A method for concentrating, separating and determining trace mercury in seawater
Concentration separation and determination of mercury in seawater by using bismethylene thiocarbohydrazide-modified silica-coated magnetic nanoparticles, combined with magnetic solid phase microextraction and electrothermal atom absorption spectrometer, the trace amount in seawater was solved The difficulty of mercury detection and pollution problems achieve efficient and simple mercury analysis.
Patent Information
- Application Number
- CN202210138491.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-02-15
AI Technical Summary
The detection of trace amounts of mercury in seawater is difficult, and the prior art is prone to contamination during sample collection, processing and analysis, resulting in increased detection difficulty.
The silica-modified silica-coated magnetic nanoparticles were used as adsorbent, and the concentration separation and determination of mercury were performed by combining magnetic solid-phase microextraction and electrothermal atom absorption spectrometer.
Efficient concentration separation and determination of mercury in seawater is achieved, simplified operation, reduced sample and reagent consumption, improved analytical characteristics, and reduced laboratory residue generation.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of mercury measurement, and in particular relates to a method for concentrating, separating and measuring trace mercury in seawater. Background Art
[0002] Mercury is a global environmental pollutant. The ocean is the source and sink of atmospheric mercury. In the marine environment, mercury can be converted into more toxic methylmercury through biological methylation. The concentration of methylmercury in carnivorous fish can reach 10,000 to 100,000 times the concentration of mercury in seawater. Mercury has become one of the most toxic elements to marine life. Mercury in seawater is at trace and ultra-trace levels, and is seriously contaminated during sample collection, processing and analysis, which increases the difficulty of mercury detection. Summary of the invention
[0003] The purpose of the present invention is to overcome the above-mentioned shortcomings and provide a method for concentrating, separating and determining trace mercury in seawater, which can determine the content of mercury in seawater.
[0004] In order to achieve the above object, the present invention comprises the following steps:
[0005] S1, preparation of di-methylenethiocarbohydrazide-modified silica-coated magnetic nanoparticles;
[0006] S2, using di-methylenethiocarbohydrazide-modified silica-coated magnetic nanoparticles as adsorbent materials for concentrating and separating trace mercury in seawater samples;
[0007] S3, the concentration of mercury in the adsorbent was determined by coupling magnetic solid phase microextraction with electrothermal atomic absorption spectrometry.
[0008] The specific method of S1 is as follows:
[0009] S11, preparing silica-coated magnetic nanoparticles by coprecipitation method;
[0010] S12, using 50 mL of 1% aminopropyltriethoxysilane and 95% ethanol by volume, dilute the obtained silica-coated magnetic nanoparticles to 150 mL, and adjust the pH value of the solution to 4.5 with acetic acid.
[0011] S13, stirring and heating at 60 °C for 2 h under nitrogen atmosphere to obtain nanospheres;
[0012] S14, washing the nanospheres and drying them into powder to obtain aminopropyl magnetic nanoparticles;
[0013] S15, mixing the obtained aminopropyl magnetic nanoparticles with 25 mL of a mixture of 3% diglutaraldehyde and deionized water, adding 2-4 mL of acetic acid, and refluxing the reaction mixture to obtain solid glutaraldehyde aminopropyl magnetic nanoparticles;
[0014] S16, decanting the solid glutaraldehyde aminopropyl magnetic nanoparticles under the action of a magnet, washing them, mixing them with 25 mL of 1.5% thiocarbohydrazide, adding 2-4 mL of acetic acid, boiling and refluxing to obtain thiocarbohydrazide glutaraldehyde aminopropyl magnetic nanoparticles, decanting them, and washing them;
[0015] S17, suspending the obtained thiocarbohydrazide glutaraldehyde aminopropyl magnetic nanoparticles in 45 mL of ethanol with a mass volume ratio of 2% of di-2-pyridone, and refluxing to obtain dimethocarbohydrazide modified silica-coated magnetic nanoparticles, washing and drying to obtain dimethocarbohydrazide modified silica-coated magnetic nanoparticles.
[0016] In S14, the nanospheres were washed three times with deionized water and then washed twice with methanol.
[0017] In S14, the drying is performed under vacuum at room temperature.
[0018] In S15, reflux for 4 hours;
[0019] In S16, boiling and reflux for 24 hours;
[0020] In S17, reflux is performed for 24 hours.
[0021] In S17, the magnetic nanoparticles coated with silica modified with dimethocarbonyl hydrazide are poured out by a magnet and then washed.
[0022] In S3, when determining the concentration of mercury in the adsorbent, the sample flow rate is 4.0 mL / min, the eluent flow rate is 0.6 mL / min, and the reducing agent flow rate is 1.2 mL / min.
[0023] In S3, after the concentration of mercury in the adsorbent is determined, the liquid is sent to a liquid separation device, which uses a membrane with a pore size of 0.5 μm and a nitrogen flow rate of 100 mL / min.
[0024] Compared with the prior art, the prepared di-methylenethiocarbohydrazide-modified silica-coated magnetic nanoparticles have magnetism, and can easily achieve phase separation of magnetic nanoparticles by applying an external magnetic field. The method is simple to operate, has a high sample throughput, improved analytical characteristics, and reduced consumption of samples and reagents. The method is fast, easy to use, automatic and selective, and has good analytical characteristics. The method is a relatively cheap method, requires a small amount of sample and reagent, and reduces the generation of laboratory residues. DETAILED DESCRIPTION
[0025] The present invention will be further described below in conjunction with the embodiments.
[0026] The present invention comprises the following steps:
[0027] S1, preparation of di-methylenethiocarbohydrazide-modified silica-coated magnetic nanoparticles;
[0028] S11, preparing silica-coated magnetic nanoparticles by coprecipitation method;
[0029] S12, using 50 mL of 1% aminopropyltriethoxysilane and 95% ethanol by volume, dilute the obtained silica-coated magnetic nanoparticles to 150 mL, and adjust the pH value of the solution to 4.5 with acetic acid.
[0030] S13, stirring and heating at 60 °C for 2 h under nitrogen atmosphere to obtain nanospheres;
[0031] S14, washing the nanospheres with deionized water for three times and then with methanol for two times, and drying them into powder under vacuum at room temperature to obtain aminopropyl magnetic nanoparticles;
[0032] S15, mixing the obtained aminopropyl magnetic nanoparticles with 25 mL of a mixture of 3% diglutaraldehyde and deionized water, adding 2-4 mL of acetic acid, and refluxing the reaction mixture for 4 hours to obtain solid glutaraldehyde aminopropyl magnetic nanoparticles;
[0033] S16, decanting the solid glutaraldehyde aminopropyl magnetic nanoparticles under the action of a magnet, washing them, mixing them with 25 mL of 1.5% thiocarbohydrazide, adding 2-4 mL of acetic acid, boiling and refluxing for 24 hours to obtain thiocarbohydrazide glutaraldehyde aminopropyl magnetic nanoparticles, decanting them and washing them;
[0034] S17, suspending the obtained thiocarbohydrazide glutaraldehyde aminopropyl magnetic nanoparticles in 45 mL of ethanol with a mass volume ratio of 2% of di-2-pyridone, and refluxing for 24 hours to obtain dimethocarbonylthiohydrazide-modified silica-coated magnetic nanoparticles, pouring out the dimethocarbonylthiohydrazide-modified silica-coated magnetic nanoparticles through a magnet, washing and drying to obtain dimethocarbonylthiohydrazide-modified silica-coated magnetic nanoparticles.
[0035] S2, using di-methylenethiocarbohydrazide-modified silica-coated magnetic nanoparticles as adsorbent materials for concentrating and separating trace mercury in seawater samples;
[0036] S3, the concentration of mercury in the adsorbent was determined by coupling magnetic solid phase microextraction with electrothermal atomic absorption spectrometer. When determining the concentration of mercury in the adsorbent, the sample flow rate was 4.0 mL / min, the eluent flow rate was 0.6 mL / min, and the reductant flow rate was 1.2 mL / min. The capture time of mercury vapor on the coated graphite tube was at least 90 seconds, the optimal atomization temperature was 1200°C, the adsorption temperature was 20°C, and the holding time was 3 seconds.
[0037] S4, after determining the concentration of mercury in the adsorbent, the liquid is sent to a liquid separation device, which uses a membrane with a pore size of 0.5 μm and a nitrogen flow rate of 100 mL / min. The loading time is set to 120 s to ensure reasonable sensitivity.
[0038] Embodiment 1:
[0039] S1, 2 g of silica-coated magnetic nanoparticles were prepared by coprecipitation method;
[0040] S2, using 50 mL of 1% aminopropyltriethoxysilane and 95% ethanol by volume, dilute 2 g of silica-coated magnetic nanoparticles to 150 mL, and adjust the pH value of the solution to 4.5 with acetic acid.
[0041] S3, stirring and heating at 60 °C for 2 h under nitrogen atmosphere to obtain nanospheres;
[0042] S4, washing the nanospheres with deionized water for three times and then with methanol for two times, and drying them into powder under vacuum at room temperature to obtain aminopropyl magnetic nanoparticles;
[0043] S5, mixing the obtained aminopropyl magnetic nanoparticles with 25 mL of a mixture of 3% diglutaraldehyde and deionized water, adding 2-4 mL of acetic acid, and refluxing the reaction mixture for 4 hours to obtain solid glutaraldehyde aminopropyl magnetic nanoparticles;
[0044] S6, decanting the solid glutaraldehyde aminopropyl magnetic nanoparticles under the action of a magnet, washing them, mixing them with 25 mL of 1.5% thiocarbohydrazide, adding 2-4 mL of acetic acid, boiling and refluxing for 24 hours to obtain thiocarbohydrazide glutaraldehyde aminopropyl magnetic nanoparticles, decanting them and washing them;
[0045] S7, suspending the obtained thiocarbohydrazide glutaraldehyde aminopropyl magnetic nanoparticles in 45 mL of ethanol with a mass volume ratio of 2% of di-2-pyridone, and refluxing for 24 hours to obtain dimethocarbonylthiohydrazide-modified silica-coated magnetic nanoparticles, pouring out the dimethocarbonylthiohydrazide-modified silica-coated magnetic nanoparticles through a magnet, washing and drying to obtain dimethocarbonylthiohydrazide-modified silica-coated magnetic nanoparticles.
[0046] S8, using di-methylenethiocarbohydrazide-modified silica-coated magnetic nanoparticles as adsorbent materials for concentrating and separating trace mercury in seawater samples;
[0047] S9, the concentration of mercury in the adsorbent was determined by coupling magnetic solid phase microextraction with electrothermal atomic absorption spectrometer. When determining the concentration of mercury in the adsorbent, the sample flow rate was 4.0 mL / min, the eluent flow rate was 0.6 mL / min, and the reductant flow rate was 1.2 mL / min. The capture time of mercury vapor on the coated graphite tube was 100 seconds, the optimal atomization temperature was 1200°C, the adsorption temperature was 20°C, and the holding time was 3 seconds.
[0048] S10, after determining the concentration of mercury in the adsorbent, the liquid is sent to a liquid separation device, which uses a membrane with a pore size of 0.5 μm and a nitrogen flow rate of 120 mL / min. The loading time is set to 130 s to ensure reasonable sensitivity.
[0049] Embodiment 2:
[0050] S1, 3 g of silica-coated magnetic nanoparticles were prepared by coprecipitation method;
[0051] S2, using 60 mL of 1% aminopropyltriethoxysilane and 95% ethanol by volume, dilute 2 g of silica-coated magnetic nanoparticles to 180 mL, and adjust the pH value of the solution to 4.5 with acetic acid.
[0052] S3, stirring and heating at 60 °C for 2 h under nitrogen atmosphere to obtain nanospheres;
[0053] S4, washing the nanospheres with deionized water for three times and then with methanol for two times, and drying them into powder under vacuum at room temperature to obtain aminopropyl magnetic nanoparticles;
[0054] S5, mixing the obtained aminopropyl magnetic nanoparticles with 35 mL of a mixture of 3% diglutaraldehyde and deionized water, adding 3-5 mL of acetic acid, and refluxing the reaction mixture for 4 hours to obtain solid glutaraldehyde aminopropyl magnetic nanoparticles;
[0055] S6, decanting the solid glutaraldehyde aminopropyl magnetic nanoparticles under the action of a magnet, washing them, mixing them with 35 mL of 1.5% thiocarbohydrazide, adding 3-5 mL of acetic acid, boiling and refluxing for 24 hours to obtain thiocarbohydrazide glutaraldehyde aminopropyl magnetic nanoparticles, decanting them and washing them;
[0056] S7, suspending the obtained thiocarbohydrazide glutaraldehyde aminopropyl magnetic nanoparticles in 50 mL of ethanol with a mass volume ratio of 2% of di-2-pyridone, and refluxing for 24 hours to obtain dimethocarbonylthiohydrazide-modified silica-coated magnetic nanoparticles, pouring out the dimethocarbonylthiohydrazide-modified silica-coated magnetic nanoparticles through a magnet, washing and drying to obtain dimethocarbonylthiohydrazide-modified silica-coated magnetic nanoparticles.
[0057] S8, using di-methylenethiocarbohydrazide-modified silica-coated magnetic nanoparticles as adsorbent materials for concentrating and separating trace mercury in seawater samples;
[0058] S9, the concentration of mercury in the adsorbent was determined by coupling magnetic solid phase microextraction with electrothermal atomic absorption spectrometry. When determining the concentration of mercury in the adsorbent, the sample flow rate was 3.8 mL / min, the eluent flow rate was 0.65 mL / min, and the reductant flow rate was 1.3 mL / min. The capture time of mercury vapor on the coated graphite tube was 110 seconds, the atomization temperature was 1250°C, the adsorption temperature was 25°C, and the holding time was 4 seconds.
[0059] S10, after determining the concentration of mercury in the adsorbent, the liquid is sent to a liquid separation device, which uses a membrane with a pore size of 0.5 μm and a nitrogen flow rate of 130 mL / min. The loading time is set to 140 s to ensure reasonable sensitivity.
[0060] Embodiment 3:
[0061] S1, 4 g of silica-coated magnetic nanoparticles were prepared by coprecipitation method;
[0062] S2, using 60 mL of 1% aminopropyltriethoxysilane and 95% ethanol, dilute 2 g of silica-coated magnetic nanoparticles to 200 mL, and adjust the pH value of the solution to 4.5 with acetic acid.
[0063] S3, stirring and heating at 60 °C for 2 h under nitrogen atmosphere to obtain nanospheres;
[0064] S4, washing the nanospheres with deionized water for three times and then with methanol for two times, and drying them into powder under vacuum at room temperature to obtain aminopropyl magnetic nanoparticles;
[0065] S5, mixing the obtained aminopropyl magnetic nanoparticles with 40 mL of a mixture of 3% diglutaraldehyde and deionized water, adding 4-6 mL of acetic acid, and refluxing the reaction mixture for 4 hours to obtain solid glutaraldehyde aminopropyl magnetic nanoparticles;
[0066] S6, decanting the solid glutaraldehyde aminopropyl magnetic nanoparticles under the action of a magnet, washing them, mixing them with 40 mL of 1.5% thiocarbohydrazide, adding 4-6 mL of acetic acid, boiling and refluxing for 24 hours to obtain thiocarbohydrazide glutaraldehyde aminopropyl magnetic nanoparticles, decanting them and washing them;
[0067] S7, suspending the obtained thiocarbohydrazide glutaraldehyde aminopropyl magnetic nanoparticles in 60 mL of ethanol with a mass volume ratio of 2% of di-2-pyridone, and refluxing for 24 hours to obtain dimethocarbonylthiohydrazide-modified silica-coated magnetic nanoparticles, pouring out the dimethocarbonylthiohydrazide-modified silica-coated magnetic nanoparticles through a magnet, washing and drying to obtain dimethocarbonylthiohydrazide-modified silica-coated magnetic nanoparticles.
[0068] S8, using di-methylenethiocarbohydrazide-modified silica-coated magnetic nanoparticles as adsorbent materials for concentrating and separating trace mercury in seawater samples;
[0069] S9, the concentration of mercury in the adsorbent was determined by coupling magnetic solid phase microextraction with electrothermal atomic absorption spectrometer. When determining the concentration of mercury in the adsorbent, the sample flow rate was 4.0 mL / min, the eluent flow rate was 0.7 mL / min, and the reductant flow rate was 1.4 mL / min. The capture time of mercury vapor on the coated graphite tube was 120 seconds, the optimal atomization temperature was 1300°C, the adsorption temperature was 25°C, and the holding time was 4.5 seconds.
[0070] S10, after determining the concentration of mercury in the adsorbent, the liquid is sent to a liquid separation device, which uses a membrane with a pore size of 0.5 μm and a nitrogen flow rate of 140 mL / min. The loading time is set to 150 s to ensure reasonable sensitivity.
Claims
1. A method for concentrating, separating and determining trace amounts of mercury in seawater. It is characterized in that The following steps are involved: S1, preparing di-methylenethiocarbohydrazide-modified silica-coated magnetic nanoparticles, the specific method is as follows: S11, preparing silica-coated magnetic nanoparticles by coprecipitation method; S12, using 50 mL of 1% aminopropyltriethoxysilane and 95% ethanol to dilute the obtained silica-coated magnetic nanoparticles to 150 mL, and adjusting the pH value of the diluted solution to 4.5 with acetic acid; S13, stirring and heating at 60 °C for 2 h under nitrogen atmosphere to obtain nanospheres; S14, washing the nanospheres and drying them into powder to obtain aminopropyl magnetic nanoparticles; S15, mixing the obtained aminopropyl magnetic nanoparticles with 25 mL of a mixture of 3% diglutaraldehyde and deionized water, adding 2-4 mL of acetic acid, and refluxing the reaction mixture to obtain solid glutaraldehyde aminopropyl magnetic nanoparticles; S16, decanting the solid glutaraldehyde aminopropyl magnetic nanoparticles under the action of a magnet, washing them, mixing them with 25 mL of 1.5% thiocarbohydrazide, adding 2-4 mL of acetic acid, boiling and refluxing to obtain thiocarbohydrazide glutaraldehyde aminopropyl magnetic nanoparticles, decanting them, and washing them; S17, suspending the obtained thiocarbohydrazide glutaraldehyde aminopropyl magnetic nanoparticles in 45 mL of ethanol with a mass volume ratio of 2% of di-2-pyridone, refluxing to obtain di-methylene thiocarbohydrazide modified silica-coated magnetic nanoparticles, washing and drying to obtain di-methylene thiocarbohydrazide modified silica-coated magnetic nanoparticles; S2, using di-methylenethiocarbohydrazide-modified silica-coated magnetic nanoparticles as adsorbent materials for concentrating and separating trace mercury in seawater samples; S3, the concentration of mercury in the adsorbent was determined by coupling magnetic solid phase microextraction with electrothermal atomic absorption spectrometry.
2. A method for concentrating, separating and determining trace mercury in seawater according to claim 1, It is characterized in that In S14, the nanospheres were washed three times with deionized water and then washed twice with methanol.
3. A method for concentrating, separating and determining trace mercury in seawater according to claim 1, It is characterized in that In S14, the drying is performed under vacuum at room temperature.
4. A method for concentrating, separating and determining trace mercury in seawater according to claim 1, It is characterized in that In S15, reflux for 4 hours; In S16, boiling and reflux for 24 hours; In S17, reflux is performed for 24 hours.
5. A method for concentrating, separating and determining trace mercury in seawater according to claim 1, It is characterized in that In S17, the magnetic nanoparticles coated with silica modified with dimethocarbonyl hydrazide are poured out by a magnet and then washed.
6. A method for concentrating, separating and determining trace mercury in seawater according to claim 1, It is characterized in that In S3, when determining the concentration of mercury in the adsorbent, the sample flow rate was 4.0 mL / min, the eluent flow rate was 0.6 mL / min, and the reducing agent flow rate was 1.2 mL / min.
7. The method for concentrating, separating and determining trace mercury in seawater according to claim 1, It is characterized in that In S3, after the concentration of mercury in the adsorbent is determined, the liquid is sent to a liquid separation device, which uses a membrane with a pore size of 0.5 μm and a nitrogen flow rate of 100 mL / min.