Circuit substrate, printed circuit board

By introducing a polymer layer into the circuit substrate and using thermosetting polyphenylene ether resin and thermoplastic resin to form a semi-interpenetrating polymer network structure, the problem of performance attenuation of printed circuit boards in hot and humid environments is solved, and higher resistance to humid and heat is achieved. Aging performance and stability.

CN114554682BActive Publication Date: 2024-10-18ZHEJIANG WAZAM NEW MATERIAL CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202011347429.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-26
Publication Date
2024-10-18
Estimated Expiration
2040-11-26

AI Technical Summary

Technical Problem

The performance of the dielectric layer of existing printed circuit boards is attenuated in hot and humid environments, resulting in insufficient stability of the circuit substrate and inability to meet usage requirements.

Method used

Introducing a polymer layer into the circuit substrate, using thermosetting polyphenylene ether resin and high molecular weight thermoplastic resin to form a semi-interpenetrating polymer network structure, enhancing the resistance to moisture and heat aging, and improving adhesion through hydrophobic groups and reactive groups performance and avoid direct exposure of the dielectric layer to the environment.

Benefits of technology

It significantly improves the humidity and heat aging resistance and peel strength of the circuit substrate, reduces the roughness requirements of the conductive layer, reduces the PIM value of the passive intermodulation value in each frequency band, and ensures the stability of the dielectric performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114554682B_ABST
    Figure CN114554682B_ABST
Patent Text Reader

Abstract

The present invention relates to a circuit substrate, comprising a dielectric layer and a conductive layer stacked on at least one surface of the dielectric layer, a polymer layer is further arranged between the dielectric layer and the conductive layer, the material of the polymer layer comprises a thermosetting polyphenylene ether resin and a thermoplastic resin, and the mass percentage of the thermosetting polyphenylene ether resin in the polymer layer is greater than the mass percentage of the thermoplastic resin in the polymer layer. The present invention also relates to a printed circuit board made of the circuit substrate. The circuit substrate of the present invention has excellent resistance to wet and hot aging, so the printed circuit board made of the circuit substrate of the present invention can meet the use requirements in a wet and hot environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic industry, in particular to a circuit substrate and a printed circuit board. Background Art

[0002] During the processing of printed circuit boards (PCBs), the copper foil on the surface of the circuit substrate will be damaged, exposing the dielectric layer of the circuit substrate directly to the environment. Since the resin system of the dielectric layer is generally epoxy resin, phenolic resin, amino resin, unsaturated polyester resin and polysilicone resin, these resins have excellent performance at room temperature, but they also have certain limitations. For example, the molecular structure has strong polarity or contains a large number of unreacted unsaturated functional groups. In a long-term hot and humid environment, the water absorption is too high or it is easy to react with oxygen in the air, resulting in serious attenuation of the performance of the dielectric layer, thereby affecting the performance stability of the PCB and failing to meet the use requirements. Summary of the invention

[0003] Based on this, it is necessary to provide a circuit substrate and a printed circuit board with stable performance to address the above problems.

[0004] A circuit substrate comprises a dielectric layer and a conductive layer stacked on at least one surface of the dielectric layer, a polymer layer is further arranged between the dielectric layer and the conductive layer, the material of the polymer layer comprises a thermosetting polyphenylene ether resin and a thermoplastic resin, and the mass percentage of the thermosetting polyphenylene ether resin in the polymer layer is greater than the mass percentage of the thermoplastic resin in the polymer layer.

[0005] In one embodiment, the thermosetting polyphenylene ether resin has an unsaturated double bond at the end of its molecular chain.

[0006] In one embodiment, the unsaturated double bond includes at least one of a vinyl group, a ketocarbonyl group, a methacryl group, a methacryl group, and an ester group.

[0007] In one embodiment, the thermoplastic resin includes at least one of thermoplastic polyphenylene ether resin, polyamide, polyolefin, saturated polyester resin and unsaturated polyester resin, and the molecular weight of the thermoplastic resin is 8000-40000.

[0008] In one embodiment, the molecular chain of the thermosetting polyphenylene ether resin contains at least one of a hydrophobic group and a reactive group;

[0009] And / or, the thermoplastic resin contains at least one of a hydrophobic group and a reactive group in the molecular chain.

[0010] In one embodiment, the hydrophobic group includes at least one of a C10-C20 hydrocarbon group, a hydrocarbon group containing an aromatic group, a hydrocarbon group containing an ester group, a hydrocarbon group containing an ether group, a hydrocarbon group containing an amine group, a hydrocarbon group containing an amide group, a hydrocarbon group containing a double bond, a polyoxypropylene group, a long-chain perfluoroalkyl group, and a polysiloxane group.

[0011] In one embodiment, the reactive group includes at least one of an unsaturated double bond group, an amino group, a carboxyl group, and an aldehyde group.

[0012] In one of the embodiments, the mass percentage of the thermoplastic resin in the polymer layer is 3%-33%.

[0013] In one embodiment, the difference between the dielectric constant of the polymer layer and the dielectric constant of the dielectric layer is negative 2.0-2.0.

[0014] In one embodiment, the thickness of the polymer layer is 3 μm-100 μm.

[0015] In one embodiment, the polymer layer further includes a dielectric filler, and the particle size of the dielectric filler is smaller than the thickness of the polymer layer.

[0016] In one of the embodiments, the roughness of the conductive layer is less than or equal to 5.1 μm.

[0017] In the circuit substrate of the present invention, a polymer layer is arranged between the dielectric layer and the conductive layer, and the polymer layer is mainly made of thermosetting polyphenylene ether resin, supplemented by a high molecular weight thermoplastic resin, so that the molecular chains of the two can form a semi-interpenetrating polymer network structure, thereby making the polymer layer have excellent resistance to moisture and heat aging, and at the same time have excellent bonding properties with the dielectric layer and the conductive layer. During the circuit processing of the PCB, even if the conductive layer is damaged, the polymer layer can prevent the dielectric layer from being directly exposed to the environment, thereby effectively improving the moisture and heat aging resistance of the circuit substrate.

[0018] In addition, the polymer layer can also effectively increase the polymer content of the surface of the dielectric layer, while improving the flatness of the surface of the dielectric layer, increasing the effective contact area with the conductive layer, thereby improving the peel strength of the circuit substrate, and further reducing the requirements for the roughness of the conductive layer, so that the dielectric properties of the circuit substrate are stable, and the passive intermodulation (PIM) value is significantly reduced in all frequency bands.

[0019] A printed circuit board is made of the circuit substrate.

[0020] Since the printed circuit board of the present invention is made of the circuit substrate, the printed circuit board of the present invention has stable resistance to moisture and heat aging and can meet the use requirements in a moisture and heat environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic structural diagram of the circuit substrate of the present invention.

[0022] In the figure: 101, dielectric layer; 102, conductive layer; 103, polymer layer. DETAILED DESCRIPTION

[0023] The circuit substrate and printed circuit board provided by the present invention will be further described below.

[0024] like Figure 1 As shown, a circuit substrate according to an embodiment of the present invention is provided, and the circuit substrate is mainly used for preparing PCB.

[0025] The circuit substrate includes a dielectric layer 101 and a conductive layer 102 stacked on at least one surface of the dielectric layer 101, and a polymer layer 103 is further arranged between the dielectric layer 101 and the conductive layer 102, so that during the circuit processing of the PCB, even if the conductive layer 102 is damaged, the polymer layer 103 can prevent the dielectric layer 101 from being directly exposed to the environment, thereby effectively improving the moisture and heat aging resistance of the circuit substrate.

[0026] The material of the polymer layer 103 includes thermosetting polyphenylene ether resin and thermoplastic resin, and the mass percentage of the thermosetting polyphenylene ether resin in the polymer layer is greater than the mass percentage of the thermoplastic resin in the polymer layer.

[0027] Thermosetting polyphenylene ether resin has excellent resistance to moisture and heat aging. However, the pure thermosetting polyphenylene ether resin layer is relatively brittle and has poor bonding effect with the dielectric layer 101 and the conductive layer 102. Therefore, the present invention mainly uses thermosetting polyphenylene ether resin and supplements it with a high molecular weight thermoplastic resin to match it, so that the molecular chains of the two can form a semi-interpenetrating polymer network structure, reduce the curing crosslinking density while increasing the toughness of the polymer layer 103, avoid the polymer layer 103 from breaking during use, and increase the interface compatibility between the polymer layer 103 and the resin in the dielectric layer 101, so that the polymer layer 103 has excellent resistance to moisture and heat aging, and has excellent bonding performance with the dielectric layer 101 and the conductive layer 102, and achieves excellent bonding effect with the dielectric layer 101 and the conductive layer 102.

[0028] Therefore, during the circuit processing of the PCB, even if the conductive layer 102 of the circuit substrate is damaged, the polymer layer 103 can prevent the dielectric layer 101 from being directly exposed to the environment, thereby effectively improving the moisture and heat aging resistance of the circuit substrate.

[0029] It should be noted that polyphenylene ether resin is a thermoplastic resin, and the thermosetting polyphenylene ether resin refers to a polyphenylene ether resin that is modified and then cross-linked and cured by chemical reaction under heating, pressurization or under the action of a curing agent or ultraviolet light to become an insoluble and infusible substance.

[0030] In the present invention, the thermosetting polyphenylene ether resin can be a capped modified polyphenylene ether resin, preferably containing an unsaturated double bond at the end of the polyphenylene ether molecular chain, wherein the unsaturated double bond includes at least one of a vinyl group, a ketone carbonyl group, a methacrylic group, a methacrylic linear group, and an ester group, so as to ensure that the polymer layer 103 can chemically react with the dielectric layer 101 to form a tight bond. At the same time, since the unsaturated double bond only exists at the end of the thermosetting polyphenylene ether resin molecular chain, the resin itself still has excellent resistance to moisture and heat aging, so that it can also protect the dielectric layer 101 in a moisture and heat environment.

[0031] In one or more embodiments, the thermoplastic resin includes at least one of thermoplastic polyphenylene ether resin, polyamide, polyolefin, saturated polyester resin, and unsaturated polyester resin. In order to further ensure the performance of the polymer layer 103 and achieve a better bonding effect with the dielectric layer 101 and the conductive layer 102, the mass percentage of the thermoplastic resin in the polymer layer 103 is 3%-33%, and the molecular weight of the thermoplastic resin is further preferably 8000-400000.

[0032] In order to further improve the performance stability of the polymer layer 103 in a hot and humid environment, the molecular chain of the thermosetting polyphenylene ether resin may contain a hydrophobic group; and / or the molecular chain of the thermoplastic resin may contain a hydrophobic group. The hydrophobic group includes at least one of a C10-C20 hydrocarbon group, a hydrocarbon group containing an aromatic group, a hydrocarbon group containing an ester group, a hydrocarbon group containing an ether group, a hydrocarbon group containing an amine group, a hydrocarbon group containing an amide group, a hydrocarbon group containing a double bond, a polyoxypropylene group, a long-chain perfluoroalkyl group, and a polysiloxane group.

[0033] The dielectric layer 101 is generally made of a polymer matrix and a dielectric filler, and the polymer matrix includes at least one of epoxy resin, phenolic resin, amino resin, unsaturated polyester resin, and polysilicone ether resin. In order to make the polymer layer 103 and the dielectric layer 101 better bonded and improve the peel strength of the circuit substrate, the polymer layer 103 needs to have a certain compatibility or reactivity with the dielectric layer 101.

[0034] For example, the thermosetting polyphenylene ether resin or thermoplastic resin of the polymer layer 103 and the polymer substrate of the dielectric layer 101 are polymers with the same or similar molecular structures, so that the polymer layer 103 and the dielectric layer 101 can be well bonded or fused by the bonding force between molecules.

[0035] Alternatively, when the polymer matrix of the dielectric layer 101 includes at least one of the functional groups such as vinyl, epoxy, amino, and hydroxyl, the molecular chain of the thermosetting polyphenylene ether resin in the polymer layer 103 may contain reactive groups, and / or the molecular chain of the thermoplastic resin may contain reactive groups, or the polymer layer 103 may contain reactive groups by surface treatment methods such as plasma treatment. The reactive groups include at least one of unsaturated double bond groups, amino groups, carboxyl groups, and aldehyde groups.

[0036] For example, when the polymer matrix of the dielectric layer 101 contains vinyl, the material of the polymer layer 103 needs to include at least one of unsaturated groups such as vinyl, ketocarbonyl, methacrylic, methacrylic, and ester groups; when the polymer matrix of the dielectric layer 101 contains hydroxyl, the material of the polymer layer 103 needs to include at least one of amino, carboxyl, and aldehyde groups. This allows a chemical reaction to occur between the polymer layer 103 and the dielectric layer 101, achieving connection between layers through chemical bonds, and improving the peel strength of the circuit substrate.

[0037] It should be noted that at this time, the conductive layer 102 can also be surface treated by surface treatment methods such as plasma treatment, so that the surface of the conductive layer 102 also contains reactive groups such as hydroxyl groups, so that a chemical reaction can also occur between the conductive layer 102 and the polymer layer 103, and the connection between the layers is achieved through chemical bonds.

[0038] Furthermore, the polymer layer 103 is preferably made of a thermosetting polyphenylene ether resin containing reactive groups and hydrophobic groups and a thermoplastic polymer containing reactive groups and hydrophobic groups, so as to simultaneously improve the peel strength and moisture and heat resistance stability of the circuit substrate.

[0039] In the circuit substrate of the present invention, the thickness of the polymer layer 103 is greater than or equal to 3 μm. On the one hand, the polymer layer 103 can effectively cover the dielectric layer 101 and block the direct contact between the dielectric layer 101 and the external environment; on the other hand, the polymer layer 103 can also effectively increase the polymer content of the surface of the dielectric layer 101, while improving the flatness of the surface of the dielectric layer 101, increasing the effective contact area with the conductive layer 102, and improving the peel strength of the circuit substrate.

[0040] At the same time, in order to reduce the influence of the polymer layer 103 on the dielectric properties of the circuit substrate, the thickness of the polymer layer 103 is less than or equal to 100 μm, and more preferably 5 μm-50 μm. When the two opposite surfaces of the dielectric layer 101 are provided with polymer layers 103, the sum of the thicknesses of the two polymer layers 103 is less than or equal to 100 μm.

[0041] In the circuit substrate of the present invention, the dielectric constant of the polymer layer 103 may be greater than or equal to the dielectric constant of the dielectric layer 101, or may be less than or equal to the dielectric constant of the dielectric layer 101, in order to reduce the influence of the polymer layer 103 on the dielectric constant of the circuit substrate, so that the dielectric properties of the circuit substrate remain substantially unchanged and the dielectric properties are stable. In one or more embodiments, the difference between the dielectric constant of the polymer layer 103 and the dielectric constant of the dielectric layer 101 is preferably negative 2.0-2.0, more preferably negative 1.0-1.0, and more preferably less than or equal to negative 0.5-0.5.

[0042] The dielectric constant of the polymer layer 103 can be adjusted by dielectric fillers, so the polymer layer 103 can also include dielectric fillers. Of course, the particle size of the dielectric fillers is smaller than the thickness of the polymer layer 103 to avoid the dielectric fillers protruding from the polymer layer 103 and affecting the bonding performance between the polymer layer 103 and the dielectric layer 101 and the conductive layer 102.

[0043] Furthermore, the circuit substrate of the present invention can reduce the requirement for the roughness of the conductive layer 102. In one or more embodiments, the roughness of the conductive layer 102 can be reduced to within the range of VLP (less than or equal to 5.1 μm), and further reduced to within the range of HVLP (less than or equal to 3.1 μm).

[0044] In one or more embodiments, the conductive layer 102 is preferably copper foil.

[0045] Therefore, the present invention can effectively improve the peel strength and moisture-heat aging resistance of the circuit substrate as a whole. After aging in a high-temperature and moisture-heat environment at 80°C for more than one month, the performance of the circuit substrate remains basically unchanged. At the same time, the dielectric constant of the circuit substrate can be basically unchanged, and the passive intermodulation value of the circuit substrate can be significantly reduced in each frequency band, and the PIM value meets -100dBm to -160dBm.

[0046] The present invention also provides a printed circuit board, which is made of the circuit substrate.

[0047] Since the printed circuit board of the present invention is made of the circuit substrate, the printed circuit board of the present invention has stable resistance to moisture and heat aging and can meet the use requirements in a moisture and heat environment.

[0048] Hereinafter, the circuit substrate and the printed circuit board will be further described through the following specific embodiments.

[0049] Example 1

[0050] A dielectric layer with a Dk of 3.01 and a Df of 0.0037 is provided, wherein the polymer matrix of the dielectric layer is polybutadiene and the dielectric layer contains a vinyl functional group.

[0051] The terminal vinyl-modified polyphenylene ether resin and the thermoplastic polyphenylene ether are mixed in a mass ratio of 90:10, and the mixed resin is coated on the surface of the substrate by a spraying process. The thickness of the polymer film is controlled to be 30 μm through the process, and the dielectric constant of the polymer film is 2.5.

[0052] Then, copper foil is coated on the surface of the polymer layer. The copper foil is treated with a coupling agent, and the surface layer contains vinyl functional groups. The roughness of the copper foil is VLP grade (Ra: 4.2μm). After the lamination process, chemical reactions occur between the copper foil and the polymer film, and between the polymer film and the dielectric layer to obtain a circuit substrate. The conditions of the lamination process are: temperature 260°C, time 5 hours, and pressure 650psi.

[0053] The circuit substrate is prepared into a printed circuit board through the process of drilling, hole filling, micro-etching, pre-impregnation, activation, acceleration, chemical copper and copper thickening.

[0054] After inspection: Under normal conditions, the dielectric constant of the obtained circuit substrate is 2.96, the dielectric loss is 0.0025, the PIM is -114dBm, and the peel strength is 1.4N / mm; after aging for 6 weeks at 85°C and 85% relative humidity, the aging dielectric constant of the circuit substrate is 2.99; after aging at 200°C for 7 days, the peel strength of the circuit substrate is 1.2N / mm.

[0055] Example 2

[0056] The dielectric layer, polymer film and the surface treatment method of the polymer film are the same as those in Example 1.

[0057] Then, copper foil is coated on the surface of the polymer layer. The copper foil is treated with a coupling agent, and the surface layer contains vinyl functional groups. The roughness of the copper foil is HVLP grade (Ra: 3.0 μm). After the lamination process, chemical reactions occur between the copper foil and the polymer film, and between the polymer film and the dielectric layer to obtain a circuit substrate. The conditions of the lamination process are: temperature 260°C, time 5 hours, and pressure 650 psi.

[0058] The circuit substrate is prepared into a printed circuit board through the process of drilling, hole filling, micro-etching, pre-impregnation, activation, acceleration, chemical copper and copper thickening.

[0059] After inspection: Under normal conditions, the dielectric constant of the obtained circuit substrate is 2.96, the dielectric loss is 0.0025, the PIM is -116dBm, and the peel strength is 1.1N / mm; after aging for 6 weeks at 85°C and 85% relative humidity, the aging dielectric constant of the circuit substrate is 2.99; after aging at 200°C for 7 days, the peel strength of the circuit substrate is 0.9N / mm.

[0060] Example 3

[0061] A dielectric layer with a Dk of 3.01 and a Df of 0.0037 is provided, wherein the polymer matrix of the dielectric layer is polybutadiene and the dielectric layer contains a vinyl functional group.

[0062] The terminal vinyl-modified polyphenylene ether resin and the thermoplastic styrene maleic anhydride copolymer with a molecular weight of 10,000 are mixed in a mass ratio of 90:10, and the mixed resin is coated on the surface of the substrate by a spraying process. The thickness of the polymer film is controlled to be 30 μm through the process, and the dielectric constant of the polymer film is 2.5.

[0063] Then, copper foil is coated on the surface of the polymer layer. The copper foil is treated with a coupling agent, and the surface layer contains vinyl functional groups. The roughness of the copper foil is VLP grade (Ra: 4.2μm). After the lamination process, chemical reactions occur between the copper foil and the polymer film, and between the polymer film and the dielectric layer to obtain a circuit substrate. The conditions of the lamination process are: temperature 260°C, time 5 hours, and pressure 650psi.

[0064] The circuit substrate is prepared into a printed circuit board through the process of drilling, hole filling, micro-etching, pre-impregnation, activation, acceleration, chemical copper and copper thickening.

[0065] After inspection: Under normal conditions, the dielectric constant of the obtained circuit substrate is 2.93, the dielectric loss is 0.0024, the PIM is -114dBm, and the peel strength is 1.2N / mm; after aging for 6 weeks at 85°C and 85% relative humidity, the aging dielectric constant of the circuit substrate is 2.96; after aging at 200°C for 7 days, the peel strength of the circuit substrate is 1.0N / mm.

[0066] Example 4

[0067] The only difference between Example 4 and Example 1 is that the thickness of the polymer layer is 5 μm.

[0068] The circuit substrate is prepared into a printed circuit board through the process of drilling, hole filling, micro-etching, pre-impregnation, activation, acceleration, chemical copper and copper thickening.

[0069] After inspection: Under normal conditions, the dielectric constant of the obtained circuit substrate is 3.00, the dielectric loss is 0.0030, the PIM is -114dBm, and the peel strength is 0.9N / mm; after aging for 6 weeks at 85°C and 85% relative humidity, the aging dielectric constant of the circuit substrate is 3.05; after aging at 200°C for 7 days, the peel strength of the circuit substrate is 0.7N / mm.

[0070] Example 5

[0071] The only difference between Example 5 and Example 1 is that the thickness of the polymer layer is 50 μm.

[0072] The circuit substrate is prepared into a printed circuit board through the process of drilling, hole filling, micro-etching, pre-impregnation, activation, acceleration, chemical copper and copper thickening.

[0073] After inspection: Under normal conditions, the dielectric constant of the obtained circuit substrate is 2.90, the dielectric loss is 0.0023, the PIM is -114dBm, and the peel strength is 1.4N / mm; after aging for 6 weeks at 85°C and 85% relative humidity, the aging dielectric constant of the circuit substrate is 2.93; after aging at 200°C for 7 days, the peel strength of the circuit substrate is 1.2N / mm.

[0074] Example 6

[0075] The only difference between Example 6 and Example 1 is that the thickness of the polymer layer is 100 μm.

[0076] The circuit substrate is prepared into a printed circuit board through the process of drilling, hole filling, micro-etching, pre-impregnation, activation, acceleration, chemical copper and copper thickening.

[0077] After inspection: Under normal conditions, the dielectric constant of the obtained circuit substrate is 2.84, the dielectric loss is 0.0020, the PIM is -114dBm, and the peel strength is 1.4N / mm; after aging for 6 weeks at 85°C and 85% relative humidity, the aging dielectric constant of the circuit substrate is 2.88; after aging at 200°C for 7 days, the peel strength of the circuit substrate is 1.2N / mm.

[0078] Example 7

[0079] The only difference between Example 7 and Example 1 is that the Dk of the dielectric layer is 3.55, the Df is 0.0040, the polymer substrate of the dielectric layer is polybutadiene, and the dielectric layer contains a vinyl functional group.

[0080] The circuit substrate is prepared into a printed circuit board through the process of drilling, hole filling, micro-etching, pre-impregnation, activation, acceleration, chemical copper and copper thickening.

[0081] After inspection: Under normal conditions, the dielectric constant of the obtained circuit substrate is 3.44, the dielectric loss is 0.0029, the PIM is -114dBm, and the peel strength is 1.2N / mm; after aging for 6 weeks at 85°C and 85% relative humidity, the aging dielectric constant of the circuit substrate is 3.48; after aging at 200°C for 7 days, the peel strength of the circuit substrate is 1.0N / mm.

[0082] Example 8

[0083] The only difference between Example 8 and Example 1 is that the Dk of the dielectric layer is 4.51, the Df is 0.0057, the polymer substrate of the dielectric layer is polybutadiene, and the dielectric layer contains vinyl functional groups.

[0084] The circuit substrate is prepared into a printed circuit board through the process of drilling, hole filling, micro-etching, pre-impregnation, activation, acceleration, chemical copper and copper thickening.

[0085] After inspection: Under normal conditions, the dielectric constant of the obtained circuit substrate is 4.02, the dielectric loss is 0.0049, the PIM is -114dBm, and the peel strength is 1.0N / mm; after aging for 6 weeks at 85°C and 85% relative humidity, the aging dielectric constant of the circuit substrate is 4.13; after aging at 200°C for 7 days, the peel strength of the circuit substrate is 0.7N / mm.

[0086] Comparative Example 1

[0087] The only difference between Comparative Example 1 and Example 1 is that there is no polymer layer between the copper foil and the dielectric layer.

[0088] The circuit substrate is prepared into a printed circuit board through the process of drilling, hole filling, micro-etching, pre-impregnation, activation, acceleration, chemical copper and copper thickening.

[0089] After inspection: Under normal conditions, the dielectric constant of the obtained circuit substrate is 3.01, the dielectric loss is 0.0037, the PIM is -112dBm, and the peel strength is 0.6N / mm; after aging for 6 weeks at 85°C and 85% relative humidity, the aging dielectric constant of the circuit substrate is 3.20; after aging at 200°C for 7 days, the peel strength of the circuit substrate is 0.4N / mm.

[0090] Comparative Example 2

[0091] The only difference between Comparative Example 2 and Example 1 is that there is no polymer layer between the copper foil and the dielectric layer, and the roughness grade of the copper foil is the HVLP grade (Ra is 3.1 μm).

[0092] The circuit substrate is prepared into a printed circuit board through the process of drilling, hole filling, micro-etching, pre-impregnation, activation, acceleration, chemical copper and copper thickening.

[0093] After inspection: Under normal conditions, the dielectric constant of the obtained circuit substrate is 3.01, the dielectric loss is 0.0037, the PIM is -116dBm, and the peel strength is 0.5N / mm; after aging for 6 weeks at 85°C and 85% relative humidity, the aging dielectric constant of the circuit substrate is 3.20; after aging at 200°C for 7 days, the peel strength of the circuit substrate is 0.2N / mm.

[0094] Comparative Example 3

[0095] The only difference between Comparative Example 3 and Example 1 is that the modified polyphenylene ether resin and the thermoplastic polyphenylene ether are mixed in a mass ratio of 10:90.

[0096] The circuit substrate is prepared into a printed circuit board through the process of drilling, hole filling, micro-etching, pre-impregnation, activation, acceleration, chemical copper and copper thickening.

[0097] After inspection: Under normal conditions, the dielectric constant of the obtained circuit substrate is 3.01, the dielectric loss is 0.0035, the PIM is -114dBm, and the peel strength is 0.7N / mm; after aging for 6 weeks at 85°C and 85% relative humidity, the aging dielectric constant of the circuit substrate is 3.20; after aging at 200°C for 7 days, the peel strength of the circuit substrate is 0.5N / mm.

[0098] Comparative Example 4

[0099] The only difference between Comparative Example 4 and Example 1 is that the mass percentage of the thermoplastic polyphenylene ether resin in the polymer layer is 100%.

[0100] The circuit substrate is prepared into a printed circuit board through the process of drilling, hole filling, micro-etching, pre-impregnation, activation, acceleration, chemical copper and copper thickening.

[0101] After inspection: Under normal conditions, the dielectric constant of the obtained circuit substrate is 3.01, the dielectric loss is 0.0033, the PIM is -114dBm, and the peel strength is 0.1N / mm; after aging for 6 weeks at 85°C and 85% relative humidity, the aging dielectric constant of the circuit substrate is 3.20; after aging at 200°C for 7 days, the peel strength of the circuit substrate is 0.1N / mm.

[0102] Comparative Example 5

[0103] The only difference between Comparative Example 5 and Example 1 is that in the polymer layer, the molecular weight of the thermoplastic polyphenylene ether resin is 5,000.

[0104] The circuit substrate is prepared into a printed circuit board through the process of drilling, hole filling, micro-etching, pre-impregnation, activation, acceleration, chemical copper and copper thickening.

[0105] After inspection: Under normal conditions, the dielectric constant of the obtained circuit substrate is 3.01, the dielectric loss is 0.0034, the PIM is -114dBm, and the peel strength is 0.7N / mm; after aging for 6 weeks at 85°C and 85% relative humidity, the aging dielectric constant of the circuit substrate is 3.20; after aging at 200°C for 7 days, the peel strength of the circuit substrate is 0.5N / mm.

[0106] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0107] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A circuit substrate, comprising a dielectric layer and a conductive layer stacked on at least one surface of the dielectric layer, characterized in that: A polymer layer is further arranged between the dielectric layer and the conductive layer, the material of the polymer layer includes a thermosetting polyphenylene ether resin and a thermoplastic resin, the mass percentage of the thermosetting polyphenylene ether resin in the polymer layer is greater than the mass percentage of the thermoplastic resin in the polymer layer, the molecular chains of the thermosetting polyphenylene ether resin and the thermoplastic resin both contain hydrophobic groups, the hydrophobic groups include at least one of a C10-C20 hydrocarbon group, a hydrocarbon group containing an aromatic group, a hydrocarbon group containing an ester group, a hydrocarbon group containing an ether group, a hydrocarbon group containing an amine group, a hydrocarbon group containing an amide group, a hydrocarbon group containing a double bond, a polyoxypropylene group, a long-chain perfluoroalkyl group, and a polysiloxane group, the thermoplastic resin includes at least one of a thermoplastic polyphenylene ether resin, a polyamide, a saturated polyester resin, and an unsaturated polyester resin, and the molecular weight of the thermoplastic resin is 8000-40000; Wherein, the thickness of the polymer layer is 50 μm-100 μm, and the roughness of the conductive layer is less than or equal to 5.1 μm.

2. The circuit substrate according to claim 1, characterized in that: The thermosetting polyphenylene ether resin contains an unsaturated double bond at the end of the molecular chain.

3. The circuit substrate according to claim 2, characterized in that: The unsaturated double bonds include at least one of vinyl, ketocarbonyl, methacryl, methacryl and ester groups.

4. The circuit substrate according to claim 1, characterized in that: The thermosetting polyphenylene ether resin also contains reactive groups in its molecular chain; And / or, the thermoplastic resin further contains reactive groups in its molecular chain.

5. The circuit substrate according to claim 4, characterized in that: The reactive group includes at least one of an unsaturated double bond group, an amino group, a carboxyl group, and an aldehyde group.

6. The circuit substrate according to claim 1, characterized in that: The mass percentage of the thermoplastic resin in the polymer layer is 3%-33%.

7. The circuit substrate according to claim 1, characterized in that: The difference between the dielectric constant of the polymer layer and the dielectric constant of the dielectric layer is -2.0 to 2.

0.

8. The circuit substrate according to claim 1, wherein: The polymer layer further includes a dielectric filler, and the particle size of the dielectric filler is smaller than the thickness of the polymer layer.

9. A printed circuit board, characterized in that: The printed circuit board is made of the circuit substrate according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Copper foil having adhesive agent adhered thereto, copper-clad laminated plate, and wiring substrate

    CN110463363A

  • Functional conducting layer, circuit substrate and printed circuit board

    CN111808542A

  • Preimpregnation sandwich body reaches circuit substrate, printed circuit board by its preparation for circuit substrate

    CN204887693U

  • Metal-clad laminate, method for producing same, metal foil with resin, and printed wiring board

    US20170164469A1