speed is set at 200rpm and the torque is 6-7Nm. The extruder is equipped with a circular die with a diameter of 3 mm. After the sample strip is extruded from the die and air-cooled, it is cut into cylindrical yellow particles with a length of about 3 mm by a pelletizer, namely PGA modified particles D. The melt index is measured to be 19.8 g / 10 min. The particles are collected and packaged for later use.

[0085] [Example 5]

[0086] The polyglycolic acid (PGA) used in the present invention is from Corbin Purac. The monomer styrene is of Chinese medicine reagent grade. The initiator is dicumyl peroxide (DCP). The three are pre-blended in a mass ratio of 97.8:2:0.2, and the blend is prepared using PolyLab HAAKE from Thermo Fisher Scientific, USA. TM Rheomex OS PTW16 co-rotating twin-screw extruder (screw diameter 16mm, L / D=40) was used for extrusion granulation. The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. After calibration, the feeder is used to feed the PGA blend into the twin screws at a feed rate of 2000g / hr. The temperatures of sections 2-11 of the extruder are 200°C, 220°C, 230°C, 230°C, 240°C, 250°C, 250°C, 240°C, 230°C and 220°C, respectively. The screw speed is set at 200rpm and the torque is 6-7Nm. The extruder is equipped with a circular die with a diameter of 3 mm. After the sample strip is extruded from the die and air-cooled, it is cut into cylindrical yellow particles with a length of about 3 mm by a pelletizer, namely PGA modified particles E. The melt index is measured to be 35.8 g / 10 min. The particles are collected and packaged for later use.

[0087] [Example 6]

[0088] The polyglycolic acid (PGA) used in the present invention comes from Corbin Purac. Polyethylene glycol methyl acrylate (PEGMA), with a relative molecular weight of about 500, comes from Sigma-Aldrich. The initiator is dicumyl peroxide (DCP). The three are pre-blended in a mass ratio of 95.6:4:0.4, and the blend is prepared using PolyLab HAAKE from Thermo Fisher Scientific, USA. TMRheomex OS PTW16 co-rotating twin-screw extruder (screw diameter 16mm, L / D=40) was used for extrusion granulation. The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. After calibration, the feeder is used to feed the PGA blend into the twin screws at a feed rate of 2000g / hr. The temperatures of sections 2-11 of the extruder are 200°C, 220°C, 230°C, 230°C, 240°C, 250°C, 250°C, 240°C, 230°C and 220°C, respectively. The screw speed is set at 200rpm and the torque is 6-7Nm. The extruder is equipped with a circular die with a diameter of 3 mm. After the sample is extruded from the die and cooled by air, it is cut into cylindrical yellow particles with a length of about 3 mm by a pelletizer, namely PGA modified particles F. The melt index is measured to be 30.8 g / 10 min. The particles are collected and packaged for later use.

[0089] [Comparative Example 1]

[0090] The polyglycolic acid (PGA) used in the present invention comes from Corbin Purac. PolyLab HAAKE from ThermoFisher Technology Company of the United States was used. TM Rheomex OS PTW16 co-rotating twin-screw extruder (screw diameter 16mm, L / D=40) was used for extrusion granulation. The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. After calibration, the feeder is used to feed the PGA raw material into the twin screw, and the feeding rate is 2000g / hr. The temperatures of sections 2-11 of the extruder are: 200℃, 220℃, 230℃, 230℃, 240℃, 250℃, 250℃, 240℃, 230℃ and 220℃, respectively. The screw speed is set at 200rpm and the torque is 7-8Nm. The extruder is equipped with a circular die with a diameter of 3mm. After the spline is extruded from the die and air-cooled, it is cut into cylindrical yellow particles with a length of about 3mm by a pelletizer, namely PGA particles. After measurement, its melt index is 15g / 10min. Collect the particles and package them for later use.

[0091] [Comparative Example 2]

[0092] The polyglycolic acid (PGA) used in the present invention is from Corbin Purac. The monomer diethyl maleate is of Chinese medicine reagent grade. The initiator is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, of Chinese medicine reagent grade. The three are pre-blended in a mass fraction of 97.3:2:0.7, and the blend is prepared using PolyLabHAAKE from Thermo Fisher Scientific, USA. TMRheomex OS PTW16 co-rotating twin-screw extruder (screw diameter 16mm, L / D=40) was used for extrusion granulation. The extruder has 11 sections from the feed port to the die, numbered 1-11, of which the first section only serves to feed the material and cannot be heated. After calibration, the feeder is used to feed the PGA blend into the twin screws at a feed rate of 2000g / hr. The temperatures of sections 2-11 of the extruder are 200°C, 220°C, 230°C, 230°C, 240°C, 250°C, 250°C, 240°C, 230°C and 220°C, respectively. The screw speed is set at 200rpm and the torque is 6-7Nm. The extruder is equipped with a circular die with a diameter of 3 mm. After the sample strip is extruded from the die and air-cooled, it is cut into cylindrical yellow particles with a length of about 3 mm by a pelletizer, namely PGA modified particles E. The melt index is measured to be 127 g / 10 min. The particles are collected and packaged for later use.

[0093] Product performance testing

[0094] 1) Take the eight particles prepared in Examples 1 to 6 and Comparative Examples 1 to 2 and perform a thermogravimetric analysis (TGA) test according to the steps described above. The results are as follows: Figure 1 The specific values ​​are listed in Table 1.

[0095] Table 1 Thermogravimetric temperature of each particle

[0096]

[0097] As shown in Table 1 and Figure 1 The results show that the decomposition temperature of the graft-modified PGA particles with a 5% mass reduction is generally about 10°C higher than the decomposition temperature of the unmodified particles (Comparative Example 1), and the highest is about 18°C ​​(Example 3). It can be seen that the graft modification significantly increases the decomposition temperature of PGA, which is beneficial to the stability of PGA during the melt processing. However, when the initiator content continues to increase (Comparative Example 2), it will easily cause the occurrence of various side reactions such as polymer degradation, and the decomposition temperature of PGA will not increase significantly, thereby failing to achieve the technical effect of significantly improving thermal stability. The content / range of the initiator and monomer to be added needs to be repeatedly determined through experimental implementation. Even those skilled in the art cannot predict it and need to conduct a large number of experimental plans to determine it.

[0098] 2) Take the six kinds of particles prepared in Examples 1 to 4 and Comparative Examples 1 to 2, and perform thermal performance analysis (DSC) test according to the steps described above. The first cooling curve and the second heating curve are shown in FIG. Figure 2 and Figure 3 , crystallization temperature (T c ), melting temperature (T m The specific values ​​of enthalpy change (ΔH) are listed in Table 2.

[0099] Table 2 Thermal performance parameters of each particle obtained by DSC results

[0100]

[0101]

[0102] From the thermal stability results, we can see that the structure of the polyglycolic acid resin obtained by the extrusion reaction has changed, and the thermal stability has improved. The DSC results also show that the melting temperature and crystallization temperature have a downward trend, and the crystallization enthalpy change and melting enthalpy change are both reduced. This is because the side chains formed by grafting are difficult to enter the crystallization area of ​​the PGA main chain during the crystallization process, which destroys the linear easy movement of the PGA molecular main chain and the properties of arrangement in the lattice, hinders the folding of the PGA molecular chain, and the resulting crystal size becomes smaller and the crystallinity decreases. At the same time, the imperfect crystals formed by this begin to melt at a lower temperature during the melting process, and the corresponding melting peak shifts to the low temperature range, and the melting enthalpy also decreases significantly.

[0103] 3) The particles obtained in Comparative Example 1 and Examples 3 and 4 were melted and hot pressed into thin sheets of about 150 μm. The molten thin sheets were immersed in liquid nitrogen for rapid cooling. The obtained thin films after liquid nitrogen treatment were sampled for thermal analysis. The curve of the first heating process is as follows: Figure 4 shown.

[0104] The curve of the first heating process can be observed from the comparison of the crystallization process of polyvinyl alcohol from the molten state to the liquid nitrogen for rapid cooling, and the difference before and after grafting is significant. It can be seen that the film of comparative example 1 is transparent after rapid cooling by liquid nitrogen. g The molecular chain segments move around (around 80°C) to produce recrystallization, and then at T m The nearby crystals melted and a melting peak appeared. Examples 3 and 4 did not show significant or very low recrystallization peaks, indicating that the crystallization process was significantly different during the cooling process in the liquid nitrogen environment, and the change in the molecular structure of the grafted polyglycolic acid led to significant differences in the crystallization process.

[0105] 4) The filaments retained during the processing of Example 4 were dissolved in a hexafluoroisopropanol solvent and subjected to ultrasonic treatment for about 2 hours, and then the solution was poured into tetrahydrofuran (THF) for precipitation, and the unreacted monomers and homopolymers were removed by dissolution. The resulting precipitate was PGA and PGA graft copolymer. The infrared spectra of the unmodified PGA are shown in FIG. Figure 5 shown.

[0106] The infrared spectrum data obtained were normalized and the results were as follows: Figure 5 As shown, it can be seen that compared with Comparative Example 1, Example 4 has a -1The methyl peak signal nearby is significantly enhanced, indicating that the GMA monomer is grafted onto the main chain of polyglycolic acid to form a polyglycolic acid graft copolymer. The change in molecular chain structure has a significant impact on its crystallization process and thermal stability.

Claims

1. A polyglycolic acid graft copolymer with high thermal stability, wherein the main chain is a polyglycolic acid homopolymer or a copolymer of glycolide and other cyclic monomers, and the side chain is at least one of a monomer derivative, an oligomer or a polymer generated by graft polymerization; The 5% thermal weight loss temperature of the polyglycolic acid graft copolymer is at least 10 higher than that of the ungrafted polyglycolic acid. o C; The polyglycolic acid graft copolymer with high thermal stability is prepared by a method comprising the following steps: The components including the polyglycolic acid homopolymer or copolymer of glycolide and other cyclic monomers, monomers, oligomers or polymers having at least one α, β-unsaturated group, and a free radical initiator are melt-blended and reacted and extruded to obtain the polyglycolic acid graft copolymer with high thermal stability.

2. The polyglycolic acid graft copolymer with high thermal stability according to claim 1, characterized in that The main chain of the polyglycolic acid graft copolymer accounts for 80 to 99% of the total mass, and the side chain accounts for 1 to 20% of the total mass.

3. The polyglycolic acid graft copolymer with high thermal stability according to claim 1, characterized in that The main chain of the polyglycolic acid graft copolymer is a polyglycolic acid homopolymer.

4. The polyglycolic acid graft copolymer with high thermal stability according to claim 1, characterized in that The main chain of the polyglycolic acid graft copolymer is a copolymer of glycolide and other cyclic monomers.

5. The polyglycolic acid graft copolymer with high thermal stability according to claim 1, characterized in that The side chain of the polyglycolic acid graft copolymer is a graft-polymerized monomer derivative, oligomer or polymer having at least one α, β-unsaturated group.

6. The polyglycolic acid graft copolymer with high thermal stability according to claim 5, characterized in that The α, β-unsaturated group is at least one of a vinyl group, an acrylate group, a methacrylate group, an allyl group, and an acetylene group.

7. The polyglycolic acid graft copolymer with high thermal stability according to claim 1, characterized in that The monomer derivative, oligomer or polymer of the side chain of the polyglycolic acid graft copolymer carries at least one polar group, and the polar group is selected from at least one of hydroxyl, carboxyl, carbonyl, ester, amino, thiol, sulfonic acid, ether bond, halogen, peptide bond and anhydride bond.

8. The polyglycolic acid graft copolymer with high thermal stability according to claim 5, characterized in that The α, β-unsaturated groups of the monomer derivatives, oligomers or polymers of the side chains of the polyglycolic acid graft copolymer are at least one of maleic anhydride, acrylic acid, methacrylic acid, acrylates, methacrylates, acrylamides and methacrylamides.

9. The polyglycolic acid graft copolymer with high thermal stability according to any one of claims 1 to 8, characterized in that: Obtained by polymerization of the following components in weight percentage: (1) 80-97% of the polyglycolic acid homopolymer or the copolymer of glycolide and other cyclic monomers; (2) 1-19% of at least one of the monomers, oligomers or polymers having at least one α, β-unsaturated group; (3) 0.05-2% free radical initiator; The mass ratio of the free radical initiator to the monomer, oligomer or polymer having at least one α, β-unsaturated group is ≤0.3:

1.

10. The polyglycolic acid graft copolymer with high thermal stability according to claim 9, characterized in that: The mass ratio of the free radical initiator to the monomer, oligomer or polymer having at least one α, β-unsaturated group is (0.01-0.3):

1.

11. The polyglycolic acid graft copolymer with high thermal stability according to claim 9, characterized in that: Obtained by polymerization of the following components in weight percentage: (1) 90-97% of the polyglycolic acid homopolymer or the copolymer of glycolide and other cyclic monomers; (2) 2-10% of at least one monomer, oligomer or polymer having at least one α, β-unsaturated group; (3) 0.1-1% free radical initiator.

12. The polyglycolic acid graft copolymer with high thermal stability according to claim 9, characterized in that: The free radical initiator is selected from at least one of acyl peroxides, alkyl peroxides, aromatic substituted alkyl peroxides, peresters, ketone peroxides and azo compounds.

13. The polyglycolic acid graft copolymer with high thermal stability according to claim 12, characterized in that: The alkyl peroxide is a dialkyl peroxide.

14. The polyglycolic acid graft copolymer with high thermal stability according to claim 12, characterized in that: The aromatic hydrocarbon-substituted alkyl peroxide is an aromatic hydrocarbon-substituted dialkyl peroxide.

15. The polyglycolic acid graft copolymer with high thermal stability according to claim 12, characterized in that: The alkyl peroxide is alkyl hydroperoxide.

16. The polyglycolic acid graft copolymer with high thermal stability according to claim 12, characterized in that: The acyl peroxide is selected from benzoyl peroxide; and / or, The alkyl peroxide or aromatic hydrocarbon-substituted alkyl peroxide is at least one selected from di-tert-butyl peroxide, diisopropylphenyl peroxide, isopropylphenyl peroxide butyl, 3,3,5-trimethylcyclohexane-1,1-diperoxy-tert-butyl, and 2,5-di-tert-butyl peroxyhexane; and / or, The perester is selected from at least one of tert-butyl perpivalate, tert-butyl per-2-ethylhexanoate and tert-butyl perbenzoate; and / or The ketone peroxide is selected from methyl ethyl ketone peroxide; and / or, The azo compound is selected from azobisisobutyronitrile.

17. The polyglycolic acid graft copolymer with high thermal stability according to claim 15, characterized in that: The alkyl hydroperoxide is selected from at least one of tert-butyl hydroperoxide and cumene hydroperoxide.

18. A method for preparing the polyglycolic acid graft copolymer with high thermal stability according to any one of claims 1 to 17, characterized in that The following steps are involved: The components including the polyglycolic acid homopolymer or copolymer of glycolide and other cyclic monomers, monomers, oligomers or polymers having at least one α, β-unsaturated group, and a free radical initiator are melt-blended and reacted and extruded to obtain the polyglycolic acid graft copolymer with high thermal stability.

19. The method for preparing a polyglycolic acid graft copolymer with high thermal stability according to claim 18, characterized in that: The temperature of the reaction extrusion is 160-280 o C, speed is 50-1200 rpm.

20. The method for preparing a polyglycolic acid graft copolymer with high thermal stability according to claim 19, characterized in that: The temperature of the reaction extrusion is 180-260 o C, speed is 100-500 rpm.

21. The polyglycolic acid graft copolymer resin with high thermal stability obtained by the preparation method according to claim 18.

22. Use of the polyglycolic acid graft copolymer with high thermal stability according to any one of claims 1 to 17 in melt processing.

23. Use of the polyglycolic acid graft copolymer with high thermal stability according to any one of claims 1 to 17 in blown film, cast film, multilayer film, sheet, fiber, and injection molded products.