Biaxially oriented tube

By using multiphase propylene copolymers and a specific stretching method to prepare biaxially oriented tubes, the problems of long-term hydrostatic performance and uneven wall thickness in the prior art have been solved, achieving excellent hydrostatic performance and uniform wall thickness.

CN114502633BActive Publication Date: 2024-11-19SABIC GLOBAL TECHNOLOGIES BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080069607.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-04
Filing Date
2020-10-02
Publication Date
2024-11-19
Estimated Expiration
2040-10-02

AI Technical Summary

Technical Problem

Existing technologies make it difficult to simultaneously achieve good long-term hydrostatic performance and uniform wall thickness in biaxially oriented polypropylene pipes, and too much or too little rubber content will affect the tensile effect.

Method used

A biaxially oriented tube is prepared by using a polymer composition containing a multiphase propylene copolymer, wherein the propylene-based polymer consists of a propylene matrix and a dispersed ethylene-α-olefin copolymer, through specific axial and circumferential stretching steps, with the rubber content controlled in the range of 2.0-30 wt%.

Benefits of technology

Excellent long-term hydrostatic performance and uniform wall thickness of biaxially oriented tubes were achieved, improving the tube's resistance to internal pressure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005078517160000061
    Figure GDA0005078517160000061
  • Figure GDA0005078517160000181
    Figure GDA0005078517160000181
  • Figure GDA0005078517160000182
    Figure GDA0005078517160000182
Patent Text Reader

Abstract

The present invention relates to a biaxially oriented tube made from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of: (a1) a propylene based matrix, wherein the propylene based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene based matrix, and (a2) a dispersed ethylene-α-olefin copolymer, wherein the sum of the total amount of the propylene based matrix and the total amount of the dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) is 2.0-30.0 wt% relative to the propylene based polymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a pipe produced by biaxial stretching of a polypropylene composition. Background Art

[0002] It is known that physical and mechanical properties of polymeric materials can be improved by orienting the material. In many cases, orienting the material in one direction to improve properties can result in degradation of the same property in a direction perpendicular to the orientation direction. In order to adjust the properties in two directions, biaxial orientation of the material can be applied. Biaxial orientation means that the polymeric material is oriented in two mutually perpendicular directions. The tube can be oriented in both the axial and circumferential directions (annular directions) to improve properties such as long-term hydrostatic performance and low temperature impact resistance.

[0003] Pipes prepared by biaxial stretching of polypropylene compositions are known. US5910346 describes stretched pipes prepared from isotropic polypropylene pipes (ICI grade GSE 108). Morath et al., in Biaxially oriented polypropylene pipes, Plastics, Rubber and Composites 2006 vol 35 no 10, p. 447-454, describe biaxially oriented polypropylene pipes prepared from random polypropylene copolymers having a melt flow rate of 0.3 dg / min and an ethylene content of 4%.

[0004] One of the most important properties of a pipe is its resistance to crack growth.

[0005] An object of the present invention is to provide a biaxially oriented polypropylene pipe having good long term hydrostatic properties.

[0006] Accordingly, the present invention provides a biaxially oriented tube made from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0007] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0008] (a2) dispersed ethylene-α-olefin copolymer, wherein the sum of the total amount of propylene-based matrix and the total amount of dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) is 2.0-30.0 wt% relative to the propylene-based polymer.

[0009] The biaxially oriented tube prepared from the polymer composition refers to a biaxially oriented tube prepared by a method comprising the following steps:

[0010] a) forming the polymer composition into a pipe, and

[0011] b) stretching the tube of step a) in axial and circumferential directions to obtain a biaxially oriented tube.

[0012] Preferably, the biaxially oriented tube consists of a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0013] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0014] (a2) dispersed ethylene-α-olefin copolymers, wherein the sum of the total amount of propylene-based matrix and the total amount of dispersed ethylene-α-olefin copolymers in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) is 2.0-30 wt% relative to the propylene-based polymer;

[0015] and wherein the biaxially oriented tube is prepared by a process comprising the steps of:

[0016] a) forming the polymer composition into a pipe, and

[0017] b) stretching the tube of step a) in axial and circumferential directions to obtain a biaxially oriented tube.

[0018] The terms "tube" and "tube" are understood here as hollow elongated articles which may have a cross section of various shapes. The cross section may be, for example, annular, elliptical, square, rectangular or triangular. The term "diameter" is understood here as the largest dimension of the cross section.

[0019] It has surprisingly been found that the biaxially oriented tubes of the present invention have good long term hydrostatic properties.

[0020] According to the present invention, the propylene-based polymer in the polymer composition used to prepare the biaxially oriented tube comprises a heterophasic propylene copolymer. It has been found that the preparation of a biaxially oriented tube from a polymer composition having a certain amount of dispersed ethylene-α-olefin copolymer ('rubber' content) will obtain excellent long-term hydrostatic pressure properties. When the 'rubber' content in the composition is too low, the biaxial stretching step cannot be successfully carried out. When the 'rubber' content in the composition is too high, it is difficult to obtain a biaxially stretched tube. In addition, when the 'rubber' content in the composition is too high, fluctuations in the wall thickness of the obtained biaxially oriented tube will be observed.

[0021] Suitable rubber content in the propylene based polymer can be achieved by using a heterophasic propylene copolymer containing 2.0-30 wt% dispersed ethylene-α-olefin copolymer. Alternatively, if the amount of dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is not 2.0-30 wt%, additional components such as propylene homopolymers can be added to adjust the 'rubber' content of the composition.

[0022] The amount of (a2) is 2.0-30 wt %, such as at least 3.0 wt %, at least 4.0 wt %, at least 5.0 wt %, at least 7.0 wt % or at least 9.0 wt % relative to the propylene-based polymer. The amount of (a2) is preferably at most 25 wt %, more preferably at most 20 wt %, more preferably at most 15 wt %, more preferably at most 13 wt %, more preferably at most 10 wt % relative to the propylene-based polymer. The amount of (a2) is most preferably 4.0-7.0 wt % relative to the propylene-based polymer. The biaxially oriented tube thus formed has excellent long-term hydrostatic pressure properties and uniform wall thickness.

[0023] Propylene polymer

[0024] A) Heterophasic propylene copolymer

[0025] Heterophasic propylene copolymers are typically prepared by polymerizing propylene and subsequently polymerizing an ethylene-α-olefin mixture in the presence of a catalyst in one or more reactors. The resulting polymer material is heterophasic, but the specific morphology usually depends on the preparation process applied and the monomer ratios.

[0026] The heterophasic propylene copolymer used in the present invention can be produced by any conventional technique known to those skilled in the art, such as a multistage polymerization process, such as bulk polymerization, gas phase polymerization, slurry polymerization, solution polymerization or any combination thereof. Any conventional catalyst system can be used, such as Ziegler-Natta or metallocene catalysts. These techniques and catalysts are described, for example, in the following documents: WO06 / 010414; Polypropylene and other Polyolefins, by Ser van der Ven, Studies in Polymer Science 7, Elsevier 1990; WO06 / 010414, US4399054 and US4472524. The heterophasic propylene copolymer is preferably prepared using a Ziegler-Natta catalyst.

[0027] The heterophasic propylene copolymer may be prepared by a process comprising the steps of:

[0028] - polymerizing propylene and optionally ethylene and / or α-olefins in the presence of a catalyst system to obtain a propylene-based substrate, and

[0029] - subsequently polymerizing ethylene and α-olefins in a propylene-based matrix in the presence of a catalyst system to obtain a dispersed ethylene-α-olefin copolymer. These steps are preferably carried out in different reactors. The catalyst system used for the first and second steps may be the same or different.

[0030] The heterophasic propylene copolymer of the composition of the present invention consists of a propylene-based matrix and a dispersed ethylene-α-olefin copolymer. The propylene-based matrix usually forms a continuous phase in the heterophasic propylene copolymer. As is well known in the art, the amount of the propylene-based matrix and the dispersed ethylene-α-olefin copolymer can be varied by: 13 Confirmed by C-NMR.

[0031] The propylene-based matrix is ​​composed of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer is composed of at least 70 wt% of propylene monomer units and at most 30 wt% of comonomer units, based on the total weight of the propylene-based matrix, wherein the comonomer units are selected from ethylene monomer units and α-olefin monomer units having 4 to 10 carbon atoms, for example, the propylene copolymer is composed of at least 80 wt% of propylene monomer units and at most 20 wt% of comonomer units, at least 90 wt% of propylene monomer units and at most 10 wt% of comonomer units, or at least 95 wt% of propylene monomer units and at most 5 wt% of comonomer units.

[0032] The comonomer in the propylene copolymer of the propylene base is preferably selected from ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene and 1-decene, and is preferably ethylene.

[0033] The propylene-based matrix preferably consists of a propylene homopolymer. The fact that the propylene-based matrix consists of a propylene homopolymer is advantageous because a higher stiffness can be obtained compared to the case where the propylene-based matrix is ​​a propylene-α-olefin copolymer.

[0034] The melt flow index (MFI) of the propylene-based matrix (before mixing the heterophasic propylene copolymer into the composition of the present invention) is measured according to ISO 1133 (2.16 kg / 230°C), i.e., MFI PP For example it may be at least 0.1 dg / min, at least 0.2 dg / min, at least 0.3 dg / min, at least 0.5 dg / min and / or for example at most 20 dg / min, at most 10 dg / min, at most 5.0 dg / min, at most 3.0 dg / min, at most 1.0 dg / min.

[0035] The propylene based matrix is ​​preferably present in an amount of 60 to 98 wt%, such as up to 97 wt%, up to 96 wt%, up to 95 wt%, up to 93 wt% or up to 91 wt%, based on the total heterophasic propylene copolymer. The propylene based matrix is ​​preferably present in an amount of at least 70 wt%, more preferably at least 75 wt%, more preferably at least 80 wt%, more preferably at least 85 wt%, more preferably at least 87 wt%, more preferably at least 90 wt%, based on the total heterophasic propylene copolymer. The propylene based matrix is ​​most preferably present in an amount of 93 to 96 wt%, based on the total heterophasic propylene copolymer.

[0036] The propenyl matrix is ​​preferably semi-crystalline, i.e. not 100% amorphous, nor 100% crystalline. For example, the propenyl matrix contains at least 40% crystalline, such as at least 50%, such as at least 60% crystalline, and / or such as up to 80% crystalline, such as up to 70% crystalline. For example, the crystallinity of the propenyl matrix is ​​60-70%. For the purposes of the present invention, the crystallinity of the propenyl matrix is ​​measured using differential scanning calorimetry (DSC) according to ISO 11357-1 and ISO 11357-3 of 1997, using a scan rate of 10°C / min, a sample of 5 mg and a second heating curve using 207.1 J / g of 100% crystalline material as a theoretical standard.

[0037] In addition to the propylene-based matrix, the heterophasic propylene copolymer also comprises a dispersed ethylene-α-olefin copolymer. The dispersed ethylene-α-olefin copolymer is also referred to herein as 'dispersed phase'. The dispersed phase is embedded in the heterophasic propylene copolymer in a discontinuous form. The particle size of the dispersed phase is generally 0.05-2.0 microns, which can be measured by a transmission electron microscope (TEM). The amount of the dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is sometimes referred to herein as RC.

[0038] The amount of ethylene monomer units in the ethylene-α-olefin copolymer is preferably 34-60 wt%, preferably 40-60 wt%, 45-60 wt% or 50-60 wt%.The amount of ethylene monomer units in the dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is sometimes referred to herein as RCC2.

[0039] Preferably, the biaxially oriented tube is prepared from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0040] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0041] (a2) a dispersed ethylene-α-olefin copolymer, wherein the sum of the total amount of the propylene-based matrix and the total amount of the dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) relative to the propylene-based polymer is 2.0-30 wt%; and wherein the amount of ethylene monomer units in the ethylene-α-olefin copolymer of (a2) is 34-60 wt%, preferably 40-60 wt%, 45-60 wt% or 50-60 wt%.

[0042] The α-olefin in the ethylene-α-olefin copolymer is preferably selected from α-olefins having 3-8 carbon atoms. Examples of suitable α-olefins having 3-8 carbon atoms include, but are not limited to, propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene and 1-decene. The α-olefin in the ethylene-α-olefin copolymer is more preferably selected from α-olefins having 3-4 carbon atoms and any mixture thereof, and the α-olefin is more preferably propylene, in which case the ethylene-α-olefin copolymer is an ethylene-propylene copolymer.

[0043] Preferably, the biaxially oriented tube is prepared from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0044] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0045] (a2) a dispersed ethylene-α-olefin copolymer, wherein the sum of the total amount of propylene-based matrix and the total amount of dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) relative to the propylene-based polymer is 2.0-30 wt%; and wherein the amount of ethylene monomer units in the ethylene-α-olefin copolymer of (a2) is 34-60 wt%, preferably 40-60 wt%, 45-60 wt% or 50-60 wt%, and wherein the α-olefin in the ethylene-α-olefin copolymer (a2) is preferably selected from α-olefins having 3 to 8 carbon atoms.

[0046] MFI of the dispersed ethylene α-olefin copolymer (before the heterophasic propylene copolymer is mixed into the composition of the present invention) MFI 橡胶 For example, it may be at least 0.001 dg / min, at least 0.03 dg / min or at least 0.05 dg / min and / or for example at most 0.1 dg / min or 0.01 dg / min. MFI 橡胶 Calculate according to the following general formula:

[0047]

[0048] in

[0049] MFI 多相 is the MFI (dg / min) of the heterophasic propylene copolymer measured according to ISO 1133 (2.16 kg / 230°C),

[0050] MFI 基质 is the MFI (dg / min) of the propylene-based matrix measured according to ISO1133 (2.16 kg / 230°C),

[0051] The matrix content is the fraction of propylene-based matrix in the heterophasic propylene copolymer.

[0052] The rubber content is the fraction of the ethylene-α-olefin copolymer dispersed in the heterophasic propylene copolymer. The sum of the matrix content and the rubber content is 1. For the avoidance of doubt, in the general formula Log means log 10 .

[0053] The amount of dispersed ethylene-α-olefin copolymer is preferably 2.0-40wt%, such as at least 3.0wt%, at least 4.0wt%, at least 5.0wt%, at least 7.0wt% or at least 9.0wt%. Based on the total heterophasic propylene copolymer, the amount of dispersed ethylene-α-olefin copolymer is preferably at most 30wt%, more preferably at most 25wt%, more preferably at most 20wt%, more preferably at most 15wt%, more preferably at most 13wt%, more preferably at most 10wt%. When the amount of dispersed ethylene-α-olefin copolymer based on the total heterophasic propylene copolymer is at most 30wt%, the composition can be composed of heterophasic propylene copolymer. Most preferably, the amount of dispersed ethylene-α-olefin copolymer based on the total heterophasic propylene copolymer is 4.0-7.0wt%.

[0054] Preferably, the biaxially oriented tube is prepared from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0055] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0056] (a2) dispersed ethylene-α-olefin copolymer, wherein the sum of the total amount of propylene-based matrix and the total amount of dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) is 2.0-30 wt% relative to the propylene-based polymer; and wherein (a2) is present in an amount of 2.0-40 wt%, such as at least 3.0 wt%, at least 4.0 wt%, at least 5.0 wt%, at least 7.0 wt% or at least 9.0 wt% or up to 30 wt%, more preferably up to 25 wt%, more preferably up to 20 wt%, more preferably up to 15 wt%, more preferably up to 13 wt%, more preferably up to 10 wt%, based on the total heterophasic propylene copolymer.

[0057] In the heterophasic propylene copolymer of the composition of the present invention the sum of the total weight of the propylene based matrix and the total weight of the dispersed ethylene-α-olefin copolymer is 100 wt% of the heterophasic propylene copolymer.

[0058] Preferably, the heterophasic propylene copolymer has a p-xylene soluble fraction (CXS) at 25 °C measured according to ISO 16152:2005 of 20 to 5 wt%, such as 18 to 7%.

[0059] The amount of ethylene monomer units in the heterophasic propylene copolymer (sometimes referred to as TC2) is preferably in the range of 1.0 to 16 wt%, such as 2.0 to 14 wt%, 3.0 to 12 wt% or 4.0 to 10 wt% of the heterophasic propylene copolymer.

[0060] The heterophasic propylene copolymer preferably has an MFI measured according to ISO 1133-1:2011 (MFI 230°C / 2.16 kg) of 0.1 to 10.0 g / 10 min, more preferably 0.1 to 4.0 g / 10 min, especially 0.1 to 1.0 g / 10 min.

[0061] Preferably, in the heterophasic propylene copolymer of the present invention the comonomer in the propylene-α-olefin copolymer is selected from ethylene and α-olefins having 4-10 carbon atoms, and the α-olefin in the ethylene-α-olefin copolymer is selected from α-olefins having 3-8 carbon atoms.

[0062] Most preferably, in the heterophasic propylene copolymer of the present invention the comonomer in the propylene-α-olefin copolymer is ethylene and the α-olefin in the ethylene-α-olefin copolymer is propylene.

[0063] Preferably, the amount of A) is 30-100 wt%, such as at least 40 wt%, at least 50 wt%, greater than 50 wt%, at least 55 wt%, at least 60 wt%, at least 70 wt%, at least 80 wt%, at least 90 wt%, at least 95 wt%, at least 98 wt%, at least 99 wt% or 100 wt%, relative to the propylene-based polymer.

[0064] In a preferred embodiment, the propylene-based polymer consists of A), wherein the amount of (b) is 2.0-30 wt% relative to A). This is advantageous because the pipe can be prepared by a simple process using a single type of propylene-based polymer.

[0065] Preferably, the biaxially oriented tube is prepared from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0066] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0067] (a2) a dispersed ethylene-α-olefin copolymer, wherein the sum of the total amount of propylene-based matrix and the total amount of dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) is 2.0-30 wt% relative to the propylene-based polymer; and wherein the amount of A) is 30-100 wt% relative to the propylene-based polymer, such as at least 40 wt%, at least 50 wt%, greater than 50 wt%, at least 55 wt%, at least 60 wt%, at least 70 wt%, at least 80 wt%, at least 90 wt%, at least 95 wt%, at least 98 wt%, at least 99 wt% or 100 wt%.

[0068] Preferably, the biaxially oriented tube is prepared from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0069] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0070] (a2) a dispersed ethylene-α-olefin copolymer, wherein the sum of the total amount of propylene-based matrix and the total amount of dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) relative to the propylene-based polymer is 2.0-30 wt%; and wherein the amount of A) relative to the propylene-based polymer is 30-100 wt%, preferably 90-100 wt%, and wherein (a2) is present in an amount of 2.0-40 wt%, preferably 4.0-15 wt%, based on the total heterophasic propylene copolymer.

[0071] B) Propylene homopolymer

[0072] The propylene-based polymer may also contain B) a propylene homopolymer. This can be used to adjust the rubber content in the propylene-based polymer to ensure excellent long-term hydrostatic pressure performance. When the amount of (a2) is greater than 30 wt% relative to A), the propylene-based polymer contains B) so that the amount of (a2) is at most 30 wt% relative to the propylene-based polymer. The use of B) is advantageous because pipes with different properties can be prepared from a single grade of heterophasic propylene copolymers by using different amounts of homopolymers.

[0073] The amount of B) is preferably 0-70 wt%, such as at least 5 wt%, at least 10 wt%, at least 15 wt%, at least 20 wt% or at least 25 wt% and / or at most 65 wt%, at most 60 wt%, at most 55 wt%, at most 50 wt%, at most 45 wt% or at most 40 wt% relative to the propylene-based polymer. For example, the amount of B) can be 5-30 wt% or 30-70 wt% relative to the propylene-based polymer.

[0074] The melt flow index of the propylene homopolymer measured according to ISO 1133-1:2011 (230° C. / 2.16 kg) is preferably 0.1 to 10.0 g / 10 min, more preferably 0.1 to 4.0 g / 10 min, particularly preferably 0.1 to 1.0 g / 10 min.

[0075] The total amount of A) and B) is preferably at least 80 wt%, at least 90 wt%, at least 95 wt%, at least 98 wt%, at least 99 wt% or 100 wt%.

[0076] C) Random propylene copolymer

[0077] The propylene-based polymer may also comprise C) a random copolymer of propylene and a comonomer which is ethylene and / or an α-olefin having 4 to 10 carbon atoms. When the amount of (a2) is relatively small relative to the propylene-based polymer, this component may be used, for example, to adjust the properties of a pipe.

[0078] The amount of C) relative to the propylene-based polymer is generally not too large, such as up to 20 wt%, such as 1-10 wt%. In some embodiments, the propylene-based polymer does not include C) a random copolymer of propylene and a comonomer, wherein the comonomer is ethylene and / or an α-olefin having 4-10 carbon atoms.

[0079] In some embodiments, the comonomer content of the random copolymer is less than 3.8 wt% based on the random copolymer. When the comonomer content of the random copolymer is less than 3.8 wt%, the comonomer content is preferably at least 0.1 wt%, preferably 0.5-3.5 wt%, 0.5-3.0 wt% or 1.0-2.0 wt% based on the random copolymer.

[0080] In some embodiments, the random copolymer has a comonomer content of at least 3.8 wt% based on the random copolymer. When the random copolymer has a comonomer content of at least 3.8 wt%, the comonomer content can be 3.8-10.0 wt%, such as 4.0-8.0 wt% or 4.2-6.0 wt% based on the random copolymer.

[0081] The term "comonomer content" is understood herein as the amount of comonomer derived units. The sum of the comonomer content and the amount of propylene derived units in the random propylene copolymer is 100%.

[0082] The comonomer is preferably ethylene, 1-butene, 1-hexene and / or 1-octene. The most preferred comonomer is ethylene.

[0083] The random propylene copolymer preferably has a melt flow index of 0.1 to 10.0 g / 10 min, more preferably 0.1 to 4.0 g / 10 min, more preferably 0.1 to 1.0 g / 10 min, as measured according to ISO 1133-1:2011 (230° C. / 2.16 kg).

[0084] The total amount of A), B) and C) is typically at least 95 wt%, at least 98 wt%, at least 99 wt% or 100 wt%, based on the propylene-based polymer.

[0085] Preferred embodiments

[0086] In some preferred embodiments, the propylene-based polymer consists of A), wherein the amount of (b) is 2.0-30 wt%, preferably 4.0-15 wt%, relative to the propylene-based polymer.

[0087] In some preferred embodiments, the propylene-based polymer consists of A) and B), wherein the amount of (b) is 4.0-15 wt% relative to the propylene-based polymer, and the amount of (b) is not greater than 30 wt% relative to A).

[0088] In some preferred embodiments, the propylene-based polymer consists of A) and B), wherein the amount of (b) is 4.0-15 wt% relative to the propylene-based polymer, and the amount of (b) is up to 30 wt% relative to A).

[0089] In some preferred embodiments, the propylene-based polymer consists of A) and B), wherein the amount of (b) is 4.0-15 wt% relative to A), wherein the amount of A) is 75-90 wt% relative to the propylene-based polymer, and the amount of B) is 10-25 wt% relative to the propylene-based polymer.

[0090] In some preferred embodiments, the propylene-based polymer consists of A) and B), wherein the amount of (b) is 4.0-15 wt% relative to A), wherein the amount of A) is 50-75 wt% relative to the propylene-based polymer, and the amount of B) is 25-50 wt% relative to the propylene-based polymer.

[0091] The polymer composition containing a propylene-based polymer preferably contains substantially no other polymers than the propylene-based polymer.

[0092] The amount of propylene-based polymer relative to the total amount of polymers in the polymer composition may be at least 95 wt%, at least 98 wt%, at least 99 wt% or 100 wt%.

[0093] Preferably, the biaxially oriented tube is prepared from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0094] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0095] (a2) dispersed ethylene-α-olefin copolymers, wherein the sum of the total amount of propylene-based matrix and the total amount of dispersed ethylene-α-olefin copolymers in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) relative to the propylene-based polymer is 2.0-30 wt%; and wherein the amount of propylene-based polymer relative to the total amount of polymers in the polymer composition can be at least 95 wt%, at least 98 wt%, at least 99 wt% or 100 wt%.

[0096] Preferably, the biaxially oriented tube is prepared from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0097] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0098] (a2) dispersed ethylene-α-olefin copolymers, wherein the sum of the total amount of propylene matrix and the total amount of dispersed ethylene-α-olefin copolymers in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) relative to the propylene based polymer is 2.0-30 wt%; and wherein the amount of A) relative to the propylene based polymer is 30-100 wt%, preferably 90-100 wt%, and wherein the amount of propylene based polymer relative to the total amount of polymers in the polymer composition can be at least 95 wt%, at least 98 wt%, at least 99 wt% or 100 wt%.

[0099] Preferably, the biaxially oriented tube is prepared from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0100] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0101] (a2) a dispersed ethylene-α-olefin copolymer, wherein the sum of the total amount of propylene-based matrix and the total amount of dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) relative to the propylene-based polymer is 2.0-30 wt%; and wherein the amount of A) relative to the propylene-based polymer is 30-100 wt%, preferably 90-100 wt%, and wherein (a2) is present in an amount of 2.0-40 wt%, preferably 4.0-15 wt%, based on the total heterophasic propylene copolymer.

[0102] Preferably, the biaxially oriented tube is prepared from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0103] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0104] (a2) a dispersed ethylene-α-olefin copolymer, wherein the sum of the total amount of propylene-based matrix and the total amount of dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) relative to the propylene-based polymer is 2.0-30 wt%; and wherein the amount of A) relative to the propylene-based polymer is 30-100 wt%, preferably 90-100 wt%, and wherein (a2) is present in an amount of 2.0-40 wt%, preferably 4.0-15 wt%, based on the total heterophasic propylene copolymer, and wherein the amount of propylene-based polymer relative to the total amount of polymers in the polymer composition may be at least 95 wt%, at least 98 wt%, at least 99 wt% or 100 wt%.

[0105] The polymer composition may contain components other than the propylene-based polymer, such as additives and fillers.

[0106] Examples of additives include: nucleating agents, stabilizers such as heat stabilizers; antioxidants; UV stabilizers; colorants such as pigments and dyes; clarifying agents; surface tension modifiers; lubricants; flame retardants; mold release agents; flow improvers; plasticizers; antistatic agents; external elastic impact modifiers; foaming agents; and / or components that enhance the interface connection between the polymer and the filler, such as maleated polyethylene. The amount of additives is generally 0-5wt%, such as 1-3wt%, relative to the total amount of the composition.

[0107] Examples of fillers include glass fiber, talc, mica, nanoclay. The amount of filler is generally 0-40 wt%, such as 5-30 wt% or 10-25 wt%, relative to the total amount of the composition.

[0108] Therefore, in some embodiments, the polymer composition further comprises 0-5 wt% of additives and 0-40 wt% of fillers.

[0109] The polymer composition may be obtained by melt mixing the polyolefin and any other optional components.

[0110] Preferably, the total amount of the propylene-based polymer and the optional additives and the optional filler is 100 wt% relative to the total amount of the composition.

[0111] Method steps

[0112] A biaxially oriented tube is prepared by a process comprising the steps of:

[0113] a) forming the polymer composition into a pipe, and

[0114] b) stretching the tube of step a) in axial and circumferential directions to obtain a biaxially oriented tube.

[0115] The process for producing the pipe can be carried out as a continuous process or as a batch process. A continuous process is understood here to be a process in which the polymer composition is fed continuously for the pipe production step a) while the stretching step b) is carried out continuously.

[0116] The polymer composition may be formed into a tube by any known method such as extrusion or injection molding (step a). Biaxial stretching (step b) may be performed by any known method.

[0117] A method of forming a polymer composition into a tube and biaxially stretching the tube is described in US6325959:

[0118] Conventional devices for extruding plastic pipes include an extruder, a nozzle, a calibrator, a cooling device, a pulling device, and a device for cutting or winding the pipe. The molten material of the polymer passes from the extruder through the nozzle and reaches the calibrator, and the cooling and finished pipe is subjected to shearing and stretching along the axial direction of the pipe, and a pipe with a substantially uniaxial orientation along its axial direction will be obtained. Another reason that contributes to the orientation of the polymer material along the direction of material flow is that the pipe can withstand the tension associated with the preparation.

[0119] In order to achieve biaxial orientation, the device can be supplemented downstream of the traction device with equipment for controlling the temperature of the tube to a temperature suitable for biaxial orientation of the tube, orientation equipment, calibration equipment, cooling equipment and traction equipment for providing the biaxially oriented tube to a cutting device or a winder.

[0120] It is also possible to carry out the biaxial orientation after extrusion directly in connection with a first calibration device, in which case the above-mentioned supplementary device follows the first calibration device.

[0121] Biaxial orientation of the tube can be accomplished in a variety of ways, such as mechanically by an internal mandrel or by an internal pressurized fluid such as air or water or the like. Other methods are orienting the tube by rollers, such as by placing the tube on a mandrel and rotating the mandrel and tube relative to one or more pressure rollers engaged with the tube, or by internally disposed pressure rollers rotating relative to the tube against an externally disposed die or calibration device.

[0122] In addition, Morath et al., Biaxially oriented polypropylene pipes, Plastics, Rubber and Composites 2006 vol 35 no 10, p. 447-454, describe a method for preparing biaxially oriented tubes from random propylene copolymers.

[0123] Conditions of step b)

[0124] Those skilled in the art can select suitable conditions such as temperature of step b) to obtain a biaxially oriented tube. Step b) is carried out at a stretching temperature that orients the propylene-based polymer in the polymer composition.

[0125] The stretching temperature is selected according to the melting point of the propylene-based polymer in the polymer composition.

[0126] The stretching temperature is defined here as the temperature at the surface of the tube in step a) just before step b). Before step b), the mandrel and the tube in step a) are heated so that they have the desired stretching temperature. This can also be achieved by soaking the mandrel and the tube in step a) in the stretching temperature for a sufficient time (e.g. 30 minutes) to reach thermal equilibrium (the temperature is preferably controlled within ±1°C).

[0127] Melting points are measured by differential scanning calorimetry according to ASTM D3418. DSC measurements are performed using a DSC TA Q20 and a mechanical refrigerator capable of reaching -90°C. To avoid degradation, the measurements can be performed under a nitrogen flow. The method followed is:

[0128] First heating: -40℃ to 230℃@10℃ / min (maintain at the end temperature for 3min)

[0129] Cooling: 230℃ to -40℃@10℃ / min

[0130] Second heating: -40℃ to 230℃@10℃ / min

[0131] The sample used is 3-5 mg

[0132] The melting point was recorded from the second heating cycle.

[0133] The stretching temperature may be selected to be below the melting point of the propylene-based polymer in the polymer composition.

[0134] The stretching temperature may be 1-30°C lower than the melting point of the propylene-based polymer in the polymer composition, for example 2-20°C or 3-10°C lower.

[0135] When the propylene-based polymer comprises different propylene-based polymers having different melting points, the stretching temperature may be determined so as to orient most of the propylene-based polymers. Those skilled in the art may appropriately determine a suitable stretching temperature according to the type and amount of the propylene-based polymer present in the polymer composition.

[0136] Generally, it is possible to select the stretching temperature within a suitable temperature range based on the melting point of each propylene-based polymer present in the polymer composition.

[0137] When the melting points of the propylene-based polymers present in the polymer composition vary greatly, the stretching temperature can be selected based on the propylene-based polymers present in large amounts. For example, the stretching temperature can be selected based on the melting point of the propylene-based polymer present in the largest amount in the polymer composition. When determining the stretching temperature, it is possible to ignore the propylene-based polymers present in small amounts (e.g., less than 5 wt % of the polymer composition).

[0138] In some embodiments, step b) is carried out at a stretching temperature of 140-160°C, preferably 145-155°C.

[0139] Stretch ratio

[0140] Typically, step b) is carried out at an axial stretch ratio of 1.1 to 5.0 and an average hoop stretch ratio of 1.1 to 3.0.

[0141] Preferably, the biaxially oriented tube is prepared from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0142] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0143] (a2) dispersed ethylene-α-olefin copolymers, wherein the sum of the total amount of propylene-based matrix and the total amount of dispersed ethylene-α-olefin copolymers in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) is 2.0-30 wt% relative to the propylene-based polymer;

[0144] and wherein the biaxially oriented tube is prepared by a process comprising the steps of:

[0145] a) forming the polymer composition into a pipe, and

[0146] b) stretching the tube of step a) in axial and circumferential directions to obtain a biaxially oriented tube, wherein step b) is performed at an axial stretching ratio of 1.1-5.0 and an average hoop stretching ratio of 1.1-3.0.

[0147] More preferably, the biaxially oriented tube is prepared from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0148] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0149] (a2) dispersed ethylene-α-olefin copolymers, wherein the sum of the total amount of propylene-based matrix and the total amount of dispersed ethylene-α-olefin copolymers in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) is 2.0-30 wt% relative to the propylene-based polymer;

[0150] and wherein the biaxially oriented tube is prepared by a process comprising the steps of:

[0151] a) forming the polymer composition into a pipe, and

[0152] b) stretching the tube of step a) in axial and circumferential directions to obtain a biaxially oriented tube, wherein step b) is carried out at a stretching temperature of 140-160°C, preferably 145-155°C, and an axial stretch ratio of 1.1-5.0 and an average hoop stretch ratio of 1.1-3.0.

[0153] More preferably, the biaxially oriented tube is prepared from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0154] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0155] (a2) a dispersed ethylene-α-olefin copolymer, wherein the sum of the total amount of propylene-based matrix and the total amount of dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) relative to the propylene-based polymer is 2.0-30 wt%; and wherein the amount of propylene-based polymer relative to the total amount of polymers in the polymer composition may be at least 95 wt%, at least 98 wt%, at least 99 wt% or 100 wt%;

[0156] and wherein the biaxially oriented tube is prepared by a process comprising the steps of:

[0157] a) forming the polymer composition into a pipe, and

[0158] b) stretching the tube of step a) in axial and circumferential directions to obtain a biaxially oriented tube, wherein step b) is carried out at a stretching temperature of 140-160°C, preferably 145-155°C, and an axial stretch ratio of 1.1-5.0 and an average hoop stretch ratio of 1.1-3.0.

[0159] Preferably, the biaxially oriented tube is prepared from a polymer composition comprising a propylene based polymer, wherein the propylene based polymer comprises A) a heterophasic propylene copolymer, wherein the heterophasic propylene copolymer consists of:

[0160] (a1) a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and

[0161] (a2) a dispersed ethylene-α-olefin copolymer, wherein the sum of the total amount of propylene-based matrix and the total amount of dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is 100 wt%, wherein the amount of (a2) relative to the propylene-based polymer is 2.0-30 wt%; and wherein the amount of A) relative to the propylene-based polymer is 30-100 wt%, preferably 90-100 wt%, and wherein (a2) is present in an amount of 2.0-40 wt%, preferably 4.0-15 wt%, based on the total heterophasic propylene copolymer, and wherein the amount of propylene-based polymer relative to the total amount of polymers in the polymer composition may be at least 95 wt%, at least 98 wt%, at least 99 wt% or 100 wt%,

[0162] and wherein the biaxially oriented tube is prepared by a process comprising the steps of:

[0163] a) forming the polymer composition into a pipe, and

[0164] b) stretching the tube of step a) in axial and circumferential directions to obtain a biaxially oriented tube, wherein step b) is performed at an axial stretching ratio of 1.1-5.0 and an average hoop stretching ratio of 1.1-3.0.

[0165] The average hoop stretch ratio is preferably 1.1-2.0.

[0166] The axial stretch ratio is preferably 1.1-4.0, such as 1.1-3.6 or 1.1-3.2. For obtaining a biaxially oriented tube with a larger outer diameter, the axial stretch ratio is usually larger.

[0167] The axial stretch ratio of the stretched tube is defined as the ratio of the cross-sectional area of ​​the starting isotropic tube to the cross-sectional area of ​​the biaxially oriented tube (i.e., the product), i.e.:

[0168]

[0169] OD stands for outside diameter and ID stands for inside diameter.

[0170] In the case of expansion tube stretching, the hoop stretch ratio of the product varies from the inner wall to the outer wall. These stretch ratios are defined as:

[0171]

[0172] The average hoop stretch ratio can be defined as:

[0173]

[0174] in:

[0175] Biaxially oriented tube

[0176] The biaxially oriented tube of the present invention can be a pressure tube or a non-pressure tube. The preferred tube is a pressure tube.

[0177] The wall thickness of the biaxially oriented tube can generally be 0.3mm to 10cm. The outer diameter of the biaxially oriented tube can generally be 10-2000mm. In some embodiments, the outer diameter of the biaxially oriented tube is 10mm to 10cm, and the thickness is 0.3-3mm or 1-3mm. In some instances, the outer diameter of the biaxially oriented tube is 10-50cm, and the thickness is 1mm to 1cm. In some instances, the outer diameter of the biaxially oriented tube is 50cm to 2m, and the thickness is 5mm to 10cm.

[0178] The biaxially oriented tube of the present invention preferably has a time to failure measured according to ISO 1167-1 at a stress level of 20 MPa and a temperature of 20° C. of at least 100 hours, preferably at least 400 hours, more preferably at least 1000 hours.

[0179] It should be noted that the present invention relates to all possible combinations of features described herein. It should therefore be understood that all combinations of features relating to the compositions of the present invention, all combinations of features relating to the methods of the present invention, and all combinations of features relating to the compositions of the present invention and all combinations of features relating to the methods of the present invention are described herein.

[0180] It should also be noted that the term 'comprising' does not exclude the presence of other elements. However, it should be understood that the description of a product / composition comprising a certain component also discloses a product / composition consisting of these components. A product / composition consisting of these components may be advantageous because it provides a simpler and more economical method for preparing the product / composition. Similarly, it should also be understood that the description of a method comprising certain steps also discloses a method consisting of these steps. A method consisting of these steps may be advantageous because it provides a simpler and more economical method.

[0181] When lower and upper numerical limits for parameters are mentioned, it is also understood that the range resulting from the combination of the lower and upper values ​​is disclosed.

[0182] The present invention will now be described by way of the following examples, but the present invention is not limited thereto.

[0183] Material:

[0184] rPP1: propylene-ethylene copolymer with a comonomer content of 4 wt% and MFR 230°C / 2.16kg of 0.3 g / 10 min, Tm = 142.1°C

[0185] IPC1: a heterophasic propylene copolymer consisting of 84.5 wt% of a propylene homopolymer (MFI 230°C / 2.16 kg of 0.55 dg / min) and 15.5 wt% of an ethylene-propylene copolymer, wherein the amount of ethylene-derived units in the ethylene-propylene copolymer is 55 wt%, MFI 230°C / 2.16 kg of 0.3 dg / min

[0186] IPC2: a heterophasic propylene copolymer consisting of 91.0 wt% of a propylene homopolymer (MFI 230°C / 2.16 kg of 0.43 dg / min) and 9.0 wt% of an ethylene-propylene copolymer, wherein the amount of ethylene-derived units in the ethylene-propylene copolymer is 58 wt%, and the MFI 230°C / 2.16 kg is 0.3 dg / min

[0187] hPP1: propylene homopolymer, MFI 230°C / 2.16kg: 0.30 dg / min.

[0188] Production of Biaxially Oriented Tubes:

[0189] The heterophasic propylene copolymer was pelletized using a twin screw extruder. The processing temperature and screw profile were standard for polypropylene compounding. Standard additives for propylene based pipes were added during pelletization.

[0190] Thick tubular structures having dimensions of about 32 mm outer diameter and about 16 mm inner diameter were produced using these compounded pellets. These thick tubes were stretched over an expanding tapered mandrel having an outlet diameter of 32 mm and a half angle of 15 degrees at the temperatures shown in Table 1. The tubes stretched very uniformly through the thickness and could be stretched to relatively low axial stretch ratios.

[0191] These thick tubes were stretched at a stretching speed of 100 mm / min over an expanded tapered mandrel with an outlet diameter of 61-65 mm and a half angle of 15 degrees at the temperature shown in Table 1. The axial stretch ratio was 3 and the average annular stretch ratio was 1.3.

[0192] The internal pressure resistance of the pipes was measured according to ISO 1167-1 at a stress level of 20 MPa at 20° C. The failure times of the pipes are given in Table 1 below.

[0193] Table 1

[0194]

[0195] Some fluctuations in the wall thickness of the biaxially oriented tube obtained were observed for Example 7. No fluctuations in the wall thickness of the biaxially oriented tube obtained were observed for Examples 8, 9 and 10.

[0196] It is appreciated that biaxially oriented tubes made from compositions comprising heterophasic propylene copolymers have a longer time to failure than biaxially oriented tubes or unstretched tubes made from random propylene-ethylene copolymers.

[0197] It is also understood that the lower the amount of dispersed phase in the heterophasic propylene copolymer, the longer the time to failure. By adding homopolymers the amount of dispersed phase in the heterophasic propylene copolymer relative to the total composition can be adjusted, which influences the time to failure (Examples 8, 9 and 10).

Claims

1. A biaxially oriented tube prepared from a polymer composition, wherein the polymer composition comprises a propylene-based polymer, the amount of the propylene-based polymer relative to the total amount of polymers in the polymer composition is at least 95 wt%, and the propylene-based polymer comprises A) a heterophasic propylene copolymer, wherein the amount of the heterophasic propylene copolymer relative to the propylene-based polymer is 30 to 100 wt%, and wherein the heterophasic propylene copolymer, based on its total amount, consists of: (a1) 60 to 98 wt% of a propylene-based matrix, wherein the propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer, wherein the propylene copolymer consists of at least 70 wt% of propylene monomer units and at most 30 wt% of ethylene and / or α-olefin monomer units, based on the total weight of the propylene-based matrix, and (a2) a dispersed ethylene-α-olefin copolymer, wherein the amount of the dispersed ethylene-α-olefin copolymer is 2.0-20.0 wt% relative to the propylene-based polymer, the amount of ethylene monomer units in the dispersed ethylene-α-olefin copolymer is 34-60 wt%, wherein the sum of the total amount of the propylene-based matrix and the total amount of the dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer is 100 wt%; The polymer composition further comprises 0-5 wt% of additives and 0-40 wt% of fillers, wherein the additives include: Nucleating agent; stabilizer; colorant; clarifying agent; surface tension modifier; lubricant; flame retardant; mold release agent; flow improver; plasticizer; antistatic agent; external elastic impact modifier; foaming agent; and / or a component that enhances the interface connection between the polymer and the filler; and the filler is selected from glass fiber, talc, mica and nano clay, The biaxially oriented tube is prepared by a method comprising the following steps: a) forming the polymer composition into a pipe, and b) stretching the tube of step a) in the axial and circumferential directions to obtain a biaxially oriented tube, The step b) is carried out at a stretching temperature of 140-160° C., an axial stretching ratio of 1.1-5.0 and an average hoop stretching ratio of 1.1-3.

0.

2. The biaxially oriented tube of claim 1, wherein the amount of (a2) the dispersed ethylene-α-olefin copolymer is 4.0-13 wt% relative to the propylene-based polymer.

3. The biaxially oriented tube according to claim 1 or 2, wherein the amount of (a2) dispersed ethylene-α-olefin copolymer is 2.0-40 wt% relative to A) heterophasic propylene copolymer.

4. The biaxially oriented tube of claim 1 or 2, wherein the (a1) propylene-based matrix is ​​a propylene homopolymer and the (a2) dispersed ethylene-α-olefin copolymer is an ethylene-propylene copolymer.

5. The biaxially oriented tube of claim 1 or 2, wherein the propylene-based polymer has a melt flow index of 0.1 to 10.0 g / 10 min as measured at 230°C / 2.16 kg according to ISO 1133-1:2011.

6. The biaxially oriented tube of claim 1 or 2, wherein the amount of the propylene-based polymer is 100 wt% relative to the total amount of polymers in the polymer composition.

7. The biaxially oriented tube of claim 1 or 2, wherein the polymer composition further comprises 1-3 wt% of an additive and 5-30 wt% of a filler.

8. The biaxially oriented tube of claim 1 or 2, wherein step b) is carried out at a stretching temperature of 145-155°C, an axial stretch ratio of 1.1-4.0 and an average hoop stretch ratio of 1.1-2.

0.

9. The biaxially oriented tube of claim 1 or 2, wherein the biaxially oriented tube has a time to failure of at least 100 hours measured according to ISO 1167-1 at a stress level of 20 MPa and a temperature of 20°C.

10. The biaxially oriented tube of claim 1 or 2, wherein the amount of A) the heterophasic propylene copolymer is 40-100 wt% relative to the propylene-based polymer.

11. The biaxially oriented tube of claim 1 or 2, wherein the propylene-based polymer consists of A) a heterophasic propylene copolymer, wherein the amount of (a2) dispersed ethylene-α-olefin copolymer is 2.0-20 wt% relative to A) the heterophasic propylene copolymer.

12. The biaxially oriented tube of claim 1 or 2, wherein the propylene-based polymer further comprises: B) 0-70 wt% of a propylene homopolymer, and / or C) 0-20 wt% of a random copolymer of propylene and a comonomer, wherein the comonomer is ethylene and / or an α-olefin having 4 to 10 carbon atoms, The total amount of A), B) and C) is 100 wt% relative to the propylene-based polymer.

13. The biaxially oriented tube of claim 12, wherein the amount of B) the propylene homopolymer is 5.0-70 wt% relative to the propylene-based polymer.

14. The biaxially oriented tube of claim 12, wherein the amount of C) the random copolymer of propylene and the comonomer is 1.0-20 wt% relative to the propylene-based polymer.