An organic memristor with ultra-low operating voltage and a method for preparing the same

The organic memristor prepared by aqueous solution processing method solves the problems of high operating voltage and poor stability of organic memristors, realizes an ultra-low operating voltage and high stability of organic memristors, advances its research process and is artificial Neural networks provide reliable prototype devices.

CN114512609BActive Publication Date: 2024-11-05NANJING UNIV OF POSTS & TELECOMM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210037716.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-13
Publication Date
2024-11-05
Estimated Expiration
2042-01-13

AI Technical Summary

Technical Problem

The existing organic memristor has high operating voltage and poor stability, which hinders its research progress.

Method used

The organic memristor with ultra-low operating voltage was prepared by aqueous solution processing. The nanofilm was prepared by dissolving chlorophyll copper sodium in ultra-pure water to form a solution, spin coating, and vacuum deposition of the top electrode to form an organic memory of a vertical sandwich structure. Resistor.

Benefits of technology

The ultra-low operating voltage (<100mV), high switching ratio (106), long retention characteristics (>1×104s) and high read-write erasing cycle tolerance (>6000 times) of the organic memristor, and The process is simple, non-toxic and harmless, and is suitable for the development of low-cost and high-stability artificial neural networks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114512609B_ABST
    Figure CN114512609B_ABST
Patent Text Reader

Abstract

The present invention discloses an organic memristor with ultra-low operating voltage and a preparation method thereof. The memristor is a vertical sandwich structure, and includes a substrate, a bottom electrode, an organic functional layer and a top electrode from bottom to top; wherein the organic functional layer is a nanofilm prepared by spin coating an organic functional layer solution on the bottom electrode, and the organic functional layer solution is formed by dissolving sodium copper chlorophyllin in ultrapure water, and the structural formula of the sodium copper chlorophyllin is shown in formula (I). The present invention uses small and medium-sized molecules-sodium copper chlorophyllin (organic salt), and solves the problem of easy crystallization in the spin coating process of sodium copper chlorophyllin by controlling the spin coating process parameters, successfully spin coating in water solvent to prepare a uniform and smooth film comparable to the evaporation method, and prepares a vertical sandwich structure device based on ITO / sodium copper chlorophyllin / Ag, and finally achieves ultra-low operating voltage, high switching ratio, high retention characteristics, and read-write-erase cycles>6000 times.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of organic electronics and information technology, and relates to an organic diode memristor device, and in particular to an organic memristor with an ultra-low operating voltage and a preparation method thereof. Background Art

[0002] With the failure of Moore's Law, the future is about to enter the post-Moore's Law era. The continuous growth of data storage and processing needs urgently requires an emerging technology to take up the banner. Memristors provide new opportunities to overcome the shortcomings of traditional memory chips. They can be used as non-volatile memory. Their device composition is simple, RRAM has fast operation speed and low power consumption; long write-erase endurance and retention characteristics, and different operation methods can realize multi-value storage of RRAM devices; they have excellent scalability and good compatibility with current CMOS processes, providing potential for high-density integration and low-cost manufacturing. More importantly, people hope to effectively simulate the work of the brain through the integrated network of memristor devices to achieve storage and computing integration.

[0003] Organic materials have the advantages of simple film formation (such as inkjet printing, dip coating and spin coating), low cost, flexible and stretchable, and biocompatible. More importantly, their electronic properties can be regulated by molecular design. However, organic materials also face huge challenges. For example, toxic and harmful solvents are required for spin coating, which is not environmentally friendly. In addition, the operating voltage of organic memristor devices is large, and the device stability and uniformity are poor. This is also the main reason that hinders the research progress of organic memristors. Summary of the invention

[0004] In view of the deficiencies of the prior art, the present invention provides an organic memristor with ultra-low operating voltage and a preparation method thereof, wherein an organic (salt) small and medium-sized molecular nanofilm with low roughness is obtained by an aqueous solution processing method, and an organic memristor with ultra-low operating voltage is prepared. The problem of high operating voltage and poor stability of the existing organic memristor is effectively solved, which is conducive to promoting the research progress of organic memristors.

[0005] The present invention is achieved through the following technical solutions:

[0006] An organic memristor with an ultra-low operating voltage, the memristor is a vertical sandwich structure, and includes a substrate, a bottom electrode, an organic functional layer and a top electrode from bottom to top; wherein the organic functional layer is a nanofilm prepared by spin coating an organic functional layer solution on the bottom electrode, the organic functional layer solution is formed by dissolving sodium copper chlorophyllin in ultrapure water, and the structural formula of the sodium copper chlorophyllin is shown in formula (I):

[0007]

[0008] Preferably, the material of the substrate is glass; the material of the bottom electrode is indium tin oxide; and the material of the top electrode is metal Ag.

[0009] Preferably, the thickness of the bottom electrode is 185 nm; the thickness of the organic functional layer is 40-50 nm; and the thickness of the top electrode is 40-50 nm.

[0010] A method for preparing an organic memristor with ultra-low operating voltage comprises the following steps:

[0011] Step 1) preparing an organic functional layer solution: dissolving the sodium copper chlorophyllin material in an ultrapure water solvent at a concentration of 20 mg / mL, and heating at 60° C. to completely dissolve it to obtain an organic functional layer solution;

[0012] Step 2) a bottom electrode layer is formed on the substrate material, and the substrate is cleaned with an ITO cleaning agent and ultrapure water ultrasonic cleaning in sequence, the cleaned substrate is first blown dry with ordinary nitrogen, and then placed in an oven at 120° C. for 1 hour to remove the remaining moisture;

[0013] Step 3) placing the cleaned substrate after the treatment in step 2) under ultraviolet ozone treatment for 30 minutes;

[0014] Step 4) using a pipette to draw 150-200 μL of the organic functional layer solution prepared in step 1) and spin-coating it on the substrate treated in step 3) to form a film, placing the spin-coated sample in a vacuum oven at room temperature and gradually heating it to 60° C., annealing for 30 minutes, removing excess solvent, and obtaining an organic functional layer;

[0015] Step 5) Vacuum evaporation of the top electrode on the organic functional layer prepared in step 4) with the vacuum degree controlled at 4×10 -4 Pa~5×10 -4 Pa;

[0016] Step 6) After the vacuum evaporation is completed, the vacuum state is maintained and the top electrode is cooled to room temperature for 30 minutes to obtain the organic memristor with ultra-low operating voltage.

[0017] Preferably, the heating time in step 1) is 5 hours.

[0018] Preferably, the ultrasonic cleaning process in step 2) is: first cleaning with an ITO cleaning agent, then cleaning twice with ultrapure water, and the ultrasonic cleaning time is 30 minutes.

[0019] Preferably, the spin coating process in step 4) is: first adjust the rotation speed to 500 rpm for 9 seconds, then adjust the rotation speed to 3000 rpm for 30 seconds, and spin coating in air with the air humidity controlled below 60%.

[0020] Preferably, the evaporation rate of the vacuum evaporation in step 5) is

[0021] The beneficial effects of the present invention are as follows:

[0022] (1) The organic memristor of the present invention has the characteristics of simple structural design and easy preparation. The solution processing method adopted by the present invention is different from the prior art (organic solvent) in that ultrapure water is used as the solvent for spin coating, which is non-toxic and harmless.

[0023] (2) The present invention effectively solves the problem of easy crystallization of organic small and medium-sized molecular materials during spin coating, and prepares a nano-thin film with a roughness (Ra=1.02nm) comparable to that of the evaporation method.

[0024] (3) The organic memristor of the present invention has the characteristics of ultra-low operating voltage and ultra-stability. The prepared organic memristor has ultra-low operating voltage (<100mV), high switching ratio (10 6 ), high retention characteristics (>1×10 4 s, only test time, actual life span exceeds 10 years), read-write-erase cycle>6000 times.

[0025] (4) The organic memristor structure of the present invention is easy to design, has a simple process, high yield, and is universal. It has opened up a new material strategy for reliable ultra-low operating voltage artificial synapses to operate stably in an air environment, providing technical reserves and reliable prototype devices for building low-cost, high-stability artificial neural networks, thereby promoting a more precise realization of the development of artificial intelligence devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of the structure of an organic memristor device with ultra-low operating voltage;

[0027] Figure 2 The AFM surface morphology of the organic functional layer nanofilm in Example 1;

[0028] Figure 3 is a SEM cross-sectional view of the organic memristor in Example 1;

[0029] Figure 4 is the IV curve of the organic memristor in Example 1;

[0030] Figure 5 is the read-write-erase cycle characteristic curve of the organic memristor in Example 1;

[0031] Figure 6 is a holding time characteristic curve of the organic memristor in Example 1;

[0032] Figure 7is a distribution diagram of the IV curve SET Voltage of the organic memristor in Example 1;

[0033] Figure 8 is a morphology image of the organic functional layer nanofilm in Example 2 under an optical microscope;

[0034] Fig. 9 is the IV curve of the organic memristor in Example 2;

[0035] Fig.10 is the AFM surface morphology of the organic functional layer nanofilm in Example 3;

[0036] Fig.11 is the IV curve of the organic memristor in Example 3;

[0037] Fig.12 is a distribution diagram of Set Voltage of different devices of the organic memristor in Example 3;

[0038] Fig.13 3 is a distribution diagram of the Reset Voltage of different devices of the organic memristor in Example 3. DETAILED DESCRIPTION

[0039] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may extend based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0040] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.

[0041] Example 1

[0042] An organic memristor with ultra-low operating voltage, such as Figure 1 As shown, the memristor is a vertical sandwich structure, which includes a substrate, a bottom electrode, an organic functional layer and a top electrode from bottom to top; wherein, the organic functional layer is a nanofilm prepared by spin-coating an organic functional layer solution on the bottom electrode, and the organic functional layer solution is formed by dissolving sodium copper chlorophyll in ultrapure water.

[0043] The preparation method of the organic memristor comprises the following specific steps:

[0044] (1) Preparation of organic functional layer solution: Sodium copper chlorophyllin material was dissolved in ultrapure water solvent at a concentration of 20 mg / mL, and heated at 60° C. for 5 h to completely dissolve it, thereby obtaining an organic functional layer solution.

[0045] The structural formula of sodium copper chlorophyllin is shown in the following formula (I), which is a stable structure of porphyrin.

[0046]

[0047] (2) Glass is selected as a substrate, and a layer of indium tin oxide with a thickness of 185 nm is generated on the glass to form ITO conductive glass. The ITO conductive glass is cleaned with an ITO cleaning agent (once) and ultrapure water (twice) for 30 minutes, then blown dry with ordinary nitrogen and placed in an oven at 120°C for 30 minutes to remove residual moisture.

[0048] (3) The dried ITO conductive glass is treated with UV-ozone for 30 minutes.

[0049] (4) Place the substrate at the center of the spin coating table, use a pipette to draw 150-200 μL of the organic functional layer solution and evenly spread it on the substrate, adjust the rotation speed and time (first adjust the rotation speed to 500 rpm for 9 seconds, then adjust the rotation speed to 3000 rpm for 30 seconds) and spin coat in air. The air humidity is controlled below 60%. Place the spin-coated sample in a vacuum oven at room temperature and gradually heat it to 60°C. Anneal for 30 minutes to remove excess solvent to obtain an organic functional layer nanofilm with a thickness of 40-50 nm.

[0050] (5) Place the substrate with the nanofilm into the vacuum evaporation equipment and control the pressure in the vacuum chamber to 4×10 -4 Pa~5×10 -4 Pa, vacuum evaporation of metal Ag anode began, the evaporation rate was The thickness is 40-50 nm; the thickness of the film is measured using a step profiler and further confirmed by SEM.

[0051] (6) After the evaporation experiment is completed, the metal Ag anode is cooled to room temperature in the vacuum chamber for 30 minutes to complete all the preparation processes of the organic memristor. Then, the chamber is opened to take out the wafer and conduct relevant electrical performance tests on the device.

[0052] After the device is prepared, the electrical performance of the organic memristor device prepared in this embodiment is tested using Keithley 4200, and the prepared organic memristor is characterized. The specific test results are as follows:

[0053] Figure 2 This is an AFM morphology image of the organic nanofilm prepared in this embodiment. From the image, it can be found that the roughness of the nanofilm of small and medium-sized molecule sodium copper chlorophyllin prepared by solution heating treatment and aqueous solution spin coating is about Ra=1.02nm, which is comparable to the small molecule film deposited by vapor deposition.

[0054] Figure 3 This is a SEM image of the organic memristor device prepared in this embodiment. From the image, it can be found that the ITO electrode at the bottom is about 185nm, the thickness of the sodium copper chlorophyll nanofilm in the middle is about 40-50nm, and the thickness is uniform, and the thickness of the evaporated silver electrode on the top is 40-50nm.

[0055] Figure 4 The IV curve of the organic memristor prepared in this embodiment after 100 cycles is shown in FIG. 1 . The organic memristor can realize stable switching between high and low resistance states. It can be seen from the figure that the SET voltage of the memristor is less than 100 mV, and the switching ratio is about 10 6 .

[0056] Figure 5 The organic memristor prepared in this embodiment was subjected to 6000 read-write-erase cycle tests, and it can be seen that no obvious changes occurred, indicating that the memristor has strong cycle tolerance.

[0057] Figure 6 The data retention capability of the organic memristor prepared in this embodiment was tested. There was no obvious charge leakage after 10,000 seconds of retention. From the retention time theory, it can be inferred that the memristor can be maintained for more than 10 years without obvious attenuation.

[0058] Figure 7 This is a distribution curve of the SET voltage of the 100-cycle IV curve of the organic memristor prepared in this embodiment. It can be seen from the figure that the SET voltage distribution is relatively uniform (the variance of the SET voltage is 0.01581), and the average value of the SET voltage is about 60mV.

[0059] Example 2

[0060] A method for preparing an organic memristor, the specific steps are as follows:

[0061] (1) Preparation of organic functional layer solution: Dissolve the sodium copper chlorophyllin material in ultrapure water solvent at a concentration of 20 mg / mL to obtain an organic functional layer solution.

[0062] (2) Glass was selected as a substrate, and a layer of indium tin oxide with a thickness of 185 nm was generated on the glass to form ITO conductive glass. The ITO conductive glass was cleaned with an ITO cleaning agent (once) and ultrapure water (twice) for 30 min, then dried with ordinary nitrogen and placed in an oven at 120° C. for 30 min.

[0063] (3) The dried ITO conductive glass is treated with UV-ozone for 30 minutes.

[0064] (4) Place the substrate at the center of the spin coating table, use a pipette to draw 150-200 μL of the organic functional layer solution and evenly spread it on the substrate, adjust the rotation speed and time (first adjust the rotation speed to 500 rpm for 9 seconds, then adjust the rotation speed to 3000 rpm for 30 seconds) for spin coating, place the spin-coated sample in a vacuum oven at room temperature and gradually heat it to 60°C, anneal for 30 minutes, remove excess solvent, and obtain an organic functional layer nanofilm with a thickness of about 40 nm.

[0065] (5) Place the substrate with the nanofilm into the vacuum evaporation equipment and control the pressure in the vacuum chamber to 4×10 -4 Pa~5×10 -4 Pa range, the evaporation of metal Ag anode begins, and the evaporation rate is The thickness is 40-50 nm; the thickness of the film is measured using a step profiler.

[0066] (6) After the evaporation experiment is completed, the metal Ag anode is cooled to room temperature in the vacuum chamber, and all the preparation processes of the memristor are completed. Then the chamber is opened to take out the wafer and conduct relevant electrical performance tests on the device.

[0067] After the device is prepared, the electrical performance of the organic memristor device prepared in this embodiment is tested using Keithley 4200, and the prepared organic memristor is characterized. The specific test results are as follows:

[0068] Figure 8 This is the morphology of the organic nanofilm prepared in this example under an optical microscope. From the figure, it can be seen that the spin coating of small and medium-sized molecules of sodium copper chlorophyllin in aqueous solution without heating treatment will encounter the common problem of small molecule spin coating (easy crystallization).

[0069] Fig. 9 The IV curve of the organic memristor prepared in this embodiment shows that the nanofilm with severe crystallization will produce fatal pinholes, which seriously damages the insulation of the organic nanofilm. Therefore, its IV curve shows a direct conduction state, which reflects that the preparation method of Example 1 effectively improves the performance of the device.

[0070] Example 3

[0071] A method for preparing an organic memristor, the specific steps are as follows:

[0072] (1) Preparation of organic functional layer solution: Sodium copper chlorophyllin material was dissolved in ultrapure water solvent at a concentration of 17.5 mg / mL, and heated at 60° C. for 5 h to completely dissolve it, thereby obtaining an organic functional layer solution.

[0073] (2) Glass is selected as a substrate, and a layer of indium tin oxide with a thickness of 185 nm is generated on the glass to form ITO conductive glass. The ITO conductive glass is cleaned with an ITO cleaning agent (once) and ultrapure water (twice) for 30 minutes, then blown dry with ordinary nitrogen and placed in an oven at 120°C for 30 minutes for drying.

[0074] (3) The dried ITO conductive glass is treated with UV-ozone for 30 minutes.

[0075] (4) Place the substrate at the center of the spin coating table, use a pipette to draw 150-200 μL of the organic functional layer solution and evenly spread it on the substrate, adjust the rotation speed and time (first adjust the rotation speed to 500 rpm for 9 seconds, then adjust the rotation speed to 3000 rpm for 30 seconds) for spin coating, place the spin-coated sample in a vacuum oven at room temperature and gradually heat it to 60°C, anneal for 30 minutes, remove excess solvent, and obtain an organic functional layer nanofilm with a thickness of about 40 nm.

[0076] (5) Place the substrate with the nanofilm into the vacuum evaporation equipment and control the pressure in the vacuum chamber to 4×10 -4 Pa~5×10 -4 Pa, and began to evaporate the metal Ag anode at a rate of The thickness is 40-50 nm; the thickness of the film is measured using a step profiler.

[0077] (6) After the evaporation experiment is completed, the metal Ag anode is cooled to room temperature in the vacuum chamber, and all the preparation processes of the memristor are completed. Then the chamber is opened to take out the wafer and conduct relevant electrical performance tests on the device.

[0078] After the device is prepared, the electrical performance of the organic memristor device prepared in this embodiment is tested using Keithley 4200, and the prepared organic memristor is characterized. The specific test results are as follows:

[0079] Fig.10 This is an AFM morphology image of the organic nanofilm prepared in this example. It can be seen from the image that the roughness of the film is also very low (Ra=0.502 nm).

[0080] Fig.11This is the IV curve of the organic memristor prepared in this embodiment. It can be found from the figure that the device exhibits obvious RRAM performance, and its switching voltage is also less than 100mV, indicating that the device can be transformed from volatile to non-volatile by changing the concentration of sodium copper chlorophyllin solution.

[0081] Fig.12 , Fig.13 The distribution curves of SET voltage and RESET voltage of 64 different devices prepared in this embodiment are shown. It can be seen from the figure that the voltage distribution of the device is very uniform, and the voltage is less than 100mV. Although a film with lower roughness can be obtained by reducing the concentration of sodium copper chlorophyllin, the uniformity and yield of the device are also improved, but the read, write and erase tolerance, and maintenance stability of the device are significantly reduced compared with Example 1.

[0082] All the characterization results show that the organic memristor with ultra-low operating voltage prepared in Example 1 has excellent memristor performance, is low-priced, non-toxic and harmless to process, and can be prepared on a large scale.

[0083] Although the present invention has been illustrated and described with reference to certain preferred embodiments of the present invention, it should be understood by those skilled in the art that the above contents are further detailed descriptions of the present invention in conjunction with specific embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. Those skilled in the art may make various changes in form and details, including making several simple deductions or substitutions, without departing from the spirit and scope of the present invention.

Claims

1. A method for preparing an organic memristor with ultra-low operating voltage, characterized in that: The following steps are involved: Step 1) preparing an organic functional layer solution: dissolving the sodium copper chlorophyllin material in an ultrapure water solvent at a concentration of 20 mg / mL, and heating at 60° C. to completely dissolve it to obtain an organic functional layer solution; Step 2) a bottom electrode layer is formed on the substrate material, and the substrate is cleaned with an ITO cleaning agent and ultrapure water ultrasonic cleaning in sequence, the cleaned substrate is first blown dry with ordinary nitrogen, and then placed in an oven at 120° C. for 1 hour to remove the remaining moisture; Step 3) placing the cleaned substrate after the treatment in step 2) under ultraviolet ozone treatment for 30 minutes; Step 4) using a pipette to draw 150-200 μL of the organic functional layer solution prepared in step 1) and spin-coating it on the substrate treated in step 3) to form a film, placing the spin-coated sample in a vacuum oven at room temperature and gradually heating it to 60° C., annealing for 30 minutes, removing excess solvent, and obtaining an organic functional layer; Step 5) Vacuum evaporation of the top electrode on the organic functional layer prepared in step 4) with the vacuum degree controlled at 4×10 -4 Pa~5×10 -4 Pa; Step 6) After the vacuum evaporation is completed, the vacuum state is maintained and the top electrode is cooled to room temperature for 30 minutes to obtain the organic memristor with ultra-low operating voltage.

2. The method for preparing an organic memristor with ultra-low operating voltage according to claim 1, characterized in that: The heating time in step 1) is 5 hours.

3. The method for preparing an organic memristor with ultra-low operating voltage according to claim 1, characterized in that: Step 2) The ultrasonic cleaning process is: first cleaning with an ITO cleaning agent, then cleaning twice with ultrapure water, and the ultrasonic cleaning time is 30 minutes.

4. The method for preparing an organic memristor with ultra-low operating voltage according to claim 1, characterized in that: Step 4) The spin coating process is: first adjust the rotation speed to 500 rpm for 9 seconds, then adjust the rotation speed to 3000 rpm for 30 seconds, and spin coating in air with the air humidity controlled below 60%.

5. The method for preparing an organic memristor with ultra-low operating voltage according to claim 1, characterized in that: Step 5) The evaporation rate of the vacuum evaporation 6. An organic memristor with ultra-low operating voltage obtained by the preparation method according to any one of claims 1 to 5, characterized in that: The memristor is a vertical sandwich structure, which includes a substrate, a bottom electrode, an organic functional layer and a top electrode from bottom to top; wherein the organic functional layer is a nanofilm prepared by spin coating an organic functional layer solution on the bottom electrode, and the organic functional layer solution is formed by dissolving sodium copper chlorophyllin in ultrapure water, and the structural formula of the sodium copper chlorophyllin is shown in formula (I):

7. The organic memristor with ultra-low operating voltage according to claim 6, characterized in that: The material of the substrate is glass; the material of the bottom electrode is indium tin oxide; and the material of the top electrode is metal Ag.

8. The organic memristor with ultra-low operating voltage according to claim 6, characterized in that: The thickness of the bottom electrode is 185 nm; the thickness of the organic functional layer is 40-50 nm; and the thickness of the top electrode is 40-50 nm.