Resin composition for sintering, inorganic fine particle dispersion slurry composition, and inorganic fine particle dispersion sheet
By using a combination of high molecular weight (meth)acrylic resin and water-soluble surfactant, the problem of high decomposition temperature of the binder resin in ceramic capacitors and large residual carbon amount after firing is solved, and low-temperature and efficient firing are achieved High-strength finished product, suitable for multilayering and thinning of ceramic laminates.
Patent Information
- Application Number
- CN202080069553.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-17
- Filing Date
- 2020-12-10
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-12-10
AI Technical Summary
In the manufacturing of existing ceramic capacitors, the binder resin used is high in decomposition temperature during low temperature firing, which makes it impossible to use in combination with metals that are prone to oxidation or low melting point glass. The residual carbon amount after firing is large, and the yield is low. The existing acrylic resin has poor sintering properties and insufficient sheet strength.
A high molecular weight (meth)acrylic resin containing a specific substituent is used as a resin composition for sintering, combined with a water-soluble surfactant, polymerizes through a water-soluble radical polymerization initiator to form a high molecular weight resin for manufacturing inorganic particles. Disperse the sheet to achieve low temperature decomposition and high strength forming.
It realizes efficient sintering at low temperatures, reduces residual carbon, improves the strength and yield of the ceramic laminate, takes into account both sintering properties and sheet strength, and is suitable for multilayering and thin filmization.
Smart Images

Figure BDA0003580552210000251 
Figure BDA0003580552210000261 
Figure BDA0003580552210000291
Abstract
Description
Technical Field
[0001] The present invention relates to a sintering resin composition, an inorganic fine particle dispersion slurry composition containing the sintering resin composition, and an inorganic fine particle dispersion sheet formed using the sintering resin composition or the inorganic fine particle dispersion slurry composition. Background Art
[0002] In recent years, compositions in which inorganic fine particles such as ceramic powder and glass particles are dispersed in a binder resin have been used for production of laminated electronic components such as ceramic capacitors.
[0003] Such ceramic capacitors are generally manufactured by the following method: First, additives such as a plasticizer and a dispersant are added to a solution obtained by dissolving a binder resin in an organic solvent, and then ceramic raw material powder is added and uniformly mixed using a ball mill or the like to obtain an inorganic fine particle dispersion composition.
[0004] The obtained inorganic fine particle dispersion composition is cast on a support surface such as a release-treated polyethylene terephthalate film or a SUS plate using a doctor blade or a reverse roll coater, and after volatile components such as an organic solvent are distilled off, the composition is peeled off from the support to obtain a ceramic green sheet.
[0005] Next, a conductive paste that will become an internal electrode is applied to the obtained ceramic green sheets by screen printing or the like, and a plurality of sheets are stacked, heated, and pressed to obtain a laminate. The so-called degreasing treatment is performed, that is, the obtained laminate is heated to thermally decompose and remove components such as a binder resin, and then fired to obtain a ceramic fired body with internal electrodes. Furthermore, external electrodes are applied to the end faces of the obtained ceramic fired body and fired to complete a laminated ceramic capacitor.
[0006] For example, Patent Document 1 describes a ceramic molding binder composition comprising 60 to 99 wt % of isobutyl methacrylate, 1 to 39 wt % of 2-ethylhexyl methacrylate, and 1 to 15 wt % of a methacrylate having a hydroxyl group at the β-position or ω-position, and having a molecular weight of 160,000 to 180,000.
[0007] Patent Document 2 describes that methyl methacrylate, isobutyl methacrylate, and crosslinkable bifunctional methacrylate are emulsified and polymerized starting from seed particles to obtain an acrylic resin for a fired paste having a high viscosity sufficient for screen printing, and a fired paste composition containing the acrylic resin.
[0008] Patent Document 3 describes a water-based binder resin composition for firing, which contains a polymerization reaction product (E) produced by emulsifying and polymerizing an acrylic monomer (D1) in the presence of polyethylene oxide (A) and a polyoxyalkylene ether surfactant (b).
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 10-167836
[0012] Patent Document 2: Japanese Patent No. 5594508
[0013] Patent Document 3: Japanese Patent Application Publication No. 2018-2991 Summary of the invention
[0014] Problems to be solved by the invention
[0015] Here, in the inorganic fine particle dispersion slurry composition used to make ceramic green sheets, polyvinyl alcohol resin and polyvinyl acetal resin are generally used as binders. However, these resins have a high decomposition temperature and therefore cannot be used for applications where low-temperature sintering is desired, such as in combination with easily oxidized metals such as copper, low-melting-point glass, etc.
[0016] Inorganic fine particle dispersed sheets are also required to be able to be degreased without leaving carbon in the center during firing, and to have a high yield stress and elongation at break before firing.
[0017] Typically, when using common binders such as polyvinyl alcohol resin, polyvinyl butyral resin, and cellulose resin, oxygen is required to degrease these binder resins. A large amount of residual carbon will remain in the center of the molded body where oxygen cannot reach, and cracks and expansion will occur during firing, which will cause a decrease in the yield.
[0018] Therefore, the use of (meth)acrylic resins that can be fired at low temperatures and have a small amount of residual carbon content after firing has been studied.
[0019] The binder resin described in Patent Document 1 is produced by solution polymerization and has a molecular weight of less than 200,000. Therefore, it is brittle as a whole and has a problem of not being able to obtain sufficient sheet strength.
[0020] In the acrylic resin for calcined paste described in Patent Document 2, a dispersant with poor sintering properties is added during emulsion polymerization, so there is a problem that coal ash (Japanese: coal) is easily formed during calcination. In addition, there is a problem that when the acrylic resin obtained in this way is dissolved in an organic solvent to prepare an inorganic fine particle dispersed slurry composition, the emulsifier will remain in the form of foreign matter to produce white turbidity, or sufficient sheet strength cannot be obtained when a sheet is prepared.
[0021] In Patent Document 3, an ether-based material with good sintering properties is used as an emulsifier, thereby improving the decomposability of the obtained polymerization reaction product. However, since the polymerization reaction product is obtained by emulsion polymerization, there is a problem that the emulsifier remains in the form of foreign matter, or the molecular weight of the obtained polymerization reaction product is low, and sufficient sheet strength cannot be obtained.
[0022] The object of the present invention is to provide a sintering resin composition, which has excellent decomposability at low temperatures and can obtain a high-strength molded product, realize further multilayering and thin filming, and can manufacture a ceramic laminate with excellent characteristics. In addition, the object of the present invention is to provide an inorganic particle dispersion slurry composition containing the sintering resin composition, and an inorganic particle dispersion sheet formed using the sintering resin composition or the inorganic particle dispersion slurry composition.
[0023] Means for solving problems
[0024] The present invention is a sintering resin composition, which includes a binder resin, wherein the binder resin contains a (meth) acrylic resin (A), wherein the (meth) acrylic resin (A) has at least one selected from a sulfonic group (Japanese: suruhon group), an alkylsulfonyl group, an aromatic sulfonyl group, a sulfinic acid group, an imidazoline group, a carboxyl group, an amide group, an amino group and a hydroxyl group at at least one molecular end of the main chain, and has a weight average molecular weight (Mw) of 1 million or more, and the content of a water-soluble surfactant is 0 weight part or more and 0.02 weight part or less relative to 100 weight parts of the binder resin.
[0025] The present invention is described in detail below.
[0026] The present inventors have found that by using a sintering resin composition containing a (meth) acrylic resin having a specific substituent at the molecular end and a weight average molecular weight of more than 1,000,000 and a water-soluble surfactant in a predetermined amount, sinterability and sheet strength can be taken into account. In addition, it has been found that when such a sintering resin composition is used to manufacture an inorganic particle dispersed sheet, it is easy to form a film, the degreasing property is excellent, and a formed body of the film can be obtained with a good yield, thereby completing the present invention.
[0027] The sintering resin composition of the present invention contains a binder resin.
[0028] The binder resin contains a (meth)acrylic resin (A).
[0029] The (meth)acrylic resin (A) has at least one selected from the group consisting of a sulfonic group, an alkylsulfonyl group, an aromatic sulfonyl group, a sulfinic acid group, an imidazoline group, a carboxyl group, an amide group, an amino group and a hydroxyl group at at least one molecular end of the main chain, and has a weight average molecular weight (Mw) of 1,000,000 or more.
[0030] The (meth)acrylic resin (A) has at least one group selected from sulfo group, alkylsulfonyl group, aromatic sulfonyl group, sulfinic acid group, imidazoline group, carboxyl group, amide group, amino group and hydroxyl group at at least one molecular terminal of the main chain.
[0031] By using the (meth)acrylic resin having the above-mentioned specific substituent, it is possible to achieve both sinterability and sheet strength.
[0032] The (meth)acrylic resin (A) mentioned above only needs to have the above functional group at at least one molecular end of the main chain. As a (meth)acrylic resin (A) having a carboxyl group, in addition to the carboxyl group, it may have a carboxyalkylamino group such as a carboxyethylamino group, a carboxyalkylamidino group such as a carboxyethylamidino group, etc., at the molecular end.
[0033] The (meth)acrylic resin (A) having a hydroxyl group may have a hydroxyalkylamino group such as a hydroxyethylamino group, or a hydroxyalkylamide group such as a hydroxyethylamide group, in addition to the hydroxyl group at the molecular terminal.
[0034] The sulfonic group may be a salt or an ester. Examples of the salt include ammonium salts, sodium salts, potassium salts, and the like. Examples of the ester include esters having an aliphatic group having 1 to 12 carbon atoms and an aromatic group having 6 to 12 carbon atoms, and alkyl esters are more preferred.
[0035] Examples of the alkylsulfonyl group include sulfonyl groups having an alkyl group having 1 to 12 carbon atoms, and specific examples thereof include a methylsulfonyl group, an ethylsulfonyl group, and a propylsulfonyl group.
[0036] Examples of the aromatic sulfonyl group include sulfonyl groups having an aromatic group having 12 or less carbon atoms, and specific examples thereof include a phenylsulfonyl group and the like.
[0037] The sulfinic acid group may be a salt or an ester. Examples of the salt include ammonium salts, sodium salts, potassium salts, and the like. Examples of the ester include esters having an aliphatic group having 1 to 12 carbon atoms and an aromatic group having 6 to 12 carbon atoms, and alkyl esters are more preferred.
[0038] The amino group may be a monoamino group, a diamino group, or a triamino group having 1 to 10 carbon atoms (preferably 1 to 5 carbon atoms, more preferably 1 to 3 carbon atoms).
[0039] Among them, the (meth)acrylic resin (A) preferably has a sulfone group at a molecular terminal.
[0040] In a preferred embodiment of the present invention, the specific substituent in at least one molecular terminal of the main chain of the (meth)acrylic resin (A) is preferably derived from a polymerization initiator.
[0041] The (meth)acrylic resin (A) preferably has a segment derived from isobutyl methacrylate.
[0042] Since the (meth)acrylic resin is depolymerized by heat and decomposed into monomers, residual carbon is less likely to remain, and the presence of a segment derived from isobutyl methacrylate can further improve low-temperature decomposability.
[0043] The preferred lower limit of the content of the segment derived from isobutyl methacrylate in the (meth)acrylic resin (A) is 40% by weight, and the preferred upper limit is 70% by weight.
[0044] When the content of the segment derived from isobutyl methacrylate is within the preferred range, the low-temperature decomposability can be further improved.
[0045] A more preferred lower limit of the content of the segment derived from isobutyl methacrylate is 50% by weight, and a more preferred upper limit is 60% by weight.
[0046] The (meth)acrylic resin (A) preferably further has a segment derived from at least one selected from methyl methacrylate, n-butyl methacrylate and ethyl methacrylate from the viewpoints of low-temperature decomposability, high strength, and ease of multilayering and thin film formation.
[0047] In order to maintain high yield stress, the glass transition temperature of the (meth)acrylic resin is preferably 40°C or higher. By copolymerizing with methyl methacrylate or ethyl methacrylate (these homopolymers have higher glass transition temperatures than isobutyl methacrylate), the yield stress of the obtained sheet can be increased.
[0048] On the other hand, in order to improve the brittleness of the inorganic microparticle dispersed sheet, it is desirable to add a plasticizer, but the plasticizers such as isobutyl methacrylate, methyl methacrylate, and ethyl methacrylate, which have short ester substituents, have poor retention and are prone to plasticizer exudation when processed into an inorganic microparticle dispersed sheet. Therefore, in order to maintain a high glass transition temperature and improve the retention of the plasticizer, it is desirable to copolymerize n-butyl methacrylate.
[0049] The preferred lower limit of the total content of the segment composed of methyl methacrylate, the segment composed of n-butyl methacrylate and the segment composed of ethyl methacrylate in the (meth)acrylic resin (A) is 20% by weight, more preferably 30% by weight, and still more preferably 40% by weight, and the preferred upper limit is 60% by weight, and more preferably 50% by weight.
[0050] By setting it as the said range, low-temperature decomposability can be exhibited.
[0051] The preferred lower limit of the total content of the segment derived from isobutyl methacrylate, the segment composed of methyl methacrylate, the segment composed of n-butyl methacrylate, and the segment composed of ethyl methacrylate in the (meth)acrylic resin (A) is 50% by weight, and the preferred upper limit is 100% by weight.
[0052] When the total content is 50 wt % or more, an inorganic fine particle dispersed sheet having improved yield stress and stiffness can be obtained. When the total content is 100 wt % or less, both low temperature decomposability and sheet strength can be achieved.
[0053] A more preferred lower limit of the above-mentioned total content is 55% by weight, a further preferred lower limit is 60% by weight, a further more preferred lower limit is 65% by weight, a particularly preferred lower limit is 70% by weight, a particularly more preferred lower limit is 80% by weight, a particularly preferred lower limit is 85% by weight, a very preferred lower limit is 90% by weight, and a more preferred upper limit is 97% by weight, a further preferred upper limit is 95% by weight.
[0054] The (meth)acrylic resin (A) may have a segment derived from a (meth)acrylate having 8 or more carbon atoms in the ester substituent. It should be noted that the ester substituent having 8 or more carbon atoms means that the total number of carbon atoms in the (meth)acrylate other than carbon atoms constituting the (meth)acryloyl group is 8 or more.
[0055] By having a segment derived from a (meth)acrylate having 8 or more carbon atoms in the ester substituent, the decomposition completion temperature of the (meth)acrylic resin can be sufficiently lowered, and the obtained inorganic fine particle dispersed sheet can be made tough.
[0056] Regarding the (meth)acrylate having 8 or more carbon atoms in the ester substituent, it is preferred that the ester substituent has a branched structure.
[0057] The upper limit of the number of carbon atoms in the ester substituent is preferably 30, more preferably 20, and still more preferably 10.
[0058] Examples of the (meth)acrylate having a linear or branched alkyl group include 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-lauryl (meth)acrylate, isolauryl (meth)acrylate, n-stearyl (meth)acrylate, and isostearyl (meth)acrylate.
[0059] Among them, (meth)acrylates having a branched alkyl group having 8 or more carbon atoms are preferred, and 2-ethylhexyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, and isostearyl (meth)acrylate are more preferred.
[0060] 2-Ethylhexyl methacrylate and isodecyl methacrylate are particularly excellent in decomposability compared with other long-chain alkyl methacrylates.
[0061] The content of the segment derived from the (meth)acrylic ester having 8 or more carbon atoms in the ester substituent in the (meth)acrylic resin (A) is preferably 1% by weight, more preferably 5% by weight, and preferably 15% by weight, more preferably 12% by weight, and even more preferably 10% by weight.
[0062] The (meth)acrylic resin (A) may have segments derived from other (meth)acrylates in addition to segments derived from isobutyl methacrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, and (meth)acrylates having 8 or more carbon atoms in the ester substituent.
[0063] Examples of the other (meth)acrylates include (meth)acrylate alkyl esters having an alkyl group having 2 to 6 carbon atoms, graft monomers having a polyalkylene ether chain in an ester substituent, multifunctional (meth)acrylates, and (meth)acrylates having a hydroxyl group.
[0064] A (meth)acrylic resin containing a (meth)acrylate having a carboxyl group can improve the sheet strength, but decomposability is poor, and therefore copolymerization of a (meth)acrylate having a carboxyl group is not preferred.
[0065] In a preferred embodiment of the present invention, the (meth)acrylic resin (A) preferably does not have a segment derived from a monomer having a polar functional group such as a carboxyl group or a hydroxyl group.
[0066] Examples of the alkyl (meth)acrylate having an alkyl group having 2 to 6 carbon atoms include n-propyl (meth)acrylate, n-pentyl (meth)acrylate, and n-hexyl (meth)acrylate.
[0067] Examples of the graft monomer having a polyalkylene ether chain in the ester substituent include polytetramethylene glycol monomethacrylate, etc. In addition, examples include poly(ethylene glycol·polytetramethylene glycol) monomethacrylate, poly(propylene glycol·tetramethylene glycol) monomethacrylate, propylene glycol·polybutylene glycol monomethacrylate, etc. In addition, examples include methoxypolytetramethylene glycol monomethacrylate, methoxypoly(ethylene glycol·polytetramethylene glycol) monomethacrylate, methoxypoly(propylene glycol·tetramethylene glycol) monomethacrylate, methoxypropylene glycol·polybutylene glycol monomethacrylate, etc.
[0068] Examples of the (meth)acrylate having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate.
[0069] The (meth)acrylic resin (A) may contain a segment derived from a (meth)acrylate having a glycidyl group or an epoxy group.
[0070] The content of the segment derived from the (meth)acrylate having a glycidyl group or an epoxy group in the (meth)acrylic resin (A) is preferably 0 to 10% by weight, more preferably 0 to 5% by weight, further preferably 0 to 3% by weight, further more preferably 0 to 2% by weight, and particularly preferably 0% by weight.
[0071] When the content of the segment derived from (meth)acrylate having a glycidyl group or an epoxy group in the (meth)acrylic resin (A) is within the above range, sintering properties can be further improved.
[0072] In order to promote the decomposability of the resin, a graft monomer having a polyalkylene ether chain in an ester substituent may be included as a copolymerization component, but a graft monomer having a hydroxyl group at the end is not preferred because it includes a bifunctional monomer esterified with methacrylate.
[0073] The graft monomer having a polyalkylene ether chain as an ester substituent is preferably a graft monomer having a polyalkylene ether chain as an ester substituent in which the end of the diol chain is ethoxylated or methoxylated.
[0074] If a crosslinkable polyfunctional (meth)acrylate is included as a copolymerization component, polymerization of the (meth)acrylic resin becomes non-uniform, and therefore the (meth)acrylic resin preferably does not include a segment derived from the polyfunctional (meth)acrylate.
[0075] The weight average molecular weight (Mw) of the (meth)acrylic resin (A) is 1,000,000 or more.
[0076] When the weight average molecular weight (Mw) of the (meth)acrylic resin (A) is 1,000,000 or more, the elongation at break of the obtained sheet can be increased.
[0077] The weight average molecular weight (Mw) of the (meth)acrylic resin (A) has a preferred lower limit of 1.5 million, a more preferred lower limit of 2 million, and a preferred upper limit of 7 million, a more preferred upper limit of 6 million, and a further preferred upper limit of 5 million.
[0078] When the weight average molecular weight (Mw) is 2 million to 5 million, an inorganic fine particle dispersed sheet having less residual carbon and easy thin film processing can be obtained, which is preferred.
[0079] The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the (meth)acrylic resin (A) is preferably 2.0 or less, and more preferably 1.9 or less.
[0080] By setting it as such a range, the viscosity of the inorganic fine particle dispersion slurry composition can be made appropriate, and productivity can be improved. In addition, the strength of the obtained sheet can be made appropriate.
[0081] The weight average molecular weight (Mw) and the number average molecular weight (Mn) can be measured by GPC measurement using, for example, Column LF-804 (manufactured by Showa Denko K.K.) as a column.
[0082] Regarding the glass transition temperature (Tg) of the (meth)acrylic resin (A), the glass transition temperature is preferably 40° C. or higher.
[0083] When the glass transition temperature is within the above range, the amount of the plasticizer added can be reduced, and the low-temperature decomposability of the (meth)acrylic resin can be improved.
[0084] The glass transition temperature (Tg) has a more preferred lower limit of 40°C, a further preferred lower limit of 45°C, and a preferred upper limit of 60°C, a more preferred upper limit of 55°C, and a further preferred upper limit of 50°C.
[0085] The glass transition temperature (Tg) can be measured using, for example, a differential scanning calorimeter (DSC) or the like.
[0086] The preferred upper limit of the 90% by weight decomposition temperature of the (meth)acrylic resin (A) when heated at 10°C / min is 280°C.
[0087] By setting the 90% by weight decomposition temperature to 280° C. or lower, extremely high low-temperature decomposition properties can be achieved, and the time required for degreasing can be shortened.
[0088] The preferred lower limit of the above-mentioned 90 wt % decomposition temperature is 230°C, the more preferred lower limit is 250°C, and the more preferred upper limit is 270°C.
[0089] In addition, the said 90 weight% decomposition temperature can be measured using TG-DTA etc., for example.
[0090] The (meth)acrylic resin (A) preferably has a maximum stress of 30 N / mm in a tensile test when formed into a sheet having a thickness of 20 μm. 2 above.
[0091] The (meth)acrylic resin (A) preferably exhibits a yield stress when formed into a sheet having a thickness of 20 μm and a breaking elongation of 50% or more, and more preferably a breaking elongation of 100% or more.
[0092] It should be noted that a sheet having a thickness of 20 μm can be obtained by applying a resin solution obtained by dissolving a sintering resin composition in a butyl acetate solution to a release-treated PET film using an applicator, and drying the film in a 100° C. air-supplied oven for 10 minutes. The maximum stress can be measured by a tensile test based on an AUTOGRAPH, for example, at 23° C. and 50 RH using a tensile testing machine (e.g., Autograph AG-IS, manufactured by Shimadzu Corporation) with a distance between the clamps of 3 cm and a tensile speed of 10 mm / min.
[0093] Generally, (meth)acrylic resins are hard and brittle, so when formed into a sheet and stretched, they break at a strain of less than 5% and do not exhibit yield stress. On the other hand, by adjusting the composition of the (meth)acrylic resin, the (meth)acrylic resin (A) exhibits yield stress when formed into a sheet and stretched.
[0094] The Z average particle size of the (meth)acrylic resin (A) is preferably 100 nm or more, more preferably 200 nm or more, and is preferably 1000 nm or less, more preferably 700 nm or less.
[0095] The CV value of the particle size of the (meth)acrylic resin (A) is preferably 20% or less, more preferably 15% or less, and further preferably 10% or less. The lower limit is not particularly limited, but is preferably 3% or more, and more preferably 4% or more.
[0096] The smaller the CV value of the particle size, the narrower the molecular weight distribution of the (meth)acrylic resin and the smaller the Mw / Mn. If the CV value of the particle size is within the above range, it is easy to control the viscosity when processed into a resin solution, and when used in the production of electronic products such as laminated ceramic capacitors, the production conditions can be precisely controlled to manufacture products with better performance.
[0097] In addition, the CV value of the particle size can be calculated by the following formula.
[0098] CV value (%) = [(standard deviation of particle size) / (average particle size)] × 100
[0099] The Z average particle size and the CV value of the particle size can be measured by using, for example, a ZETASIZER or the like.
[0100] Examples of a method for producing the (meth)acrylic resin (A) include a method of dispersing a raw material monomer mixture such as isobutyl methacrylate, methyl methacrylate, n-butyl methacrylate, ethyl methacrylate, etc. in water, and adding a specific polymerization initiator and, if necessary, a water-soluble surfactant to a monomer mixed solution to carry out polymerization.
[0101] In the production of conventional (meth)acrylic resins, monomers are polymerized in dispersant micelles by emulsion polymerization, but in order to obtain a high molecular weight resin, it is necessary to form giant micelles, and thus a large amount of dispersant needs to be added. Therefore, the obtained (meth)acrylic resin contains a large amount of dispersant, and as a result, there are problems such as poor sinterability and insufficient sheet strength.
[0102] In the present invention, by polymerizing the raw material monomers dispersed in water using a specific polymerization initiator, a particulate (meth)acrylic resin can be produced without using a dispersant, and a (meth)acrylic resin having a molecular weight higher than that of ordinary emulsion polymerization can be produced.
[0103] As the polymerization initiator, a water-soluble radical polymerization initiator having at least one selected from a sulfo group, a sulfonyl group, a sulfinic acid group, an imidazoline group, a carboxyl group, an amide group, and a hydroxyl group can be used.
[0104] By using the water-soluble radical polymerization initiator in the polymerization using the polymerization initiator, a high molecular weight (meth)acrylic resin can be produced without adding a large amount of a dispersant as in the usual emulsion polymerization.
[0105] In the above-mentioned polymerization reaction, the monomers dispersed in water are polymerized with the above-mentioned water-soluble free radical polymerization initiator as a starting point. At this time, dispersion polymerization is carried out at a low concentration in a manner that each monomer does not collide or adhere. By reacting in this way, a polymer with uniform composition and consistent particle size can be obtained. This is because: in the above-mentioned method, by using the above-mentioned water-soluble free radical polymerization initiator, polymerization is carried out at a low concentration, so that the reaction that becomes the cause of inhomogenization such as hydrogen abstraction can be suppressed to a minimum, and multiple polymers in the reaction system are not easy to grow.
[0106] Examples of the water-soluble radical polymerization initiator include: 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] sulfate hydrate, acid mixtures of imidazole azo compounds such as 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis(2-methylpropionamidine) dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] sulfate hydrate, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], etc. -azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 4,4'-azobis-4-cyanovaleric acid and other water-soluble azo compounds, potassium persulfate (potassium peroxodisulfate), ammonium persulfate (ammonium peroxodisulfate), sodium persulfate (sodium peroxodisulfate) and other oxygen-containing acids, hydrogen peroxide, peracetic acid, performic acid, perpropionic acid and other peroxides, etc.
[0107] Among them, acid mixtures of imidazole-based azo compounds, water-soluble azo compounds, and oxoacids are preferred. In addition, 2,2'-azobis[2-(2-imidazoline-2-yl)propane] dihydrochloride, 2,2'-azobis(2-methylpropionamidine) dihydrochloride (Japanese: ジハイドロクロライド), 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], potassium persulfate, ammonium persulfate, and sodium persulfate are more preferred from the aspect of being able to reduce residues.
[0108] These water-soluble radical polymerization initiators may be used alone or in combination of two or more.
[0109] In addition, the above method can produce a (meth)acrylic resin having a weight average molecular weight within a predetermined range, and the weight average molecular weight of the (meth)acrylic resin can be adjusted by adding a chain transfer agent or a polymerization terminator.
[0110] The chain transfer agent and the polymerization terminator are not particularly limited, and examples thereof include sodium 3-mercapto-1-propanesulfonate, mercaptosuccinic acid, mercaptopropylene glycol, (allylsulfonyl)benzene, ethyl 2-mercaptoethanesulfinate, and 3-mercaptopropionamide.
[0111] By adding the chain transfer agent and the polymerization terminator, a (meth)acrylic resin having at least one selected from a sulfonic group, a sulfonyl group, a sulfinic acid group, an imidazoline group, a carboxyl group, an amide group and a hydroxyl group at at least one molecular end of the main chain and having a weight average molecular weight within a predetermined range can be prepared.
[0112] The amount of the water-soluble radical polymerization initiator added is preferably 0.03 to 0.2 parts by weight, more preferably 0.05 to 0.15 parts by weight, based on 100 parts by weight of the raw material monomers.
[0113] By setting the added amount to 0.03 parts by weight or more, the reaction rate of the raw material monomers can be sufficiently increased. By setting the added amount to 0.2 parts by weight or less, the molecular weight of the (meth)acrylic resin can be sufficiently increased.
[0114] In addition, by setting the above range, a (meth)acrylic resin having at least one selected from a sulfonic group, a sulfonyl group, a sulfinic acid group, an imidazoline group, a carboxyl group, an amide group and a hydroxyl group at the molecular terminal (ω position) can be dispersed in water at a low concentration to obtain a resin having a uniform particle size.
[0115] In addition, in the usual emulsion polymerization, more than 1 part by weight of a water-soluble surfactant is added relative to 100 parts by weight of the raw monomer, but the water-soluble surfactant exists as a foreign matter in the case of forming a resin sheet, so it is less desirable. However, when only the water-soluble surfactant is reduced, it is difficult to polymerize a resin with a high molecular weight. By setting the addition amount of the water-soluble free radical polymerization initiator to the above range, even if almost no emulsifier is added, the polymerization region (Japanese: overlapped domain) can also be kept dispersed in water, and a (meth) acrylic resin with a very high molecular weight can be produced.
[0116] The amount of the raw material monomer added is preferably 50 to 300 parts by weight based on 1000 parts by weight of water.
[0117] By setting it as the said range, aggregation during polymerization or adhesion of resin to a reaction container can be prevented.
[0118] The amount of the raw material monomer added is more preferably 70 to 200 parts by weight based on 1000 parts by weight of water.
[0119] By setting it as the said range, residual monomer can be reduced and the polymerization can be uniformly performed.
[0120] As a method for dispersing the raw material monomer mixture in water, there is a method of stirring at 100 to 250 rpm using a stirring blade.
[0121] The temperature during the polymerization is preferably 50 to 100°C.
[0122] By setting the temperature to 50° C. or higher, the polymerization reaction can be favorably advanced. When the temperature is 80° C. or lower, the resin can be prevented from sticking together, thereby obtaining uniform resin particles.
[0123] In addition, by maintaining the predetermined temperature for several hours during the polymerization, the polar functional groups at the terminals of the monomers can be dispersed in water to form more uniform resin particles.
[0124] The CV value of the particle size of the resin particles obtained by the usual synthesis in water is about 15 to 40%. In contrast, the CV value of the particle size of the resin particles obtained by the above method is less than 20%, which can form more uniform resin particles. The CV value is a value that represents the ratio of the standard deviation to the average particle size. When the CV value is large, it implies the following situation: when making resin particles, the supply of monomers to the polymerization area growing in water is uneven, and the areas that are easy to grow and the areas that are not easy to grow are mixed. Therefore, the average molecular weight of the obtained resin remains at around 1 million.
[0125] In the (meth)acrylic resin of the present invention, the ratio of the initiator to the monomer is optimized, and the monomer is supplied uniformly and evenly to each polymerization zone, so that a resin having an average molecular weight of 2 million or more can be synthesized.
[0126] In addition, the average particle size of the (meth) acrylic resin obtained by the above method is as small as 0.01 to 0.2 μm, so it is difficult to recover using a filter material such as a filter cloth, and it is preferably recovered by centrifugation, freeze drying, spray drying, etc. In addition, the following methods can also be used: a method of adding an alcohol such as butanol and hexanol, an organic solvent such as methyl acetate, etc. to a solution containing resin particles after the reaction to swell and condense the resin and recover it; a method of adding an organic salt such as sodium acetate and sodium sulfonate to precipitate the resin; a method of dehydrating the solution after the reaction under reduced pressure to increase the resin concentration and precipitate and dry the resin, etc.
[0127] The binder resin may contain a (meth)acrylic resin (B) having a weight average molecular weight (Mw) of 1,000,000 or less.
[0128] By containing the (meth)acrylic resin (B), there is an advantage that the physical properties of the sheet can be easily adjusted.
[0129] The weight average molecular weight (Mw) of the (meth)acrylic resin (B) is preferably less than 1,000,000, more preferably 500,000 or less, further preferably 300,000 or less, and further preferably 100,000 or less.
[0130] Examples of the monomer components constituting the (meth)acrylic resin (B) include the same monomer components as those for the (meth)acrylic resin (A).
[0131] The weight ratio of the (meth)acrylic resin (A) to the (meth)acrylic resin (B) in the binder resin is preferably 99:1 to 50:50.
[0132] By setting it as the said range, there exists an advantage that both a high yield stress and a high elongation at break can be easily achieved.
[0133] The weight ratio is more preferably 70:30 to 50:50.
[0134] The content of the water-soluble surfactant in the sintering resin composition of the present invention is 0 parts by weight or more and 0.02 parts by weight or less based on 100 parts by weight of the binder resin.
[0135] The water-soluble surfactant is preferably a surfactant having a solubility in water at 25° C. of 10 g / 100 g or more.
[0136] When the content of the water-soluble surfactant is set to 0.02 parts by weight or less, for example, even when the (meth)acrylic resin is dissolved in an organic solvent, the haze value is low, and both sinterability and sheet strength can be achieved.
[0137] The content of the water-soluble surfactant is preferably 0.015 parts by weight or less based on 100 parts by weight of the binder resin.
[0138] In addition, the lower limit is 0 parts by weight or more. In addition, by adding a very small amount of a water-soluble surfactant, the resin can be inhibited from adhering to the polymerization kettle or blades, so it can be added in a very small amount, for example, preferably 0.000005 parts by weight or more, more preferably 0.00005 parts by weight or more, and further preferably 0.005 parts by weight or more.
[0139] The method for measuring the content of the water-soluble surfactant is not particularly limited, and the content of the water-soluble surfactant can be measured, for example, by a method using liquid chromatography represented by HPLC, or by a method of extraction using methanol, etc. Alternatively, the content of the water-soluble surfactant can be measured using a thermogravimetric mass spectrometer based on the amount of decomposition gas at 400 to 600° C. resulting from the combustion of the water-soluble surfactant and the amount of decomposition gas at 200 to 300° C. resulting from the decomposition of the (meth)acrylic resin.
[0140] The water-soluble surfactant is used as a dispersant added during emulsion polymerization, and examples thereof include anionic surfactants such as alkyl sulfonates, and polymer surfactants such as polyvinyl alcohol, polyvinyl butyral, and polyalkylene glycol.
[0141] Examples of the alkylsulfonate include sodium salts, potassium salts, and ammonium salts of octylsulfonic acid, decylsulfonic acid, and dodecylsulfonic acid.
[0142] When the sintering resin composition of the present invention is converted into a resin solution, the resin solution may become cloudy even if the amount of the water-soluble surfactant is very small. In addition, since the (meth)acrylic resin (A) has a very high molecular weight, the resin solution may become cloudy even if the solubility in the solvent is poor.
[0143] Therefore, whether the resin solution is suitable for forming an inorganic fine particle dispersed sheet can be determined by evaluating the haze value. A resin solution having a haze value of 10% or more at room temperature containing 10% by weight of the resin component is not suitable for forming an inorganic fine particle dispersed sheet.
[0144] The sintering resin composition of the present invention may further contain an organic solvent.
[0145] The organic solvent is not particularly limited, and examples thereof include toluene, ethyl acetate, butyl acetate, amyl acetate, hexyl acetate, ethyl butyrate, butyl butyrate, amyl butyrate, hexyl butyrate, isopropyl alcohol, methyl isobutyl ketone, methyl ethyl ketone, methyl isobutyl ketone, ethylene glycol ethyl ether, ethylene glycol monobutyl ether, ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoisobutyl ether, trimethylpentanediol monoisobutyrate, butyl carbitol, butyl carbitol acetate, terpineol, terpineol acetate, dihydroterpineol, dihydroterpineol acetate, Texanol, isophorone, butyl lactate, dioctyl phthalate, dioctyl adipate, benzyl alcohol, phenylpropylene glycol, cresol, and the like. Among them, butyl acetate, terpineol, terpineol acetate, dihydroterpineol, dihydroterpineol acetate, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoisobutyl ether, butyl carbitol, butyl carbitol acetate, and Texanol are preferred. In addition, butyl acetate, terpineol, terpineol acetate, dihydroterpineol, and dihydroterpineol acetate are more preferred. It should be noted that these organic solvents may be used alone or in combination of two or more.
[0146] The boiling point of the organic solvent is preferably 70° C. or higher.
[0147] When the boiling point is 70° C. or higher, premature evaporation does not occur, and excellent handling properties can be achieved.
[0148] The boiling point is more preferably 90 to 230°C, further preferably 95 to 200°C, further preferably 100 to 180°C, and particularly preferably 105 to 150°C.
[0149] By setting it as the said range, the strength of the obtained sheet can be improved.
[0150] From the viewpoint of low-temperature sintering properties, the sintering resin composition of the present invention preferably contains substantially no polymerization initiator.
[0151] The sintering resin composition of the present invention preferably has a haze of less than 10% when the content of the binder resin is adjusted to 10% by weight.
[0152] By setting it as the said range, there exists an advantage that the sheet strength becomes high.
[0153] The haze is preferably 0% or more, more preferably 9% or less, further preferably 7% or less, and further more preferably 5% or less.
[0154] The sintering resin composition of the present invention preferably has a maximum stress of 30 N / mm in a tensile test when formed into a sheet having a thickness of 20 μm. 2 above.
[0155] The sintering resin composition of the present invention preferably exhibits a yield stress when formed into a sheet having a thickness of 20 μm and a breaking elongation of 50% or more, and more preferably a breaking elongation of 100% or more.
[0156] It should be noted that a sheet having a thickness of 20 μm can be obtained by applying a resin solution obtained by dissolving the calcining resin composition of the present invention in a butyl acetate solution to a release-treated PET film using an applicator, and drying in a 100° C. air-blowing oven for 10 minutes. The maximum stress can be measured by the same method as the tensile test of the (meth)acrylic resin (A).
[0157] Generally, (meth)acrylic resins are hard and brittle, so when formed into a sheet and stretched, they break at a strain of less than 5% and do not show yield stress. On the other hand, by adjusting the composition of the sintering resin composition, the sintering resin composition of the present invention also shows yield stress when formed into a sheet and stretched.
[0158] The Z average particle size of the sintering resin composition of the present invention is preferably 100 nm or more, more preferably 200 nm or more, and is preferably 1000 nm or less, more preferably 700 nm or less.
[0159] The CV value of the particle size of the sintering resin composition of the present invention is preferably 20% or less, more preferably 15% or less, and further preferably 10% or less. The lower limit is not particularly limited, but is preferably 3% or more, and more preferably 4% or more.
[0160] The smaller the CV value of the particle size, the narrower the molecular weight distribution of the (meth)acrylic resin and the smaller the Mw / Mn. If the CV value of the particle size is within the above range, it is easy to control the viscosity when processed into a resin solution, and when used in the production of electronic products such as laminated ceramic capacitors, the production conditions can be precisely controlled to manufacture products with better performance.
[0161] The Z average particle size and the CV value of the particle size can be measured by using, for example, a ZETASIZER or the like.
[0162] Furthermore, an inorganic fine particle-dispersed slurry composition can be prepared using the sintering resin composition of the present invention containing a binder resin and an organic solvent, and inorganic fine particles.
[0163] The present invention also includes an inorganic fine particle-dispersed slurry composition containing the sintering resin composition of the present invention and inorganic fine particles.
[0164] The content of the binder resin in the inorganic fine particle dispersion slurry composition of the present invention is not particularly limited, but the preferred lower limit is 5% by weight and the preferred upper limit is 30% by weight.
[0165] By setting the content of the binder resin within the above range, it is possible to obtain an inorganic fine particle dispersed slurry composition that can be degreased even when fired at a low temperature.
[0166] A more preferred lower limit of the content of the binder resin is 6% by weight, and a more preferred upper limit is 12% by weight.
[0167] The inorganic fine particle dispersion slurry composition of the present invention contains the above-mentioned organic solvent.
[0168] The content of the organic solvent in the inorganic fine particle dispersion slurry composition of the present invention is not particularly limited, but the preferred lower limit is 10 wt % and the preferred upper limit is 60 wt %. By setting the content within the above range, the coating properties and the dispersibility of the inorganic fine particles can be improved.
[0169] The inorganic fine particle-dispersed slurry composition of the present invention contains inorganic fine particles.
[0170] The inorganic fine particles are not particularly limited, and examples thereof include glass powder, ceramic powder, phosphor fine particles, silicon oxide, and metal fine particles.
[0171] The above-mentioned glass powder is not particularly limited. For example, it may include: glass powders such as bismuth oxide glass, silicate glass, lead glass, zinc glass, boron glass, or glass powders of various silicon oxides such as CaO-Al2O3-SiO2 system, MgO-Al2O3-SiO2 system, LiO2-Al2O3-SiO2 system, etc.
[0172] In addition, as the above-mentioned glass powder, the following can also be used: SnO-B2O3-P2O5-Al2O3 mixture, PbO-B2O3-SiO2 mixture, BaO-ZnO-B2O3-SiO2 mixture, ZnO-Bi2O3-B2O3-SiO2 mixture, Bi2O3-B2O3-BaO-CuO mixture, Bi2O3-ZnO-B2O3-Al2O3-SrO mixture, ZnO-Bi2O3-B2O3 mixture, Bi2O3-SiO2 mixture, P2O5-Na2O-CaO-BaO-Al2O3-B2O3 mixture, P2O5-SnO mixture, P2O5-SnO-B2O3 mixture, P2O5-SnO-SiO2 mixture, CuO-P2O5-RO mixture, SiO2-B2O3-ZnO-Na2O-Li2O-NaF-V2O5 mixture, P2O5-ZnO-SnO-R2O-RO mixture, B2O3-SiO2-ZnO mixture, B2O3-SiO2-Al2O3-ZrO2 mixture, SiO2-B2O3-ZnO-R2O-RO mixture, SiO2-B2O3-Al2O3-RO-R2O mixture, SrO-ZnO-P2O5 mixture, SrO-ZnO-P2O5 mixture, BaO-ZnO-B2O3-SiO2 mixture, etc. It should be noted that R is an element selected from Zn, Ba, Ca, Mg, Sr, Sn, Ni, Fe, and Mn.
[0173] Particularly preferably, it is a glass powder of PbO-B2O3-SiO2 mixture, or a lead-free glass powder such as BaO-ZnO-B2O3-SiO2 mixture or ZnO-Bi2O3-B2O3-SiO2 mixture without lead.
[0174] The above-mentioned ceramic powder is not particularly limited. For example, it may include: alumina, ferrite, zirconia, zircon, barium zirconate, calcium zirconate, titanium oxide, barium titanate, strontium titanate, calcium titanate, magnesium titanate, zinc titanate, lanthanum titanate, neodymium titanate, lead zirconate titanate (Japanese: チタン酸ジルコン鉛), aluminum nitride, silicon nitride, boron nitride, boron carbide, barium stannate, calcium stannate, magnesium silicate, mullite, steatite, cordierite, forsterite, etc.
[0175] In addition, ITO, FTO, niobium oxide, vanadium oxide, tungsten oxide, lanthanum strontium manganate, lanthanum strontium cobalt ferrite, yttrium-stabilized zirconia, gadolinium-doped cerium oxide, nickel oxide, lanthanum chromate, etc. can also be used.
[0176] The phosphor particles are not particularly limited. For example, blue phosphors, red phosphors, green phosphors, etc., which are known as phosphors for displays, can be used as phosphor materials. For example, MgAl 10 O 17 :Eu、Y2SiO5:Ce series、CaWO4:Pb series、BaMgAl 14 O 23 :Eu series, BaMgAl 16 O 27 :Eu series, BaMg2Al 14 O 23 :Eu series, BaMg2Al 14 O 27 As the red phosphor material, for example, Y2O3:Eu system, Y2SiO5:Eu system, Y3Al5O 12 :Eu series, Zn3(PO4)2:Mn series, YBO3:Eu series, (Y,Gd)BO3:Eu series, GdBO3:Eu series, ScBO3:Eu series, LuBO3:Eu series. As green phosphor materials, for example, Zn2SiO4:Mn series, BaAl 12 O 19 :Mn series, SrAl 13 O 19 : Mn series, CaAl 12 O 19 :Mn series, YBO3:Tb series, BaMgAl 14 O 23 :Mn series, LuBO3:Tb series, GdBO3:Tb series, ScBO3:Tb series, Sr6Si3O3Cl4:Eu series phosphor materials. In addition, ZnO:Zn series, ZnS:(Cu,Al) series, ZnS:Ag series, Y2O2S:Eu series, ZnS:Zn series, (Y,Cd)BO3:Eu series, BaMgAl 12 O 23 : Eu-based phosphor material.
[0177] The metal fine particles are not particularly limited, and examples thereof include powders containing copper, nickel, palladium, platinum, gold, silver, aluminum, tungsten, or alloys thereof.
[0178] In addition, metals such as copper and iron that have good adsorption characteristics with carboxyl groups, amino groups, amide groups, etc. and are easily oxidized can also be used appropriately. These metal powders may be used alone or in combination of two or more.
[0179] In addition to the metal complex, various carbon blacks, carbon nanotubes, and the like can also be used.
[0180] The inorganic fine particles preferably contain lithium or titanium. Specifically, for example, low melting point glass such as LiO2·Al2O3·SiO2 inorganic glass, Li2S-M x S y (M=B, Si, Ge, P) and other lithium chalcogenide glasses, lithium cobalt composite oxides such as LiCoO2, lithium manganese composite oxides such as LiMnO4, lithium nickel composite oxides, lithium vanadium composite oxides, lithium zirconium composite oxides, lithium hafnium composite oxides, lithium silicophosphate (Li 3.5 Si 0.5 P 0.5 O4), lithium titanium phosphate (LiTi2(PO4)3), lithium titanate (Li4Ti5O 12 )、Li 4 / 3 Ti 5 / 3O4, Lithium Germanium Phosphate (LiGe2(PO4)3), Li2-SiS Glass, Li4GeS4-Li3PS4 Glass, LiSiO3, LiMn2O4, L i2 S-P2S5 glass and ceramics, Li2O-SiO2, Li2O-V2O5-SiO2, LiS-SiS2-Li4SiO4 glass, LiPON and other ion conductive oxides, Li2O-P2O5-B2O3, Li2O-GeO2Ba and other lithium oxide compounds, Li x Al y Ti z (PO4)3 series glass, La x Li y TiO z Glass, Li x Ge y P z O4 series glass, Li7La3Zr2O 12 Glass, Li v Si w P x S y Cl z Glass, lithium niobium oxides such as LiNbO3, lithium aluminum oxide compounds such as Li-β-alumina, Li14 Lithium zinc oxides such as Zn(GeO4)4, etc.
[0181] The content of the inorganic particles in the inorganic particle dispersion slurry composition of the present invention is not particularly limited, and the preferred lower limit is 10% by weight, and the preferred upper limit is 90% by weight. By setting it to more than 10% by weight, it is possible to have sufficient viscosity and excellent coating properties, and by setting it to less than 90% by weight, it is possible to make the dispersibility of the inorganic particles excellent.
[0182] The inorganic fine particle-dispersed slurry composition of the present invention preferably contains a plasticizer.
[0183] Examples of the plasticizer include monomethyl adipate, di(butoxyethyl adipate), dibutoxyethoxyethyl adipate, triethylene glycol bis(2-ethylhexanoate), triethylene glycol dicaproate, acetyl triethyl citrate, hexadecyl tributyl citrate, and dibutyl sebacate.
[0184] By using these plasticizers, the amount of plasticizer added can be reduced compared to the case of using ordinary plasticizers (about 30% by weight added to the binder resin can be reduced to 25% by weight or less, and further reduced to 20% by weight or less).
[0185] Among them, it is preferred to use a non-aromatic plasticizer, and it is more preferred to contain a component derived from adipic acid, triethylene glycol or citric acid. It should be noted that a plasticizer having an aromatic ring is not preferred because it easily burns to form coal ash.
[0186] The boiling point of the plasticizer is preferably 240° C. or higher and lower than 390° C. By setting the boiling point to 240° C. or higher, the plasticizer is easily evaporated during the drying process and can be prevented from remaining in the molded body. In addition, by setting the boiling point to lower than 390° C., the generation of residual carbon can be prevented. It should be noted that the boiling point is the boiling point at normal pressure.
[0187] The content of the plasticizer in the inorganic fine particle dispersion slurry composition of the present invention is not particularly limited, but the preferred lower limit is 0.1% by weight and the preferred upper limit is 3.0% by weight. By setting the content within the above range, the burning residue of the plasticizer can be reduced.
[0188] The viscosity of the inorganic fine particle dispersion slurry composition of the present invention is not particularly limited, but when measured at 20° C. using a B-type viscometer with a probe rotation speed of 5 rpm, the preferred lower limit of the viscosity is 0.1 Pa·s, and the preferred upper limit is 100 Pa·s.
[0189] By setting the viscosity to 0.1 Pa·s or more, the inorganic fine particle dispersed sheet obtained can maintain a predetermined shape after being coated by die coating printing method, etc. In addition, by setting the viscosity to 100 Pa·s or less, it is possible to prevent the coating trace of the die from disappearing, thereby achieving excellent printability.
[0190] The method for preparing the inorganic fine particle dispersion slurry composition of the present invention is not particularly limited, and examples thereof include a known stirring method. Specifically, for example, examples thereof include a method in which the sintering resin composition of the present invention, the inorganic fine particles, an organic solvent added as needed, a plasticizer, and other components are stirred using a three-roll mill or the like.
[0191] An inorganic fine particle dispersed sheet can be produced by applying the inorganic fine particle dispersed slurry composition of the present invention onto a support film subjected to a one-side release treatment, drying the organic solvent and forming the film into a sheet. Such an inorganic fine particle dispersed sheet is also one of the present invention.
[0192] The inorganic fine particle dispersed sheet of the present invention preferably has a thickness of 1 to 20 μm.
[0193] The supporting film used in manufacturing the inorganic microparticle-dispersed sheet of the present invention is preferably a resin film having heat resistance and solvent resistance and flexibility. By making the supporting film flexible, the inorganic microparticle-dispersed slurry composition can be applied to the surface of the supporting film by a roll coater, a knife coater, etc., and the obtained inorganic microparticle-dispersed sheet-formed film can be stored and supplied in a state of being wound into a roll.
[0194] Examples of the resin forming the support film include polyethylene terephthalate, polyester, polyethylene, polypropylene, polystyrene, polyimide, polyvinyl alcohol, fluorine-containing resins such as polyvinyl chloride and polyvinyl fluoride, nylon, and cellulose.
[0195] The thickness of the supporting film is preferably, for example, 20 to 100 μm.
[0196] In addition, it is preferable to subject the surface of the supporting film to a release treatment, whereby the peeling operation of the supporting film can be easily performed in the transfer step.
[0197] By using the inorganic particle dispersion slurry composition and inorganic particle dispersion sheet of the present invention as materials for the positive electrode, solid electrolyte, and negative electrode of an all-solid battery, an all-solid battery can be manufactured. In addition, by using the inorganic particle dispersion slurry composition and inorganic particle dispersion sheet of the present invention for dielectric green sheets and electrode pastes, a laminated ceramic capacitor can be manufactured.
[0198] The manufacturing method of the above-mentioned all-solid-state battery preferably has the following steps: a step of forming a slurry for an electrode active material layer containing an electrode active material and a binder for the electrode active material layer to produce an electrode active material sheet; a step of stacking the electrode active material sheet with the inorganic microparticle dispersed sheet of the present invention to produce a stacked body; and a step of sintering the stacked body.
[0199] The electrode active material is not particularly limited, and for example, the same material as the inorganic fine particles can be used.
[0200] As the binder for the electrode active material layer, the above-mentioned binder resin can be used.
[0201] Examples of a method for laminating the electrode active material sheet and the inorganic fine particle dispersed sheet of the present invention include a method of cutting them into sheets and then subjecting them to thermal compression bonding or thermal lamination by hot pressing.
[0202] In the calcining step, the heating temperature preferably has a lower limit of 250°C and an upper limit of 350°C.
[0203] Through the above-mentioned manufacturing method, an all-solid-state battery can be obtained.
[0204] The all-solid-state battery preferably has a structure in which a positive electrode layer containing a positive electrode active material, a negative electrode layer containing a negative electrode active material, and a solid electrolyte layer formed between the positive electrode layer and the negative electrode layer are stacked.
[0205] The method for producing a laminated ceramic capacitor preferably comprises the steps of: printing a conductive paste on the inorganic fine particle dispersed sheet of the present invention and drying the printed conductive paste to produce a dielectric sheet; and laminating the dielectric sheets.
[0206] The above-mentioned conductive paste contains conductive powder.
[0207] The material of the conductive powder is not particularly limited as long as it has conductivity, and examples thereof include nickel, palladium, platinum, gold, silver, copper, and alloys thereof. These conductive powders may be used alone or in combination of two or more.
[0208] As the binder resin and the organic solvent used in the conductive paste, the same ones as those in the inorganic fine particle dispersion slurry composition of the present invention can be used.
[0209] The method for printing the conductive paste is not particularly limited, and examples thereof include screen printing, die coating printing, offset printing, gravure printing, and inkjet printing.
[0210] In the method for producing the above-mentioned multilayer ceramic capacitor, the multilayer ceramic capacitor can be obtained by stacking dielectric sheets on which the above-mentioned conductive paste is printed.
[0211] Effects of the Invention
[0212] According to the present invention, a sintering resin composition can be provided, which has excellent decomposability at low temperatures, can obtain a high-strength molded product, realizes further multilayering and thin filming, and can manufacture a ceramic laminate with excellent characteristics. In addition, an inorganic particle dispersion slurry composition containing the sintering resin composition, and an inorganic particle dispersion sheet formed using the sintering resin composition or the inorganic particle dispersion slurry composition can be provided. DETAILED DESCRIPTION
[0213] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.
[0214] (Example 1)
[0215] A 2L separable flask equipped with a stirrer, a cooler, a thermometer, a hot water bath, and a nitrogen inlet was prepared. 900 parts by weight of water, 70 parts by weight of isobutyl methacrylate (iBMA) and 30 parts by weight of ethyl methacrylate (EMA) as monomers were added to the 2L separable flask. Then, the monomers were dispersed in the water by stirring with a stirring blade at 150 rpm to obtain a monomer mixed solution.
[0216] The obtained monomer mixture was bubbled with nitrogen for 20 minutes to remove dissolved oxygen, and then the inside of the separable flask was replaced with nitrogen, and the temperature was raised while stirring until the hot water bath reached 80°C. Then, a solution in which 0.01 parts by weight of ammonium dodecylsulfonate (DSA, solubility in water at 25°C: 10 g / 100 g) as a water-soluble surfactant and 0.08 parts by weight of ammonium persulfate (APS) as a polymerization initiator were dissolved in 20 parts by weight of water was added to initiate polymerization. After initiating the polymerization for 7 hours, the polymerization was terminated by cooling to room temperature, and an aqueous solution containing a (meth) acrylic resin having a sulfonic group at one molecular terminal of the main chain was obtained.
[0217] 2 g of the obtained resin aqueous solution was dried in an oven at 150° C., and the resin solid content was evaluated. As a result, it was confirmed that the resin solid content concentration in the aqueous solution was 10% by weight, indicating that all the monomers used had reacted.
[0218] The obtained aqueous solution was dried using a spray dryer to obtain a resin composition for firing.
[0219] (Examples 2 to 14, Comparative Examples 1 to 9)
[0220] A resin composition for firing was obtained in the same manner as in Example 1 except that the types and addition amounts of monomers, water-soluble surfactants, polymerization initiators, chain transfer agents, and polymerization terminators were as shown in Tables 1 and 2. The chain transfer agent and polymerization initiator were added at the same time as the monomers were added to water.
[0221] In addition, the following substances were used as a monomer, a water-soluble surfactant, a polymerization initiator, a chain transfer agent, and a polymerization terminator.
[0222] <Single body>
[0223] MMA: Methyl Methacrylate
[0224] nBMA: n-butyl methacrylate
[0225] 2EHMA: 2-Ethylhexyl Methacrylate
[0226] iDMA: Isodecyl Methacrylate
[0227] HEMA: 2-Hydroxyethyl Methacrylate
[0228] MPOMA: Methoxypolypropylene glycol methacrylate
[0229] <Water-soluble surfactant>
[0230] DSN: sodium dodecyl sulfate, solubility in water at 25°C 10g / 100g
[0231] PVA: GOHSENOL Z-210 (manufactured by Mitsubishi Chemical Corporation), solubility in water at 25°C: 30 g / 100 g
[0232] <Polymerization initiator>
[0233] KPS: Potassium persulfate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0234] NaPS: Sodium persulfate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0235] VA-044: 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0236] V-50: 2,2'-azobis(2-methylpropionamidine) dihydrochloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0237] VA-057: 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0238] VA-086: 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide] (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0239] PEROYL SA: Disuccinic acid peroxide (manufactured by NOF Corporation)
[0240] PEROYL IPP: diisopropyl peroxydicarbonate (manufactured by NOF Corporation)
[0241] <Polymerization terminator>
[0242] ASB: (allylsulfonyl)benzene
[0243] AC: Allyl Octanoate
[0244] <Chain transfer agent>
[0245] MESE: 2-Mercaptoethanesulfinic acid ethyl ester
[0246] MPA: 3-Mercaptopropionamide
[0247]
[0248]
[0249] <Evaluation>
[0250] The following evaluations were performed on the (meth)acrylic resins and the resin compositions for firing obtained in the Examples and Comparative Examples. The results are shown in Tables 5 and 6. It should be noted that, regarding Comparative Example 2, since PVA was used as a water-soluble surfactant, the monomer micelles in the reaction system became larger, and when a small amount of polymerization initiator was added, the polymerization initiator could not be fully distributed to the micelles, the monomers could not be fully grown into polymers, and the (meth)acrylic resin could not be obtained, so no evaluation was performed.
[0251] (1) Z average particle size and CV value of particle size
[0252] In Examples and Comparative Examples, the aqueous solution containing the (meth)acrylic resin obtained after polymerization was supplied to ZETASIZER to measure the particle size, and the CV value of the particle size was calculated using the following calculation formula.
[0253] CV value (%) = standard deviation / average particle size × 100
[0254] (2) Average molecular weight
[0255] The obtained (meth)acrylic resin was measured for its weight average molecular weight (Mw) and number average molecular weight (Mn) in terms of polystyrene by gel permeation chromatography using LF-804 (manufactured by SHOKO Corporation) as a column.
[0256] (3) Glass transition temperature (Tg)
[0257] The glass transition temperature (Tg) of the obtained (meth)acrylic resin was measured using a differential scanning calorimeter (DSC). Specifically, the temperature was evaluated at a temperature increase rate of 5°C / min from room temperature to 150°C in a nitrogen atmosphere at a flow rate of 50 mL / min.
[0258] (4) Water-soluble surfactant content
[0259] The content of the water-soluble surfactant was calculated using a thermogravimetric mass spectrometer (TG-MS device, manufactured by Netzsch) for the obtained resin composition for calcination based on the amount of decomposition gas at 400 to 600° C. resulting from the combustion of the water-soluble surfactant and the amount of decomposition gas at 200 to 300° C. resulting from the decomposition of the (meth)acrylic resin.
[0260] (5) Tensile test
[0261] The obtained resin solution obtained by dissolving the obtained calcining resin composition in a butyl acetate solution was applied to a release-treated PET film using an applicator and dried in a 100°C air-blown oven for 10 minutes to prepare a resin sheet with a thickness of 20 μm. A graph paper was used as a cover film, and a 1 cm wide strip test piece was prepared using scissors.
[0262] The obtained test piece was subjected to a tensile test at 23°C and 50RH using Autograph AG-IS (manufactured by Shimadzu Corporation) with a chuck distance of 3 cm and a tensile speed of 10 mm / min to confirm stress-strain characteristics (presence of yield stress, maximum stress, and elongation at break).
[0263] (6) Sinterability
[0264] (6-1) Preparation of Conductive Paste
[0265] The sintering resin composition obtained in the examples and comparative examples was dissolved in a terpineol solvent so that the resin solid content was 11% by weight to obtain a resin composition solution. To 44 parts by weight of the obtained resin composition solution, 1 part by weight of oleic acid as a dispersant and 55 parts by weight of nickel powder ("NFP201", manufactured by JFE Minerals Co., Ltd.) as conductive fine particles were added and mixed using a three-roll mill to obtain a conductive paste.
[0266] (6-2) Preparation of ceramic green sheets
[0267] The firing resin compositions obtained in Examples and Comparative Examples, inorganic fine particles, a plasticizer, and an organic solvent were added to form the compositions shown in Tables 3 and 4, and mixed using a ball mill to obtain inorganic fine particle-dispersed slurry compositions.
[0268] The obtained inorganic fine particle dispersion slurry composition was applied onto a release treated polyester film so as to have a thickness of 1 μm after drying, dried at room temperature for 1 hour, then dried at 80° C. for 3 hours using a hot air dryer, and then dried at 120° C. for 2 hours to obtain a ceramic green sheet.
[0269] Note that barium titanate ("BT-02", manufactured by Sakai Chemical Industry Co., Ltd., average particle size 0.2 μm) was used as the inorganic fine particles, and butyl acetate was used as the organic solvent.
[0270] [Table 3]
[0271]
[0272] [Table 4]
[0273]
[0274] (6-3) Preparation of Sintered Ceramic Body
[0275] The conductive paste was applied to one side of the ceramic green sheet by screen printing to a thickness of 1.5 μm after drying, and dried to form a conductive layer, thereby obtaining a ceramic green sheet with a conductive layer. The ceramic green sheet with a conductive layer was cut into 5 cm squares, 100 pieces were stacked, and the mixture was heated at a temperature of 70°C and a pressure of 150 kg / cm 2 The mixture was heated and pressed for 10 minutes under the conditions of , to obtain a laminate.
[0276] The obtained laminate was heated to 400°C at a heating rate of 3°C / min in a nitrogen atmosphere and maintained for 5 hours, then heated to 1350°C at a heating rate of 5°C / min and maintained for 10 hours to obtain a ceramic fired body.
[0277] (6-4) Sinterability Evaluation
[0278] The obtained ceramic fired body was cut and the cross section was observed with an electron microscope and evaluated based on the following criteria.
[0279] It should be noted that when the sintering resin compositions of Comparative Examples 1 and 4 were used, a laminated body could not be prepared, and a ceramic sintered body could not be produced.
[0280] ○: There are no voids, cracks or peeling in the ceramic fired body, and each layer is closely attached.
[0281] ×: Voids, cracks, and peeling were observed in the ceramic fired body. In addition, a ceramic fired body could not be obtained.
[0282] (7) Solution haze
[0283] The obtained resin composition for firing was dissolved in butyl acetate to adjust the resin concentration to 10% by weight, and the haze value was measured using a haze meter ("HM-150", manufactured by Murakami Color Research Laboratory Co., Ltd.).
[0284] (8) Surface roughness
[0285] The center line average roughness (Ra) of the surface of the ceramic green sheet obtained in "(6) Sinterability" was measured using a stylus roughness meter ("Surfcom 1400D", manufactured by Tokyo Seimitsu Co., Ltd.) by a method in accordance with JIS B 0601, and evaluated according to the following criteria. The case where Ra was 0.05 μm or less was evaluated as ◎, the case where Ra was 0.1 μm or less was evaluated as ○, and the case where Ra was greater than 0.1 μm was evaluated as ×.
[0286] ◎: Ra is 0.05 μm or less.
[0287] ○: Ra exceeds 0.05 μm and is 0.1 μm or less.
[0288] ×: Ra exceeds 0.1 μm.
[0289]
[0290]
[0291] Excellent properties were confirmed in any evaluation of Examples 1 to 7. On the other hand, in Comparative Examples 1 and 4, the sheet was brittle in the tensile test and only a small elongation at break was obtained, so the handling of the ceramic green sheet was poor and a laminate could not be obtained. In addition, the glass transition temperature (Tg) of the (meth) acrylic resin obtained in Comparative Example 3 was low, the ceramic green sheet had no stiffness, and the thickness of the sheet was uneven, and interlayer peeling was observed in the ceramic sintered body. In addition, in Comparative Example 5, voids caused by the decomposition gas of residual carbon were confirmed in the center of the ceramic sintered body.
[0292] Industrial Applicability
[0293] According to the present invention, a sintering resin composition can be provided, which has excellent decomposability at low temperatures, can obtain a high-strength molded product, realizes further multilayering and thin filming, and can manufacture a ceramic laminate with excellent characteristics. In addition, an inorganic particle dispersion slurry composition containing the sintering resin composition, and an inorganic particle dispersion sheet formed using the sintering resin composition or the inorganic particle dispersion slurry composition can be provided.
Claims
1. A sintering resin composition comprising a binder resin, The binder resin contains a (meth)acrylic resin (A), The (meth)acrylic resin (A) has at least one selected from a sulfonic group, an alkylsulfonyl group, an aromatic sulfonyl group and a sulfinic acid group at at least one molecular end of the main chain, and has a weight average molecular weight Mw of 1 million to 8 million. The content of the water-soluble surfactant is 0 parts by weight or more and 0.02 parts by weight or less based on 100 parts by weight of the binder resin.
2. The sintering resin composition according to claim 1, wherein The weight average molecular weight Mw of the (meth)acrylic resin (A) is 1,000,000 or more and 7,000,000 or less.
3. The sintering resin composition according to claim 1 or 2, wherein The glass transition temperature Tg of the (meth)acrylic resin (A) is 40° C. or higher.
4. The sintering resin composition according to claim 1 or 2, characterized in that: The CV value of the particle size of the (meth)acrylic resin (A) is 10% or less.
5. The sintering resin composition according to claim 1 or 2, wherein The (meth)acrylic resin (A) contains 40% by weight or more of a segment derived from isobutyl methacrylate.
6. The sintering resin composition according to claim 1 or 2, wherein The (meth)acrylic resin (A) has a segment derived from at least one selected from methyl methacrylate, n-butyl methacrylate, and ethyl methacrylate.
7. The sintering resin composition according to claim 1 or 2, wherein The ratio Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn of the (meth)acrylic resin (A) is 2.0 or less.
8. The sintering resin composition according to claim 1 or 2, wherein The (meth)acrylic resin (A) exhibited a yield stress when formed into a sheet having a thickness of 20 μm, and the maximum stress was 30 N / mm. 2 The elongation at break is 50% or more. 9 . The sintering resin composition according to claim 1 , further comprising an organic solvent having a boiling point of 70° C. or higher.
10. The sintering resin composition according to claim 9, wherein When the content of the binder resin was adjusted to 10% by weight, the haze was less than 10%. 11 . An inorganic fine particle-dispersed slurry composition comprising the sintering resin composition according to claim 1 , and inorganic fine particles. 12 . An inorganic fine particle dispersed sheet produced using the sintering resin composition according to claim 1 or the inorganic fine particle dispersed slurry composition according to claim 11 .
Citation Information
Patent Citations
Binder resin for compacting ceramic
JP1998167836A
Adhesive tape
CN105324453A
Process for producton of water-soluble (method) acrylic polymers, water-soluble (meth) acrylic polymers, and use thereof
CN1533405A
Ceramic slurry and production and use thereof
JP1997011212A
Binder, ceramic slurry, and ceramic green sheet, and adjustment of flowability of ceramic slurry
JP2000063181A