Permanent ferrite rotor
Through the uniform mixing of modified polyphenylene sulfide and permanent magnet ferrite magnetic powder, the problem of uneven mixing of toughener agents in ferrite injection molded rotors is solved, which significantly improves mechanical strength and toughness, and achieves better performance improvement .
Patent Information
- Application Number
- CN202210225389.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-03-09
AI Technical Summary
The existing ferrite injection molded rotors have problems with uneven mixing of toughening enhancers, resulting in insufficient mechanical strength and toughness.
Modified polyphenylene sulfide and permanent magnet ferrite powder are used to form modified polyphenylene sulfide through the combination of polyurethane elastomer, reinforcement, toughening agent and coupling agent, and are manufactured through a screw extruder. Particles ensure uniform distribution of components and improve the mechanical strength and toughness of the molded rotor.
The mechanical strength, toughness and high temperature resistance of the molded rotor are significantly improved, ensuring the uniformity of component distribution and performance improvement.
Smart Images

Figure BDA0003539011940000031 
Figure BDA0003539011940000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of motors, and in particular to a permanent magnet ferrite rotor. Background Art
[0002] For motor rotors, the more popular process is injection molding. Usually, magnetic powder is uniformly mixed with binders such as nylon and polyphenylene sulfide, granulated and injected into a mold to form a rotor. It has the advantages of low cost and simple preparation process, but also has disadvantages such as poor mechanical strength and easy cracking. A ferrite injection molding scheme is disclosed in the authorized invention patent document with domestic authorization announcement number CN111210964B, which mixes magnetic powder with polyphenylene sulfide, coupling agent, reinforcing and toughening agent to form ferrite materials, and then can be injection molded into rotors and other devices. After testing, the rotor under this scheme has multiple properties such as high mechanical strength and not easy to crack. The disadvantage is that the mixing of toughening and strengthening agents occurs unevenly, which is easy to affect the performance of the molded magnet and needs to be improved. Summary of the invention
[0003] To solve at least one of the above technical defects, the present invention provides the following technical solutions:
[0004] The present application document discloses a permanent ferrite rotor, which is injection molded. The rotor comprises the following components by mass:
[0005] 80-88 parts of permanent ferrite magnetic powder;
[0006] Modified polyphenylene sulfide, 10-15 parts, 80-85 parts of polyphenylene sulfide, 10-15 parts of polyurethane elastomer, 4-6 parts of reinforcing agent, 5-8 parts of toughening agent, 0.2-0.4 parts of lubricant, 0.1-0.3 parts of coupling agent are mixed and melted to form modified polyphenylene sulfide, and the melt viscosity is 30-45 Pa.S;
[0007] Coupling agent 0.2-0.5 parts;
[0008] Dispersant 0.02-0.05 parts.
[0009] In this scheme, polyurethane elastomer, reinforcing agent, toughening agent, coupling agent, etc. are mixed with polyphenylene sulfide for modification, and the prepared modified polyphenylene sulfide is mixed with magnetic powder for injection molding of the rotor. The reinforcing agents, toughening agents, etc. are evenly distributed. After testing, the rotor has better mechanical strength, toughness, high temperature resistance and other properties.
[0010] Furthermore, the reinforcing agent is a mixture of glass fiber, calcium stearate and barium stearate, wherein the glass fiber has a length of 2-4 mm and a diameter of 7-12 μm. When the glass fiber, calcium stearate, barium stearate and the like are mixed in a predetermined proportion, the modification effect on polyphenylene sulfide is better and the performance of the molded rotor is greatly increased.
[0011] Furthermore, the mass ratio of glass fiber, calcium stearate and barium stearate in the reinforcing agent is 10-8:1:1.
[0012] Furthermore, the toughening agent is a terpolymer of ethylene-methyl acrylate-glycidyl methacrylate, and the toughening modification performed with the terpolymer has a more excellent effect after testing.
[0013] Furthermore, the coupling agent is KH550, KH560 or KH792.
[0014] Furthermore, in the preparation of the modified polyphenylene sulfide, polyphenylene sulfide, polyurethane elastomer, reinforcing agent, toughening agent, lubricant and coupling agent are mixed and granulated by a screw extruder, and the temperature ranges of each section of the screw extruder are: zone 1 220-235°C, zone 2 235-270°C, zone 3 270-310°C, zone 4 310-325°C, zone 5 310-325°C, zone 6 310-325°C, zone 7 310-325°C, zone 8 310-325°C, zone 9 310-325°C, zone 10 310-325°C.
[0015] Furthermore, during mixing, polyphenylene sulfide and polyurethane elastomer are first mixed, and then coupling agent, lubricant, reinforcing agent and toughening agent are added in sequence, which helps to evenly distribute the material components.
[0016] Further, the injection molding of the rotor includes:
[0017] The step of mixing permanent ferrite magnetic powder with a coupling agent and a dispersant;
[0018] The step of mixing the modified polyphenylene sulfide, the dispersant and the permanent ferrite magnetic powder mixture and extruding and granulating the mixture;
[0019] The step of injection molding the prepared particles into a rotor.
[0020] As for the injection molding parameters, conventional ones can be used, such as controlling the temperature at 315-345°C and the pressure at 1600-2100 bar, which is basically consistent with the scheme recorded in the authorization announcement No. CN111210964B.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention mixes modified polyphenylene sulfide with magnetic powder, etc., reduces the components of the mixed material, distributes the materials evenly, and greatly improves the performance of the molded rotor. DETAILED DESCRIPTION
[0023] The present invention will be further described below in conjunction with specific embodiments.
[0024] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments, unless otherwise specified, are conventional methods or conventional process parameters in the art.
[0025] When preparing the following examples, polyphenylene sulfide: melt viscosity (310°C, 1200S -1 ) is 33Pa.S;
[0026] The dispersant is consistent with that used in CN111210964B;
[0027] Permanent ferrite magnetic powder, average particle size (Fischer permeability method) D50 is 1.53μm, Br is 2815Gs and HCj is 28640e measured by rubber refining method, which is basically consistent with that used in CN111210964B;
[0028] The polyurethane elastomer is a homemade type, which is made by reacting polypropylene glycol 2000, toluene diisocyanate, ethylene glycol, propylene glycol, etc. The polyurethane elastomer in the following embodiment is as follows: 20 parts of polypropylene glycol 2000 are taken by mass, and vacuum dehydrated at 100°C for 2 hours with stirring. After cooling, 50 parts of toluene diisocyanate are added, and the reaction is carried out at 70°C for 1 hour. Then 11 parts of ethylene glycol and 11 parts of propylene glycol are added, and the reaction is carried out at 80°C for 10 minutes. After vacuum degassing, the mixture is cured at a curing temperature of 70°C, and the mixture is kept warm for 12 hours. The mixture is heated to 100°C and kept warm for 10 hours. After cooling, the polyurethane elastomer can be obtained.
[0029] The particle size of calcium stearate and barium stearate is 18-25 μm, the length of glass fiber is 2-4 mm, and the diameter is 8-10 μm.
[0030] The toughening agent is a terpolymer of ethylene-methyl acrylate-glycidyl methacrylate, the lubricant is liquid paraffin, and the coupling agent is dissolved in isopropanol in a ratio of 1:10.
[0031] The formula of the rotor in the following examples is shown in the following table:
[0032] Table 1
[0033]
[0034] in
[0035] The preparation of modified polyphenylene sulfide in Example 1 is as follows: polyphenylene sulfide is first mixed with a polyurethane elastomer, and then a coupling agent, a lubricant, a reinforcing agent, and a toughening agent are added in sequence and mixed evenly, and then melt granulated by a screw extruder. The temperature range of each section of the screw extruder is: zone 1 220-235°C, zone 2 235-270°C, zone 3 270-310°C, zone 4 310-325°C, zone 5 310-325°C, zone 6 310-325°C, zone 7 310-325°C, zone 8 310-325°C, zone 9 310-325°C, zone 10 310-325°C.
[0036] 80 parts of polyphenylene sulfide, 10 parts of polyurethane elastomer, 0.1 parts of coupling agent, 0.2 parts of lubricant, 4 parts of reinforcing agent, 5 parts of toughening agent, the mass ratio of glass fiber, calcium stearate and barium stearate in the reinforcing agent is 10:1:1.
[0037] The preparation of modified polyphenylene sulfide in Example 2 is as follows: the preparation method is consistent with that in Example 1, and the component ratios are as follows:
[0038] 83 parts of polyphenylene sulfide, 12 parts of polyurethane elastomer, 0.2 parts of coupling agent, 0.3 parts of lubricant, 5 parts of reinforcing agent, 6 parts of toughening agent, the mass ratio of glass fiber, calcium stearate and barium stearate in the reinforcing agent is 9:1:1.
[0039] The preparation of modified polyphenylene sulfide in Example 3 is as follows: the preparation method is consistent with that in Example 1, and the component ratios are as follows:
[0040] 85 parts of polyphenylene sulfide, 15 parts of polyurethane elastomer, 0.3 parts of coupling agent, 0.4 parts of lubricant, 6 parts of reinforcing agent, 8 parts of toughening agent, the mass ratio of glass fiber, calcium stearate and barium stearate in the reinforcing agent is 8:1:1.
[0041] The preparation of the permanent magnet ferrite rotor in the embodiment is as follows:
[0042] The permanent ferrite magnetic powder, coupling agent and 2 / 3 dispersant are mixed in a powder mixing tank at 100°C for 50 minutes, and the moisture content of the magnetic powder is controlled within 1000ppm.
[0043] Modified polyphenylene sulfide and 1 / 3 dispersant are added and mixed, and the powder is mixed for 30 minutes at 120° C. The moisture content of the mixture is controlled within 300 ppm.
[0044] The final mixture was added into a screw extruder for granulation, and the granulation temperature was controlled at 320°C.
[0045] The pellets are injection molded at 330°C and 1850 bar pressure.
[0046] Can directly mold rotors and dumbbell-shaped splines (convenient for mechanical strength testing).
[0047] A comparative example 1 is set up: compared with Example 1, there is no pre-modified preparation of modified polyphenylene sulfide in this comparative example, and the components for preparing modified polyphenylene sulfide are directly added after the permanent magnet ferrite powder is mixed, and the formula components and other steps are consistent with Example 1.
[0048] The dumbbell-shaped splines injection molded by each embodiment and comparative example were tested. The test conditions were consistent with those in CN111210964B. The test performance data are shown in the following table.
[0049] Table 2
[0050]
[0051] It can be seen from the data in the above table that the process scheme of pre-modifying polyphenylene sulfide and then mixing granulation and injection molding can further improve the mechanical properties of the workpiece.
[0052] The above are only preferred embodiments of the present invention. The protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A permanent ferrite rotor, characterized in that: The rotor is injection molded, and the rotor comprises the following components by mass: 80-88 parts of permanent ferrite magnetic powder; Modified polyphenylene sulfide, 10-15 parts, 80-85 parts of polyphenylene sulfide, 10-15 parts of polyurethane elastomer, 4-6 parts of reinforcing agent, 5-8 parts of toughening agent, 0.2-0.4 parts of lubricant, 0.1-0.3 parts of coupling agent are mixed and melted to form modified polyphenylene sulfide, and the melt viscosity is 30-45 Pa.S; Coupling agent 0.2-0.5 parts; Dispersant 0.02-0.05 parts; The reinforcing agent is a mixture of glass fiber, calcium stearate and barium stearate, wherein the glass fiber has a length of 2-4 mm and a diameter of 7-12 μm; The mass ratio of glass fiber, calcium stearate and barium stearate in the reinforcing agent is 10-8:1:1; The preparation of the modified polyphenylene sulfide comprises mixing polyphenylene sulfide, polyurethane elastomer, reinforcing agent, toughening agent, lubricant and coupling agent and then granulating the mixture by a screw extruder, wherein the temperature ranges of each section of the screw extruder are: 220-235° C. in zone 1, 235-270° C. in zone 2, 270-310° C. in zone 3, 310-325° C. in zone 4, 310-325° C. in zone 5, 310-325° C. in zone 6, 310-325° C. in zone 7, 310-325° C. in zone 8, 310-325° C. in zone 9 and 310-325° C. in zone 10; The toughening agent is ethylene-methyl acrylate-glycidyl methacrylate terpolymer; The injection molding of the rotor comprises: The step of mixing permanent ferrite magnetic powder with a coupling agent and a dispersant; The step of mixing the modified polyphenylene sulfide, the dispersant and the permanent ferrite magnetic powder mixture and extruding and granulating the mixture; The step of injection molding the prepared particles into a rotor.
2. The permanent magnet ferrite rotor according to claim 1, characterized in that: The coupling agent is KH550, KH560 or KH792.
3. The permanent magnet ferrite rotor according to claim 2, characterized in that: During mixing, polyphenylene sulfide and polyurethane elastomer are first mixed, and then coupling agent, lubricant, reinforcing agent and toughening agent are added in sequence.