Soft magnetic composite material and preparation method thereof
By using core-shell structure and physical vapor deposition technology in soft magnetic materials, combined with an insulating layer, the problems of low resistivity, large eddy current loss and high hardness of existing soft magnetic materials are solved, and soft magnetic properties with high magnetic and mechanical properties are achieved. Composite materials for electronic devices.
Patent Information
- Application Number
- CN202210215366.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-04
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-03-04
AI Technical Summary
Existing soft magnetic materials have low resistivity, large eddy current loss, low saturation magnetic induction intensity, and excessive hardness, which affects their application in electronic equipment.
It adopts a soft magnetic composite material with a core-shell structure. The core is an amorphous or nanocrystalline soft magnetic material, and the outer shell is a crystalline metal soft magnetic material. It is formed by physical vapor deposition method and combined with an insulating layer to improve the magnetic and mechanical properties.
It achieves excellent magnetic and mechanical properties of soft magnetic composite materials, reduces eddy current losses, increases saturation magnetization and magnetic permeability, simplifies the molding process, and expands the scope of application.
Smart Images

Figure CN114496444B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of magnetic materials, and specifically relates to soft magnetic composite materials and preparation methods thereof. Background Art
[0002] Soft magnetic materials are easy to magnetize and demagnetize, and are widely used in electronic devices. At present, some soft magnetic materials have low resistivity and large eddy current loss, and some soft magnetic materials have low saturation magnetic induction, which is not conducive to the use of electronic devices; some soft magnetic materials have too high hardness, which is not conducive to the molding and preparation of magnetic parts, affecting their application in electronic devices. Therefore, the development of soft magnetic materials with excellent magnetic properties and suitable mechanical properties has become an urgent problem to be solved. Summary of the invention
[0003] In view of this, the present application provides a soft magnetic composite material and a preparation method thereof.
[0004] In the first aspect, the present application provides a soft magnetic composite material, comprising a core and a shell that at least partially wraps the core, the core is made of a first soft magnetic material, the shell is made of a second soft magnetic material, the first soft magnetic material is an amorphous soft magnetic material or a nanocrystalline soft magnetic material, and the second soft magnetic material is a crystalline metallic soft magnetic material.
[0005] In a second aspect, the present application provides a method for preparing a soft magnetic composite material, comprising:
[0006] Placing the core material and the target material in a container, wherein the inner cavity cross section of the container is polygonal, and the core material comprises a first soft magnetic material, which is an amorphous soft magnetic material or a nanocrystalline soft magnetic material;
[0007] The container is rotated around a direction perpendicular to the inner cavity cross section, the target material is kept fixed, and the material of the target material is deposited on the surface of the core material by physical vapor deposition to form a shell that at least partially wraps the core material, so as to obtain soft magnetic composite particles, wherein the material of the shell includes a second soft magnetic material, and the second soft magnetic material is a crystalline metal soft magnetic material.
[0008] The present application provides a soft magnetic composite material with a core-shell structure, wherein the material of the core includes a first soft magnetic material, and the material of the shell includes a second soft magnetic material. The first soft magnetic material and the second soft magnetic material have different microscopic morphologies, resulting in different performances of the core and the shell, so that the soft magnetic composite material has the performance advantages of both the core and the shell, and the soft magnetic composite material has excellent magnetic properties and mechanical properties, thereby expanding its application range; the preparation method of the soft magnetic composite material is simple, the operation is convenient, and it is conducive to its use. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] In order to more clearly illustrate the technical solutions in the implementation modes of the present application, the drawings required for use in the implementation modes of the present application will be described below.
[0010] Figure 1 A schematic diagram of the structure of a soft magnetic composite material provided in one embodiment of the present application.
[0011] Figure 2 A schematic structural diagram of a soft magnetic composite material provided in another embodiment of the present application.
[0012] Figure 3 A schematic structural diagram of a soft magnetic composite material provided in yet another embodiment of the present application.
[0013] Figure 4 A schematic flow chart of a method for preparing a soft magnetic composite material provided in one embodiment of the present application.
[0014] Figure 5 A schematic cross-sectional view of a container provided in accordance with one embodiment of the present application.
[0015] Figure 6 This is a schematic diagram of a container in use according to one embodiment of the present application.
[0016] Figure 7 A schematic flow chart of a method for preparing a soft magnetic composite material provided in yet another embodiment of the present application.
[0017] Description of labels:
[0018] Core-11, shell-12, first shell-12', second shell-12", insulating layer-13, soft magnetic composite material-10, inner cavity-21, container-20, core material-30, target material-40. DETAILED DESCRIPTION
[0019] The following are preferred implementations of the present application. It should be noted that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.
[0020] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application. In addition, the present application can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the various specific processes and material examples provided by the present application, but those of ordinary skill in the art can appreciate the application of other processes and / or the use of other materials.
[0021] See also Figure 1 , is a schematic structural diagram of a soft magnetic composite material provided in one embodiment of the present application, the soft magnetic composite material 10 includes a core 11 and a shell 12 at least partially wrapping the core 11, the material of the core 11 includes a first soft magnetic material, the material of the shell 12 includes a second soft magnetic material, the first soft magnetic material is an amorphous soft magnetic material or a nanocrystalline soft magnetic material, and the second soft magnetic material is a crystalline metal soft magnetic material.
[0022] It is understandable that soft magnetic materials generally refer to magnetic materials with a coercive force (Hc) of no more than 1000A / m. The microscopic morphology of soft magnetic materials includes three states: crystalline, amorphous and nanocrystalline. At present, the performance of soft magnetic materials still needs to be improved. For example, the resistivity of iron is low, and the eddy current loss is large under the alternating magnetic field. By adding other elements to form an iron-based crystalline alloy, the resistivity is increased and the eddy current loss is reduced, but the saturation magnetization intensity is also reduced at the same time; the coercive force of amorphous soft magnetic materials is low and the loss is small. The saturation magnetization intensity and magnetic permeability of nanocrystalline soft magnetic materials are improved compared with amorphous soft magnetic materials, and the resistivity is equivalent to that of amorphous soft magnetic materials, but the hardness of amorphous soft magnetic materials and nanocrystalline soft magnetic materials is high and the plasticity is low, which increases the difficulty of forming magnetic parts. The soft magnetic composite material 10 of the present application has a core-shell structure, the core 11 has an amorphous soft magnetic material or a nanocrystalline soft magnetic material, that is, the microscopic morphology of the first soft magnetic material is amorphous or nanocrystalline, the atomic arrangement in the amorphous soft magnetic material has a state of short-range order and long-range disorder, and the nanocrystalline is a state containing grains in the amorphous state, which is different from the crystalline state and the amorphous state. The amorphous soft magnetic material or the nanocrystalline soft magnetic material has a low coercive force and small loss, which helps to reduce the loss of the soft magnetic composite material 10; the shell 12 has a crystalline metal soft magnetic material, that is, the microscopic morphology of the second soft magnetic material is crystalline, the atoms in the crystalline soft magnetic material are orderly arranged, and the crystalline metal soft magnetic material not only has high saturation magnetization and permeability, but also has excellent plasticity, which helps to improve the saturation magnetization and permeability of the soft magnetic composite material 10, and at the same time improves the plasticity of the soft magnetic composite material 10, which is conducive to the processing and molding of the soft magnetic composite material 10, thereby improving the comprehensive magnetic properties and comprehensive mechanical properties of the soft magnetic composite material 10, and helping the application of the soft magnetic composite material 10.
[0023] The saturation magnetization and magnetic permeability of the crystalline soft magnetic material are high. The crystalline metal soft magnetic material not only has high saturation magnetization and magnetic permeability, but also has good plasticity, which is helpful for the processing and forming of the soft magnetic composite material 10. In the embodiment of the present application, the crystalline metal soft magnetic material includes at least one of iron, nickel, cobalt, iron-silicon alloy, iron-aluminum alloy, iron-nickel alloy and iron-cobalt alloy. In one embodiment, the silicon content in the iron-silicon alloy can be 0.5%-4%, such as 1%, 2%, 3% or 4%. In one embodiment, the aluminum content in the iron-aluminum alloy can be 6%-16%, such as 11.7%, 12%, 15%, 15.9% or 16%. Further, the iron-aluminum alloy can also contain molybdenum; the content of molybdenum can be 2%-3%, such as 2%, 2.4%, 2.8% or 3%. In one embodiment, the nickel content in the iron-nickel alloy can be 35%-90%, such as 45%, 50%, 68% or 78.5%. Furthermore, the iron-nickel alloy may also contain molybdenum; the content of molybdenum is less than or equal to 5%, such as 2%, 3%, 4% or 5%. In one embodiment, the content of cobalt in the iron-cobalt alloy may be 30%-70%, such as 40%, 50%, 60% or 65%. Furthermore, the iron-cobalt alloy may also contain vanadium; the content of vanadium is less than or equal to 5%, such as 1%, 1.5%, 2% or 2.5%.
[0024] In the embodiment of the present application, the amorphous soft magnetic material includes at least one of an iron-based amorphous soft magnetic material, a cobalt-based amorphous soft magnetic material, and an iron-nickel-based amorphous soft magnetic material. In one embodiment, the iron-based amorphous soft magnetic material may include at least one of an FeB amorphous material, an FeBC amorphous material, an FeSiB amorphous material, an FeSiBC amorphous material, an FeNbSiB amorphous material, an FeCrSiB amorphous material, an FeCrSiBC amorphous material, and FeCoBSi, such as Fe 80 B 20 , Fe 84 B 10 C6, Fe 86 B7C7、Fe 78 Si 13 B9, Fe 82 Si 10 B8, Fe 84 Si 10 B6, Fe 81 Si 3.5 B 13.5 C2、Fe 67 Co 18 B 14In one embodiment, the cobalt-based amorphous soft magnetic material may include at least one of CoFeSiB amorphous material, CoFeCrSiB amorphous material, CoFeMoSiB amorphous material, CoFeNiSiB amorphous material and CoFeNiNbSiB amorphous material, such as Co 65.7 Fe 4.3 Si 17 B 13 、Co 70.3 Fe 4.7 Si 10 B 15 、Co 66 Fe5Cr9Si5B 15 、Co 66 Fe4Mo2Si 16 B 12 、Co 71.6 Fe 4.2 Ni 4.2 Si 10 B 10 、Co 66 Fe 4.5 Ni 2.3 Nb 2.2 Si 10 B 15 In one embodiment, the iron-nickel-based amorphous soft magnetic material may include at least one of FeNiBP amorphous material, FeNiMoB amorphous material, FeNiSiB amorphous material and FeNiMoSiB amorphous material, such as Fe 40 Ni 40 B6P 14 , Fe 40 Ni 38 Mo4B 18 , Fe 46.8 Ni 31.2 Si 10 B 12 , Fe 62.4 Ni 15.6 Mo2Si8B 12 wait.
[0025] In the embodiment of the present application, the nanocrystalline soft magnetic material includes at least one of FeZrB nanocrystalline material, FeZrCuB nanocrystalline material, FeHfB nanocrystalline material, FeNbB nanocrystalline material, FeNbZrCuB nanocrystalline material, FeNbCuSiB nanocrystalline material and FeCuSiBP nanocrystalline material, such as Fe 91 Zr7B2、Fe 90 Zr7B3、Fe 89 Zr7CuB3、Fe 86Zr7CuB6、Fe 89 Hf7B4、Fe 84 Nb7B9、Fe 73.5 Nb3CuSi 13.5 B9, Fe 74 Nb3CuSi 16 B6, etc. In the present application, the nanocrystalline soft magnetic material has nanocrystalline grains, and the particle size of the nanocrystalline grains may be, but is not limited to, less than 15 nm, such as 6 nm-8 nm, 8 nm-10 nm, or 10 nm-12 nm.
[0026] In the embodiment of the present application, the particle size of the core 11 is 2μm-50μm, which ensures the performance of the soft magnetic composite material 10 and is conducive to the coating of the shell 12. Specifically, the particle size of the core 11 can be, but is not limited to, 2μm, 8μm, 15μm, 20μm, 25μm, 32μm, 37μm, 40μm, 45μm or 50μm. In one embodiment, the particle size of the core 11 is 2μm-10μm. In another embodiment, the particle size of the core 11 is 20μm-30μm. In yet another embodiment, the particle size of the core 11 is 40μm-50μm.
[0027] In the embodiment of the present application, the thickness of the shell 12 is 5nm-1000nm. Specifically, the thickness of the shell 12 may be, but is not limited to, 5nm, 50nm, 180nm, 300nm, 500nm, 750nm, 830nm, 950nm or 1000nm. In one embodiment, the thickness of the shell 12 is 5nm-100nm. In another embodiment, the thickness of the shell 12 is 300nm-500nm. In yet another embodiment, the thickness of the shell 12 is 800nm-1000nm. It is understandable that the soft magnetic composite material 10 may include a single layer of shell 12 or multiple layers of shell 12 (such as two layers, three layers, four layers, five layers, six layers, etc.), and the materials of the multiple layers of shell 12 may be the same or different. Please refer to Figure 2 , is a structural schematic diagram of a soft magnetic composite material 10 provided in another embodiment of the present application, wherein the soft magnetic composite material 10 includes a core 11 and two shells 12 wrapping the core 11, the two shells 12 are respectively a first shell 12' and a second shell 12", the first shell 12' wraps the core 11, and the second shell 12" wraps the first shell 12'. Figure 2The case where the soft magnetic composite material 10 has two layers of outer shell 12 is shown. It can be understood that the soft magnetic composite material 10 can also have three or more layers of outer shell 12, which will not be repeated here. In one embodiment, the soft magnetic composite material 10 includes multiple layers of outer shell 12, and the materials of adjacent outer shells 12 are different, so as to further improve the magnetic properties and mechanical properties of the soft magnetic composite material 10. In the present application, the outer shell 12 can completely cover the inner core 11, that is, the coverage rate is 100%; the outer shell 12 can also cover part of the inner core 11, such as the coverage rate is greater than 80%, greater than 90%, greater than 95%, greater than 98%, greater than 99%, etc.
[0028] Amorphous / nanocrystalline soft magnetic materials have high hardness and low plasticity. When using them to prepare magnetic parts, resin and other substances need to be added to form them, so as to avoid the amorphous / nanocrystalline soft magnetic materials from breaking during the pressing process and affecting their magnetic properties. However, the addition of resin and other substances reduces the magnetic properties of the magnetic parts. The present application can reduce the eddy current loss of the soft magnetic composite material 10 by using amorphous / nanocrystalline soft magnetic materials, and the high magnetic induction intensity and magnetic permeability of the soft magnetic composite material 10 can be guaranteed by using crystalline metal soft magnetic materials. At the same time, the crystalline metal soft magnetic material is used for wrapping, which improves the plasticity of the soft magnetic composite material 10, is conducive to the pressing of the soft magnetic composite material 10, reduces the difficulty of pressing, and is conducive to the processing and molding operation of the soft magnetic composite material 10. In addition, there is no addition of other non-magnetic substances, which ensures the content of soft magnetic materials in the soft magnetic composite material 10, which helps to improve its magnetic properties. In one embodiment of the present application, the first soft magnetic material is an amorphous soft magnetic material, and the second soft magnetic material is a crystalline metal soft magnetic material. In another embodiment of the present application, the first soft magnetic material is a nanocrystalline soft magnetic material, and the second soft magnetic material is a crystalline metal soft magnetic material. In one embodiment, the crystalline metal soft magnetic material includes at least one of iron, iron-nickel alloy and iron-cobalt alloy. The above-mentioned crystalline metal soft magnetic material has high magnetic induction intensity and magnetic permeability, and excellent plasticity, which is conducive to subsequent compression molding operations. In a specific embodiment, the crystalline metal soft magnetic material is an iron-nickel alloy. Selecting the iron-nickel alloy can make the shell 12 have high plasticity, which is conducive to subsequent compression molding operations.
[0029] In the embodiment of the present application, the hardness of the first soft magnetic material is greater than the hardness of the second soft magnetic material, and the plasticity of the second soft magnetic material is greater than the plasticity of the first soft magnetic material. The plasticity can be characterized by elongation. The use of soft magnetic materials with different mechanical properties to form the soft magnetic composite material 10 is conducive to the pressing of the soft magnetic composite material 10, thereby facilitating the preparation of magnetic parts.
[0030] See also Figure 3 , which is a schematic structural diagram of a soft magnetic composite material 10 provided in another embodiment of the present application, Figure 1The two embodiments are roughly the same, except that the soft magnetic composite material 10 also includes an insulating layer 13, and the insulating layer 13 at least partially wraps the outer shell 12. By providing the insulating layer 13, the resistivity of the soft magnetic composite material 10 is increased, and the eddy current loss of the soft magnetic composite material 10 under the magnetic field is reduced, which is beneficial for its use in a high-frequency environment. In the present application, the insulating layer 13 can completely cover the outer shell 12, that is, the coverage rate is 100%; the insulating layer 13 can also partially cover the outer shell 12, such as the coverage rate is greater than 80%, greater than 90%, greater than 95%, greater than 98%, greater than 99%, etc. In one embodiment, the insulating layer 13 completely covers the outer shell 12 to reduce the eddy current loss of the soft magnetic composite material 10 as much as possible.
[0031] In the embodiment of the present application, the material of the insulating layer 13 includes at least one of a ceramic material and a ferrite. The insulating layer 13 has the properties of high temperature resistance, high toughness, and high resistivity, which can not only play an insulating role, reduce the eddy current loss of the soft magnetic composite material 10, but also facilitate the subsequent pressing and molding operation. When the organic insulating layer is formed by coating resin, the content of the soft magnetic material in the soft magnetic composite material 10 will be reduced, resulting in a decrease in magnetic permeability and an increase in hysteresis loss, and affecting the temperature of pressing and molding; when other inorganic metals or non-metallic materials are used to form the insulating layer, the surface hardness of the soft magnetic composite material will be increased, and such an insulating layer may even crack during the molding process of the magnetic part, further increasing the difficulty of molding. In one embodiment, the ceramic material includes at least one of zirconium oxide, yttrium oxide, aluminum oxide, and silicon carbide. The above ceramic materials have both high resistivity and excellent insulation and toughness, which are beneficial to improving the performance of the soft magnetic composite material 10. In one embodiment, the insulating layer 13 is made of zirconium oxide and yttrium oxide, wherein yttrium oxide plays a role in stabilizing zirconium oxide, so that the insulating layer 13 has excellent insulation and high temperature resistance. Ferrite is a soft magnetic material whose main component is iron oxide and is compounded with other metal oxides such as ZnO, NiO, MnO, etc. It is a ceramic metal oxide material. Ferrite has a very high resistivity, especially when ferrite contains divalent metal oxides such as manganese, nickel, cobalt, zinc, etc., ferrite can have a high resistivity (such as 10 4 Ω·cm, etc.). Specifically, the ferrite may include at least one of manganese ferrite, zinc ferrite, manganese zinc ferrite, manganese magnesium zinc ferrite, nickel zinc ferrite and copper zinc ferrite. For example, the saturation magnetization intensity of nickel zinc ferrite is 0.2T-0.8T. In one embodiment, the material of the insulating layer 13 is ferrite. By using ferrite as the insulating layer 13, the content of soft magnetic material in the soft magnetic composite material 10 is increased, and the ferrite is resistant to high temperature, which helps to increase the molding temperature, helps to reduce the residual stress in the pressing molding process and reduce the coercive force, which is beneficial to the use of the soft magnetic composite material 10.
[0032] In the embodiment of the present application, the thickness of the insulating layer 13 is 5nm-100nm, which is beneficial to improve the resistivity of the soft magnetic composite material 10, thereby reducing its eddy current loss, and improving its high temperature resistance, ensuring its performance. Specifically, the thickness of the insulating layer 13 can be but is not limited to 5nm, 10nm, 20nm, 33nm, 40nm, 45nm, 55nm, 70nm, 80nm, 95nm or 100nm. In one embodiment, the thickness of the insulating layer 13 is 5nm-20nm. In another embodiment, the thickness of the insulating layer 13 is 30nm-60nm. In yet another embodiment, the thickness of the insulating layer 13 is 80nm-100nm.
[0033] In the implementation mode of the present application, the soft magnetic composite material 10 also includes a binder, and the binder wraps the shell 12 or the insulating layer 13. By adding the binder, it is beneficial to fix the soft magnetic composite material 10 and facilitate processing and molding. In one embodiment, the mass content of the binder in the soft magnetic composite material 10 is 1%-10%, such as the mass content of the binder in the soft magnetic composite material 10 is 1%-7%, 1%-5% or 2%-3%, etc., which is beneficial to the compression molding of the soft magnetic composite material 10 and does not reduce the density of the soft magnetic material in the soft magnetic composite material 10. In the present application, a viscous substance can be selected as a binder. In one embodiment, the binder can be a resin, such as at least one of a polyimide resin, an epoxy resin, a silicone resin, and a fluororesin. In a specific embodiment, the binder can be a thermosetting resin.
[0034] The present application also provides a method for preparing a soft magnetic composite material, which is used to prepare the soft magnetic composite material 10 in any of the above embodiments. Figure 4 , is a schematic flow chart of a method for preparing a soft magnetic composite material provided in one embodiment of the present application, comprising:
[0035] S101: placing a core material and a target material in a container, wherein the inner cavity cross-section of the container is a polygon, and the core material comprises a first soft magnetic material, and the first soft magnetic material is an amorphous soft magnetic material or a nanocrystalline soft magnetic material.
[0036] S102: Rotate the container in a direction perpendicular to the inner cavity cross section, keep the target material fixed, and deposit the target material on the surface of the core material by physical vapor deposition to form a shell that at least partially wraps the core material, so as to obtain soft magnetic composite particles, wherein the material of the shell includes a second soft magnetic material, and the second soft magnetic material is a crystalline metal soft magnetic material.
[0037] In S101, see Figure 5, is a schematic cross-sectional view of a container 20 provided in one embodiment of the present application, wherein the container 20 has an inner cavity 21, and the cross-section of the inner cavity 21 is a polygon. Figure 6 , is a schematic diagram of a container 20 provided in an embodiment of the present application during use, wherein a core material 30 and a target material 40 are placed in the container 20 so as to form a shell 12 on the surface of the core material 30. It can be understood that the core material 30 is the core 11 of the soft magnetic composite material 10, and the selection of its material, microscopic morphology, particle size, etc. is not repeated here. In one embodiment, the cross section of the inner cavity 21 of the container 20 is parallel to the direction of gravity. In another embodiment, the cross section of the inner cavity 21 of the container 20 is perpendicular to the direction of gravity. In the embodiment of the present application, a target material seat is provided in the inner cavity 21 of the container 20, and the target material seat is used to place the target material 40. In the present application, the inner cavity 21 of the container 20 is a vacuum chamber, which is convenient for the deposition of the target material 40, and the selection of the target material 40 is determined according to the material of the shell 12. In the embodiment of the present application, when the shell 12 is an alloy material, the target material 40 can be an alloy target or a plurality of single metal targets.
[0038] In the present application, the core material 30 can be prepared or directly purchased. In one embodiment, the amorphous soft magnetic material can be prepared by a magnetic film crushing method or a water mist spraying method, and then the prepared amorphous soft magnetic material can be used as the first soft magnetic material. The magnetic film crushing method is to crush and grind an amorphous alloy magnetic film with a thickness of micrometer level (such as tens of micrometers) into a metal powder state to obtain an amorphous soft magnetic material. The water mist spraying method is to spray and atomize liquid metal in a high-temperature molten state and high-pressure water or air at the same time, and the high-temperature liquid metal is rapidly cooled to form amorphous fine particles to obtain an amorphous soft magnetic material. The water mist spraying method can obtain an amorphous soft magnetic material with good sphericity, which is more conducive to the deposition and coating of the target material 40. In a specific embodiment, the amorphous soft magnetic material is prepared by the water mist spraying method, and the particle size of the amorphous soft magnetic material is 2μm-50μm. In one embodiment, a small amount of elements such as Zr, Cu, Hf, and Nb may be added to the amorphous soft magnetic material, and a crystallization treatment may be performed at an appropriate temperature to precipitate a portion of the nanoscale crystal phase to obtain a nanocrystalline soft magnetic material.
[0039] In S102, the container 20 rotates around a direction perpendicular to the cross section of the inner cavity 21. During the rotation, the core material 30 in the inner cavity 21 will continuously flip under the action of gravity, so that by setting the material of the target material 40, physical vapor deposition is performed, and the target material 40 is deposited on the surface of the core material 30 to finally form the desired outer shell 12; and because the core material 30 is constantly moving in the rotating inner cavity 21 and under the action of gravity during the deposition process, the target material 40 can be evenly deposited on the surface of the core material 30 to form an outer shell 12 that evenly covers the core material 30. It can be understood that by replacing the material of the target material 40, an outer shell 12 with different material compositions and multiple layers can be obtained, and by controlling the deposition time, an outer shell 12 of the desired thickness can be obtained. The target material 40 is fixed, and the movement range of the core material 30 in the inner cavity 21 overlaps with the deposition range of the target material 40, thereby ensuring the formation of the outer shell 12. The container 20 can rotate with its central axis as the rotation axis to Figure 6 As shown in the example, the container 20 can rotate counterclockwise, can rotate clockwise, or can rotate clockwise and counterclockwise alternately. In the embodiment of the present application, the rotation speed of the container 20 is 20rpm-40rpm, so as to ensure that the core material 30 will move during the rotation of the container 20, and the displacement will not be too large, which is conducive to the deposition of the target material 40. Specifically, the rotation speed of the container 20 is 20rpm, 25rpm, 30rpm, 35rpm or 40rpm, etc.
[0040] In the present application, physical vapor deposition can be but not limited to vacuum evaporation, vacuum sputtering, ion plating and the like, and the process conditions of physical vapor deposition can be selected according to the properties of the deposited target material 40. In this way, the core material 30 and the target material 40 can be selected as needed to obtain a soft magnetic composite material 10 with excellent comprehensive performance. In the embodiment of the present application, the target material 40 is set, the gas is introduced, and the output power and the pressure of the inner cavity 21 are adjusted to perform physical vapor deposition. Specifically, the output power can be 100W-300W, such as 100W, 160W, 200W, 250W, 270W or 300W; the pressure of the inner cavity 21 can be 0.1Pa-5Pa, such as 0.1Pa, 0.5Pa, 1Pa, 1.5Pa, 2Pa, 3Pa, 4Pa or 5Pa; when the material of the outer shell 12 does not contain oxygen or carbon, the introduced gas is an inert gas; when the material of the outer shell 12 contains oxygen, a mixed gas is introduced, and the mixed gas includes an inert gas and oxygen, and the oxygen content in the mixed gas can be 20%-50%, such as 20%, 25%, 30%, 35%, 40%, 45% or 50%, etc. The inert gas can be but is not limited to argon, helium, nitrogen, etc. In the embodiment of the present application, the core material 30 is heated during the physical vapor deposition process, so that the temperature of the core material 30 is 100°C-400°C (such as 100°C, 150°C, 200°C, 250°C, 300°C, 350°C or 400°C, etc.), which is conducive to the deposition of the target material 40 and improves the bonding force between the core 11 and the shell 12. In the embodiment of the present application, the core material 30 and the target material 40 are placed in the container 20, and the target material 40 is an iron-nickel alloy, wherein the nickel content in the iron-nickel alloy can be 50%-80%; inert gas is introduced, and the pressure of the inner cavity 21 is adjusted to 0.1Pa-5.0Pa, and physical vapor deposition is performed at an output power of 100W-300W and a rotation speed of the container 20 of 20rpm-40rpm to obtain soft magnetic composite particles, namely, the soft magnetic composite material 10, and the shell 12 of the soft magnetic composite material 10 is an iron-nickel alloy.
[0041] In one embodiment, the core material 30 and the target material 40 are placed in a container 20, the inner cavity 21 of the container 20 has a polygonal cross section, the core material 30 is an iron-based amorphous soft magnetic material, and the target material 40 is an iron-nickel alloy, wherein the nickel content of the iron-nickel alloy can be 50%-80%; the inner cavity 21 of the container 20 is vented to an internal pressure of 8×10 -4Pa, argon gas is introduced to adjust the internal pressure to 0.1Pa-5.0Pa, and sputtering is performed at an output power of 100W-300W. At the same time, the container 20 starts to rotate at a speed of 20rpm-40rpm. After the sputtering is completed, nitrogen gas is introduced into the inner cavity 21 to atmospheric pressure, and the soft magnetic composite material 10 is taken out. The core 11 of the soft magnetic composite material 10 is made of iron-based amorphous soft magnetic material, and the outer shell 12 is an iron-nickel alloy layer. The saturation magnetization intensity of the iron-based amorphous soft magnetic material is 1.2T-1.4T, and the maximum magnetic permeability is about 6×10 4 The saturation magnetization of the iron-nickel alloy is 0.7T-0.8T, and the maximum magnetic permeability is about 3×10 4 The saturation magnetization intensity of the soft magnetic composite material 10 is 1T-1.4T, and the maximum magnetic permeability is 3×10 4 The soft magnetic composite material 10 obtained by the method provided by the present application has excellent comprehensive magnetic properties, and the iron-nickel alloy improves the plasticity of the soft magnetic composite material 10, which is beneficial to the improvement of the magnetic properties and preparation of magnetic parts.
[0042] See also Figure 7 , which is a schematic flow chart of a method for preparing a soft magnetic composite material provided in another embodiment of the present application, comprising:
[0043] S201: placing a core material and a target material in a container, wherein the inner cavity cross-section of the container is a polygon, and the core material comprises a first soft magnetic material, and the first soft magnetic material is an amorphous soft magnetic material or a nanocrystalline soft magnetic material.
[0044] S202: Rotate the container in a direction perpendicular to the inner cavity cross section, keep the target material fixed, and deposit the target material on the surface of the core material by physical vapor deposition to form a shell that at least partially wraps the core material, wherein the shell is made of a second soft magnetic material, and the second soft magnetic material is a crystalline metal soft magnetic material.
[0045] S203: forming an insulating layer on the surface of the shell, wherein the insulating layer at least partially wraps the shell, thereby obtaining soft magnetic composite particles.
[0046] For S201 and S202, please refer to the description of S101 and S102 above.
[0047] In S203, an insulating layer 13 may also be formed on the surface of the housing 12. In the present application, the insulating layer 13 is formed by a physical vapor deposition method. Specifically, by setting a target material 40 of a desired material, the desired insulating layer 13 is obtained. This method can increase the selection range of the material of the insulating layer 13, and is more conducive to selecting a material that improves the performance of the soft magnetic composite material 10, and the controllability of the entire process and the structure of the soft magnetic composite material 10 is high.
[0048] In the embodiment of the present application, the material of the insulating layer includes at least one of a ceramic material and a ferrite. In the embodiment of the present application, a core material 30 and a target material 40 having a shell 12 are placed in a container 20; a gas is introduced, and the pressure of the inner cavity 21 is adjusted to 0.1Pa-5.0Pa (such as 0.1Pa, 0.5Pa, 1Pa, 1.5Pa, 2Pa, 3Pa, 4Pa or 5Pa, etc.), and physical vapor deposition is performed at an output power of 1000W-4000W (such as 1000W, 1500W, 2000W, 3000W, 3600W or 4000W, etc.) and a rotation speed of the container 20 of 20rpm-40rpm, and an insulating layer 13 is deposited on the surface of the shell 12 to obtain a soft magnetic composite material 10, and the material of the insulating layer 13 is a ceramic material. In one embodiment, a target material 40 containing zirconium and yttrium elements is used, and a mixed gas containing an inert gas and oxygen is introduced into the inner cavity 21 of the container 20, so that the pressure of the inner cavity 21 is 0.1Pa-5.0Pa, and an insulating layer 13 is deposited on the surface of the outer shell 12. The material of the insulating layer 13 includes zirconium oxide and yttrium oxide. Optionally, the mixed gas includes an inert gas and oxygen, and the oxygen content in the mixed gas is 20%-50%, such as 20%, 25%, 30%, 35%, 40%, 45% or 50%. Among them, the number of target materials 40 can be single or multiple, such as the target material 40 includes a zirconium target and a yttrium target. In a specific embodiment, the target material 40 is an alloy containing zirconium and yttrium, and the inner cavity 21 of the container 20 is evacuated to an internal pressure of 8×10 -4 Pa, introduce a mixed gas of argon and oxygen, the oxygen content in the mixed gas is 20%-50%, adjust the internal pressure to 0.1Pa-5.0Pa, and perform sputtering at an output power of 1000W-4000W, while the container 20 starts to rotate at a speed of 20rpm-40rpm, and an insulating layer 13 is formed on the surface of the shell 12; after the sputtering is completed, introduce nitrogen into the inner cavity 21 to atmospheric pressure, and take out the soft magnetic composite material 10; the soft magnetic composite material 10 has an insulating layer 13. The molar ratio of zirconium to yttrium in the target material 40 can be, but is not limited to, 4.
[0049] In an embodiment of the present application, a core material 30 having a shell 12 and a target material 40 are placed in a container 20, wherein the target material 40 is an iron alloy target; a mixed gas is introduced, and the pressure of the inner cavity 21 is adjusted to 0.1Pa-5.0Pa (such as 0.1Pa, 0.5Pa, 1Pa, 1.5Pa, 2Pa, 3Pa, 4Pa or 5Pa, etc.), and physical vapor deposition is performed at an output power of 100W-300W (such as 100W, 160W, 200W, 250W, 270W or 300W, etc.) and a rotation speed of the container 20 of 20rpm-40rpm, and an insulating layer 13 is deposited on the surface of the shell 12 to obtain a soft magnetic composite material 10, the insulating layer 13 is made of ferrite, the mixed gas includes an inert gas and oxygen, and the oxygen content in the mixed gas is 20%-50% (such as 20%, 25%, 30%, 35%, 40%, 45% or 50%, etc.). In one embodiment, an iron-nickel-zinc alloy is used as the target material 40, and a mixed gas containing an inert gas and oxygen is introduced into the inner cavity 21 of the container 20 to make the pressure of the inner cavity 21 be 0.1Pa-5.0Pa, and an insulating layer 13 is deposited on the surface of the shell 12. The material of the insulating layer 13 includes nickel-zinc ferrite. In a specific embodiment, the core material 30 and the target material 40 are placed in the container 20, the cross section of the inner cavity 21 of the container 20 is polygonal, the core material 30 is an amorphous soft magnetic material, and the target material 40 is an iron-nickel alloy, wherein the nickel content of the iron-nickel alloy can be 50%-80%; the inner cavity 21 of the container 20 is vented to an internal pressure of 8×10 -4 Pa, argon gas is introduced to adjust the internal pressure to 0.1Pa-5.0Pa, and sputtering is performed at an output power of 100W-300W. At the same time, the container 20 starts to rotate at a speed of 20rpm-40rpm; then the target material 40 is replaced with Fe 63 Ni 13 Zn 24 , introduce a mixed gas of argon and oxygen into the inner cavity 21 of the container 20, the oxygen content in the mixed gas is 20%-50%, adjust the internal pressure to 0.1Pa-5.0Pa, and perform sputtering at an output power of 100W-300W, and at the same time, the container 20 starts to rotate at a rotation speed of 20rpm-40rpm; after the sputtering is completed, introduce nitrogen into the inner cavity 21 to atmospheric pressure, and take out the soft magnetic composite material 10; the core 11 of the soft magnetic composite material 10 is made of amorphous soft magnetic material, the outer shell 12 is made of iron-nickel alloy outer shell, and the insulating layer 13 is made of nickel-zinc ferrite.
[0050] In the embodiment of the present application, the preparation method of the soft magnetic composite material 10 also includes dispersing the soft magnetic composite particles into a binder and performing compression molding. Furthermore, the mass content of the binder in the soft magnetic composite material 10 is 1%-10%, which is conducive to the compression molding of the soft magnetic composite material 10 and does not reduce the density of the soft magnetic composite particles in the soft magnetic composite material 10. It can be understood that when the compression molding operation is not performed, the soft magnetic composite particles are the soft magnetic composite material 10. Specifically, compression molding can be performed in a mold but is not limited to it. The soft magnetic composite particles in which the shell 12 wraps the core 11, or the insulating layer 13 wraps the shell 12 and the core 11 are obtained by physical vapor deposition. After a plurality of soft magnetic composite particles are mixed with a binder, they are compressed to obtain a soft magnetic composite material 10 with a certain shape, which can be used in electronic equipment, such as as a part of an inductor, a filter, or a transformer. Due to the wrapping of the outer shell 12 and / or the insulating layer 13, the soft magnetic composite particles have excellent mechanical properties. During the pressing process, external forces will not damage the structure of the soft magnetic composite particles, thereby reducing the difficulty of forming the soft magnetic composite material 10. The soft magnetic composite material 10 can be formed in one time, and the operation is simple and convenient, which is conducive to obtaining soft magnetic composite materials 10 of different shapes, such as E-type, U-type, L-type, ring-shaped, etc.
[0051] The preparation method of the soft magnetic composite material 10 provided in the present application is simple, easy to operate, has strong process controllability, and is green and environmentally friendly. At the same time, it expands the range of choices for the materials of the core 11 and the shell 12, is more suitable for large-scale production of the soft magnetic composite material 10, has a high product yield and excellent magnetic properties, and is more conducive to its application.
[0052] The above is a detailed introduction to the contents provided in the implementation mode of the present application. This article explains and illustrates the principles and implementation modes of the present application. The above explanation is only used to help understand the method and core idea of the present application. At the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation mode and application scope. In summary, the contents of this specification should not be understood as limiting the present application.
Claims
1. A soft magnetic composite material, It is characterized in that It includes a core, a shell that at least partially wraps the core, and an insulating layer that at least partially wraps the shell, the core is made of a first soft magnetic material, the shell is made of a second soft magnetic material, the first soft magnetic material is an amorphous soft magnetic material or a nanocrystalline soft magnetic material, the second soft magnetic material is a crystalline metal soft magnetic material, the insulating layer is made of at least one of a ceramic material and a ferrite, the ceramic material includes at least one of zirconium oxide, yttrium oxide, aluminum oxide and silicon carbide, and the thickness of the insulating layer is 5nm-100nm.
2. The soft magnetic composite material according to claim 1, It is characterized in that The amorphous soft magnetic material includes at least one of an iron-based amorphous soft magnetic material, a cobalt-based amorphous soft magnetic material and an iron-nickel-based amorphous soft magnetic material; the iron-based amorphous soft magnetic material includes at least one of an FeB amorphous material, an FeBC amorphous material, an FeSiB amorphous material, an FeSiBC amorphous material, an FeNbSiB amorphous material, an FeCrSiB amorphous material, an FeCrSiBC amorphous material and FeCoB; the cobalt-based amorphous soft magnetic material includes at least one of a CoFeSiB amorphous material, a CoFeCrSiB amorphous material, a CoFeMoSiB amorphous material, a CoFeNiSiB amorphous material and a CoFeNiNbSiB amorphous material; the iron-nickel-based amorphous soft magnetic material includes at least one of a FeNiBP amorphous material, a FeNiMoB amorphous material, a FeNiSiB amorphous material and a FeNiMoSiB amorphous material; The nanocrystalline soft magnetic material comprises at least one of FeZrB nanocrystalline material, FeZrCuB nanocrystalline material, FeHfB nanocrystalline material, FeNbB nanocrystalline material, FeNbZrCuB nanocrystalline material, FeNbCuSiB nanocrystalline material and FeCuSiBP nanocrystalline material; The crystalline metallic soft magnetic material comprises at least one of iron, nickel, cobalt, iron-silicon alloy, iron-aluminum alloy, iron-nickel alloy and iron-cobalt alloy.
3. The soft magnetic composite material according to claim 1, It is characterized in that The particle size of the core is 2 μm-50 μm, and the thickness of the shell is 5 nm-1000 nm.
4. The soft magnetic composite material according to claim 1, It is characterized in that The soft magnetic composite material includes multiple layers of shells, and adjacent shells are made of different materials.
5. The soft magnetic composite material according to claim 1, It is characterized in that The ferrite includes at least one of manganese ferrite, zinc ferrite, manganese-zinc ferrite, manganese-magnesium-zinc ferrite, nickel-zinc ferrite and copper-zinc ferrite.
6. A method for preparing a soft magnetic composite material, It is characterized in that include: Placing the core material and the target material in a container, wherein the inner cavity cross section of the container is polygonal, and the core material comprises a first soft magnetic material, which is an amorphous soft magnetic material or a nanocrystalline soft magnetic material; The container is rotated in a direction perpendicular to the cross section of the inner cavity, the target material is kept stationary, and the material of the target material is deposited on the surface of the core material by physical vapor deposition to form a shell that at least partially wraps the core material; An insulating layer is formed on the surface of the shell, and the insulating layer at least partially wraps the shell to obtain soft magnetic composite particles, wherein the material of the shell includes a second soft magnetic material, and the second soft magnetic material is a crystalline metal soft magnetic material. The material of the insulating layer includes at least one of a ceramic material and a ferrite, and the ceramic material includes at least one of zirconium oxide, yttrium oxide, aluminum oxide and silicon carbide. The thickness of the insulating layer is 5nm-100nm.
7. The preparation method according to claim 6, It is characterized in that The rotation speed of the container is 20rpm-40rpm; The core material is heated during the physical vapor deposition process so that the temperature of the core material is 100° C.-400° C.
8. The preparation method according to claim 6, It is characterized in that The target material containing zirconium and yttrium elements is used, and a mixed gas containing inert gas and oxygen is introduced into the inner cavity of the container to make the pressure of the inner cavity 0.1Pa-5.0Pa, and the insulating layer is deposited on the surface of the outer shell. The material of the insulating layer includes zirconium oxide and yttrium oxide.
9. The preparation method according to claim 6, It is characterized in that An iron-nickel-zinc alloy is used as the target material, a mixed gas containing an inert gas and oxygen is introduced into the inner cavity of the container to make the pressure of the inner cavity 0.1Pa-5.0Pa, and the insulating layer is deposited on the surface of the outer shell. The material of the insulating layer includes nickel-zinc ferrite.
10. The preparation method according to claim 6, It is characterized in that The amorphous soft magnetic material is prepared by a water mist spraying method, wherein the particle size of the amorphous soft magnetic material is 2 μm-50 μm; The target material is an iron-nickel alloy, and the content of nickel in the iron-nickel alloy is 50%-80%.
11. The preparation method according to claim 6, It is characterized in that The method also includes dispersing the soft magnetic composite particles into a binder and performing compression molding, wherein the mass content of the binder in the soft magnetic composite material is 1%-10%.
Citation Information
Patent Citations
Method for preparing covering type compound powder for thermal spraying by vacuum magnetron sputtering
CN103046012A
Composite particle, method for producing composite particle, powder core, magnetic element, and electronic device