An organic field effect transistor memory based on polyvinyl alcohol and a preparation method thereof

By introducing a hydrophobic film layer into the organic field effect transistor memory, the defects formed by PVA materials at the interface are solved, the memory storage capacity and stability are improved, and the high current switching ratio and stability are achieved, which are suitable for the organic storage field. technological advancements.

CN114512606BActive Publication Date: 2024-11-05NANJING UNIV OF POSTS & TELECOMM
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210038652.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-13
Publication Date
2024-11-05
Estimated Expiration
2042-01-13

AI Technical Summary

Technical Problem

There is room for improvement in existing airport effect transistor memories in terms of storage capacity and stability, especially because defects formed by PVA materials at the interface affect charge transfer and device stability.

Method used

The hydrophobic film is introduced through solution processing to prevent the hydrogen bonding force between PVA and silicon wafers and improve the quality of PVA films. Polytetrafluoroethylene and polyvinyl alcohol spin coating technology are used to prepare high dielectric constant and good solution processing properties. Hydrophobic film layer to improve device performance.

Benefits of technology

It realizes a high current switching ratio at a low operating voltage, has second-order storage capability and stability, has no obvious problems in 100 read and write erase cycle tests, and is stable in the air, providing new technical ideas in the field of organic storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114512606B_ABST
    Figure CN114512606B_ABST
Patent Text Reader

Abstract

The present invention discloses an organic field effect transistor memory based on polyvinyl alcohol and a preparation method thereof, wherein the structure of the memory sequentially includes a source-drain electrode, an organic semiconductor layer, a charge storage layer, a gate insulating layer and a gate electrode as a substrate from top to bottom; wherein a hydrophobic film layer is further provided between the charge storage layer and the gate insulating layer; the hydrophobic film layer is prepared by spin coating a hydrophobic film solution on the gate insulating layer, wherein the hydrophobic film solution is formed by dispersing polytetrafluoroethylene in water; the charge storage layer is prepared by spin coating a polyvinyl alcohol solution on the hydrophobic film layer. The present invention introduces a polytetrafluoroethylene film between a silicon wafer and a polyvinyl alcohol film by spin coating, isolates the hydrogen bonding force between the PVA and the silicon wafer, hinders the formation of a surface dipole, and the spin-coated polytetrafluoroethylene acts as a hydrophobic film, which greatly improves the quality of the upper PVA film and improves the morphology of the PVA film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor memory, and in particular relates to an organic field effect transistor memory based on polyvinyl alcohol and a preparation method thereof. Background Art

[0002] The increasing data traffic and the rapid iteration of data storage technology have put forward an urgent need to improve the performance of storage devices. At present, the high-density integration of semiconductor memory has reached its physical limit. It will be difficult to further increase the storage capacity by reducing the size of the device for a long time in the future. Faced with the contradiction between the increasing storage demand and the inability to continue the miniaturization of semiconductor devices, it is undoubtedly an excellent solution to use organic materials with excellent performance and low price to improve the performance of the device on the basis of the original size. As a basic and important electronic component, organic field-effect transistor memory can realize storage and can be non-volatile through regulation. It has quickly become a research hotspot and has achieved many achievements. However, there is still a lot of room for improvement in its storage capacity and storage stability.

[0003] According to the working principle and device structure, the organic non-volatile memory currently studied at home and abroad can be divided into floating gate type, electret type and ferroelectric type memory devices based on the structure of organic field effect transistor. The main characterization parameters of organic field effect transistor memory are transfer curve, output curve, carrier mobility, storage window, read-write erase cycle, maintenance time, etc. Nowadays, a lot of work is devoted to finding a new material with high storage density, high transmission speed, multi-level storage, and photoelectric coordinated regulation. PVA, as a common dielectric layer material, has a high dielectric constant and good solution processability. These characteristics effectively reduce the operating voltage of organic field effect transistor memory. And PVA has mechanical flexibility, non-toxicity and biodegradability, which further highlights its potential in organic field effect transistor polymer materials. However, due to the limitation of hydroxyl groups, PVA will form defects at the interface, thereby hindering the transfer of charge in the organic field effect transistor, thereby affecting the storage rate and stability of the device. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides an organic field effect transistor memory based on polyvinyl alcohol and a preparation method thereof, which is a method for introducing a hydrophobic film through a solution processing method, which effectively blocks the hydrogen bonding force between PVA and a silicon wafer, hinders the formation of a surface dipole, and improves the quality of an upper PVA film and improves the morphology of the PVA film, which is conducive to advancing the research progress of organic field effect transistor non-volatile memory.

[0005] The present invention is achieved through the following technical solutions:

[0006] A polyvinyl alcohol-based organic field effect transistor memory, the structure of the memory comprising, from top to bottom, a source-drain electrode, an organic semiconductor layer, a charge storage layer, a gate insulating layer and a gate electrode as a substrate; wherein a hydrophobic film layer is further provided between the charge storage layer and the gate insulating layer; the hydrophobic film layer is prepared by spin coating a hydrophobic film solution on the gate insulating layer, the hydrophobic film solution being formed by dispersing polytetrafluoroethylene in water; the charge storage layer is prepared by spin coating a polyvinyl alcohol solution on the hydrophobic film layer.

[0007] Preferably, the polyvinyl alcohol solution is formed by dissolving polyvinyl alcohol in dimethyl sulfoxide solvent.

[0008] Preferably, the material of the source and drain electrodes is metal Cu; the material of the organic semiconductor layer is pentacene; the material of the gate insulating layer is silicon dioxide; and the gate electrode is highly doped silicon.

[0009] Preferably, the thickness of the source-drain electrode is 100 nm; the thickness of the organic semiconductor layer is 30-50 nm; the thickness of the charge storage layer is 20-30 nm; and the thickness of the gate insulating layer is 50 nm.

[0010] A method for preparing an organic field effect transistor memory based on polyvinyl alcohol comprises the following steps:

[0011] Step 1) preparing a hydrophobic film layer material solution: dispersing a polytetrafluoroethylene suspension in water to a concentration of 6% to 17% after dilution, and ultrasonically treating for 15 minutes to obtain a hydrophobic film solution for standby use;

[0012] Step 2) preparing a charge storage layer material solution: dissolving polyvinyl alcohol in dimethyl sulfoxide solvent at a concentration of 3 mg / mL, heating at 80° C. to completely dissolve it, and allowing it to stand to obtain a polyvinyl alcohol solution for later use;

[0013] Step 3) using the gate electrode and the gate insulating layer grown thereon as a substrate, and sequentially washing with acetone, ethanol, and deionized water, and drying;

[0014] Step 4) placing the cleaned substrate after treatment in step 3) under ultraviolet ozone treatment for 5 to 10 minutes;

[0015] Step 5) filtering the hydrophobic film solution prepared in step 1) through a 0.22 μm filter, aspirating with a syringe and injecting it onto the substrate treated in step 4) to form a film by spin coating, placing the spin-coated sample in an oven at 80° C. for 30 minutes to remove excess solvent, thereby obtaining a hydrophobic film layer;

[0016] Step 6) cooling the sample obtained in step 5) to room temperature, drawing the polyvinyl alcohol solution prepared in step 2) into a syringe and spin coating the solution on the hydrophobic film layer obtained in step 5) to form a film, placing the spin-coated sample in an oven at 80° C. for 30 minutes, removing excess solvent, and obtaining a charge storage layer;

[0017] Step 7) Vacuum-evaporating an organic semiconductor layer and a source-drain electrode sequentially on the charge storage layer obtained in step 6) to obtain the result.

[0018] Preferably, the spin coating process in step 5) is: adjusting the rotation speed to 3000 rpm and rotating at a constant speed for 30 seconds; and the spin coating process in step 6) is: adjusting the rotation speed to 1500 rpm and rotating at a constant speed for 60 seconds.

[0019] Preferably, the vacuum evaporation process in step 7) is: the evaporation rate The vacuum degree is controlled at 4×10 -4 Pa~5×10 -4 Pa.

[0020] Preferably, the concentration after dilution in step 1) is 10%.

[0021] The beneficial effects of the present invention are as follows:

[0022] (1) The present invention introduces a polytetrafluoroethylene film between the silicon wafer and the polyvinyl alcohol film by spin coating, thereby isolating the hydrogen bonding force between the PVA and the silicon wafer and hindering the formation of surface dipoles. The spin-coated polytetrafluoroethylene acts as a hydrophobic film, which greatly improves the quality of the upper PVA film and improves the morphology of the PVA film and the upper pentacene film.

[0023] (2) The charge storage layer of the organic field effect transistor memory provided by the present invention is prepared by solution spin coating, which has the characteristics of simple preparation process and large-area preparation. In addition, the materials used in the present invention are easy to obtain and low in price.

[0024] (3) The organic field effect transistor memory provided by the present invention can achieve a higher current switching ratio under a lower operating voltage condition and has excellent transistor performance.

[0025] (4) The organic field effect transistor memory provided by the present invention has a second-order storage, is stable after 100 read-write-erase cycle tests, and has no obvious charge leakage in a 10,000 second hold time test. It has a low threshold voltage (-1.66V) and a high on / off ratio (greater than 10 4 ).

[0026] (5) The organic field effect transistor memory provided by the present invention can operate in the air. Due to the presence of the hydrophobic film, the influence of part of the water on the device is isolated, the stability of the device is improved, and it can provide new technical ideas for the future organic storage field.

[0027] (6) The organic field effect transistor memory provided by the present invention has a simple preparation process and can be prepared on a large scale to control the appearance of thin films, which is convenient for promotion and integrated commercial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a schematic diagram of the structure of the organic field effect transistor memory based on polyvinyl alcohol in Example 1;

[0029] Figure 1 Middle: 1. Source and drain electrodes; 2. Organic semiconductor layer; 3. Charge storage layer; 4. Gate insulating layer; 5. Gate electrode; 6. Hydrophobic film layer;

[0030] Figure 2 Characterization of the contact angle of the polytetrafluoroethylene film of the organic field effect transistor memory based on polyvinyl alcohol in Example 2;

[0031] Figure 3 This is the AFM surface morphology of the polytetrafluoroethylene film of the polyvinyl alcohol-based organic field effect transistor memory in Example 2.

[0032] Figure 4 The AFM surface morphology of the charge trapping layer PVA of the organic field effect transistor memory based on polyvinyl alcohol: a is the morphology of the single PVA film prepared in Comparative Example 1, and b is the morphology of the film after the lower layer spin-coated with polytetrafluoroethylene prepared in Example 2;

[0033] Figure 5 The AFM surface morphology of the organic semiconductor layer pentacene of the organic field effect transistor memory based on polyvinyl alcohol: a is the morphology of the single PVA film prepared in Comparative Example 1, and b is the morphology of the film after the lower layer spin-coated with polytetrafluoroethylene prepared in Example 2;

[0034] Figure 6 are transfer characteristic curves of organic field effect transistor memory based on polyvinyl alcohol: a is the transfer characteristic curve of the organic field effect transistor memory prepared in comparative example 1, and b is the transfer characteristic curve of the organic field effect transistor memory prepared in example 2;

[0035] Figure 7 : are output characteristic curves of organic field effect transistor memory based on polyvinyl alcohol: a is the output characteristic curve of the organic field effect transistor memory prepared in comparative example 1, and b is the output characteristic curve of the organic field effect transistor memory prepared in example 2;

[0036] Figure 8 Memory window characteristic curves of organic field effect transistor memory based on polyvinyl alcohol: a is the memory window characteristic curve of the organic field effect transistor memory prepared in comparative example 1, and b is the memory window characteristic curve of the organic field effect transistor memory prepared in example 2;

[0037] Fig. 9 is a read-write-erase cycle characteristic curve of the organic field effect transistor memory based on polyvinyl alcohol in Example 2;

[0038] Fig.10 This is the retention time characteristic curve of the organic field effect transistor memory based on polyvinyl alcohol in Example 2. DETAILED DESCRIPTION

[0039] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may extend based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0040] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.

[0041] In the following examples, polytetrafluoroethylene and polyvinyl alcohol (PVA) were purchased from Sigma, and pentacene was purchased from TCI.

[0042] Example 1

[0043] An organic field effect transistor memory based on polyvinyl alcohol, the structural diagram is as follows Figure 1 As shown, the structure of the memory includes, from top to bottom, a source-drain electrode 1, an organic semiconductor layer 2, a charge storage layer 3, a gate insulating layer 4, and a gate electrode 5 as a substrate; wherein a hydrophobic film layer 6 is further provided between the charge storage layer and the gate insulating layer; the hydrophobic film layer 6 is prepared by spin coating a hydrophobic film solution on the gate insulating layer 4, wherein the hydrophobic film solution is formed by dispersing polytetrafluoroethylene in water; the charge storage layer 3 is prepared by spin coating a polyvinyl alcohol solution on the hydrophobic film layer 6, wherein the polyvinyl alcohol solution is formed by dissolving polyvinyl alcohol in a dimethyl sulfoxide solvent.

[0044] The organic field effect transistor memory uses N-type heavily doped silicon as the gate electrode, and a 50nm thick silicon dioxide layer grown on it as the gate insulating layer; a film (hydrophobic film) is first prepared by spin coating a polytetrafluoroethylene solution dispersed in water, and then a flat film is prepared by spin coating a PVA solution dissolved in dimethyl sulfoxide on the hydrophobic film. Pentacene with a thickness of about 50nm is used as the organic semiconductor layer, and a 100nm thick metal Cu is used as the source and drain electrodes.

[0045] The preparation method of the above-mentioned organic field effect transistor memory has the following specific steps:

[0046] (1) Disperse the polytetrafluoroethylene suspension in water to dilute it to concentrations of 6%, 10%, 12.5%, and 17%, respectively. Ultrasonicate for 15 minutes before use.

[0047] (2) Dissolve polyvinyl alcohol (Mw-116000) in dimethyl sulfoxide (DMSO) solvent at a concentration of 3 mg / mL, heat at 80°C to completely dissolve it, and let it stand for later use.

[0048] (3) The silicon wafer of N-type heavily doped silicon and the 50 nm silicon dioxide gate insulating layer grown thereon was cut into pieces of 1.5 cm × 1.5 cm in size, and was cleaned in acetone for 15 min, ethanol for 15 min, and deionized water for 15 min, and then dried at 120°C.

[0049] (4) The cleaned substrate after drying is placed in an ultraviolet ozone treatment for 5 to 10 minutes.

[0050] (5) Filter the prepared polytetrafluoroethylene solution through a 0.22 μm filter, draw it up with a syringe and inject it onto a clean silicon wafer substrate to spin-coat a film (hydrophobic film), adjust the speed to 3000 rpm and rotate at a constant speed for 30 seconds, place the spin-coated sample in an oven at 80°C for 30 minutes, remove excess solvent and set aside.

[0051] (6) The prepared sample was cooled to room temperature, the prepared polyvinyl alcohol solution was sucked with a syringe and injected onto the hydrophobic film to be spin-coated again, the rotation speed was adjusted to 1500 rpm and the sample was placed in an oven at 80°C for 30 min to remove excess solvent and obtain a charge storage layer.

[0052] (7) Vacuum evaporation of pentacene and source / drain Cu electrodes on the charge storage layer in sequence at a deposition rate of The vacuum degree is controlled at 4×10 -4 Pa~5×10 -4 Pa, that is, the channel width of the mask is 1500μm and the length is 100μm.

[0053] During the above-mentioned preparation process of the organic field effect transistor memory, the room temperature in the laboratory is always kept constant at 25° C. and the humidity is kept below 50%.

[0054] Comparative Example 1

[0055] A method for preparing an organic field effect transistor memory based on polyvinyl alcohol, the specific steps are as follows:

[0056] (1) Dissolve polyvinyl alcohol (Mw-116000) in dimethyl sulfoxide (DMSO) solvent at a concentration of 3 mg / mL, heat at 60°C to completely dissolve it, and let it stand for later use.

[0057] (2) The N-type heavily doped silicon and the 50 nm silicon dioxide gate insulating layer grown thereon were cut into pieces of 1.5 cm × 1.5 cm in size, and cleaned in acetone for 15 min, ethanol for 15 min, and deionized water for 15 min, and then dried at 120°C.

[0058] (3) The cleaned substrate after drying is placed in an ultraviolet ozone treatment for 5 to 10 minutes.

[0059] (4) Use a syringe to absorb the prepared polyvinyl alcohol solution and spin-coat it on a clean substrate to form a film. Adjust the rotation speed to 1500 rpm and rotate it at a constant speed for 60 seconds. Place the spin-coated sample in an oven at 80°C for 30 minutes to remove excess solvent to obtain a charge storage layer. Figure 4 a shows the AFM morphology of the PVA film after spin coating.

[0060] (5) Vacuum evaporation of pentacene and source / drain Cu electrodes on the charge storage layer in sequence at a deposition rate of The vacuum degree is controlled at 5×10 -4 Pa~4×10 -4 Pa. The channel width of the mask is 1500μm and the length is 100μm. Figure 5 a shows the AFM morphology of pentacene film.

[0061] Example 2

[0062] A method for preparing an organic field effect transistor memory based on polyvinyl alcohol, the specific steps are as follows:

[0063] (1) Disperse the polytetrafluoroethylene suspension in water to a concentration of 10% after dilution, and ultrasonically treat for 15 minutes before use.

[0064] (2) Dissolve polyvinyl alcohol (Mw-116000) in dimethyl sulfoxide (DMSO) solvent at a concentration of 3 mg / mL, heat at 60°C to completely dissolve it, and let it stand for later use.

[0065] (3) The silicon wafer of N-type heavily doped silicon and the 50 nm silicon dioxide gate insulating layer grown thereon was cut into pieces of 1.5 cm × 1.5 cm in size, and was cleaned in acetone for 15 min, ethanol for 15 min, and deionized water for 15 min, and then dried at 120°C.

[0066] (4) The cleaned substrate after drying is placed in an ultraviolet ozone treatment for 5 to 10 minutes.

[0067] (5) Filter the prepared polytetrafluoroethylene solution through a 0.22 μm filter, draw it up with a syringe and inject it onto a clean silicon wafer substrate for spin coating. Adjust the rotation speed to 3000 rpm and rotate it at a constant speed for 30 seconds. Place the spin-coated sample in an oven at 80°C for 30 minutes to remove excess solvent.

[0068] like Figure 2 The figure shows the contact angle characterization of the polytetrafluoroethylene film. It can be seen from the figure that the polytetrafluoroethylene film provides a hydrophobic interface.

[0069] like Figure 3 The AFM morphology of the PTFE film after spin coating is shown in Figure 1. As can be seen from the figure, the PTFE film was successfully prepared, but its roughness was significantly higher.

[0070] (6) The prepared sample was cooled to room temperature, the prepared polyvinyl alcohol solution was sucked with a syringe and injected onto the hydrophobic film to be spin-coated again, the rotation speed was adjusted to 1500 rpm and the sample was placed in an oven at 80°C for 30 min to remove excess solvent and obtain a charge storage layer.

[0071] like Figure 4 b shows the AFM morphology of the PVA film after spin coating. Figure 4 a It can be seen from the comparison that the polyvinyl alcohol film spin-coated on the polytetrafluoroethylene in this embodiment is relatively flat and has a lower roughness. Compared with the comparative example 1, the roughness is lower, thereby improving the mobility of the device.

[0072] (7) Vacuum evaporation of pentacene and source / drain Cu electrodes on the charge storage layer in sequence at a deposition rate of The vacuum degree is controlled at 5×10 -4 Pa~4×10 -4 Pa, that is, the channel width of the mask is 1500μm and the length is 100μm.

[0073] like Figure 5 b shows the AFM morphology of pentacene film. Figure 5 a Comparison shows that the pentacene particles in this embodiment grow in an island shape and have a high crystallinity.

[0074] Test Example 1

[0075] After the device was prepared, the electrical properties of the organic field effect transistor memory prepared in Example 2 and Comparative Example 1 were tested using Keithley 4200, and the test results were as follows:

[0076] Figure 6 a is the transfer curve of the memory device prepared in comparative example 1. As can be seen from the figure, the carrier mobility is 0.04 cm 2 V -1 s -1 , threshold voltage (-7.02V), on / off ratio greater than 10 3 .

[0077] Figure 6 b is the transfer curve of the memory device obtained in Example 2. As can be seen from the figure, the carrier mobility is 0.16 cm 2 V -1 s -1 , threshold voltage (-1.66V), switch closed greater than 10 3 .

[0078] Figure 7 a is the output curve of the memory device obtained in comparative example 1. It can be seen from the figure that when V is fixed DS =-15V, and the output curves are tested at different gate voltage conditions of 0, -6V, -12V, -18V, -24V, and -30V. It can be seen that the device has a good field effect.

[0079] Figure 7 b is the output curve of the memory device obtained in Example 2. It can be seen from the figure that when V is fixed DS =-15V, and the output curves are tested at different gate voltage conditions of 0, -6V, -12V, -18V, -24V, and -30V. It can be seen that the device has a good field effect.

[0080] Figure 8 a is the storage window curve of the storage device prepared in comparative example 1, from which it can be seen that there is no storage window.

[0081] Figure 8 b is the storage window curve of the memory device prepared in Example 2. It can be seen from the figure that the maximum forward storage window is 15V, and increases with the increase of gate voltage, which improves the small storage window characteristic of organic field effect transistor memory based solely on PVA.

[0082] Fig. 9 The memory device prepared in Example 2 was subjected to 100 read-write-erase cycle tests. It can be seen from the figure that no obvious changes occurred, and the device showed strong stability.

[0083] Fig.10 This is a test of the data retention capability of the memory device prepared in Example 2. As can be seen from the figure, there is no obvious charge leakage phenomenon after 10,000 seconds of maintenance, indicating that the data retention capability is reliable.

[0084] According to the test results of Comparative Example 1 and Example 2, the method of improving the PVA-based organic field effect transistor memory of the present invention improves the mobility and storage window of the device, reduces the turn-on voltage of the device, and reduces the energy loss. It is also low-priced and cost-saving, and is easy to promote and integrate for commercial applications.

[0085] Although the present invention has been illustrated and described with reference to certain preferred embodiments of the present invention, it should be understood by those skilled in the art that the above contents are further detailed descriptions of the present invention in conjunction with specific embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. Those skilled in the art may make various changes in form and details, including making several simple deductions or substitutions, without departing from the spirit and scope of the present invention.

Claims

1. An organic field effect transistor memory based on polyvinyl alcohol, characterized in that: The structure of the memory includes, from top to bottom, a source-drain electrode, an organic semiconductor layer, a charge storage layer, a gate insulating layer, and a gate electrode as a substrate; wherein a hydrophobic film layer is further provided between the charge storage layer and the gate insulating layer; the hydrophobic film layer is prepared by spin coating a hydrophobic film solution on the gate insulating layer, the hydrophobic film solution being formed by dispersing polytetrafluoroethylene in water; the charge storage layer is prepared by spin coating a polyvinyl alcohol solution on the hydrophobic film layer; The polyvinyl alcohol solution is formed by dissolving polyvinyl alcohol in dimethyl sulfoxide solvent; The material of the source and drain electrodes is metal Cu; the material of the organic semiconductor layer is pentacene; the material of the gate insulating layer is silicon dioxide; and the gate electrode is highly doped silicon; The method for preparing the memory comprises the following steps: Step 1) preparing a hydrophobic film layer material solution: dispersing a polytetrafluoroethylene suspension in water to a concentration of 6% to 17% after dilution, and subjecting the solution to ultrasonic treatment for 15 min to obtain a hydrophobic film solution for later use; Step 2) Prepare a charge storage layer material solution: dissolve polyvinyl alcohol in dimethyl sulfoxide solvent at a concentration of 3 mg / mL, heat at 80°C to completely dissolve it, and let it stand to obtain a polyvinyl alcohol solution for later use; Step 3) using the gate electrode and the gate insulating layer grown thereon as a substrate, and sequentially washing with acetone, ethanol, and deionized water, and drying; Step 4) placing the cleaned substrate after treatment in step 3) under ultraviolet ozone treatment for 5 to 10 minutes; Step 5) Filter the hydrophobic film solution prepared in step 1) through a 0.22 μm filter, draw it up with a syringe and inject it onto the substrate treated in step 4) to spin-coat the film, place the spin-coated sample in an oven at 80° C. for 30 min, remove excess solvent, and obtain a hydrophobic film layer; Step 6) Cool the sample obtained in step 5) to room temperature, draw the polyvinyl alcohol solution prepared in step 2) into a syringe and spin-coat the hydrophobic film layer obtained in step 5) to form a film, place the spin-coated sample in an oven at 80° C. for 30 min, remove excess solvent, and obtain a charge storage layer; Step 7) Vacuum-evaporating an organic semiconductor layer and a source-drain electrode sequentially on the charge storage layer prepared in step 6) to obtain the result.

2. The organic field effect transistor memory based on polyvinyl alcohol according to claim 1, characterized in that: The thickness of the source-drain electrode is 100 nm; the thickness of the organic semiconductor layer is 30-50 nm; the thickness of the charge storage layer is 20-30 nm; and the thickness of the gate insulating layer is 50 nm.

3. The organic field effect transistor memory based on polyvinyl alcohol according to claim 1, characterized in that: Step 5) The spin coating process is: adjusting the rotation speed to 3000 rpm and rotating at a constant speed for 30 s; Step 6) The spin coating process is: adjusting the rotation speed to 1500 rpm and rotating at a constant speed for 60 s.

4. The organic field effect transistor memory based on polyvinyl alcohol according to claim 1, characterized in that: Step 7) The vacuum evaporation process is as follows: the evaporation rate is 0.1 Å / s, and the vacuum degree is controlled at 4×10 -4 Pa ~ 5×10 -4 Pa.

5. The organic field effect transistor memory based on polyvinyl alcohol according to claim 1, characterized in that: The concentration after dilution in step 1) is 10%.

Citation Information

Patent Citations

  • Organic field effect transistor memory based on core-shell type clustered star shaped structure polymer and preparation method thereof

    CN106169536A

  • Organic field-effect transistor memory based on polymer doped semiconductor nanoparticle

    CN106953010A

  • Nano array and tunnel structure coexisting organic field effect transistor memory and manufacturing method thereof

    CN112259684A

  • Fabrication of non-volatile organic field-effecttransistor memory using polymeric gate electret layer

    KR100680001B1

  • Non-volatile organic memory device using polymer electret and NANO floating gate, and manufacturing method thereof

    KR1020160048444A