A cathode coating material for lithium secondary batteries, a method for preparing the same, and a cathode and a lithium secondary battery comprising the coating material.

By grafting the cationic functional polymer onto the surface of graphene oxide, a positive electrode coating material for lithium secondary batteries was prepared, which solved the problem of lithium polysulfide dissolution in lithium sulfur batteries, and significantly improved the discharge capacity and life of the battery. , especially at high current density, showed significant improvement.

CN114556631BActive Publication Date: 2024-11-29LG ENERGY SOLUTION LTD +1
3 Cites 0 Cited by

Patent Information

Application Number
CN202180005894.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-10
Publication Date
2024-11-29
Estimated Expiration
2041-08-10

Smart Images

  • Figure CN114556631B_ABST
    Figure CN114556631B_ABST
Patent Text Reader

Abstract

This invention discloses a positive electrode coating material for lithium-ion batteries, its preparation method, and a positive electrode and a lithium-ion battery comprising the coating material. The positive electrode coating material for lithium-ion batteries is obtained by grafting a polymer with cationic functional groups onto the surface of graphene oxide and is used as a positive electrode coating material for lithium-ion batteries to prevent the dissolution of lithium polysulfides, thereby improving battery performance. The positive electrode coating material for lithium-ion batteries comprises graphene oxide with a surface modified with cationic functional groups.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0099787, filed on August 10, 2020, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a positive electrode coating material for a lithium secondary battery, a preparation method thereof, and a positive electrode and a lithium secondary battery comprising the coating material. More specifically, the present invention relates to a positive electrode coating material for a lithium secondary battery, which is manufactured by grafting a polymer having a cationic functional group onto the surface of graphene oxide and can improve the performance of the battery by preventing the dissolution of lithium polysulfide when used as a positive electrode coating material for a lithium secondary battery. Background Art

[0003] As interest in energy storage technology grows, research and development of electrochemical devices is increasing as its applications expand to mobile phones, tablets, laptops, and camcorders, and further to electric vehicles (EVs) and hybrid electric vehicles (HEVs). Electrochemical devices are the area of ​​greatest interest in this regard, with the development of secondary batteries such as lithium-sulfur batteries that can be charged and discharged becoming the focus of attention. In recent years, research and development has been conducted on the design of new electrodes and cells in order to increase capacity density when developing such batteries.

[0004] Among these electrochemical devices, lithium-sulfur batteries (Li-S batteries) that use lithium metal as a negative electrode and sulfur as a positive electrode have a higher theoretical capacity and energy density (usually about 2500Wh / kg) than conventional lithium-ion batteries, and because they use sulfur that can be easily obtained from nature as a positive electrode, they are also economical and affordable, and thus have attracted much attention as the next generation of secondary batteries that can replace lithium-ion batteries. In this lithium-sulfur battery, a reduction reaction of sulfur and an oxidation reaction of lithium metal occur during the discharge process. At this time, sulfur forms lithium polysulfide (LiPS) with a linear structure from S8 with a ring structure. This lithium-sulfur battery is characterized by showing a voltage that is gradually discharged until the polysulfide is completely reduced to Li2S.

[0005] However, the biggest obstacle to the commercialization of lithium-sulfur batteries is the generation of lithium polysulfide (LiPS, Li2S) during charging and discharging in batteries that use sulfur-based compounds as positive electrode active materials and alkali metals such as lithium as negative electrode active materials. x In other words, the biggest problem of lithium-sulfur batteries is the sharp drop in capacity due to the dissolution of lithium polysulfide generated at the positive electrode during charging and discharging.

[0006] More specifically, lithium polysulfide generated when sulfur used as a positive electrode is reduced during discharge has high solubility, especially in an ether-based liquid electrolyte, and is small in size, thereby being able to pass through a separator, and when it encounters lithium metal used as a negative electrode, it causes a side reaction leading to a problem of interface instability. As a result, the capacity decreases due to the irreversible loss of the positive electrode active material, and the life of the battery is shortened because sulfur particles are deposited on the surface of the lithium metal due to the side reaction. Therefore, a technology capable of preventing lithium polysulfide generated from the positive electrode from dissolving into the liquid electrolyte during battery operation is required. Summary of the invention

[0007] Technical issues

[0008] Therefore, an object of the present invention is to provide a positive electrode coating material for a lithium secondary battery, a method for producing the same, and a positive electrode and a lithium secondary battery comprising the coating material, wherein the positive electrode coating material for a lithium secondary battery is obtained by grafting a polymer having a cationic functional group onto the surface of graphene oxide, and is used as a positive electrode coating material for a lithium secondary battery, thereby preventing the dissolution of lithium polysulfide and improving the performance of the battery.

[0009] Technical Solution

[0010] In order to achieve the above object, the present invention provides a positive electrode coating material for a lithium secondary battery, which comprises graphene oxide surface-modified with a cationic functional group.

[0011] In addition, the present invention provides a method for manufacturing a positive electrode coating material for a lithium secondary battery, the method comprising the following steps:

[0012] (a) preparing a surface-modified graphene oxide by reacting graphene oxide containing one or more of a -COOH group and a -OH group on the surface with a hydrocarbon structural unit having 1 to 10 carbon atoms and containing 0 to 2 oxygen atoms, the hydrocarbon structural unit comprising a functional group forming a bond with the -COOH group or the -OH group and a functional group forming a bond with a vinyl group contained in a (meth)acrylate compound; and

[0013] (b) reacting the surface-modified graphene oxide with a (meth)acrylate structural unit grafted with a hydrocarbon group having 2 to 10 carbon atoms and containing a cationic group.

[0014] In addition, the present invention provides a positive electrode for a lithium secondary battery, comprising: a positive electrode active material; and a positive electrode coating material coated on a surface of the positive electrode active material.

[0015] In addition, the present invention provides a lithium secondary battery, which includes: a positive electrode for a lithium secondary battery; a lithium metal negative electrode; an electrolyte provided between the positive electrode and the negative electrode; and a separator.

[0016] Beneficial Effects

[0017] According to the positive electrode coating material for lithium secondary batteries, the preparation method thereof, and the positive electrode and lithium secondary battery comprising the coating material of the present invention, the advantages of the present invention are that the coating material obtained by grafting a polymer having a cationic functional group onto the surface of graphene oxide is used as a positive electrode coating material for lithium secondary batteries, thereby preventing the dissolution of lithium polysulfide and being able to improve the performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is the chemical structural formula of the positive electrode coating material for a lithium secondary battery according to an embodiment of the present invention.

[0019] Figure 2 FIG. 4 is a reaction scheme showing a process of synthesizing a cationic monomer grafted onto the surface of graphene oxide according to an embodiment of the present invention.

[0020] Figure 3 FIG. 4 is a reaction scheme showing a process of forming subsequent reaction initiation sites on the surface of graphene oxide according to an embodiment of the present invention.

[0021] Figure 4 FIG. 4 is a reaction scheme showing a process of grafting a cationic polymer to a subsequent reaction initiation site formed on the surface of graphene oxide according to an embodiment of the present invention.

[0022] Figure 5 To show the cationic monomer (QDMAEMA) prepared according to the embodiment of the present invention 1 Graph of the H NMR analysis results.

[0023] Figure 6 FIG. 5 is a graph showing the TGA analysis results of the positive electrode coating material prepared according to an embodiment of the present invention.

[0024] Figure 7 The figure shows the FT-IR analysis result of the positive electrode coating material prepared according to the embodiment of the present invention.

[0025] Figure 8 The figure shows the XRD analysis result of the positive electrode coating material prepared according to the embodiment of the present invention.

[0026] Fig. 9 FIG. 5 is a graph showing the UV-Vis analysis results of the positive electrode coating material prepared according to an embodiment of the present invention.

[0027] Fig.10 These are SEM images and EDS images of a “sulfur-carbon composite material coated with a positive electrode coating material” prepared according to an embodiment of the present invention.

[0028] Fig.11 TGA analysis graph (left) and TEM analysis graph (right) of the sulfur-carbon composite material coated with a positive electrode coating material (FGO(OH)-TFSI) prepared according to an embodiment of the present invention.

[0029] Figures 12 to 14 FIG. 1 is a graph comparing the discharge capacity and life characteristics of lithium-sulfur batteries according to the example of the present invention and the comparative example. DETAILED DESCRIPTION

[0030] Hereinafter, a positive electrode coating material for a lithium secondary battery, a preparation method thereof, and a positive electrode and a lithium secondary battery including the coating material according to the present invention will be described in detail with reference to the accompanying drawings.

[0031] Cathode coating materials

[0032] Figure 1 is the chemical structural formula of the positive electrode coating material for lithium secondary batteries according to an embodiment of the present invention. Figure 1 As shown, the positive electrode coating material for a lithium secondary battery according to the present invention includes graphene oxide whose surface is modified with a cationic functional group.

[0033] The positive electrode coating material for a lithium secondary battery according to the present invention is obtained by grafting a polymer having a cationic functional group on the surface of graphene oxide (GO) and modifying the surface of the graphene oxide with a functional group containing a cation, and because the coating material is coated on the positive electrode active material, the cationic functional group formed on the surface of the coating material inhibits the dissolution of lithium polysulfide, thereby improving the performance of the lithium secondary battery.

[0034] More specifically, the cationic functional groups of the positive electrode coating material for lithium secondary batteries are introduced into the hydroxyl groups present in large quantities on the surface of graphene oxide by atom transfer radical polymerization (ATRP), and because the cationic functional groups are introduced into the surface of graphene oxide, the dispersibility of the positive electrode coating material can be improved.

[0035] In addition, because cationic functional groups are introduced on the surface of graphene oxide, when it is applied to the positive electrode of a lithium-sulfur battery, the dissolution of lithium polysulfide is suppressed, so that the discharge capacity decreases with the cycle compared to the case where it is not applied, and the performance improvement at high current density is particularly significant.

[0036] The present invention is characterized in that the cationic functional group is bonded to graphene oxide in a state of being contained in a hydrocarbon group having 4 to 70 carbon atoms and containing 0 to 4 oxygen atoms, and the bonding to graphene oxide is completed through carbon atoms.

[0037] More specifically, it is characterized in that the hydrocarbon group having 4 to 70 carbon atoms (preferably 40 to 50 carbon atoms) and containing a cationic functional group comprises a (meth)acrylate structural unit grafted with a hydrocarbon group having 2 to 10 carbon atoms and containing a cationic group, and the (meth)acrylate structural unit has a form of bonding to a hydrocarbon structural unit having 1 to 10 carbon atoms, the hydrocarbon structural unit forms a bond with the surface of the graphene oxide, and the hydrocarbon structural unit having 1 to 10 carbon atoms contains 0 to 2 oxygen atoms.

[0038] Here, the (meth)acrylate structural unit may have a form in which 2 to 5 (meth)acrylates are polymerized, and the hydrocarbon structural unit having 1 to 10 carbon atoms that forms a bond with the surface of graphene oxide may include a carbonyl group that is bonded to graphene oxide. In addition, the cationic functional group may include one or more cations selected from the group consisting of nitrogen cations, oxygen cations, and sulfur cations, wherein at least nitrogen cations may be preferably included.

[0039] More specifically, the cationic functional group may be represented by Formula 1 below (ie, when the cationic functional group is a nitrogen cation), and the cationic functional group may further include a halogen anion as a counter ion of the cation included in the cationic functional group, as shown in Formula 1 below.

[0040] [Formula 1]

[0041]

[0042] wherein R1, R2, R3, R4 and R5 are hydrogen or an alkyl group having 1 to 4 carbon atoms,

[0043] X is a halogen group,

[0044] o, p and q are each independently an integer from 0 to 4,

[0045] n is a natural number from 1 to 5.

[0046] (Wavy Line represents the connection bond with graphene oxide).

[0047] On the other hand, as examples of the cationic functional group represented by Formula 1,

[0048]

[0049] Graphene oxide acts as an initiator, allowing a large amount of cationic polymer to be grafted on the surface of graphene oxide, and also serves to improve compatibility with a positive electrode active material when coated on a positive electrode active material such as a sulfur-carbon composite material.

[0050] As described above, the positive electrode coating material for a lithium secondary battery of the present invention is coated on the surface of a positive electrode active material to function as a physical shielding film and is used to suppress volume changes of sulfur particularly during charge and discharge of a lithium sulfur battery.

[0051] Method for preparing positive electrode coating material

[0052] The method for manufacturing a positive electrode coating material for a lithium secondary battery according to the present invention comprises the following steps:

[0053] (a) preparing a surface-modified graphene oxide by reacting a graphene oxide containing at least one selected from a -COOH group and a -OH group on the surface with a hydrocarbon structural unit having 1 to 10 carbon atoms and containing 0 to 2 oxygen atoms, the hydrocarbon structural unit comprising a functional group forming a bond with the -COOH group or the -OH group and a functional group forming a bond with a vinyl group contained in a (meth)acrylate compound; and

[0054] (b) reacting the surface-modified graphene oxide with a (meth)acrylate structural unit grafted with a hydrocarbon group having 2 to 10 carbon atoms and containing a cationic group.

[0055] Figure 2 To show the reaction scheme of the process of synthesizing the cationic monomer grafted on the surface of graphene oxide according to an embodiment of the present invention, Figure 3 To illustrate the reaction scheme of the process of forming subsequent reaction initiation sites on the surface of graphene oxide according to an embodiment of the present invention, Figure 4 In order to show the reaction scheme of the process of grafting the cationic polymer to the subsequent reaction initiation site formed on the surface of graphene oxide according to an embodiment of the present invention. Figures 2 to 4 A method for preparing a positive electrode coating material for a lithium secondary battery is described in more detail.

[0056] In the hydrocarbon structural unit having 1 to 10 carbon atoms and containing 0 to 2 oxygen atoms, which comprises a functional group forming a bond with a -COOH group or a -OH group and a functional group forming a bond with a vinyl group contained in the (meth)acrylate compound in step (a), the functional group forming a bond with the -COOH group or the -OH group may be selected from a carbonyl group substituted with a halogen group, an ether group, an ester group and a carbonate group, and the functional group forming a bond with the vinyl group contained in the (meth)acrylate compound may be selected from a halogen group, an ether group, an ester group and a carbonate group.

[0057] More specifically, the hydrocarbon structural unit having 1 to 10 carbon atoms and containing 0 to 2 oxygen atoms, which comprises a functional group which forms a bond with a -COOH group or a -OH group and a functional group which forms a bond with a vinyl group contained in a (meth)acrylate compound, may have a carbonyl group substituted with a halogen group and a carbon atom substituted with a halogen group, and more specifically, the hydrocarbon structural unit having 1 to 10 carbon atoms and containing 0 to 2 oxygen atoms, which comprises a functional group which forms a bond with a -COOH group or a -OH group and a functional group which forms a bond with a vinyl group contained in a (meth)acrylate compound, may be 2-bromoisobutyryl bromide.

[0058] In addition, in the (meth)acrylate structural unit grafted with a hydrocarbon group having 2 to 10 carbon atoms and containing a cationic group in step (b), the cationic group may include one or more cations selected from the following: nitrogen cations, oxygen cations and sulfur cations, among which at least nitrogen cations may preferably be included.

[0059] In addition, in the (meth) acrylate structural unit grafted with a hydrocarbon group having 2 to 10 carbon atoms and containing a cationic group, the hydrocarbon group having 2 to 10 carbon atoms containing a cationic group may be a compound represented by the following formula 2.

[0060] [Formula 2]

[0061]

[0062] wherein R4 and R5 are hydrogen or an alkyl group having 1 to 4 carbon atoms,

[0063] X is a halogen group,

[0064] p and q are each independently an integer from 0 to 4.

[0065] In addition, the reaction of step (b) may include a polymerization reaction, and the polymerization reaction may specifically be an atom transfer radical polymerization (ATRP) reaction. In addition, the reaction of step (b) may be carried out at a temperature of 50° C. to 90° C., preferably 60° C. to 80° C., for 24 to 72 hours, preferably 36 to 60 hours, but is not limited thereto.

[0066] In addition, in the atom transfer radical polymerization reaction of step (b), a catalyst such as CuBr / PMDETA ligand commonly used during atom transfer radical polymerization can be used.

[0067] Through the atom transfer radical polymerization reaction of step (b), cationic functional groups are introduced on the surface of graphene oxide, and the dispersibility of the positive electrode coating material can be improved by introducing cationic functional groups on the surface of graphene, and finally, by being applied to the positive electrode of a lithium-sulfur battery, the dissolution of lithium polysulfide can be suppressed.

[0068] On the other hand, after step (b), if necessary, a step of reacting the reaction product finally prepared in step (b) with a lithium salt may be further performed, and for example, by reacting the positive electrode coating material with LiTFSI in an aqueous phase, TFSI may be used. - Replace (or exchange) the halogen anion.

[0069] In addition, in step (a), the mass ratio of the hydrocarbon structural unit to the graphene oxide can be 0.7 to 1.3:1, preferably about 1:1, the hydrocarbon structural unit has 1 to 10 carbon atoms and contains 0 to 2 oxygen atoms, the hydrocarbon structural unit contains a functional group that forms a bond with a -COOH group or an -OH group and a functional group that forms a bond with a vinyl group contained in a (meth)acrylate compound, and the graphene oxide contains at least one selected from -COOH groups and -OH groups on its surface. In addition, the mass ratio of the (meth)acrylate structural unit grafted with a hydrocarbon group having 2 to 10 carbon atoms and containing a cationic group to the surface-modified graphene oxide in step (b) can be 1 to 10:1, preferably 5 to 10:1, and more preferably 6 to 8:1.

[0070] Positive electrode for lithium secondary battery

[0071] The positive electrode for a lithium secondary battery according to the present invention includes a positive electrode active material and a positive electrode coating material coated on the surface of the positive electrode active material.

[0072] That is, the positive electrode coating material is the positive electrode coating material for the lithium secondary battery, and the coating amount thereof may be 0.2 to 2 parts by weight, preferably 0.75 to 1.5 parts by weight, and more preferably 0.9 to 1.1 parts by weight relative to 100 parts by weight of the positive electrode active material. If the content of the positive electrode coating material coated on the surface of the positive electrode active material is not within the above range, the advantages obtained by using the positive electrode coating material may be less or no.

[0073] Thus, if a positive electrode coating material containing graphene oxide surface-modified with cation-containing functional groups is coated on a positive electrode active material, the compatibility between the coating and the positive electrode active material (especially the sulfur-carbon composite material) is improved, and the volume change of sulfur during the charging and discharging process of the lithium-sulfur battery can be suppressed, and most importantly, the coating material of the present invention plays a role in capturing and adsorbing lithium polysulfide, so that the lithium polysulfide generated at the positive electrode during the operation of the battery will not dissolve into the liquid electrolyte, thereby improving the battery performance.

[0074] The positive electrode active material preferably contains sulfur (S) atoms, and more preferably may be a sulfur-carbon composite material. Considering that the electrical conductivity of sulfur is about 5.0×10 -14S / cm and thus is close to a non-conductor, so it is not easy for electrochemical reactions to occur on the electrode, and considering that the overvoltage is very large, the actual discharge capacity and voltage are much lower than the theoretical values, and a conductive carbon material is used together (i.e., a structure in which sulfur is loaded in the pores of the carbon material).

[0075] The sulfur contained in the sulfur-carbon composite material may be at least one selected from the following: inorganic sulfur (S8), Li2Sn (n≥1), organic sulfur compounds and carbon-sulfur polymers [(C2S x ) n : x = 2.5 to 50, n ≥ 2], wherein inorganic sulfur (S8) can be preferably used.

[0076] In addition, the carbon material constituting the sulfur-carbon composite material can be used without particular limitation, as long as it has a porous structure or a high specific surface area and is commonly used in the art. For example, the carbon material having a porous structure can be, but is not limited to, at least one selected from the following: graphite; graphene; carbon black such as Deco black, acetylene black, Ketjen black, channel black, furnace black, lamp black and thermal black; carbon nanotubes (CNT) such as single-walled carbon nanotubes (SWCNT) and multi-walled carbon nanotubes (MWCNT); carbon fibers such as graphite nanofibers (GNF), carbon nanofibers (CNF) and activated carbon fibers (ACF); and activated carbon, and its shape can be used without limitation, as long as it is in the form of balls, rods, needles, plates, tubes or blocks and is commonly used in lithium secondary batteries.

[0077] The sulfur-carbon composite material may have a particle size of 10 μm to 50 μm. If the particle size of the sulfur-carbon composite material is less than 10 μm, there is a problem that the resistance between particles increases and overvoltage is generated in the electrode of the lithium-sulfur battery. If the particle size exceeds 50 μm, the surface area per unit weight decreases, and thus the wetted area with the electrolyte and the reaction site with lithium ions in the electrode decrease, and the amount of electron transfer relative to the size of the composite material decreases, thereby delaying the reaction, and as a result, the discharge capacity of the battery decreases.

[0078] In the positive electrode, the positive electrode coating material is preferably coated on the entire surface of the positive electrode active material, and a cationic functional group is formed in each graphene oxide of the positive electrode coating material. Therefore, it can be said that because a large number of cationic functional groups are densely distributed on the entire surface of the positive electrode active material, the ability to suppress the dissolution of lithium polysulfide is maximized.

[0079] On the other hand, the positive electrode manufactured by the method for manufacturing the positive electrode can also include a binder and a conductive material. The binder is a component that helps the combination between the positive electrode active material and the conductive material and the combination of the current collector, and for example, it can be but is not limited to at least one selected from the following: polyvinylidene fluoride (PVdF), polyvinylidene fluoride-polyhexafluoropropylene copolymer (PVdF / HFP), polyvinyl acetate, polyvinyl alcohol, polyvinyl ether, polyethylene, polyethylene oxide, alkylated polyethylene oxide, polypropylene, polymethyl (meth) acrylate, polyethyl (meth) acrylate, polytetrafluoroethylene (PTFE), polyvinyl chloride, polyacrylonitrile, polyvinyl pyridine, polyvinyl pyrrolidone, styrene-butadiene rubber, acrylonitrile-butadiene rubber, ethylene propylene diene monomer (EPDM) rubber, sulfonated EPDM rubber, styrene-butene rubber, fluororubber, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose and mixtures thereof.

[0080] The amount of the binder added is generally 1 to 50 parts by weight, preferably 3 to 15 parts by weight, relative to 100 parts by weight of the total weight of the positive electrode material containing the positive electrode active material. If the content of the binder is less than 1 part by weight, the adhesion strength between the positive electrode active material and the collector may be insufficient. If the content of the binder exceeds 50 parts by weight, the adhesion strength is improved, but the content of the positive electrode active material may be reduced accordingly, thereby reducing the capacity of the battery.

[0081] In addition, there is no particular restriction on the conductive material, as long as it does not cause side reactions in the internal environment of the lithium secondary battery and has excellent conductivity without causing chemical changes in the battery. The conductive material can generally be graphite or conductive carbon, and can be, for example, but not limited to, one selected from the following: graphite such as natural graphite or artificial graphite; carbon black materials such as carbon black, acetylene black, Ketjen black, Deco black, thermal black, channel black, furnace black, lamp black and summer black; carbon-based materials with a crystal structure of graphene or graphite; conductive fibers such as carbon fibers and metal fibers; carbon fluoride; metal powders such as aluminum powder and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive oxides such as titanium oxide; conductive polymers such as polyphenylene derivatives; and mixtures of two or more thereof.

[0082] Relative to 100 parts by weight of the total weight of the positive electrode material containing the positive electrode active material, the amount of conductive material added is generally 0.5 to 50 parts by weight, preferably 1 to 30 parts by weight. If the content of the conductive material is too low, that is, if it is less than 0.5 parts by weight, it is difficult to obtain the effect of improving conductivity, or the electrochemical characteristics of the battery may deteriorate. If the content of the conductive material exceeds 50 parts by weight, that is, if it is too much, the amount of positive electrode active material is relatively small, thereby the capacity and energy density may be reduced. There is no particular restriction on the method of incorporating the conductive material into the positive electrode material, and conventional methods known in the relevant art can be used, such as coating on the positive electrode active material. In addition, if necessary, adding a second coating having conductivity to the positive electrode active material can replace the addition of the conductive material as described above.

[0083] A filler may be selectively added to the positive electrode of the present invention as a component for suppressing the expansion of the positive electrode. There is no particular limitation on such a filler as long as it can suppress the expansion of the electrode without causing chemical changes in the battery, and examples thereof may include: olefin polymers such as polyethylene and polypropylene; and fiber materials such as glass fiber and carbon fiber.

[0084] The positive electrode current collector may be, but is not limited to, platinum (Pt), gold (Au), palladium (Pd), iridium (Ir), silver (Ag), ruthenium (Ru), nickel (Ni), stainless steel (STS), aluminum (Al), molybdenum (Mo), chromium (Cr), carbon (C), titanium (Ti), tungsten (W), ITO (In-doped SnO2), FTO (F-doped SnO2) or their alloys; or aluminum (Al) or stainless steel with surface treatment of carbon (C), nickel (Ni), titanium (Ti) or silver (Ag). The shape of the positive electrode current collector may be in the form of foil, film, sheet, stamping form, porous body, foam, etc.

[0085] Lithium secondary battery

[0086] In addition, the present invention provides a lithium secondary battery, which includes a positive electrode for a lithium secondary battery, a lithium metal negative electrode, an electrolyte provided between the positive electrode and the negative electrode, and a separator, and the lithium secondary battery is preferably a lithium sulfur battery.

[0087] Typically, a lithium secondary battery is composed of a positive electrode, the positive electrode being composed of a positive electrode material and a current collector; a negative electrode, the negative electrode being composed of a negative electrode material and a current collector; and a separator, the separator blocking the electrical contact between the positive electrode and the negative electrode and allowing lithium ions to move, and the lithium secondary battery comprising an electrolyte that conducts lithium ions by immersing therein. The negative electrode can be manufactured according to conventional methods known in the art. For example, the negative electrode is prepared by dispersing and mixing a negative electrode active material, a conductive material, a binder, and a filler if necessary, etc. in a dispersion medium (solvent) to form a slurry, and the slurry can be coated on the negative electrode collector, followed by drying and rolling.

[0088] The negative electrode active material may be lithium metal or a lithium alloy (e.g., an alloy of lithium and a metal such as aluminum, zinc, bismuth, cadmium, antimony, silicon, lead, tin, gallium, or indium). The negative electrode current collector may be, but is not limited to, platinum (Pt), gold (Au), palladium (Pd), iridium (Ir), silver (Ag), ruthenium (Ru), nickel (Ni), stainless steel (STS), copper (Cu), molybdenum (Mo), chromium (Cr), carbon (C), titanium (Ti), tungsten (W), ITO (In-doped SnO2), FTO (F-doped SnO2), or an alloy thereof; or copper (Cu) or stainless steel whose surface is treated with carbon (C), nickel (Ni), titanium (Ti), or silver (Ag). The negative electrode current collector may be in the form of a foil, a film, a sheet, a stamped form, a porous body, a foam, or the like.

[0089] The separator is arranged between the positive electrode and the negative electrode to prevent a short circuit between them and to serve as a path for lithium ions. As a separator, olefin polymers such as polyethylene and polypropylene, glass fiber, etc. can be used in the form of sheets, multilayers, microporous films, woven fabrics, non-woven fabrics, etc., but the present invention is not limited thereto. On the other hand, if a solid electrolyte such as a polymer (e.g., an organic solid electrolyte, an inorganic solid electrolyte, etc.) is used as an electrolyte, the solid electrolyte can also serve as a separator. Specifically, an insulating film with high ion permeability and mechanical strength is used. The pore size of the separator is generally in the range of 0.01 μm to 10 μm, and the thickness can generally be in the range of 5 μm to 300 μm.

[0090] As the electrolyte of the non-aqueous electrolyte (non-aqueous organic solvent), carbonate, ester, ether or ketone may be used alone or in combination of two or more thereof, but is not limited thereto. For example, aprotic organic solvents such as dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, γ-butyrolactone, n-methyl acetate, n-ethyl acetate, n-propyl acetate, triester phosphate, dibutyl ether, N-methyl-2-pyrrolidone, 1,2-dimethoxyethane, tetrahydrofuran, tetrahydrofuran derivatives such as 2-methyltetrahydrofuran, dimethyl sulfoxide, formamide, dimethylformamide, dioxolane and its derivatives, acetonitrile, nitromethane, methyl formate, methyl acetate, trimethoxymethane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, methyl propionate, ethyl propionate, etc. can be used, but are not limited thereto.

[0091] A lithium salt may be added to the electrolyte (so-called non-aqueous electrolyte containing a lithium salt). The lithium salt may include, but is not limited to, substances known to be advantageously soluble in non-aqueous electrolytes, such as LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiPF3(CF2CF3)3, LiAlCl4, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylate, lithium tetraphenylborate or lithium imide, etc. In order to improve the charge-discharge characteristics, flame retardancy, etc., the (non-aqueous) electrolyte may also contain pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, (condensed) glycol dimethyl ether, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted Oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. If necessary, a halogen-containing solvent such as carbon tetrachloride and trifluoroethylene may be added to impart nonflammability, and carbon dioxide gas may be added to improve high temperature storage characteristics.

[0092] The lithium secondary battery of the present invention can be manufactured by conventional methods in the art. For example, a lithium secondary battery can be manufactured by inserting a porous separator between the positive electrode and the negative electrode and introducing a non-aqueous electrolyte. The lithium secondary battery according to the present invention can be applied not only to battery pack batteries used as power sources for small devices, but is also particularly suitable for use as a unit cell of a battery module as a power source for medium and large devices. In this regard, the present invention also provides a battery module in which at least two lithium secondary batteries are electrically connected (in series or in parallel). Needless to say, the number of lithium secondary batteries contained in the battery module can be variously adjusted in consideration of the purpose and capacity of the battery module.

[0093] In addition, the present invention provides a battery pack in which the battery modules are electrically connected according to conventional techniques in the art. The battery modules and the battery pack can be used as a power source for at least one medium or large device selected from the following: power tools; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs); electric trucks; electric commercial vehicles; or power storage systems, but the present invention is not limited thereto.

[0094] Example

[0095] Hereinafter, preferred embodiments of the present invention will be described to help understand the present invention. However, it will be apparent to those skilled in the art that the following examples are only used to illustrate the present invention, and that various changes and variants can be accomplished within the scope and spirit of the present invention, and such changes and variants are within the scope of the appended claims.

[0096] [Example 1] Preparation of positive electrode coating material for lithium secondary battery

[0097] First, 2-(dimethylamino)ethyl methacrylate (Sigma-aldrich) was reacted with 1-bromobutane (Sigma-aldrich) at 45° C. for 18 hours to obtain quaternized 2-(dimethylamino)ethyl methacrylate (ie, cationic monomer).

[0098] Then, graphene oxide (Sigma-aldrich) was reacted with 2-bromoisobutyryl bromide (Sigma-aldrich) and triethylamine (Sigma-aldrich) to form bromine initiation sites on the surface of graphene oxide. Then, it was subjected to an atom transfer radical polymerization reaction with the cationic monomer prepared above at a mass ratio of 1:7 (reaction temperature: 70°C, reaction time: 48 hours, catalyst: CuBr / PMDETA ligand) to prepare graphene oxide (i.e., a positive electrode coating material) grafted with a cationic polymer on its surface (in addition, the prepared positive electrode coating material was reacted with LiTFSI in an aqueous phase to make the bromide anion (Br - ) and TFSI - exchange).

[0099] [Experimental Example 1] Chemical structure analysis of cationic monomer (QDMAEMA)

[0100] conduct 1 H NMR analysis was performed to confirm whether the cationic monomer prepared in Example 1 was normally synthesized. Figure 5 To show the cationic monomer (QDMAEMA) prepared according to the embodiment of the present invention 1 Graph of the H NMR analysis results.

[0101] As described above, the cationic monomer prepared in Example 1 was synthesized normally. 1 The results of HNMR analysis, such as Figure 5 As shown, the chemical structures of the expected cationic monomers are shown, thereby confirming that there is no abnormality in the synthesis of the cationic monomers.

[0102] [Experimental Example 2] Chemical structure analysis of positive electrode coating material (modified graphene oxide)

[0103] For the positive electrode coating material prepared in Example 1, in order to examine whether the cationic polymer (PQDMAEMA) was normally grafted on the surface of graphene oxide, TGA analysis, FT-IR analysis, XRD analysis and UV-Vis analysis were performed. Figure 6 This is a graph showing the TGA analysis results of the positive electrode coating material prepared according to an embodiment of the present invention. Figure 7 This is a diagram showing the FT-IR analysis results of the positive electrode coating material prepared according to an embodiment of the present invention. Figure 8 is a graph showing the XRD analysis results of the positive electrode coating material prepared according to an embodiment of the present invention, and Fig. 9 FIG. 5 is a graph showing the UV-Vis analysis results of the positive electrode coating material prepared according to an embodiment of the present invention.

[0104] As described above, for the positive electrode coating material prepared in Example 1, as a result of TGA analysis, FT-IR analysis, XRD analysis and UV-Vis analysis performed to confirm whether the cationic polymer is normally grafted on the surface of graphene oxide, Figure 6 It was confirmed that the cationic polymer (PQDMAEMA) of the positive electrode coating material was a linear polymer polymerized using only the cationic monomer (QDMAEMA) as an AIBN initiator (initiator for radical initiation).

[0105] In addition, through the FT-IR analysis Figure 7 It was confirmed that the characteristic peak of the cationic polymer (PQDMAEMA) contained in the positive electrode coating material was present; Figure 8 It was confirmed that after modification, the crystal peak of graphene oxide (GO) disappeared; and by UV-Vis analysis Fig. 9 It was confirmed that the positions of the characteristic peaks (234 nm, 300 nm) of graphene oxide changed. In summary, for the positive electrode coating material prepared in Example 1, it can be seen that the cationic polymer (PQDMAEMA) is normally grafted onto the surface of graphene oxide.

[0106] [Example 2] Preparation of positive electrode for lithium secondary battery

[0107] 0.5 mg (i.e., the content of the coating material in the total weight of the positive electrode is set to 0.25 wt% (FGO 0.25)) of the positive electrode coating material (FGO (OH) -TFSI) prepared in Example 1 was tip-sonicated for 30 minutes and dispersed in acetone, and then mixed with a sulfur-carbon composite material (prepared by mixing elemental sulfur (sulfur) and super P (carbon) in a weight ratio of 7:3, grinding with a mortar, and heat-treating at 155°C for 30 minutes) and stirred for 15 hours. Then, the stirred solution was dried at 50°C to remove acetone.

[0108] Subsequently, the sulfur-carbon composite material coated with the positive electrode coating material (FGO(OH)-TFSI), the binder (polyacrylic acid) and the conductive material (carbon black) were mixed in a weight ratio of 85:10:5, and then 0.5 wt% of PVA dispersant was added thereto, and the concentration was adjusted so that the solid content in the aqueous phase was 18 wt%, and the obtained product was mixed with a thinky mixer to prepare a positive electrode slurry. Finally, the prepared positive electrode slurry was coated on an aluminum foil with a 400 μm scraper and dried at 50 ° C for about 14 hours to prepare a positive electrode for a lithium secondary battery.

[0109] [Example 3] Preparation of positive electrode for lithium secondary battery

[0110] A positive electrode for a lithium secondary battery was prepared in the same manner as in Example 2, except that the amount of the positive electrode coating material (FGO(OH)-TFSI) prepared in Example 1 was changed from 0.5 mg to 1 mg (i.e., the content of the coating material in the total weight of the positive electrode was set to 0.5 wt % (FGO 0.5)).

[0111] [Example 4] Preparation of positive electrode for lithium secondary battery

[0112] A positive electrode for a lithium secondary battery was prepared in the same manner as in Example 2, except that the amount of the positive electrode coating material (FGO(OH)-TFSI) prepared in Example 1 was changed from 0.5 mg to 1.5 mg (i.e., the content of the coating material in the total weight of the positive electrode was set to 0.75 wt % (FGO 0.75)).

[0113] [Example 5] Preparation of positive electrode for lithium secondary battery

[0114] A positive electrode for a lithium secondary battery was prepared in the same manner as in Example 2, except that the amount of the positive electrode coating material (FGO(OH)-TFSI) prepared in Example 1 was changed from 0.5 mg to 2 mg (i.e., the content of the coating material in the total weight of the positive electrode was set to 1 wt % (FGO 1)).

[0115] [Example 6] Preparation of positive electrode for lithium secondary battery

[0116] A positive electrode for a lithium secondary battery was prepared in the same manner as in Example 2, except that the amount of the positive electrode coating material (FGO(OH)-TFSI) prepared in Example 1 was changed from 0.5 mg to 3 mg (i.e., the content of the coating material in the total weight of the positive electrode was set to 1.5 wt % (FGO 1.5)).

[0117] [Comparative Example 1] Preparation of positive electrode for lithium secondary battery

[0118] The sulfur-carbon composite material (prepared by mixing elemental sulfur (sulfur) and super P (carbon) in a weight ratio of 7:3, grinding with a mortar, and heat treating at 155°C for 30 minutes), a binder (polyacrylic acid) and a conductive material (carbon black) were mixed in a weight ratio of 85:10:5, and then 0.5 wt% of PVA dispersant was added thereto, and the concentration was adjusted so that the solid content in the aqueous phase was 18 wt%, and the obtained product was mixed with a thinky mixer to prepare a positive electrode slurry. Finally, the prepared positive electrode slurry was coated on an aluminum foil with a 400 μm scraper and dried at 50°C for about 14 hours to prepare a positive electrode for a lithium secondary battery.

[0119] [Experimental Example 3] Composition Analysis of Sulfur-Carbon Composite Material Coated with Positive Electrode Coating Material

[0120] For the positive electrode for lithium secondary battery prepared in Example 3, TEM analysis and EDS analysis were performed to confirm whether the positive electrode coating material (FGO(OH)-TFSI) was normally coated on the surface of the sulfur-carbon composite material. Fig.10 : SEM image (corresponding to the upper left figure) and EDS image of the “sulfur-carbon composite material coated with a positive electrode coating material” prepared according to an embodiment of the present invention.

[0121] As described above, for the positive electrode for lithium secondary battery prepared in Example 3, as a result of TEM analysis and EDS analysis in order to confirm whether the positive electrode coating material (FGO(OH)-TFSI) is normally coated on the surface of the sulfur-carbon composite material, elements F and N are detected, such as Fig.10 This confirmed that the surface of the sulfur-carbon composite material was normally coated with the positive electrode coating material (FGO(OH)-TFSI).

[0122] on the other hand, Fig.11 The TGA analysis diagram (left) and TEM analysis diagram (right) of the sulfur-carbon composite material coated with the positive electrode coating material (FGO(OH)-TFSI) prepared according to the embodiment of the present invention. Fig.11 As can be seen from the left figure, it was confirmed that the content of sulfur in the sulfur-carbon composite material was 70 weight %, and it was confirmed that the sulfur content was well maintained even as prepared in the present invention.

[0123] [Examples 7 to 11, Comparative Example 2] Production of lithium-sulfur batteries

[0124] The positive electrodes prepared in Examples 2 to 6 and Comparative Example 1 were placed in a manner facing the lithium metal negative electrode, and then a Celgard separator was inserted between the positive electrode and the negative electrode. Then, an electrolyte prepared by dissolving LiTFSI and LiNO3 at concentrations of 1 M and 0.2 M, respectively, in a DOL / DME solvent was injected into the shell to prepare a coin cell type lithium sulfur battery.

[0125] [Experimental Example 4] Evaluation of discharge capacity and life characteristics of lithium secondary batteries

[0126] For the lithium-sulfur batteries manufactured in Examples 7 to 11 and Comparative Example 2, discharge capacity and life characteristics were evaluated by setting the current density to 0.2C to 2C rates. Figures 12 to 14 FIG. 1 is a graph comparing the discharge capacity and life characteristics of lithium-sulfur batteries according to the example of the present invention and the comparative example.

[0127] As a result of evaluating the discharge capacity and life characteristics of the lithium-sulfur batteries manufactured in Examples 7 to 11 and Comparative Example 2 as described above, Fig.12 As shown, it was confirmed that the lithium-sulfur battery (corresponding to Fig.12 Compared with the "uncoated" in the embodiment 7 to 11, the lithium sulfur batteries of Examples 7 to 11, in which the positive electrode coating material (FGO(OH)-TFSI) is coated on the positive electrode active material, have improved battery performance. Figures 13 to 14 It can be seen that the lithium-sulfur battery of the present invention exhibits significantly improved battery performance, especially at high current density.

Claims

1. A positive electrode coating material for a lithium secondary battery, comprising graphene oxide surface-modified with a cationic functional group, wherein the cationic functional group is bonded to graphene oxide in a state contained in a hydrocarbon group having 4 to 70 carbon atoms and containing 0 to 4 oxygen atoms, and the bonding to graphene oxide is accomplished through carbon atoms, wherein the hydrocarbon group having 4 to 70 carbon atoms and containing a cationic functional group comprises a (meth)acrylate structural unit grafted with a hydrocarbon group having 2 to 10 carbon atoms and containing a cationic group, The (meth)acrylate structural unit has a form of bonding to a hydrocarbon structural unit having 1 to 10 carbon atoms, the hydrocarbon structural unit forms a bond with the surface of the graphene oxide, and the hydrocarbon structural unit having 1 to 10 carbon atoms contains 0 to 2 oxygen atoms. 2 . The positive electrode coating material for a lithium secondary battery according to claim 1 , wherein the (meth)acrylate structural unit has a form in which 2 to 5 (meth)acrylates are polymerized. 3 . The positive electrode coating material for a lithium secondary battery according to claim 2 , wherein the hydrocarbon structural unit having 1 to 10 carbon atoms that forms a bond with the surface of the graphene oxide includes a carbonyl group bonded to the graphene oxide. 4 . The positive electrode coating material for a lithium secondary battery according to claim 1 , wherein the cationic functional group comprises at least one cation selected from the group consisting of a nitrogen cation, an oxygen cation, and a sulfur cation.

5. The positive electrode coating material for lithium secondary battery according to claim 1, wherein the cationic functional group is represented by the following formula 1: [Formula 1] wherein R1, R2, R3, R4 and R5 are hydrogen or an alkyl group having 1 to 4 carbon atoms, X is a halogen group, o, p and q are each independently an integer from 0 to 4, n is a natural number from 1 to 5. 6 . The positive electrode coating material for a lithium secondary battery according to claim 1 , wherein the cationic functional group further contains a halogen anion as a counter ion of the cation contained in the cationic functional group.

7. A method for preparing the positive electrode coating material for a lithium secondary battery according to claim 1, the method comprising the following steps: (a) preparing a surface-modified graphene oxide by reacting graphene oxide containing one or more of a -COOH group and a -OH group on the surface with a hydrocarbon structural unit having 1 to 10 carbon atoms and containing 0 to 2 oxygen atoms, which contains a functional group forming a bond with the -COOH group or the -OH group and a functional group forming a bond with a vinyl group contained in a (meth)acrylate compound; and (b) reacting the surface-modified graphene oxide with a (meth)acrylate structural unit grafted with a hydrocarbon group having 2 to 10 carbon atoms and containing a cationic group.

8. The method for preparing a positive electrode coating material for a lithium secondary battery according to claim 7, wherein in the hydrocarbon structural unit having 1 to 10 carbon atoms and containing 0 to 2 oxygen atoms, which contains a functional group forming a bond with a -COOH group or a -OH group and a functional group forming a bond with a vinyl group contained in a (meth)acrylate compound, The functional group forming a bond with the -COOH group or the -OH group is selected from the group consisting of a carbonyl group substituted with a halogen group, an ether group, an ester group and a carbonate group, and The functional group forming a bond with the vinyl group contained in the (meth)acrylate compound is selected from the group consisting of a halogen group, an ether group, an ester group and a carbonate group.

9. The method for preparing a positive electrode coating material for a lithium secondary battery according to claim 7, wherein the hydrocarbon structural unit having 1 to 10 carbon atoms and containing 0 to 2 oxygen atoms, which contains a functional group forming a bond with a -COOH group or a -OH group and a functional group forming a bond with a vinyl group contained in a (meth)acrylate compound, has a carbonyl group substituted with a halogen group and a carbon atom substituted with a halogen group.

10. The method for preparing a positive electrode coating material for a lithium secondary battery according to claim 7, wherein the hydrocarbon structural unit having 1 to 10 carbon atoms and containing 0 to 2 oxygen atoms, which contains a functional group that forms a bond with a -COOH group or a -OH group and a functional group that forms a bond with a vinyl group contained in a (meth)acrylate compound, is 2-bromoisobutyryl bromide.

11. The method for preparing a positive electrode coating material for a lithium secondary battery according to claim 7, wherein in the (meth)acrylate structural unit grafted with a hydrocarbon group having 2 to 10 carbon atoms and containing a cationic group, the cationic group contains at least one cation selected from the following: a nitrogen cation, an oxygen cation and a sulfur cation.

12. The method for preparing a positive electrode coating material for a lithium secondary battery according to claim 11, wherein in the (meth)acrylate structural unit grafted with a hydrocarbon group having 2 to 10 carbon atoms and containing a cationic group, the hydrocarbon group having 2 to 10 carbon atoms and containing a cationic group is a compound represented by the following formula 2: [Formula 2] wherein R4 and R5 are hydrogen or an alkyl group having 1 to 4 carbon atoms, X is a halogen group, p and q are each independently an integer from 0 to 4. 13 . The method for preparing a positive electrode coating material for a lithium secondary battery according to claim 7 , wherein the reaction of step (b) comprises a polymerization reaction.

14. The method for preparing a positive electrode coating material for a lithium secondary battery according to claim 7, wherein the mass ratio of the hydrocarbon structural unit having 1 to 10 carbon atoms and containing 0 to 2 oxygen atoms, which contains a functional group forming a bond with a -COOH group or a -OH group and a functional group forming a bond with a vinyl group contained in a (meth)acrylate compound, to the graphene oxide containing one or more of -COOH groups and -OH groups on the surface in step (a) is 0.7 to 1.3:1, and The mass ratio of the (meth)acrylate structural unit grafted with a hydrocarbon group having 2 to 10 carbon atoms and containing a cationic group to the surface-modified graphene oxide in the step (b) is 1 to 10:

1. 15 . The method for preparing a positive electrode coating material for a lithium secondary battery according to claim 7 , wherein after the step (b), a step of reacting the reaction product finally prepared in the step (b) with a lithium salt is further performed.

16. A positive electrode for a lithium secondary battery, the positive electrode for a lithium secondary battery comprising: positive electrode active material; and The positive electrode coating material according to claim 1, wherein the positive electrode coating material is coated on the surface of the positive electrode active material. 17 . The positive electrode for a lithium secondary battery according to claim 16 , wherein the positive electrode active material is a sulfur-carbon composite material. 18 . The positive electrode for a lithium secondary battery according to claim 16 , wherein the coating amount of the positive electrode coating material is 0.2 parts by weight to 2 parts by weight relative to 100 parts by weight of the positive electrode active material.

19. A lithium secondary battery, comprising: The positive electrode for a lithium secondary battery according to claim 16; Lithium metal anode; An electrolyte disposed between the positive electrode and the negative electrode; and Diaphragm. 20 . The lithium secondary battery according to claim 19 , wherein the lithium secondary battery is a lithium sulfur battery.

Citation Information

Patent Citations

  • Non-Slip Patch for Dogs

    KR1020200099787A

  • Lithium sulfur battery based on modification of graphene oxide thin film

    CN105047982A

  • A mitochondrial-targeted nanophotosensitive immunomodulatory compound drug, its preparation method and application

    CN107158405B