A rotary die forging preparation method for ultra-light and high-strength magnesium-lithium alloy
By adding trace amounts of Ca, Zr or Ce to the magnesium lithium alloy and performing multi-pass rotary die forging deformation at room temperature, the problems of reducing strength and opposite properties of magnesium lithium alloy are solved, and ultra-light and high-strength and high elongation are prepared. Magnesium lithium alloy has achieved the improvement of mechanical properties of magnesium lithium alloy.
Patent Information
- Application Number
- CN202210177887.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-25
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-02-25
Smart Images

Figure CN114535478B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal materials, and in particular relates to a rotary die forging preparation method of an ultra-light and high-strength magnesium-lithium alloy. Background Art
[0002] Magnesium-lithium alloys have become candidate materials for aerospace, military and other fields due to their ultra-low density, good formability and damping properties. When the lithium content in magnesium alloys is 5.3-10.7% (wt.%), the alloy matrix is composed of α-Mg (HCP) and β-Li (BCC) dual phases, and the slip system activated at room temperature increases, which can better coordinate plastic deformation. Magnesium-lithium alloys have high specific strength, specific stiffness, excellent seismic resistance and resistance to high-energy particle penetration. They have great development potential in aerospace, aviation, weapons industry, nuclear industry, automobiles, 3C industry, medical equipment and other fields; but with the increase of Li content, the alloy strength decreases, limiting its wide application in industry.
[0003] At present, the most widely used commercial deformable magnesium alloy systems are AZ, AM, ZK and Mg-RE systems. AZ and AM alloys are cheap, but their absolute strength and yield strength ratio are low, so their applications are limited; ZK alloys such as ZK60 have a yield strength of 240-250MPa after extrusion, a tensile strength of 325-340MPa, and an elongation of 10-12%, but generally have a strong deformation texture and low alloy tension and compression symmetry. For Mg-RE alloys, the addition of rare earth elements can stimulate non-basal slip, thereby weakening the deformation texture and improving the mechanical properties of the alloy. However, the addition of rare earth elements increases the density of the alloy, which is not conducive to the environmental protection concept of energy conservation and emission reduction.
[0004] At present, the main method to improve the strength of magnesium-lithium alloys is through large plastic deformation, such as equal channel angle extrusion, high pressure torsion and multi-directional forging. Compared with cast magnesium alloys, deformed magnesium alloys processed by plastic forming methods such as extrusion, forging and rolling have higher strength and better ductility, which can meet the needs of more diversified structural parts. However, due to the close-packed hexagonal structure of magnesium alloys, strong basal texture is easily formed during extrusion or rolling, resulting in poor formability and plasticity of magnesium alloys, and showing anisotropy of mechanical properties and asymmetry of tensile and compressive yield, which has become a bottleneck problem hindering the large-scale application of deformed magnesium alloys. Summary of the invention
[0005] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the main purpose of the present invention is to provide a method for preparing an ultra-light and high-strength magnesium-lithium alloy by rotary die forging, which uses a Mg-Li alloy with good coordinated deformation ability, and after extrusion, it improves the strength and plasticity of the alloy by rotary die forging with small strain at room temperature, so as to prepare a magnesium-lithium alloy with good coordinated strength and plasticity.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] A rotary die forging preparation method for an ultra-light and high-strength magnesium-lithium alloy comprises the following steps:
[0008] A) obtaining the following raw materials: pure magnesium ingot, pure aluminum ingot, magnesium-lithium master alloy, magnesium-zirconium master alloy, magnesium-calcium master alloy, or magnesium-cerium master alloy;
[0009] B) placing the pure magnesium ingot, pure aluminum ingot, magnesium-lithium master alloy, magnesium-zirconium master alloy, magnesium-calcium master alloy, or magnesium-cerium master alloy obtained in step A) in a vacuum melting furnace to obtain an alloy melt;
[0010] C) casting the alloy melt prepared in step B), cooling it, and performing mechanical processing to obtain an alloy ingot;
[0011] D) preheating and extruding the alloy ingot in step C) to obtain an extruded rod of a magnesium-lithium alloy;
[0012] E) The extruded rod obtained in step D) is subjected to multiple-pass small-strain rotary forging deformation treatment at room temperature to obtain a rod-shaped ultra-light and high-strength magnesium-lithium alloy.
[0013] Preferably, the chemical element composition of the raw material includes, by mass fraction: Li: 5.0-7.0%, Al: 2.5-3.5%, Zr: 0-0.4%, Ce: 0-0.4%, Ca: 0-0.4%, and the rest is magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%.
[0014] Preferably, the chemical element composition of the raw material includes, by mass fraction, 6.0% Li, 3.0% Al, 0.4% Zr, and the rest is magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%.
[0015] Preferably, the step C) is specifically as follows: the alloy melt obtained in step B) is heated to 700-720°C, the waste residue is removed and stirred evenly, and then allowed to stand for 5-10 minutes, and then poured into a stainless steel mold with a diameter of 90 mm and a length of 300 mm to form, and then naturally cooled in a vacuum chamber and taken out, and then turned into a diameter of Alloy ingots.
[0016] Preferably, the step D) is specifically as follows: placing the alloy ingot obtained in step C) in a heating furnace for preheating, and then placing the preheated alloy ingot in an extruder After extrusion molding by a die, the extruded rod of magnesium-lithium alloy is obtained by cooling to room temperature.
[0017] Preferably, the cooling condition is air cooling by a fan.
[0018] Preferably, the preheating temperature is 265-275°C, and the time is 0.5-1 hour; the extrusion molding conditions are: extrusion ratio is (20-30):1, extrusion speed is 1-2m / min, and extrusion temperature is 265-275°C.
[0019] Preferably, the preheating temperature is 270°C, and the preheating time is 1 hour; the extrusion molding conditions are: the extrusion ratio is 25:1, the extrusion speed is 1.5 m / min; and the extrusion temperature is 270°C.
[0020] Preferably, the step E) is specifically: subjecting the extruded rod obtained in step D) to 15-24 small strain rotary forging deformation treatments at room temperature, and each forging is performed with a radial compression amount of 0.04-0.48 mm, and finally obtaining a rod with a diameter of Rod-shaped ultra-light and high-strength magnesium-lithium alloy.
[0021] Compared with the prior art, the present invention has at least the following advantages:
[0022] The rotary die forging method for preparing an ultra-light and high-strength magnesium-lithium alloy provided in the present application is to add a trace amount of Ca, Zr, or Ce to the Mg-Li-Al alloy to form Al 2 Ca, or Al 3 Zr, or Al-Ce phase, which can pin the grain boundary during hot extrusion, inhibit the growth of recrystallized grains, and ultimately achieve the effect of grain refinement; at the same time, through multi-pass small strain rotary forging deformation treatment at room temperature, high-density twins and stacking faults are introduced into the α-Mg grains, which greatly improves the comprehensive mechanical properties of magnesium-lithium alloys, and prepares ultra-light and high-strength magnesium-lithium alloys with a yield strength of 248-349MPa, a tensile strength of 344-411MPa, an elongation of 8.1-25%, and a density of 1.543-1.602g / cm 3 . BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments or the description of the prior art will be briefly introduced below.
[0024] Figure 1 OM diagram of the magnesium-lithium alloy prepared in Example 1;
[0025] Figure 2 OM diagram of the magnesium-lithium alloy prepared in Example 2;
[0026] Figure 3 OM diagram of the magnesium-lithium alloy prepared in Example 3;
[0027] Figure 4 OM diagram of the magnesium-lithium alloy prepared in Example 4;
[0028] Figure 5 OM diagram of the magnesium-lithium alloy prepared in Example 5;
[0029] Figure 6 The SEM image of the magnesium-lithium alloy prepared in Example 1 is shown;
[0030] Figure 7 The SEM image of the magnesium-lithium alloy prepared in Example 2 is shown;
[0031] Figure 8 The SEM image of the magnesium-lithium alloy prepared in Example 3 is shown;
[0032] Fig. 9 The SEM image of the magnesium-lithium alloy prepared in Example 4 is shown;
[0033] Fig.10 The SEM image of the magnesium-lithium alloy prepared in Example 5 is shown;
[0034] Fig.11 The stress-strain diagram shows the ultra-light and high-strength magnesium-lithium alloy prepared in Example 1;
[0035] Fig.12 : represents the stress-strain diagram of the ultra-light and high-strength magnesium-lithium alloy prepared in Example 2;
[0036] Fig.13 : represents the stress-strain diagram of the ultra-light and high-strength magnesium-lithium alloy prepared in Example 3;
[0037] Fig.14 4 is a stress-strain diagram showing the ultralight and high-strength magnesium-lithium alloy prepared in Example 4;
[0038] Fig.15 The stress-strain diagram of the ultra-light and high-strength magnesium-lithium alloy prepared in Example 5 is shown. DETAILED DESCRIPTION
[0039] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.
[0040] When a certain amount, concentration or other value or parameter is expressed in the form of a range, a preferred range, or a preferred upper and lower numerical limit, it should be understood that it is equivalent to specifically revealing any range by combining any pair of upper range limits or preferred numerical values with any lower range limit or preferred numerical value, regardless of whether the range is specifically disclosed. Unless otherwise indicated, the numerical range values listed herein include the endpoints of the range, and all integers and fractions within the range.
[0041] Unless otherwise indicated, all percentages, parts, ratios, etc. herein are by weight.
[0042] The materials, methods, and examples herein are illustrative and are not to be construed as limiting unless specifically stated.
[0043] The pure magnesium ingot, pure aluminum ingot, magnesium-lithium master alloy, magnesium-zirconium master alloy, magnesium-calcium master alloy and magnesium-cerium master alloy used in the embodiments of the present invention are commercially available products.
[0044] The model of the stretching machine used in the embodiment of the present invention is UTM4104, the model of the metallographic microscope is OLYMPUS PMG3; and the model of the scanning electron microscope is JSM-7800F.
[0045] In the embodiment of the present invention, the purity of the magnesium ingot is ≥99.95%, and the purity of the aluminum ingot is ≥99.97%;
[0046] In the embodiment of the present invention, the magnesium-lithium master alloy, the magnesium-zirconium master alloy, the magnesium-calcium master alloy and the magnesium-cerium master alloy are collectively referred to as magnesium master alloys, and the lithium, zirconium, calcium and cerium of the magnesium master alloys account for 10-20% of the total mass of the magnesium master alloys respectively;
[0047] In the embodiment of the present invention, the vacuum furnace is evacuated to 2.5×10 -1 Pa, and then fill in argon as a protective gas until the vacuum furnace is completely melted in the atmosphere of protective gas argon.
[0048] Example 1
[0049] The ultra-light and high-strength magnesium-lithium alloy provided by the present invention has the following components in mass fraction:
[0050] Li: 5.0%, Al: 3.0%, Ca: 0.4%, and the rest are magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%.
[0051] This embodiment also discloses a rotary die forging preparation method of the ultra-light and high-strength magnesium-lithium alloy, comprising the following steps:
[0052] 1) Obtain the following raw materials: prepare pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, and magnesium-calcium master alloys;
[0053] 2) Under the protection of argon, pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, and magnesium-calcium master alloys are placed in a crucible according to the above mass fraction ratios and placed in a vacuum furnace for heating to 720° C. until all raw materials are completely melted to obtain an alloy melt;
[0054] 3) stirring the alloy melt obtained in step 2) at a temperature of 710° C. until all raw materials are uniformly mixed, removing scum from the surface of the alloy melt, standing for 5 minutes, and then pouring into a stainless steel mold with a diameter of 90 mm and a length of 300 mm to form, and then naturally cooling in a vacuum chamber and taking it out, and then turning it into an alloy ingot with a diameter of 80 mm;
[0055] 4) The alloy ingot obtained in step 3) is placed in a heating furnace for preheating at a temperature of 265° C. for 1 hour; then the preheated alloy ingot is extruded in an extruder with an extrusion ratio of 25:1, an extrusion speed of 1-2 m / min, and an extrusion temperature of 270° C. using a die with a diameter of 16 mm, and then air-cooled to room temperature to obtain an extruded rod of a magnesium-lithium alloy.
[0056] 5) The extruded rod obtained in step 4) is subjected to 15 passes of small strain rotary forging deformation treatment at room temperature, and the specific experimental operation is as follows: the first pass pressing amount is 0.36mm; the second pass pressing amount is 0.43mm; the third pass pressing amount is 0.31mm; the fourth pass pressing amount is 0.06mm; the fifth pass pressing amount is 0.19mm; the sixth pass pressing amount is 0.05mm; the seventh pass pressing amount is 0.09mm; the eighth pass pressing amount is 0.23mm; the ninth pass pressing amount is 0.37mm; the tenth pass pressing amount is 0.05mm; the eleventh pass pressing amount is 0.26mm; the twelfth pass pressing amount is 0.21mm; the thirteenth pass pressing amount is 0.04mm; the fourteenth pass pressing amount is 0.05mm; the fifteenth pass pressing amount is 0.2mm; and finally a rod-shaped ultra-light and high-strength magnesium-lithium alloy with a diameter of 12.9-13.1mm is obtained.
[0057] In this embodiment, the mechanical properties of the magnesium-lithium alloy prepared by the extrusion process in step D) and the magnesium-lithium alloy prepared by the rotary die forging method in step E) are tested. The results are as follows: the performance indicators of the extruded rod prepared by the extrusion process are: yield strength of 156MPa, tensile strength of 250MPa, elongation of 17.8%, density of 1.602g / cm 3The performance indicators of the magnesium-lithium alloy material obtained by the rotary die forging method are: yield strength of 285MPa, tensile strength of 377.7MPa, elongation of 10.8%, and density of 1.602g / cm 3 .
[0058] The OM diagram of the ultra-light and high-strength magnesium-lithium alloy obtained by the rotary die forging method in this embodiment is as follows: Figure 1 As shown in the SEM images Figure 6 The stress-strain curve is shown in Fig.11 shown.
[0059] Example 2
[0060] The ultra-light and high-strength magnesium-lithium alloy provided by the present invention has the following components in mass fraction:
[0061] Li: 5.0%, Al: 3.0%, Ce: 0.4%, and the rest are magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%.
[0062] This embodiment also discloses a rotary die forging preparation method of the ultra-light and high-strength magnesium-lithium alloy, comprising the following steps:
[0063] 1) Obtain the following raw materials: prepare pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, and magnesium-cerium master alloys;
[0064] 2) Under the protection of argon, pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, and magnesium-cerium master alloys are placed in a crucible according to the above mass fraction ratios and placed in a vacuum furnace for heating to 720° C. until all raw materials are completely melted to obtain an alloy melt;
[0065] 3) stirring the alloy melt obtained in step 2) at a temperature of 700° C. until all raw materials are uniformly mixed, removing scum on the surface of the alloy melt, standing for 5 minutes, and then pouring it into a stainless steel mold with a diameter of 90 mm and a length of 300 mm to form, and then naturally cooling it in a vacuum chamber and taking it out, and then turning it into an alloy ingot with a diameter of 80 mm;
[0066] 4) The alloy ingot obtained in step 3) is placed in a heating furnace for preheating at a temperature of 275° C. for 0.5 hours; then the preheated alloy ingot is extruded in an extruder with an extrusion ratio of 20:1, an extrusion speed of 1-2 m / min, and an extrusion temperature of 275° C., and a mold with a diameter of 16 mm is selected, and then air-cooled to room temperature to obtain an extruded rod of a magnesium-lithium alloy.
[0067] 5) The extruded rod obtained in step 4) is subjected to 22 passes of small strain rotary forging deformation treatment at room temperature, and the specific experimental operation is as follows: the first pass pressing amount is 0.48mm; the second pass pressing amount is 0.39mm; the third pass pressing amount is 0.23mm; the fourth pass pressing amount is 0.05mm; the fifth pass pressing amount is 0.32mm; the sixth pass pressing amount is 0.09mm; the seventh pass pressing amount is 0.29mm; the eighth pass pressing amount is 0.33mm; the ninth pass pressing amount is 0.09mm; the tenth pass pressing amount is 0.28mm; the eleventh pass pressing amount is 0.15m m; the pressing amount of the twelfth pass is 0.08mm; the pressing amount of the thirteenth pass is 0.1mm; the pressing amount of the fourteenth pass is 0.11mm; the pressing amount of the fifteenth pass is 0.04mm; the pressing amount of the sixteenth pass is 0.32mm; the pressing amount of the seventeenth pass is 0.19mm; the pressing amount of the eighteenth pass is 0.12mm; the pressing amount of the nineteenth pass is 0.12mm; the pressing amount of the twentieth pass is 0.04mm; the pressing amount of the twenty-first pass is 0.11mm; the pressing amount of the twenty-second pass is 0.3mm; and finally, a rod-shaped ultra-light and high-strength magnesium-lithium alloy with a diameter of 11.70-11.91mm is obtained;
[0068] In this embodiment, the mechanical properties of the magnesium-lithium alloy prepared by the extrusion process in step D) and the magnesium-lithium alloy prepared by the rotary die forging method in step E) are tested. The results are as follows: the performance indicators of the extruded rod prepared by the extrusion process are: yield strength of 143.7MPa, tensile strength of 252.2MPa, elongation of 21.1%, density of 1.601g / cm 3 The performance indicators of the magnesium alloy material prepared by rotary die forging are: yield strength of 260.8MPa, tensile strength of 385.4MPa, elongation of 8.1%, density of 1.601g / cm 3 ;
[0069] The OM diagram of the ultra-light and high-strength magnesium-lithium alloy obtained by the rotary die forging method in this embodiment is as follows: Figure 2 As shown in the SEM images Figure 7 The stress-strain curve is shown in Fig.12 shown.
[0070] Example 3
[0071] The ultra-light and high-strength magnesium-lithium alloy provided by the present invention has the following components in mass fraction:
[0072] Li: 6.0%, Al: 3.0%, Ca: 0.4%, and the rest are magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%.
[0073] This embodiment also discloses a rotary die forging preparation method of the ultra-light and high-strength magnesium-lithium alloy, comprising the following steps:
[0074] 1) Obtain the following raw materials: prepare pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, and magnesium-calcium master alloys;
[0075] 2) Under the protection of argon, pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, and magnesium-calcium master alloys are placed in a crucible according to the above mass fraction ratios and placed in a vacuum furnace for heating to 720° C. until all raw materials are completely melted to obtain an alloy melt;
[0076] 3) stirring the alloy melt obtained in step 2) at a temperature of 710° C. until all raw materials are uniformly mixed, removing scum from the surface of the alloy melt, standing for 8 minutes, and then pouring into a stainless steel mold with a diameter of 90 mm and a length of 300 mm to form, and then naturally cooling in a vacuum chamber and taking it out, and then turning it into an alloy ingot with a diameter of 80 mm;
[0077] 4) The alloy ingot obtained in step 3) is placed in a heating furnace for preheating at a temperature of 265° C. for 0.8 hours; the preheated alloy ingot is then extruded in an extruder with an extrusion ratio of 25:1, an extrusion speed of 1-2 m / min, and an extrusion temperature of 265° C., and a mold with a diameter of 16 mm is selected, and then air-cooled to room temperature to obtain an extruded rod of a magnesium-lithium alloy.
[0078] 5) The extruded rod obtained in step 4) is subjected to 17 passes of small strain rotary forging deformation treatment at room temperature, and the specific experimental operation is as follows: the first pass has a pressing amount of 0.43 mm; the second pass has a pressing amount of 0.36 mm; the third pass has a pressing amount of 0.4 mm; the fourth pass has a pressing amount of 0.13 mm; the fifth pass has a pressing amount of 0.23 mm; the sixth pass has a pressing amount of 0.21 mm; the seventh pass has a pressing amount of 0.46 mm; the eighth pass has a pressing amount of 0.26 mm; the ninth pass has a pressing amount of 0. The pressing amount is 0.22mm; the pressing amount of the tenth pass is 0.04mm; the pressing amount of the eleventh pass is 0.09mm; the pressing amount of the twelfth pass is 0.07mm; the pressing amount of the thirteenth pass is 0.13mm; the pressing amount of the fourteenth pass is 0.24mm; the pressing amount of the fifteenth pass is 0.21mm; the pressing amount of the sixteenth pass is 0.09mm; the pressing amount of the seventeenth pass is 0.04mm; and finally, a rod-shaped ultra-light and high-strength magnesium-lithium alloy with a diameter of 12.32-12.48mm is obtained;
[0079] In this embodiment, the mechanical properties of the magnesium-lithium alloy prepared by the extrusion process in step D) and the magnesium-lithium alloy prepared by the rotary die forging method in step E) are tested. The results are as follows: the performance indicators of the extruded rod prepared by the extrusion process are: yield strength of 144.5MPa, tensile strength of 250.2MPa, elongation of 22.2%, density of 1.599g / cm 3The performance indicators of the magnesium alloy material prepared by rotary die forging are: yield strength of 248MPa, tensile strength of 353MPa, elongation of 12.3%, density of 1.599g / cm 3 .
[0080] The OM diagram of the ultra-light and high-strength magnesium-lithium alloy obtained by the rotary die forging method in this embodiment is as follows: Figure 3 As shown in the SEM images Figure 8 The stress-strain curve is shown in Fig.13 shown.
[0081] Example 4
[0082] The ultra-light and high-strength magnesium-lithium alloy provided by the present invention has the following components in mass fraction:
[0083] Li: 6.0%, Al: 3.0%, Zr: 0.4%, and the rest are magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%.
[0084] This embodiment also discloses a rotary die forging preparation method of the ultra-light and high-strength magnesium-lithium alloy, comprising the following steps:
[0085] 1) Obtain the following raw materials: prepare pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, and magnesium-zirconium master alloys;
[0086] 2) Under the protection of argon, pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, and magnesium-zirconium master alloys are placed in a crucible according to the above mass fraction ratios and placed in a vacuum furnace for heating to 720° C. until all raw materials are completely melted to obtain an alloy melt;
[0087] 3) stirring the alloy melt obtained in step 2) at a temperature of 710° C. until all raw materials are uniformly mixed, removing scum from the surface of the alloy melt, standing for 10 minutes, and then pouring into a stainless steel mold with a diameter of 90 mm and a length of 300 mm to form, and then naturally cooling in a vacuum chamber and taking it out, and then turning it into an alloy ingot with a diameter of 80 mm;
[0088] 4) The alloy ingot obtained in step 3) is placed in a heating furnace for preheating at a temperature of 270° C. for 0.5 hours; the preheated alloy ingot is then extruded in an extruder with an extrusion ratio of 25:1, an extrusion speed of 1-2 m / min, and an extrusion temperature of 270° C., and a mold with a diameter of 16 mm is selected, and then air-cooled to room temperature to obtain an extruded rod of a magnesium-lithium alloy.
[0089] 5) The extruded rod obtained in step 4) is subjected to 20 passes of small strain rotary forging deformation treatment at room temperature, and the specific experimental operation is as follows: the first pass pressing amount is 0.43mm; the second pass pressing amount is 0.33mm; the third pass pressing amount is 0.37mm; the fourth pass pressing amount is 0.23mm; the fifth pass pressing amount is 0.12mm; the sixth pass pressing amount is 0.29mm; the seventh pass pressing amount is 0.38mm; the eighth pass pressing amount is 0.04mm; the ninth pass pressing amount is 0.26mm; the tenth pass pressing amount is 0.23 mm; the pressing amount of the eleventh pass is 0.11mm; the pressing amount of the twelfth pass is 0.05mm; the pressing amount of the thirteenth pass is 0.13mm; the pressing amount of the fourteenth pass is 0.26mm; the pressing amount of the fifteenth pass is 0.23mm; the pressing amount of the sixteenth pass is 0.04mm; the pressing amount of the seventeenth pass is 0.13mm; the pressing amount of the eighteenth pass is 0.04mm; the pressing amount of the nineteenth pass is 0.17mm; the pressing amount of the twentieth pass is 0.22mm; and finally, a rod-shaped ultra-light and high-strength magnesium-lithium alloy with a diameter of 11.9-12.0mm is obtained;
[0090] In this embodiment, the mechanical properties of the magnesium-lithium alloy prepared by the extrusion process in step D) and the magnesium-lithium alloy prepared by the rotary die forging method in step E) are tested. The results are as follows: the performance indicators of the extruded rod prepared by the extrusion process are: yield strength of 144.5MPa, tensile strength of 250.2MPa, elongation of 22.2%, density of 1.593g / cm 3 The performance indicators of the magnesium alloy material prepared by rotary die forging are: yield strength of 349MPa, tensile strength of 411MPa, elongation of 15%, density of 1.593g / cm 3 ;
[0091] The OM diagram of the ultra-light and high-strength magnesium-lithium alloy obtained by the rotary die forging method in this embodiment is as follows: Figure 4 As shown in the SEM images Fig. 9 The stress-strain curve is shown in Fig.14 shown.
[0092] Example 5
[0093] The ultra-light and high-strength magnesium-lithium alloy provided by the present invention has the following components in mass fraction:
[0094] Li: 7.0%, Al: 3.0%, Ca: 0.4%, and the rest are magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%.
[0095] This embodiment also discloses a rotary die forging preparation method of the ultra-light and high-strength magnesium-lithium alloy, comprising the following steps:
[0096] 1) Obtain the following raw materials: prepare pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, and magnesium-calcium master alloys;
[0097] 2) Under the protection of argon, pure magnesium ingots, pure aluminum ingots, magnesium-lithium master alloys, and magnesium-calcium master alloys are placed in a crucible according to the above mass fraction ratios and placed in a vacuum furnace for heating to 720° C. until all raw materials are completely melted to obtain an alloy melt;
[0098] 3) stirring the alloy melt obtained in step 2) at a temperature of 710° C. until all raw materials are uniformly mixed, removing scum from the surface of the alloy melt, standing for 5 minutes, and then pouring into a stainless steel mold with a diameter of 90 mm and a length of 300 mm to form, and then naturally cooling in a vacuum chamber and taking it out, and then turning it into an alloy ingot with a diameter of 80 mm;
[0099] 4) The alloy ingot obtained in step 3) is placed in a heating furnace for preheating at a temperature of 270° C. for 1 hour; then the preheated alloy ingot is extruded in an extruder with an extrusion ratio of 25:1, an extrusion speed of 1-2 m / min, and an extrusion temperature of 270° C., and a mold with a diameter of 16 mm is selected for extrusion molding, and then air-cooled to room temperature to obtain an extruded rod of a magnesium-lithium alloy.
[0100] 5) The extruded rod obtained in step 4) is subjected to 24 passes of small strain rotary forging deformation treatment at room temperature, and the specific experimental operation is as follows: the first pass pressing amount is 0.48mm; the second pass pressing amount is 0.29mm; the third pass pressing amount is 0.39mm; the fourth pass pressing amount is 0.23mm; the fifth pass pressing amount is 0.07mm; the sixth pass pressing amount is 0.14mm; the seventh pass pressing amount is 0.27mm; the eighth pass pressing amount is 0.35mm; the ninth pass pressing amount is 0.06mm; the tenth pass pressing amount is 0.25mm; the eleventh pass pressing amount is 0.24mm; the twelfth pass pressing amount is 0.05mm; the thirteenth pass pressing amount is 0.08mm; the fourteenth pass pressing amount is 0.08mm; the fifteenth pass pressing amount is 0.1mm; the sixteenth pass pressing amount is 0.08mm; the seventeenth pass pressing amount is The pressing amount of the 18th pass is 0.13mm; the pressing amount of the 19th pass is 0.1mm; the pressing amount of the 20th pass is 0.07mm; the pressing amount of the 21st pass is 0.07mm; the pressing amount of the 22nd pass is 0.17mm; the pressing amount of the 23rd pass is 0.27mm; the pressing amount of the 24th pass is 0.19mm, and finally a rod-shaped ultra-light and high-strength magnesium-lithium alloy with a diameter of 11.58-11.75mm is obtained; in this embodiment, the mechanical properties of the magnesium-lithium alloy prepared by the extrusion process in step D) and the magnesium-lithium alloy prepared by the rotary die forging preparation method in step E) are tested, and the results are as follows: the performance indicators of the extruded rod prepared by the extrusion process are: yield strength is 165.3MPa, tensile strength is 222.1MPa, elongation is 22.6%, and density is 1.543g / cm 3 The performance indicators of the magnesium alloy material prepared by rotary die forging are: yield strength of 290MPa, tensile strength of 344MPa, elongation of 25%, density of 1.543g / cm 3 .
[0101] The OM diagram of the ultra-light and high-strength magnesium-lithium alloy obtained by the rotary die forging method in this embodiment is as follows: Figure 5 As shown in the SEM images Fig.10 The stress-strain curve is shown in Fig.15 shown.
[0102] Comparative Example 1
[0103] This comparative example relates to an ultra-light and high-strength magnesium-lithium alloy. The components of the magnesium-lithium alloy are the same as those in Example 1, and the preparation method of the magnesium-lithium alloy is basically the same as that in Example 1, except that the number of die forging passes is 10.
[0104] In this embodiment, the mechanical properties of the magnesium-lithium alloy prepared by the rotary die forging process in step E) are tested, and the results are as follows: the yield strength is 230 MPa, the tensile strength is 308.8 MPa, the elongation is 13.9%, and the density is 1.602 g / cm 3 .
[0105] Compared with Example 1, the performance of Comparative Example 1 is much lower. This is considered to be due to insufficient rotary die forging passes, and the number of dislocations, twins and stacking faults introduced into the alloy is relatively low, resulting in low mechanical properties of the alloy. This further indicates that the magnesium alloy matrix requires a sufficient number of substructures to enhance the alloy performance.
[0106] Comparative Example 2
[0107] This comparative example relates to an ultra-light and high-strength magnesium-lithium alloy. The components of the magnesium-lithium alloy are the same as those in Example 2, and the preparation method of the magnesium-lithium alloy is basically the same as that in Example 2, except that the die forging reduction is 0.50-0.54 mm.
[0108] In this embodiment, the mechanical properties of the magnesium-lithium alloy material prepared by the rotary die forging process in step E) are tested, and the results are as follows: the yield strength is 245.3 MPa, the tensile strength is 330.3 MPa, the elongation is 13%, and the density is 1.601 g / cm 3 ;
[0109] The performance of Comparative Example 2 is lower than that of Example 2. This is because the reduction in a single pass of rotary die forging is too large, which introduces a large number of cracks inside the alloy, resulting in lower mechanical properties of the alloy. This further indicates that the magnesium alloy matrix requires an appropriate single-pass reduction to enhance the alloy properties.
[0110] Comparative Example 3
[0111] This comparative example relates to an ultra-light and high-strength magnesium-lithium alloy. The components of the magnesium-lithium alloy are the same as those in Example 3, and the preparation method of the magnesium-lithium alloy is basically the same as that in Example 3, except that the first pass of die forging has a reduction of 0.54 mm, followed by rotary forging with a reduction of 0.02-0.1 mm.
[0112] In this embodiment, the mechanical properties of the magnesium-lithium alloy material prepared by the rotary die forging process in step E) are tested, and the results are as follows: the yield strength is 246.9 MPa, the tensile strength is 326.5 MPa, the elongation is 17.3%, and the density is 1.599 g / cm 3 ;
[0113] Compared with Example 3, Comparative Example 3 has lower strength but higher plasticity. This is because the large reduction in the first pass of rotary forging introduces a large number of twins, dislocations and stacking faults into the alloy. Subsequently, rotary forging is performed with a reduction of 0.02-0.1 mm, and the density of the substructure inside the alloy gradually becomes saturated, resulting in lower strength. However, these substructures can coordinate plastic deformation, which is the main reason for the higher plasticity.
[0114] Comparative Example 4
[0115] This comparative example relates to an ultra-light and high-strength magnesium-lithium alloy. The components of the magnesium-lithium alloy are the same as those in Example 4, and the preparation method of the magnesium-lithium alloy is basically the same as that in Example 4, except that the die forging reduction is 0.01-0.04 mm.
[0116] In this embodiment, the mechanical properties of the magnesium-lithium alloy material prepared by the rotary die forging process in step E) are tested, and the results are: yield strength is 340MPa, tensile strength is 401MPa, elongation is 14%, and density is 1.593g / cm 3 ;
[0117] The mechanical properties of Comparative Example 4 are similar to those of Example 4. Considering the smaller multi-pass pressing amount, high-density twins, dislocations and stacking faults are introduced into the alloy, which prevents the appearance of more cracks in the alloy and greatly improves the mechanical properties of the alloy. This shows that a smaller single-pass pressing amount is beneficial for the preparation of high-strength magnesium-lithium alloys.
[0118] Comparative Example 5
[0119] This comparative example relates to an ultra-light and high-strength magnesium-lithium alloy. The components of the magnesium-lithium alloy are the same as those in Example 5, and the preparation method of the magnesium-lithium alloy is basically the same as that in Example 5, except that the reduction amount in the 10th pass of the die forging pass is 0.54 mm, and the rotary forging is performed with a reduction amount of 0.01-0.04 mm before and after.
[0120] In this embodiment, the mechanical properties of the magnesium-lithium alloy material prepared by the rotary die forging process in step E) are tested, and the results are as follows: the yield strength is 261.7 MPa, the tensile strength is 349.8 MPa, the elongation is 22.1%, and the density is 1.543 g / cm 3 ;
[0121] Compared with Example 5, Comparative Example 5 has lower strength but higher plasticity. The reason for this is similar to that of Comparative Example 3, indicating that a larger reduction in a single pass is beneficial for preparing a magnesium-lithium alloy with higher plasticity.
[0122] The microstructure and mechanical properties of the ultra-light and high-strength magnesium-lithium alloys prepared in Examples 1-5 and / or Comparative Examples 1-5 of the present invention were tested and analyzed, as follows:
[0123] 1) Microstructure characterization
[0124] The OM and SEM images of the ultra-light and high-strength magnesium-lithium alloys prepared by the rotary die forging process in Examples 1-5 are shown in FIG. Figure 1-5 and Figure 6-10 It can be seen that after the extruded magnesium-lithium alloy material is deformed by rotary forging, there are high-density twins inside the α-Mg grains. These twins can hinder dislocation movement and maintain work hardening, which is the main reason for the high strength of magnesium-lithium alloy after rotary forging.
[0125] 2) Mechanical properties test
[0126] According to GB228-2000 standard, the ultra-light and high-strength magnesium-lithium alloy samples after rotary die forging in Examples 1-5 of the present invention and Comparative Examples 1-5 were processed into standard tensile specimens. The tensile specimens were in sheet shape with a cross-sectional area of 2 mm*3 mm and a gauge length of 8 mm. The tensile direction of the specimens was the same as the rotary forging feed direction. The specific mechanical properties are shown in Table 1, where Figure 11-15 They are stress-strain diagrams of the ultra-light and high-strength magnesium-lithium alloys in Examples 1-5 at room temperature.
[0127] Table 1 Mechanical properties of ultra-light and high-strength magnesium-lithium alloys in Examples 1-5 and Comparative Examples 1-5 at room temperature
[0128]
[0129] It can be seen from the above table that the ultra-light and high-strength magnesium-lithium alloy provided by the present invention has high strength at room temperature; this is because after the alloy undergoes multiple passes of small-strain rotary forging with a specific downward pressure at room temperature, high-density twins and stacking faults are introduced into the interior of the α-Mg grains. These twins and stacking faults can hinder dislocation movement and maintain work hardening, greatly improving the comprehensive mechanical properties of the magnesium-lithium alloy.
[0130] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.
Claims
1. A rotary die forging method for preparing an ultra-light and high-strength magnesium-lithium alloy, characterized in that: The following steps are involved: A) obtaining the following raw materials: pure magnesium ingot, pure aluminum ingot, magnesium-lithium master alloy, magnesium-calcium master alloy; B) placing the pure magnesium ingot, pure aluminum ingot, magnesium-lithium master alloy, and magnesium-calcium master alloy obtained in step A) in a vacuum melting furnace to obtain an alloy melt; C) casting the alloy melt prepared in step B), cooling it, and performing mechanical processing to obtain an alloy ingot; D) preheating and extruding the alloy ingot in step C) to obtain an extruded rod of a magnesium-lithium alloy; E) The extruded rod obtained in step D) is subjected to 15-24 passes of small strain rotary forging deformation at room temperature, and each forging is performed with a radial compression amount of 0.04-0.48 mm, and finally a diameter of The rod-shaped ultra-light and high-strength magnesium-lithium alloy; The chemical element composition of the raw materials includes, by mass fraction, 5.0-7.0% Li, 2.5-3.5% Al, 0.4% Ca, and the rest is magnesium and unavoidable impurities, and the total content of the impurities is less than or equal to 0.3%; the yield strength of the ultra-light and high-strength magnesium-lithium alloy is 248-349MPa, the tensile strength is 344-411MPa; the elongation is 8.1-25%; the density is 1.543-1.602g / cm 3 .
2. The rotary die forging preparation method of the ultra-light and high-strength magnesium-lithium alloy according to claim 1, characterized in that: The step C) is specifically as follows: the alloy melt obtained in step B) is heated to 700-720°C, the waste residue is removed, the mixture is stirred evenly, and then allowed to stand for 5-10 minutes, and then poured into a stainless steel mold with a diameter of 90 mm and a length of 300 mm to form a mold, and then naturally cooled in a vacuum chamber and taken out, and then turned into a stainless steel mold with a diameter of Alloy ingots.
3. The rotary die forging preparation method of ultra-light and high-strength magnesium-lithium alloy according to claim 2, characterized in that: The step D) is specifically as follows: placing the alloy ingot obtained in the step C) in a heating furnace for preheating, and then placing the preheated alloy ingot in an extruder. After extrusion molding by a die, the extruded rod of magnesium-lithium alloy is obtained by cooling to room temperature.
4. The rotary die forging preparation method of ultra-light and high-strength magnesium-lithium alloy according to claim 3, characterized in that: The cooling condition is air cooling by a fan.
5. The rotary die forging preparation method of ultra-light and high-strength magnesium-lithium alloy according to claim 4, characterized in that: The preheating temperature is 265-275°C, and the time is 0.5-1 hour; the extrusion molding conditions are: extrusion ratio is (20-30):1, extrusion speed is 1-2m / min, and extrusion temperature is 265-275°C.
6. The rotary die forging preparation method of the ultra-light and high-strength magnesium-lithium alloy according to claim 5, characterized in that: The preheating temperature is 270°C, and the preheating time is 1 hour; the extrusion molding conditions are: the extrusion ratio is 25:1, the extrusion speed is 1.5 m / min; and the extrusion temperature is 270°C.
Citation Information
Cited By
Lossless pure platinum bar preparation process using reducing die forging and lossless pure platinum bar
CN121103883A
Preparation process of lossless pure platinum bar by using reducing-diameter die forging and lossless pure platinum bar
CN121103883B