Anisotropic conductive film and connection structure
By using high-aspect ratio conductive particles in the insulating adhesive layer for non-contact dispersion, the problems of on-resistance deviation in the connection between the glass substrate and the FPC substrate and low capture efficiency in IC chip mounting are solved, achieving efficient conduction and Low short circuit rate.
Patent Information
- Application Number
- CN202210176664.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2016-03-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2036-03-18
AI Technical Summary
When anisotropically conductive connections are made between glass substrates and FPC substrates, an increase in the number of thermocompression bondings will cause the parallel relationship to deviate, resulting in an increase in the on-resistance value, and conductive particle capture efficiency in the installation of electronic components such as IC chips. Low, short circuit is prone to occur.
Conductive particles with an aspect ratio of 1.2 or above are used and dispersed in the insulating adhesive layer in a non-contact manner. The line contact of the conductive particles is used to increase the capture area, reduce the on-resistance deviation, and improve the connection through specific arrangement and fixation methods. reliability.
It effectively reduces the deviation of on-resistance, improves conduction reliability, reduces the incidence of short circuits, improves production efficiency, simplifies connection costs, and reduces the use of insulating spacers.
Smart Images

Figure CN114582545B_ABST
Abstract
Description
[0001] This application is a divisional application of the following invention patent application:
[0002] Invention name: Anisotropic conductive film and connection structure; Application date: March 18, 2016; Application number: 201680014149.2. Technical Field
[0003] The present invention relates to an anisotropic conductive film and a connection structure connected using the anisotropic conductive film. Background Art
[0004] Anisotropic conductive films are widely used for connection between a glass substrate of a display panel such as a liquid crystal panel or an organic EL panel and a flexible printed circuit (FPC) substrate, or for mounting electronic components such as an IC chip on a substrate.
[0005] For example, Figure 6 As shown, most of the FPC substrates 100 connected to the glass substrate of the display panel have a bump group formed by arranging a plurality of slender bumps 110 with a width of 20 μm to 600 μm, a length of 1000 μm to 3000 μm, and a height of 0.1 μm to 500 μm at a pitch of tens of μm to hundreds of μm on one side. When connecting the bump group of such an FPC substrate to the display panel, first, an anisotropic conductive film is temporarily attached to the glass substrate, the FPC substrate is placed thereon from the bump forming surface side, and after adjusting a wide heat pressing tool with a flat pressing surface in parallel to the glass substrate, a heat pressing treatment is performed from the FPC substrate side, thereby enabling anisotropic conductive connection between the FPC substrate and the glass substrate.
[0006] However, if Fig. 7A As shown, even if the heat pressing tool 115 is adjusted to be parallel to the glass substrate 120 and the FPC substrate is heat-pressed through the anisotropic conductive film 1X, if the number of heat-pressing is increased, the parallel relationship between them will deviate (refer to Figure 7B ), and one end of the hot pressing tool 115 contacts, and the on-resistance value of the anisotropic conductive connection portion on the side where one end contacts (the side pressed more strongly) and the side where one end does not contact (the side pressed relatively weakly) tends to be higher than that on the former side, and there is a problem that the on-resistance value is large and deviates due to the bumps. This problem has become more prominent in the recent process of increasing the size of display panels, because the width L of the bump group of the FPC substrate 100 (the distance from the bump at one end of the bump group to the bump at the other end) has reached several meters, and the pressing surface width of the hot pressing tool has become very wide accordingly.
[0007] In order to solve this problem, it is conceivable to adjust the parallelism of the heat pressing tool to the glass substrate each time the heat pressing process is performed, but there is a problem that productivity is significantly reduced. In contrast, it has always been desired to make a spherical insulating spacer (Patent Document 1) with a particle size smaller than that of the conductive particles, which is used to achieve both conductivity in the thickness direction and insulation in the surface direction of the anisotropic conductive film, function as a gap spacer for easing the contact of one end of the heat pressing tool and achieving uniform crushing of the conductive particles.
[0008] On the other hand, when an anisotropic conductive film is used for mounting electronic components such as IC chips, it is desirable to improve the conductive particle capture efficiency or connection reliability in a connection structure using the anisotropic conductive film and reduce the short circuit occurrence rate from the viewpoint of high-density mounting. In contrast, it has been proposed to arrange particle portions (i.e., conductive particle units) in which a plurality of conductive particles are arranged in contact or close to each other in a grid pattern in an insulating adhesive layer of an anisotropic conductive film, and to change the intervals between the conductive particle units according to an electrode pattern (Patent Document 2).
[0009] Prior Art Literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Publication No. 2006-335910
[0012] Patent document 2: Japanese Patent Application Publication No. 2002-519473. Summary of the invention
[0013] Problems to be solved by the invention
[0014] However, when the glass substrate and the FPC substrate are connected anisotropically, even if the anisotropic conductive film includes spherical insulating spacers, the spherical insulating spacers do not make point contact with the wiring or bumps with a wide surface, and thus the pressing force of the heat pressing tool cannot be fully dispersed. Therefore, there is a problem that the on-resistance value of the anisotropic conductive connection portion on the side where one end is not in contact increases to, for example, 4Ω or more.
[0015] In addition, since the conductive particles and insulating spacers are different in material or average particle size, it is not easy to disperse them evenly in the anisotropic conductive film. Also, when the conductive particles and insulating spacers are anisotropically conductively connected, they overlap and there is a concern that the initial conduction characteristics will decrease.
[0016] On the other hand, when electronic components such as IC chips are mounted on a substrate, if the anisotropic conductive film described in Patent Document 2 is used, a plurality of spherical conductive particles with high mobility are filled into the mold to form a conductive particle unit, so the filling rate of the conductive particles in the mold or the position of the conductive particles in the mold will be unstable.
[0017] In addition, regarding spherical conductive particles, when they are sandwiched between opposing terminals in an anisotropic conductive connection, first, the conductive particles and the terminal surfaces are in point contact. Therefore, if the center of the conductive particle does not exist within the opposing opposing surfaces, the conductive particle will move away from between the terminals. Therefore, there is also the problem that it is difficult to improve the capture efficiency of the conductive particles in the terminals.
[0018] Therefore, the anisotropic conductive film described in Patent Document 2 has a problem in conduction reliability.
[0019] In contrast, the present invention aims to provide an anisotropic conductive film, which uses an anisotropic conductive film to fully capture conductive particles and suppress short circuits, whether in the case of high-density mounting of fine-pitch IC chips or in the case of connecting a glass substrate and an FPC substrate of a large-scale display panel, thereby reducing the deviation of on-resistance caused by one-end contact.
[0020] Solutions to Solve Problems
[0021] The present inventor has discovered that, with respect to conductive particles used in anisotropic conductive films, if, instead of filling a mold with a plurality of spherical conductive particles to form conductive particle units, conductive particles having an aspect ratio greater than a specific value are used, the capture area of the conductive particles on the connected terminal can be increased, thereby reducing the deviation in on-resistance caused by contact at one end and improving the conduction reliability. Furthermore, when the conductive particles are arranged using a mold, since the mobility of the particles is lower than that of spherical conductive particles, the conductive particles can be arranged with high precision in the desired arrangement, thereby reducing the incidence of poor arrangement and improving the production efficiency of the anisotropic conductive film, thereby conceiving of the present invention.
[0022] That is, the present invention provides an anisotropic conductive film containing conductive particles in an insulating adhesive layer, wherein the aspect ratio of the conductive particles is greater than 1.2, the conductive particles are dispersed in a non-contact manner when viewed from above, and the angle between the film surface of the anisotropic conductive film and the long axis direction of the conductive particles is less than 40°.
[0023] The present invention also provides a connection structure in which a connection terminal of a first electronic component and a connection terminal of a second electronic component are anisotropically conductively connected using the above-mentioned anisotropic conductive film.
[0024] Furthermore, the present invention provides a connection method for anisotropically conductively connecting a first electronic component to a second electronic component using the above-mentioned anisotropic conductive film, wherein:
[0025] The anisotropic conductive film is temporarily attached to the second electronic component, the first electronic component is placed on the temporarily attached anisotropic conductive film, and thermocompression bonding is performed from the first electronic component side.
[0026] Effects of the Invention
[0027] According to the anisotropic conductive film of the present invention, since the conductive particles have an aspect ratio greater than a specific value, the terminal and the conductive particles are in line contact rather than point contact during anisotropic conductive connection, thereby increasing their contact area and improving the capture of the conductive particles in the terminal.
[0028] In addition, through this line contact, even if one end of the heat pressing tool is in contact, the pressing force is dispersed in the long axis direction of the conductive particles, so that the bumps or wiring are not damaged, and the conductive particles fully function as gap spacers. Therefore, even if one end of the heat pressing tool is in contact, a good on-resistance value can be achieved on both the side with one end in contact and the side without one end in contact.
[0029] In particular, when the conductive particles are formed of conductive columnar glass particles, the degree of anisotropic conductive connection can be easily confirmed by visual observation not only from the state of particle indentation but also from the state of glass particle crushing. Therefore, the overall anisotropic conductive connection cost including the inspection cost can be reduced.
[0030] Furthermore, in the manufacturing process of anisotropic conductive films, when filling a mold with conductive particles and arranging the conductive particles, if particles having an aspect ratio greater than a specific value are used as the conductive particles, the excessive movement of the particles can be suppressed compared to spherical particles, and thus the conductive particles are less likely to fall off the mold, and the conductive particles can be precisely configured according to the desired arrangement.
[0031] Furthermore, according to the anisotropic conductive film of the present invention, since the conductive particles are dispersed in a non-contact manner in plan view, the occurrence of short circuits in the terminals of the anisotropic conductive connection can be reduced even if the conductive particles have an aspect ratio of a specific value or more.
[0032] In addition, since there is no need to use an insulating spacer, it becomes easy to evenly disperse the conductive particles in the anisotropic conductive film. In addition, the material cost is also reduced. Furthermore, the insulating spacer and the conductive particles do not overlap in the anisotropic conductive film. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] [ Figure 1A ] Figure 1A It is a top view of the conductive particles of the anisotropic conductive film 1A of the example.
[0034] [ Figure 1B ] Figure 1B It is a cross-sectional view of conductive particles in the anisotropic conductive film 1A of the example.
[0035] [ Figure 1C ] Figure 1C It is a cross-sectional view of conductive particles in the anisotropic conductive film 1A of the example.
[0036] [ Figure 2A ] Figure 2A It is a top view of the conductive particles of the anisotropic conductive film 1B of the example.
[0037] [ Figure 2B ] Figure 2B It is a cross-sectional view of conductive particles in the anisotropic conductive film 1B of the example.
[0038] [ Figure 3A ] Figure 3A It is a top view of the conductive particles of the anisotropic conductive film 1C of the example.
[0039] [ Figure 3B ] Figure 3B It is a cross-sectional view of conductive particles in the anisotropic conductive film 1C of the example.
[0040] [ Figure 4 ] Figure 4 It is a perspective view of an anisotropic conductive film 1D according to the example.
[0041] [ Figure 5 ] Figure 5 It is a perspective view of an anisotropic conductive film 1E according to the example.
[0042] [ Figure 6 ] Figure 6 This is an enlarged view of the bump formation surface of the flexible printed circuit board.
[0043] [ Fig. 7A ] Fig. 7A This is a cross-sectional view of the heat press tool and glass substrate adjusted to be parallel to each other at the start of anisotropic conductive connection.
[0044] [ Figure 7B ] Figure 7B This is a cross-sectional view of a heat press tool and a glass substrate in contact at one end during anisotropic conductive connection. DETAILED DESCRIPTION
[0045] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings. In addition, in each figure, the same reference numeral represents the same or equivalent component.
[0046] Figure 1A 1 is a plan view showing the arrangement of conductive particles 2 in an anisotropic conductive film 1A according to an embodiment of the present invention. Figure 1B , Figure 1C is its cross-sectional view. In addition, Figure 2A FIG. 1 is a top view of an anisotropic conductive film 1B according to an embodiment in which the arrangement of conductive particles is different. Figure 2B Columnar conductive particles 2 having an aspect ratio of 1.2 or more are used in these anisotropic conductive films 1A and 1B, and the conductive particles 2 are dispersed in the insulating adhesive layer 3 in a non-contact manner in plan view.
[0047] <Material of conductive particles>
[0048] As the conductive particles 2, for example, conductive columnar glass particles can be used, in which a conductive layer is formed on at least a portion of the surface of the columnar glass, preferably on the entire surface. As the conductive layer, a thin film of gold, silver, nickel, copper, ITO, etc. formed by a method such as electroless plating and CVD can be exemplified. The thickness of the conductive layer is usually more than 5 nm, preferably 10 to 800 nm, and more preferably 100 to 500 nm. In addition, as for the degree of "at least a portion of the surface", there is no particular limitation as long as anisotropic conductive connection can be performed.
[0049] By using such conductive columnar glass particles, even if excessive pressing force is applied to the conductive particles during anisotropic conductive connection, stress can be buffered by the breakage of the conductive columnar glass particles themselves. Therefore, when one end of the hot pressing tool is in contact, the conductive particles function as gap spacers to prevent damage to the bumps or wiring, and a good on-resistance value can be achieved. Moreover, it is easy to check the indentation of the bumps after the anisotropic conductive connection. In addition, it is not easily affected by the expansion and contraction caused by heat, and corrosion caused by metal ions or migration of metal ions will not occur. Furthermore, when an ultraviolet-curing insulating adhesive is used, it is not easy to cause insufficient curing due to the transmission of ultraviolet rays to a certain extent.
[0050] In addition, as the conductive particles 2, particles in which a conductive layer is provided on the resin core can also be used. In the manufacturing process of the resin core, sometimes an agglomerate of the resin core can be obtained, but in this case, the agglomerate of the resin core is classified and the particles having the above-mentioned aspect ratio are used. That is, through the manufacturing method of the resin core, an agglomerate (secondary particle) can sometimes be obtained in its intermediate process. In this case, the agglomerated resin core is crushed. In the crushing, it is preferred to unravel the agglomerate of the resin core that is agglomerated when the solvent is dried so that the particle shape is not deformed. For such an operation, a dispersant or a surface modifier can be added in advance during the compounding, or a crushing treatment in which the particle shape is difficult to deform can be performed to make it easy to crush. The crushing treatment can be repeated, and classification can be performed between or before and after the crushing process. As an example, it can be performed by using an airflow type fine crushing device. More specifically, a table-type experimental airflow crusher (labo jet mill) A-O JET MILL or COURGETTE system (both manufactured by SEISHIN Enterprise Co., Ltd.) can be cited. A cyclone separation (cyclorubber) recovery mechanism can also be combined. Such a resin core is preferably formed of a plastic material with excellent compression deformation, for example, it can be formed of (meth) acrylic resin, polystyrene resin, styrene-(meth) acrylic copolymer resin, urethane resin, epoxy resin, phenolic resin, acrylonitrile styrene (AS) resin, benzoguanamine resin, divinylbenzene resin, styrene resin, polyester resin, etc. Because the resin core has excellent compression deformation, it becomes easy to evaluate the connection state from the indentation of the particles formed at the terminal due to the anisotropic conductive connection. The conductive layer can be formed by a known method such as electroless plating as described above. The material or thickness of the conductive layer is also roughly the same as described above.
[0051] In the case of conductive particles having protrusions on the surface, particles having a predetermined aspect ratio are classified from the agglomerates of the resin core having protrusions, and a conductive layer is provided on the surface thereof. Alternatively, the resin core having a predetermined aspect ratio may be classified and then the protruding particles may be provided on the resin core.
[0052] The anisotropic conductive film of the present invention may contain conductive particles such as metal particles of nickel, cobalt, silver, copper, gold, palladium, etc., alloy particles of solder, etc., and metal-coated resin particles used for known anisotropic conductive films in addition to the above-mentioned conductive particles within a range not impairing the effects of the invention.
[0053] <Shape of conductive particles>
[0054] ・Aspect ratio
[0055] In the anisotropic conductive film of the present invention, the aspect ratio (average major axis length / average minor axis length) of the conductive particles 2 is 1.2 or more, preferably 1.3 or more, more preferably 3 or more, and preferably 15 or less, more preferably 10 or less, and further preferably 5 or less. If the aspect ratio is too small, the capture of the conductive particles in the terminal cannot be improved during the anisotropic conductive connection, and on the contrary, if it is too large, a short circuit is likely to occur due to the width of the interval between the terminals. In addition, it is difficult to operate according to the material of the conductive particles 2, which will become a factor that increases the manufacturing cost of the anisotropic conductive film.
[0056] In particular, when the conductive particles are conductive columnar glass particles, from the viewpoint of well dispersing the pressing force of the hot pressing tool, the aspect ratio is preferably 1.33 to 20, more preferably 1.67 to 6.67. If the aspect ratio is within this range, the pressing force of the hot pressing tool can be well dispersed, and the operability becomes good.
[0057] Here, the aspect ratio refers to the ratio of the average major axis length to the average minor axis length of the conductive particles 2. In the case where the conductive particles 2 are cylindrical, prism-like columns, the major axis length L1 is the length of the height direction (i.e., the long side direction) of the conductive particles 2, which can be measured using an image observation type particle size distribution measuring device as the maximum length. The average major axis length is calculated, for example, by averaging the maximum lengths of any 50 conductive particles. The minor axis length L2 is the length with the widest width among the diameters of the cross-section of the conductive particles 2, which can be measured using a metal microscope or an electron microscope (SEM). The average minor axis length is calculated, for example, by averaging any 50 minor axis lengths. This can also be measured using a metal microscope or an electron microscope (SEM). In the case where the conductive particles are contained in the film, it can be obtained by observing from above and observing in section. In addition, in the case where only the conductive particles are measured as a sample, which is distinguished from the insulating adhesive layer, the conductive particles are placed in a manner that does not cause the conductive particles to condense into a flat surface, and the average major axis length can be obtained by observing from above. At this time, the average minor axis length is in the depth direction of the measurement sample, and thus can be obtained by adjusting the focal distance of the electron microscope (SEM).
[0058] In addition, for columnar conductive particles, the longitudinal cross-sectional shape is not limited to a rectangle, and also includes a shape in which the side surface bulges in the short side direction, or a shape in which the upper and lower end surfaces bulge in the long side direction. In these cases, the aspect ratio can also be obtained by the above method, and the average major axis length, average minor axis length, and aspect ratio in the film can also be obtained in the same way. In addition, the measurement can be performed using a laser scanning type three-dimensional shape measuring device KS-1100 (manufactured by KEYENCE).
[0059] In the anisotropic conductive film of the present invention, the aspect ratio of the conductive particles 2 is set within the above range, thereby increasing the contact area between the terminal and the conductive particles 2 and improving the capture of the conductive particles 2 in the terminal. In contrast, if the aspect ratio is too large, the conductive particles 2 are easily linked during anisotropic conductive connection, which increases the incidence of short circuits. On the other hand, if the aspect ratio is too small, the capture rate of the conductive particles in the terminal decreases, which easily increases the on-resistance.
[0060] In addition, by making the aspect ratio of the conductive particles 2 within the above range, when the conductive particles 2 are filled into the mold in the manufacturing process of the anisotropic conductive film, the conductive particles 2 can be suppressed from excessively moving, so the conductive particles 2 are difficult to fall off the mold, and the conductive particles 2 can be accurately arranged in the expected arrangement. In addition, it is preferred that the aspect ratio is roughly the same for all conductive particles 2. Specifically, with regard to the distribution of the ratio of the major axis length to the minor axis length of the conductive particles, it is preferred that more than 90% of all conductive particles exist in the range of ±20% of the ratio of the average major axis length to the average minor axis length of all conductive particles, i.e., the aspect ratio, more preferably more than 95% of all conductive particles exist in ±20%, and even more preferably more than 95% of all conductive particles exist in ±10%. By making the ratio of the major axis length to the minor axis length of each conductive particle consistent in this way, it is expected to improve capture and suppress short circuits, especially for bumps with small pitches.
[0061] ・Average major axis length
[0062] The average major axis length of the conductive particles 2 is preferably 4 μm to 60 μm, more preferably 6 μm to 20 μm. If it is this length, the operability is good, and the pressing force of the hot pressing tool can be well dispersed during anisotropic conductive connection. Therefore, even if the crimping surface of the hot pressing tool contacts one end of the connected substrate surface inclined to form a relatively strong and weak area of pressing force, the increase in on-resistance can be suppressed. The average minor axis length is preferably 1 μm or more, and in order to prevent one end from contacting when the terminals are captured, it is more preferably 2.5 μm or more, and in order to firmly clamp the terminals when the terminals are not flat and have bumps, it is further more preferably 3 μm or more.
[0063] ・Cross-sectional shape
[0064] The conductive particles 2 preferably have the above aspect ratio and a cross-sectional shape formed by a curved line such as a circle or an ellipse, etc. This can well disperse the pressing force of the heat pressing tool during anisotropic conductive connection, thereby suppressing the increase in on-resistance even when one end is in contact.
[0065] In addition, the outer shape of the short side direction and the outer shape of the long side direction in the longitudinal section shape can be straight lines or curves. When the outer shapes of the short side direction and the long side direction in the longitudinal section shape are straight lines (that is, when the longitudinal section shape is rectangular), the conductive particles 2 become columns such as cylinders and prisms, and when the faces roughly parallel to the short side direction in the longitudinal section shape are semicircular or the faces roughly parallel to the long side direction are arc-shaped, they become so-called capsule-shaped columns. From the viewpoint of the pressing force of the dispersed hot pressing tool, it is preferred that the cross section be a cylinder, an elliptical column, etc., which are formed by curves such as circles and ellipses. In addition, the sphere may be a plurality of blocks. In this case, it becomes a bulging shape when the long side direction is viewed from the side. Thus, the connection state can also be correctly evaluated by the indentation of the conductive particles in the terminal. On the other hand, from the viewpoint of improving the capture of the particles in the terminal, it may also be a hexagonal prism, a pentagonal prism, a quadrangular prism, a triangular prism, a polyhedral prism, a pentagram prism, a hexagram prism, etc. Among them, a cylindrical shape is preferred from the viewpoint of arranging the conductive particles in parallel with the bumps and facilitating the thermocompression bonding conditions when the conductive particles are brought into line contact.
[0066] ・Surface shape
[0067] Protrusions may also be formed on the surface of the conductive particles. For example, conductive particles described in Japanese Patent Application Publication No. 2015-8129 and the like may be used. By forming such protrusions, it is possible to puncture a protective film provided on the terminal during anisotropic conductive connection. The protrusions are preferably formed uniformly on the surface of the conductive particles, but defects may occur in a portion of the protrusions during the process of filling the mold with conductive particles in order to arrange the conductive particles in the manufacturing process of the anisotropic conductive film. As an example, the height of the protrusion may be 10 to 500 nm, or may be less than 10% of the length of the minor axis of the particle.
[0068] <Arrangement of conductive particles>
[0069] In the anisotropic conductive film of the present invention, it is preferred that the conductive particles 2 are dispersed in a non-contact manner when viewed from above, and that the distance L3 between any conductive particle 2a and the conductive particle 2b closest to the conductive particle 2a when viewed from above (i.e., the closest distance when viewed from above) is 0.5 times or more the minor axis length L2 of the conductive particle 2a ( Figure 1A , Figure 2A ), or preferably, any conductive particle 2a and the conductive particle 2b closest to the conductive particle 2a do not overlap in the long side direction of the anisotropic conductive film ( Figure 2A ). This makes it difficult for a short circuit to occur at the terminals of the anisotropic conductive connection.
[0070] In the anisotropic conductive film of the present invention, the major axis directions A of the conductive particles 2 may be arranged in substantially the same direction or in different directions with regularity. Figure 1A As in the anisotropic conductive film 1A shown, when the long axis direction A of the conductive particles 2 is parallel to the long side direction of the anisotropic conductive film 1A, since the aspect ratio of the conductive particles is greater than 1.2, the terminals can easily capture the conductive particles even if misalignment occurs in the long side direction of the film during the anisotropic conductive connection.
[0071] On the contrary, when the long axis direction A of the conductive particles 2 is aligned along the short side direction of the anisotropic conductive film, even if the number density of the conductive particles is increased, it is difficult to cause a short circuit during the anisotropic conductive connection. Therefore, by increasing the number density of the conductive particles, it is easy to capture the conductive particles even if there is an alignment deviation terminal.
[0072] In addition, if Figure 2A It is also preferable to make the major axis direction A of the conductive particles 2 coincide with the direction oblique to the long side direction of the film as in the anisotropic conductive film 1B shown in the figure, because generally, the bumps of anisotropic conductive connection extend in the direction perpendicular to the long side direction of the film.
[0073] By aligning the major axis directions A of the conductive particles 2 in substantially the same direction as described above, it becomes easy to determine whether a product is acceptable during product inspection.
[0074] On the other hand, the long axis direction A of each conductive particle 2 may have different directions with regularity. Thus, it is possible to take into account the effects of the anisotropic conductive film (for example, the effect of the anisotropic conductive film 1A and the effect of the anisotropic conductive film 1B) in which the long axis directions of the conductive particles 2 are regular and have different directions. Therefore, it is possible to expect a greater effect of reducing the number of conductive particles. As for what kind of regularity the arrangement of the long axis direction A of the conductive particles 2 has, it can be appropriately selected according to the layout such as the size of the bumps to be connected or the distance between the bumps.
[0075] As a method for arranging the conductive particles 2 in the anisotropic conductive film in the above-mentioned arrangement, a method of dispersing the conductive particles on a stretched film and then stretching them in an arbitrary direction, or arranging the conductive particles using a mold as described later is preferable.
[0076] In addition, as the arrangement mode of the conductive particles 2 under the top view, it is preferred to arrange the centers of the conductive particles 2 in a regular manner in the vertical and horizontal directions. As a more specific mode of regular arrangement, the centers of the conductive particles 2 can be arranged in a lattice shape such as a square lattice, a rectangular lattice, a rhombus lattice, a triangular lattice, a hexagonal lattice, etc. They can also be combined. By appropriately setting the lattice spacing, short circuits can be suppressed during anisotropic conductive connection, and the capture of the conductive particles can be improved.
[0077] When the conductive particles are arranged regularly, an arrangement axis P is formed along the short side direction of the film to arrange the center of the conductive particles 2. For the conductive particles on the arrangement axis P, it is preferred that the tangent line of any conductive particle in the short side direction of the film coincides with the tangent line of the conductive particle adjacent to the conductive particle in the short side direction of the film ( Figure 1A ), or the outer tangent line of any conductive particle in the short side direction of the film passes through the conductive particles adjacent to the conductive particle. In this way, the capture of conductive particles in the terminal during anisotropic conductive connection can be improved.
[0078] In addition, in the case of having an arrangement axis P along the short axis direction of the conductive particles 2 arranging the centers of the conductive particles 2 ( Figure 1A ), or, in the case of having an arrangement axis P that arranges the centers of the conductive particles 2 along the long axis direction of the conductive particles 2 ( Figure 2A ), preferably, the conductive particles 2 adjacent to each other in the arrangement axis P overlap in the short axis direction of the anisotropic conductive film. Thus, the capture of the conductive particles in the terminal can be improved during anisotropic conductive connection.
[0079] On the other hand, for example, the conductive particles may be dispersed instead of being regularly arranged, depending on the purpose of the anisotropic conductive film or the number density of the conductive particles in the anisotropic conductive film. For example, when the anisotropic conductive film is used for FOG connection, the number density of the conductive particles is 1 / mm 2 Above 300 pieces / mm 2 Less than, more preferably 2 / mm 2 Above 200 pieces / mm 2 Less than, more preferably 3 / mm 2 Above 50 / mm 2 In the following cases, Figure 4 As shown, the conductive particles 2 can be dispersed irregularly. In this case, it is also preferable that the conductive particles 2 are dispersed so as not to be in contact with each other in a plan view.
[0080] It can be Figure 1C As shown in FIG. 1 , the angle between the film surface S of the anisotropic conductive film and the long axis direction A of the conductive particles is set to 0°, and the long axis direction A of the conductive particles 2 is made substantially parallel to the film surface S. Alternatively, Figure 2BAs shown, the long axis direction A of the conductive particle 2 is tilted relative to the film surface S. When the long axis direction A of the conductive particle 2 is tilted relative to the film surface S, the angle θ formed by the film surface S of the anisotropic conductive film and the long axis direction A of the conductive particle is less than 40°, and more preferably within 15°. Here, the numerical value of the angle θ is such an angle, but it means that the angle is satisfied when the number ratio of the conductive particles is 80% or more, and more preferably 95% or more. The angle θ can be measured from an image of a film cross section of the anisotropic conductive film taken using an optical microscope or an electron microscope. By making the angle θ less than 40°, the long axis direction A of the conductive particle 2 can be made roughly parallel to the terminal surface by means of the thermal compression bonding of the anisotropic conductive connection, and the deviation of the conductive particles during capture can be suppressed to a minimum. That is, it is possible to suppress the parallel deviation of the pressing surface and the pressed surface of the hot pressing tool during the anisotropic conductive connection and cause one-end contact.
[0081] In addition, when one side of the electronic component connected by the anisotropic conductive film is a rigid substrate, etc., it is necessary to fill the electronic component with a relatively large amount of resin during connection, thereby increasing the thickness of the insulating adhesive layer of the anisotropic conductive film, and the angle θ can be increased according to the thickness. This is because even if the angle θ of the conductive particles in the insulating adhesive layer is large, the insulating adhesive layer will be crushed by the heating and pressing during the anisotropic conductive connection, and the angle θ of the long axis direction of the conductive particles contained therein relative to the film surface will also become smaller. In addition, when the length of the long axis direction of the conductive particles is short, the angle θ of the conductive particles in the insulating adhesive layer before the anisotropic conductive connection can also be increased for the same reason. Therefore, for example, when the thickness of the insulating adhesive layer is 3 to 50 μm, if the angle θ is within 70°, there is a situation where the long axis direction of the conductive particles can be made roughly parallel to the film surface during thermal compression.
[0082] <Conductive particle density>
[0083] In the anisotropic conductive film of the present invention, the number density of the conductive particles 2 can be adjusted to a range suitable for ensuring the reliability of conduction according to the terminal width or terminal spacing of the connection object. Generally, if more than 3, preferably more than 10 conductive particles can be captured in a set of opposing terminals, good conduction characteristics can be obtained. In actual use, in the case of FOG connection with a terminal spacing of 50 to 200 μm, the number density can be 1 particle / mm 2 Above 300 pieces / mm 2 Below, more preferably 2 pieces / mm 2 Above 200 pieces / mm 2 Below, more preferably 3 pieces / mm 2 Above 50 / mm 2In this case, the preferred amount of conductive particles (preferably conductive columnar glass particles) in the anisotropic conductive film is preferably 1 part by mass to 25 parts by mass, and more preferably 5 parts by mass to 15 parts by mass, when the total mass of the anisotropic conductive film is 100 parts by mass.
[0084] In addition, regardless of the object to be connected, if the connection is within 100 pieces / mm 2 The above can fully connect terminals with a wide terminal width (for example, about 100 to 200 μm). If 500 terminals / mm 2 If the number is 1000 / mm 2 In addition, a fine pitch (for example, the terminal width and the space between terminals are 30 μm or less) will not produce terminals that do not capture conductive particles, and in order to prevent short circuits, 50,000 / mm is preferred. 2 Below, more preferably 30000 pieces / mm 2 the following.
[0085] <Method for fixing conductive particles>
[0086] As a method for fixing the conductive particles 2 in a predetermined arrangement on the insulating adhesive layer 3, a mold having concave portions corresponding to the arrangement of the conductive particles 2 is prepared by a known method such as mechanical processing, laser processing, photolithography, etc., the conductive particles 2 are placed in the mold, the insulating adhesive layer forming composition is filled thereon, and the conductive particles 2 are taken out from the mold to transfer to the insulating adhesive layer 3. From such a mold, the mold can also be made of a material with lower rigidity.
[0087] In order to arrange the conductive particles 2 in the above arrangement on the insulating adhesive layer 3, a method may be adopted in which a member having through holes formed in a predetermined arrangement is provided on the insulating adhesive layer-forming composition layer, and the conductive particles 2 are supplied therefrom to pass through the through holes.
[0088] <Layer composition>
[0089] The anisotropic conductive film of the present invention can have various layer structures. For example, the conductive particles 2 may be arranged on a single-layer insulating adhesive layer 3 and the conductive particles 2 may be pressed into the insulating adhesive layer 3 so that the conductive particles 2 are present at a fixed depth from the interface of the insulating adhesive layer 3 as in the aforementioned anisotropic conductive film 1A.
[0090] In addition, if Figure 4 As in the anisotropic conductive film 1D shown in FIG. 1 , conductive columnar glass particles having an aspect ratio of 1.2 or more can be dispersed in an insulating adhesive as the conductive particles 2 to form a film.
[0091] When the anisotropic conductive film 1D is manufactured by applying an insulating adhesive in which the conductive particles 2 are dispersed, the film thickness of the anisotropic conductive film 1D is preferably 3 μm to 50 μm, and more preferably 5 μm to 20 μm. This is because the long axis of the conductive particles 2 is oriented substantially parallel to the film surface of the anisotropic conductive film so that the conductive particles 2 can function as good gap spacers. In addition, within this range, it is easy to orient the long axis of the conductive particles substantially parallel to the film surface.
[0092] In the present invention, after the conductive particles are arranged on the single-layer insulating adhesive layer, an insulating adhesive layer may be laminated separately to make the insulating resin layer a two-layer structure, or this may be repeated to make a structure of three or more layers. The insulating adhesive layer after the second layer is formed for the purpose of improving the tuck property or suppressing the flow of the resin and the conductive particles during anisotropic conductive connection.
[0093] In addition, if Figure 5 As shown in the anisotropic conductive film 1E, it can also have a two-layer structure of a first adhesive layer 3a containing conductive particles 2 in the insulating adhesive layer and a second adhesive layer 3b not containing conductive particles in the insulating adhesive layer. Figure 4 The second adhesive layer 3b can be formed similarly to the anisotropic conductive film 1D shown in the figure, by forming an insulating adhesive layer. More specifically, other components such as a solvent are mixed into a photocurable insulating adhesive as needed, the mixture is applied to a release film, and photocured, thereby first forming the second adhesive layer 3b. Then, other components such as conductive columnar glass particles and a solvent are mixed into the insulating adhesive as needed, the mixture is applied to the second adhesive layer 3b, and the mixture is dried to form the first adhesive layer 3a. Alternatively, the first adhesive layer 3a and the second adhesive layer 3b formed separately are laminated to manufacture a two-layer anisotropic conductive film 1E. The resin forming the insulating adhesive layer of the first adhesive layer 3a and the second adhesive layer 3b can be the same as the resin forming the insulating adhesive layer. Figure 4 The insulating adhesive layer of the single-layer anisotropic conductive film 1D shown is similar.
[0094] When the anisotropic conductive film is a two-layer structure, the thickness of the first adhesive layer 3a is preferably 1 μm to 15 μm, and more preferably 2 μm to 10 μm. If it is within this range, the long axis direction of the conductive particles 2 can be aligned within a predetermined angle relative to the film surface during the coating process, thereby improving productivity.
[0095] The thickness of the second adhesive layer 3b of the anisotropic conductive film 1E is preferably 1 μm to 50 μm, more preferably 3 μm to 20 μm. Within this range, a decrease in the conductive particle capture efficiency can be suppressed, and an excessive increase in the on-resistance can be suppressed.
[0096] According to the anisotropic conductive film 1E, Figure 4 Compared with the anisotropic conductive film 1D shown in FIG. 1 , the conductive particles 2 can be made substantially parallel to the film surface of the anisotropic conductive film at a higher level. This is because the first adhesive layer 3 a can be formed thinner by the coating method.
[0097] In addition, it is possible to include an insulating spacer in the second adhesive layer 3b. Here, the particle size of the insulating spacer is usually slightly larger than or equal to that of the conductive particles. After connection, the function as an insulating spacer can be confirmed from the state of the particle held between the terminals together with the conductive particles. Therefore, if it does not function as an insulating spacer, the particle becomes a filler such as an insulating filler. As an insulating spacer, a known material having a size roughly equal to the short axis of the conductive particle can be used. In the case where the insulating spacer is formed of a compressible resin such as a resin core, the particle size of the insulating spacer can also be larger than the short axis of the conductive particle, and in the case where the insulating spacer is a hard material such as glass, the particle size of the insulating spacer is preferably less than the short axis of the conductive particle, and more preferably less than the short axis of the conductive particle. As a result, it is possible to suppress the situation where the pressure on the long axis side of the conductive particle becomes excessive.
[0098] In order to fix the conductive particles in the insulating adhesive layer, the composition for forming the insulating adhesive layer may contain a photopolymerizable resin and a photopolymerization initiator, and the conductive particles may be fixed by light irradiation. A reactive resin that does not contribute to anisotropic conductive connection may also be used to fix the conductive particles or the above-mentioned transfer. For example, a photocurable resin may be used to fix the conductive particles, and a thermosetting resin may be used to perform an adhesive function during anisotropic conductive connection. For example, an propylene polymerizable resin may be used as the photocurable resin, and an epoxy resin may be used as the thermosetting resin.
[0099] The minimum melt viscosity of the total thickness of the anisotropic conductive film 1A is preferably 100 to 10000 Pa·s, more preferably 500 to 5000 Pa·s, and particularly preferably 1000 to 3000 Pa·s. If it is within this range, the conductive particles can be precisely arranged in the insulating adhesive layer, and the resin flow caused by the pressing during the anisotropic conductive connection can be prevented from hindering the capture of the conductive particles. The minimum melt viscosity is measured using a rheometer (manufactured by TA INSTRUMENTS, ARES), which can be obtained under the conditions of a heating rate of 5°C / min, a measurement temperature range of 50 to 200°C, and a vibration frequency of 1Hz.
[0100] <Insulating adhesive layer>
[0101] The insulating adhesive layer 3 can be formed by appropriately selecting from the insulating adhesives used in the known anisotropic conductive film according to the purpose of the anisotropic conductive film. As preferred insulating adhesives, polymerizable resins such as (meth)acrylate compounds and epoxy compounds and paste-like or film-like resins containing thermal polymerization initiators or photopolymerization initiators can be cited. Here, as photopolymerization initiators, photoradical polymerization initiators, photocationic polymerization initiators, and photoanion polymerization initiators can be cited, and as thermal polymerization initiators, thermal radical polymerization initiators, thermal cationic polymerization initiators, and thermal anion polymerization initiators can be cited. In particular, photoradical polymerizable resins containing acrylate compounds and photoradical polymerization initiators; thermal radical polymerizable resins containing acrylate compounds and thermal radical polymerization initiators; thermal cationic polymerizable resins containing epoxy compounds and thermal cationic polymerization initiators; thermal anionic polymerizable resins containing epoxy compounds and thermal anion polymerization initiators; photocationic polymerizable resins containing epoxy compounds and photocationic polymerization initiators, etc. can be cited. These resins can be used in combination. Furthermore, these resins can be polymerized separately as needed.
[0102] More specifically, for example, the thermosetting epoxy adhesive in the insulating adhesive layer can be composed of a film-forming resin, a liquid epoxy resin (curing component), a curing agent, a silane coupling agent, and the like.
[0103] As film-forming resin, phenoxy resin, epoxy resin, unsaturated polyester resin, saturated polyester resin, urethane resin, butadiene resin, polyimide resin, polyamide resin, polyolefin resin etc., these can be used in combination with more than two kinds. Among these, from the viewpoint of film-forming property, processability, connection reliability, phenoxy resin can be preferably used.
[0104] Examples of the liquid epoxy resin include bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, modified epoxy resins thereof, alicyclic epoxy resins, and the like. Two or more of these may be used in combination.
[0105] Examples of the curing agent include anionic curing agents such as polyamine and imidazole, cationic curing agents such as sulfonium salts, and latent curing agents such as phenolic curing agents.
[0106] Examples of the silane coupling agent include epoxy-based silane coupling agents, acrylic-based silane coupling agents, etc. These silane coupling agents are mainly alkoxysilane derivatives.
[0107] Thermosetting epoxy adhesives may be formulated with fillers, softeners, accelerators, antioxidants, colorants (pigments, dyes), organic solvents, ion traps, and the like as needed.
[0108] Insulating fillers such as silica particles, aluminum oxide, and aluminum hydroxide may be added to the insulating adhesive layer 3 as needed. The size of the insulating filler is set to a size that does not hinder the anisotropic conductive connection, and is usually preferably smaller than the average minor axis length of the conductive particles. The amount of the insulating filler is preferably 3 to 40 parts by mass relative to 100 parts by mass of the resin forming the insulating adhesive layer. Thus, even if the insulating adhesive layer 3 melts during the anisotropic conductive connection, the conductive particles 2 can be prevented from moving uselessly due to the melted resin.
[0109] <Film thickness>
[0110] The thickness of the anisotropic conductive film (ie, the thickness of the insulating adhesive layer 3 ) is preferably 3 μm to 50 μm, more preferably 5 μm to 20 μm, in order to obtain sufficient connection strength. Within this range, the film can be used without any practical problems.
[0111] In addition, regarding the thickness of the insulating adhesive layer 3 (i.e., the thickness of the anisotropic conductive film), when the major axis length L1 of the conductive particles 2 is 100, it is preferably 90 or less, and more preferably 25 or less, and when the minor axis length L2 of the conductive particles 2 is 100, it is preferably 100 or more, and more preferably 120 or more. This is because the major axis direction A of the conductive particles 2 is made substantially parallel to the terminal surface so that the capture state is good, and the major axis direction A of the conductive particles 2 is made substantially parallel to the film surface S of the anisotropic conductive film.
[0112] <Connection structure>
[0113] The anisotropic conductive film of the present invention can be preferably used to anisotropically connect a first electronic component such as an FPC, an IC chip, an IC module, etc. with a second electronic component such as an FPC, a rigid substrate, a ceramic substrate, a glass substrate, a plastic substrate, etc. by heat or light. In addition, the first electronic components can be anisotropically connected by stacking IC chips or IC modules. In addition, light curing can be used for connection. The connection structure obtained by such treatment is also a part of the present invention.
[0114] As a method for connecting electronic components using anisotropic conductive films, it is preferred from the viewpoint of improving connection reliability that, for example, the interface of the anisotropic conductive film on the side where the conductive particles are present in the film thickness direction is temporarily bonded to a second electronic component such as a wiring substrate, and the temporarily bonded anisotropic conductive film is thermally pressed from the first electronic component side to a first electronic component such as an IC chip. Alternatively, connection can be performed by photocuring. In addition, in this connection, from the viewpoint of connection operation efficiency, such as Figure 1A , Figure 2A As shown in FIG. 1 , it is preferable that the long-side direction of the terminal 10 of the electronic component and the short-side direction of the anisotropic conductive films 1A and 1B are aligned. Example
[0115] Hereinafter, the present invention will be specifically described based on examples.
[0116] Examples 1 to 3, Comparative Examples 1 to 3
[0117] (1) Manufacturing of anisotropic conductive films
[0118] As conductive particles A, conductive cylindrical glass particles (PF-39SSSCA, Nippon Electric Glass Co., Ltd.) (average major axis length 14 μm, average minor axis length 3.9 μm) having a surface plated with 0.3 μm thick nickel (base) and a surface plated with 0.1 μm thick gold (surface) were prepared.
[0119] In addition, by dividing and classifying the conductive particles A, conductive cylindrical glass particles B (average major axis length 8 μm, average minor axis length 3.9 μm) and conductive cylindrical glass particles C (average major axis length 5.2 μm, average minor axis length 3.9 μm) of the sizes shown in Table 1 were obtained. In addition, conductive spherical glass particles D (Sekisui Chemical Co., Ltd., AUL704, particle size 4 μm) were prepared.
[0120] On the other hand, resin compositions of the compositions shown in Table 2 were prepared respectively, applied on a PET film with a film thickness of 50 μm, and dried in an oven at 80°C for 5 minutes to form a first insulating resin layer with a thickness of 15 μm or 13 μm and a second insulating resin layer with a thickness of 3 μm or 5 μm on the PET film.
[0121] In addition, a pattern is produced, that is, when viewed from above, Figure 3A As shown, the long axis direction of the conductive particles 2 is aligned in the long side direction of the film, and the centers of the conductive particles 2 are arranged in a 4-square grid. Figure 3B The angle (inclination angle θ) formed between the film surface S shown in FIG. 1 and the long axis direction A of the conductive particles 2 is the angle and number density shown in Table 1. The mold is provided with a pattern of convex portions corresponding to the arrangement of particles. The pellets of a known transparent resin are poured into the mold in a molten state and cooled and solidified to form concave portions and concave portions. Figure 3A , Figure 3B The resin molds corresponding to the arrangement patterns shown (Examples 1 to 3, Comparative Examples 1 and 3). Regarding the size of the resin mold, in Examples 1 to 3, the size of 1.3 times the average major axis length and the average minor axis length of the conductive particles was set as the upper limit of the opening. In Comparative Example 3, the size of the opening when viewed from above was smaller than that of Example 1, and the height of the convex shape was higher than that of Example 1. The closest distance between the convex portions of Examples 1 to 3 and Comparative Example 3 was 4 μm or more.
[0122] The concave portion of the resin mold was filled with the conductive particles of Table 1, and the second insulating resin layer 4 (3 μm) was covered thereon, and pressed at 60° C. and 0.5 MPa to adhere. Then, the insulating resin was peeled off from the mold, and the first insulating resin layer 5 (15 μm) was laminated at 60° C. and 0.5 MPa on the interface of the second insulating resin layer 4 on the side where the conductive particles were present, thereby manufacturing anisotropic conductive films 1C of Examples 1 to 3 and Comparative Example 3.
[0123] The anisotropic conductive film of Comparative Example 1 was manufactured in the same manner as in Example 1 except that the shape of the concave portion in the resin mold was changed. The anisotropic conductive film of Comparative Example 2 was manufactured by dispersing conductive particles in a resin composition for a second insulating resin layer without using a resin mold, so that the second insulating resin layer was formed to have a dry thickness of 5 μm, and then laminating the first insulating resin layer of 13 μm thereon. Furthermore, the coating gap of the second insulating resin layer was made smaller than the average major axis length of the conductive particles, so that the major axis length of the conductive particles was substantially parallel to the film surface when passing through the gap, and the inclination angle θ of the conductive particles was 15° or less.
[0124] The number density and area occupancy (area ratio of the conductive particles in the plan view of the anisotropic conductive film) in Table 1 were obtained by plane observation of 200 μm×200 μm at 5 locations randomly extracted from the portion used for anisotropic conductive connection of the anisotropic conductive film.
[0125] In addition, the cross-section of the film was observed according to an arbitrary cross-section and a cross-section orthogonal thereto (observation of the respective cross-sections of the major axis and the minor axis of the conductive particles), and the length in the major axis direction and the length in the minor axis direction of 200 continuous conductive particles were measured to obtain the aspect ratio. In addition, the inclination angle θ was also measured from the cross-section. As a result, more than 90% of the total number of conductive cylindrical glass particles A, B, C and conductive spherical cylindrical glass particles D were within ±20% of the aspect ratio that can be obtained from the average major axis length and the average minor axis length.
[0126] In addition, the thickness of the second insulating resin layer in Table 1 is a value measured by a film thickness measuring instrument (Litematic VL-50 manufactured by MITUTOYO Corporation).
[0127] (2) Evaluation
[0128] The anisotropic conductive films of the respective Examples and Comparative Examples were evaluated for (a) initial conduction characteristics, (b) short circuit occurrence rate, and (c) conductive particle capture efficiency as follows. The results are shown in Table 1.
[0129] (a) Initial conduction characteristics
[0130] The anisotropic conductive film of each embodiment and comparative example was sandwiched between an IC for evaluation of initial conduction and conduction reliability and a glass substrate, and heated and pressed (180°C, 20 MPa, 5 seconds) to obtain each connection for evaluation. In this case, the long side direction of the anisotropic conductive film and the short side direction of the bump were aligned. Then, the conduction resistance of the connection for evaluation was measured, and a value of 5Ω or less was determined as "OK", and a value of more than 5Ω was determined as "NG".
[0131] Here, regarding the evaluation IC and the glass substrate, their terminal patterns correspond and their dimensions are as follows.
[0132] IC for evaluating initial conduction and conduction reliability
[0133] Appearance 0.7×20mm
[0134] Thickness 0.2mm
[0135] Bump specifications: Gold plating, height 12μm, size 15×100μm, distance between bumps 15μm Number of terminals: 1300 (650 on each long side of the IC outline).
[0136] Glass substrate
[0137] Glass material: Made by CORNING
[0138] Outer diameter 30×50mm
[0139] Thickness 0.5mm
[0140] ITO electrode wiring.
[0141] (b) Short circuit occurrence rate
[0142] The short circuit rate is determined by observing 200 bump intervals randomly selected from the evaluation connection obtained in (a) using a metal microscope and confirming the aggregation or connection of conductive particles connecting adjacent bumps. In the evaluation of the short circuit rate, the absence of such aggregation or connection is determined as "OK", and the presence of more than one is determined as "NG".
[0143] (c) Conductive particle capture efficiency
[0144] In the evaluation connection products obtained in (a) of each example and comparative example, the number of particles captured by 100 bumps was measured and the ratio of the area of the conductive particles captured per bump to the terminal area was evaluated according to the following criteria.
[0145] A: The total area of the captured conductive particles is more than 8% of the terminal area;
[0146] B: The total area of the captured conductive particles is 5% or more and less than 8% of the terminal area;
[0147] C: The total area of the captured conductive particles is less than 5% relative to the terminal area.
[0148] [Table 1]
[0149]
[0150] [Table 2]
[0151] (parts by mass)
[0152]
[0153] (*1) Nippon Steel & Sumitomo Metal Corporation, YP-50 (thermoplastic resin)
[0154] (*2) Mitsubishi Chemical Corporation, jER828 (thermosetting resin)
[0155] (*3) Sanshin Chemical Industry Co., Ltd., SI-60L (latent curing agent)
[0156] (*4) Japan AEROSIL Co., Ltd., AEROSIL RX300
[0157] As can be seen from Table 1, Examples 1 to 3, in which the aspect ratio is greater than 1.3 and the conductive particles are arranged, have good initial conduction characteristics, short circuit incidence, and conductive particle capture efficiency. In contrast, in Comparative Example 1, the conductive particle capture efficiency is poor because the conductive particles are spherical. In Comparative Example 2, the aspect ratio of the conductive particles is greater than 1.3, but the conductive particles are randomly arranged, and there are overlapping conductive particles when viewed from above, so the short circuit incidence is poor. In Comparative Example 3, the capture is reduced because the tilt angle is too large, so the initial conduction characteristics are poor.
[0158] Next, as Examples 4 to 6, the anisotropic conductive films obtained in Examples 1 to 3 were prepared as follows. Figure 2A The film was bonded to a glass substrate with the angle Φ between the long side direction of the film and the long axis direction A of the conductive particles tilted to 80°, and the evaluation was performed in the same manner. The evaluation results of Examples 4 to 6 obtained were substantially the same as those of Examples 1 to 3, and the initial conduction characteristics, short circuit occurrence rate, and conductive particle capture efficiency were all good.
[0159] Example 7
[0160] (Production of anisotropic conductive film in which conductive columnar glass particles are dispersed and retained in a single layer)
[0161] A mixed liquid was prepared with toluene using 40 parts by mass of a phenoxy resin (YP-50, Nippon Steel & Sumikin Chemical Co., Ltd.), 40 parts by mass of a liquid epoxy resin (jER828, Mitsubishi Chemical Co., Ltd.), 20 parts by mass of a microcapsule-type latent curing agent (Asahi Kasei E-MATERIALS Co., Ltd., Novacure HX3941HP), and 28 parts by mass of conductive cylindrical glass particles (PF-39SSSCA, Nippon Electric Glass Co., Ltd. (average major axis length 14 μm, average minor axis length 3.9 μm)) having a surface plated with 0.3 μm thick nickel (base) and a surface plated with 0.1 μm thick gold (surface) so that the solid content was 50% by mass. The mixed solution was applied to a polyethylene terephthalate release film (PET release film) having a thickness of 50 μm so as to have a dry thickness of 20 μm, and dried in an oven at 80° C. for 5 minutes to prepare a thermally polymerized anisotropic conductive film.
[0162] When the dispersed state of the conductive columnar glass particles in the anisotropic conductive film was observed with an optical microscope, all the conductive particles were not in contact with each other in a plan view.
[0163] Example 8
[0164] (Production of an anisotropic conductive film having a two-layer structure in which a second adhesive layer is laminated on a first adhesive layer containing conductive columnar glass particles)
[0165] (Formation of the first adhesive layer)
[0166] A mixed solution was prepared with toluene to obtain a solid content of 50% by mass of 40 parts by mass of a phenoxy resin (YP-50, Nippon Steel Chemical Co., Ltd.), 40 parts by mass of a liquid epoxy resin (jER828, Mitsubishi Chemical Co., Ltd.), 20 parts by mass of a microcapsule type latent curing agent (Novacure HX3941HP, Asahi Kasei E-Materials Co., Ltd.), and 14 parts by mass of conductive cylindrical glass particles (PF-39SSSCA, Nippon Electric Glass Co., Ltd. (average major axis length 14 μm, average minor axis length 3.9 μm)) with a surface plated with 0.3 μm thick nickel (base) and a surface plated with 0.1 μm thick gold (surface). The mixed solution was applied to a polyethylene terephthalate release film (PET release film) having a thickness of 50 μm to obtain a dry thickness of 5 μm, and dried in an oven at 80°C for 5 minutes to form a first adhesive layer.
[0167] (Formation of the Second Adhesive Layer)
[0168] Next, 40 parts by mass of phenoxy resin (YP-50, Nippon Steel Chemical Co., Ltd.), 40 parts by mass of liquid epoxy resin (jER828, Mitsubishi Chemical Co., Ltd.), and 20 parts by mass of microcapsule type latent curing agent (Asahi Kasei E-MATERIALS Co., Ltd., Novacure HX3941HP) were prepared with toluene so that the solid content was 50% by mass. The mixed solution was applied to a polyethylene terephthalate release film (PET release film) having a thickness of 50 μm so that the dry thickness was 15 μm, and dried in an oven at 80°C for 5 minutes, thereby forming a relatively thick second adhesive layer.
[0169] (Lamination of the first adhesive layer and the second adhesive layer)
[0170] A relatively thick second adhesive layer was laminated on the first adhesive layer thus obtained under the conditions of 60° C. and 0.5 MPa to obtain an anisotropic conductive film.
[0171] When the dispersed state of the conductive columnar glass particles in the anisotropic conductive film was observed with an optical microscope, all the conductive particles were not in contact with each other in a plan view.
[0172] Comparative Example 4
[0173] (Manufacturing of anisotropic conductive film in which spherical conductive particles are dispersed and retained in a single layer)
[0174] Example 7 was repeated to prepare a mixed solution, except that 12 parts by mass of conductive particles having an average particle size of 4 μm (Ni / Au-plated resin particles, AUL704, Sekisui Chemical Co., Ltd.) were used instead of 28 parts by mass of the "conductive cylindrical glass particles" in Example 7, and the mixed solution was then used to prepare a thermally polymerized anisotropic conductive film.
[0175] Comparative Example 5
[0176] (Manufacturing of anisotropic conductive film in which spherical conductive particles and spherical spacers are dispersed and retained in a single layer)
[0177] Comparative Example 4 was repeated except that 15 parts by mass of spherical spacers (Si filler) having an average particle size of 1 μm were further added to the mixed solution of Comparative Example 4 to obtain a thermally polymerizable anisotropic conductive film.
[0178] Comparative Example 6
[0179] (Manufacture of anisotropic conductive film having a two-layer structure in which a first adhesive layer and a second adhesive layer containing spherical spacers and conductive particles are laminated)
[0180] Example 8 was repeated to form the first adhesive layer, except that 7.5 parts by mass of spherical insulators (Si filler) with an average particle size of 1 μm and 6 parts by mass of conductive particles (Ni / Au-plated resin particles, AUL704, Sekisui Chemical Co., Ltd.) with an average particle size of 4 μm were used instead of 14 parts by mass of the "conductive cylindrical glass particles" in Example 8. In addition, for the formation of a relatively thick second adhesive layer and their lamination, a thermal polymerization type anisotropic conductive film was obtained by repeating Example 8.
[0181] <Evaluation>
[0182] The anisotropic conductive films of Examples 7 and 8 and Comparative Examples 4, 5, and 6 were subjected to the following experiment to evaluate the initial on-resistance. The obtained results are shown in Table 3.
[0183] (Initial on-resistance)
[0184] The anisotropic conductive film (1.5 mm in length × 40 mm in width) of each embodiment and comparative example was sandwiched between a glass substrate for evaluating the initial on-resistance value and a flexible printed circuit substrate (FPC substrate), and heated and pressed (200°C, 5 MPa, 15 seconds) using a hot press tool to obtain an evaluation connector, and the on-resistance value of the evaluation connector was measured using a digital multimeter 7557 (Yokogawa Electric Co., Ltd.). The glass substrate and FPC substrate used for evaluation are described below. In practice, it is best to be 4Ω or less.
[0185] "Glass substrate for evaluating initial on-resistance value"
[0186] Glass material: Alkali glass (manufactured by CORNING)
[0187] Outer diameter: 30×50mm
[0188] Thickness: 0.7mm
[0189] Electrode: Indium tin oxide (ITO) solid electrode with a thickness of 220 nm.
[0190] "FPC substrate"
[0191] Membrane material: Polyimide film with a thickness of 38μm (polyimide type)
[0192] Width of film at connection: 1.5mm
[0193] Bump size: 2500μm in length, 25μm in width, 8μm in height, copper / nickel bump
[0194] Bump arrangement: 15 bumps (No. 1 on the left and No. 15 on the right) are arranged in parallel at a 50 μm pitch in the center of the film in the width direction (see Figure 6 ).
[0195] "Hot pressing tool with a flat pressing surface"
[0196] Pressing surface size: 100mm×1.5mm (long side direction is consistent with the width direction of FPC film)
[0197] One-end contact condition: For the glass substrate, the right end is tilted by 0.2° so as to make contact.
[0198] [Table 3]
[0199]
[0200] In the center of the FPC substrate, bumps No. 6 to 10 are formed, which are considered to receive normal pressure. On the non-one-end contact side (left side), bumps No. 1 to 5 are formed, which are considered to receive less pressure than normal due to one-end contact. On the one-end contact side (right side), bumps No. 11 to 15 are formed, which are considered to receive greater pressure than normal due to one-end contact. As a whole, it is considered that the pressing force gradually increases from bump No. 1 to bump No. 15.
[0201] As can be seen from Comparative Example 4 in Table 3, in the case of the conventional anisotropic conductive film without using conductive columnar glass particles, the on-resistance value particularly on the non-one-end contact side increases significantly as the pressing force decreases, and bumps No. 1 to 3 show on-resistance values exceeding 4Ω.
[0202] In addition, the anisotropic conductive film of Comparative Example 5 further includes spherical spacers in the single-layer anisotropic conductive film of Comparative Example 4, but the on-resistance value of the non-one-end contact side increases as the pressing force decreases. The degree of increase is greater than that of Comparative Example 4, and the bumps No. 1 to 5 show an on-resistance value exceeding 4Ω, and the bumps No. 1 to 3 especially exceed 10Ω.
[0203] The anisotropic conductive film of Comparative Example 6 has a two-layer structure in which the thinner adhesive layer contains spherical spacers and conductive particles. However, the on-resistance value on the non-one-end contact side increases as the pressing force decreases, and bumps No. 1 to 15 show on-resistance values exceeding 9Ω.
[0204] On the other hand, in the anisotropic conductive films of Examples 7 and 8, the on-resistance value of the non-one-end contact side slightly increases as the pressing force decreases, but both show an on-resistance value of less than 4Ω, and either one can obtain sufficient conduction performance. In particular, the anisotropic conductive film of Example 8 adopts a two-layer structure of a thinner adhesive layer and a thicker adhesive layer, and the thinner adhesive layer contains conductive columnar glass particles, and the thicker adhesive layer is not mixed with conductive particles. Therefore, compared with Example 7, there is a tendency for one-end contact to be further improved. In addition, the conductive columnar glass particles in Examples 7 and 8 are roughly parallel to the plane of the film, but the one side of Example 8 is more parallel. In addition, in Example 8, even if the amount of conductive columnar glass particles mixed is half of that in Example 7, better characteristics can be obtained for one-end contact. This is believed to be because the layer containing the conductive columnar glass particles is sufficiently thin relative to the long axis of the conductive columnar glass particles, so it becomes more parallel to the plane of the film when applied, making the effect easier to manifest.
[0205] Description of symbols
[0206] 1A, 1B, 1C, 1D, 1E anisotropic conductive film; 1X existing anisotropic conductive film; 2, 2a, 2b conductive particles; 3, 3a, 3b insulating adhesive layer or adhesive layer; 4 second insulating resin layer; 5 first insulating resin layer; 10 terminal; 100 flexible printed circuit (FPC) substrate; 110 bump; 115 hot pressing tool; 120 glass substrate; A long axis direction of conductive particles; L width of bump group of FPC substrate; L1 long axis length of conductive particles; L2 short axis length of conductive particles; L3 closest distance between conductive particles when viewed from above; P arrangement axis of conductive particles; S film surface; θ angle between film surface and long axis direction of conductive particles.
Claims
1. An anisotropic conductive film, comprising conductive particles in an insulating adhesive layer, wherein: The aspect ratio of the conductive particles is 1.2 or more, the conductive particles are dispersed in a non-contact manner when viewed from above, the angle between the film surface of the anisotropic conductive film and the long axis direction of the conductive particles is less than 40°, and when the anisotropic conductive film is used to anisotropically conductively connect the connection terminal of the first electronic component and the connection terminal of the second electronic component, the connection terminal of the first electronic component and the connection terminal of the second electronic component are pressed into the insulating adhesive layer by thermal compression to sandwich the conductive particles between the connection terminal of the first electronic component and the connection terminal of the second electronic component in a line contact manner, The insulating adhesive layer contains a polymerizable resin and a thermal polymerization initiator or a photopolymerization initiator. The conductive particles are arranged regularly when viewed from above. A tangent line of a conductive particle in the short-side direction of the anisotropic conductive film coincides with a tangent line of a conductive particle adjacent to the conductive particle in the short-side direction of the anisotropic conductive film or penetrates the conductive particle adjacent to the conductive particle.
2. An anisotropic conductive film, comprising conductive particles in an insulating adhesive layer, wherein: The aspect ratio of the conductive particles is 1.2 or more, the conductive particles are dispersed in a non-contact manner when viewed from above, the angle between the film surface of the anisotropic conductive film and the long axis direction of the conductive particles is less than 40°, and when the anisotropic conductive film is used to anisotropically conductively connect the connection terminal of the first electronic component and the connection terminal of the second electronic component, the connection terminal of the first electronic component and the connection terminal of the second electronic component are pressed into the insulating adhesive layer by thermal compression to sandwich the conductive particles between the connection terminal of the first electronic component and the connection terminal of the second electronic component in a line contact manner, The insulating adhesive layer contains a polymerizable resin and a thermal polymerization initiator or a photopolymerization initiator. The major axis directions of the respective conductive particles regularly have different directions.
3. The anisotropic conductive film according to claim 1 or 2, wherein: The conductive particles are present at a fixed depth from the interface of the insulating adhesive layer, and the fixed depth is a depth greater than zero.
4. The anisotropic conductive film according to claim 1 or 2, wherein: The conductive particles are conductive columnar glass particles having a conductive layer on a part or the entirety of the surface.
5. The anisotropic conductive film according to claim 1 or 2, wherein: The conductive particles are cylindrical in shape.
6. The anisotropic conductive film according to claim 1 or 2, wherein: The aspect ratio of the conductive particles is 1.3 or more and 20 or less.
7. The anisotropic conductive film according to claim 1 or 2, wherein: The average major axis length of the conductive particles is 4 μm or more and 60 μm or less.
8. The anisotropic conductive film according to claim 1 or 2, wherein: The distance between any conductive particle and the conductive particle closest to the conductive particle in a plan view is 0.5 times or more the minor axis length of the conductive particle.
9. The anisotropic conductive film according to claim 1 or 2, wherein: Any conductive particle and the conductive particle closest to the conductive particle do not overlap in the longitudinal direction of the anisotropic conductive film.
10. The anisotropic conductive film according to claim 1 or 2, wherein: The angle formed by the film surface of the anisotropic conductive film and the major axis direction of the conductive particles is within 15°.
11. The anisotropic conductive film according to claim 10, wherein The major axis direction of the conductive particles is oriented in parallel with the film surface of the anisotropic conductive film.
12. The anisotropic conductive film according to claim 1 or 2, wherein: The major axis direction of the conductive particles is uniformly parallel to or oblique to the long side direction of the anisotropic conductive film in a plan view.
13. The anisotropic conductive film according to claim 2, wherein: The conductive particles are regularly arranged when viewed from above.
14. The anisotropic conductive film according to claim 1, wherein The conductive particles are arranged in a lattice shape when viewed from above.
15. The anisotropic conductive film according to claim 13, wherein The conductive particles are arranged in a lattice shape when viewed from above.
16. The anisotropic conductive film according to claim 15, wherein Among the conductive particles arranged on the axis in the film short-side direction, the tangent line in the film short-side direction of any conductive particle coincides with the tangent line in the film short-side direction of a conductive particle adjacent to the conductive particle.
17. The anisotropic conductive film according to claim 15, wherein Among the conductive particles arranged on the axis in the film short-side direction, an external tangent line in the film short-side direction of any conductive particle penetrates a conductive particle adjacent to the conductive particle.
18. The anisotropic conductive film according to any one of claims 1 to 17, wherein The insulating adhesive layer is composed of a plurality of insulating adhesive layers.
19. The anisotropic conductive film according to claim 1, wherein The adhesive layer has a two-layer structure of an insulating adhesive layer containing conductive particles and an insulating adhesive layer containing insulating spacers. 20 . A connection structure comprising anisotropically conductively connecting a connection terminal of a first electronic component and a connection terminal of a second electronic component using the anisotropic conductive film according to claim 1 .
21. A method for anisotropically conductively connecting a first electronic component to a second electronic component using the anisotropic conductive film according to any one of claims 1 to 19, wherein: The anisotropic conductive film is temporarily attached to the second electronic component, the first electronic component is placed on the temporarily attached anisotropic conductive film, and thermocompression bonding is performed from the first electronic component side.
22. A method for manufacturing a connection structure, wherein: The method comprises the step of anisotropically conductively connecting a connection terminal of a first electronic component and a connection terminal of a second electronic component using the anisotropic conductive film according to any one of claims 1 to 19.
Citation Information
Patent Citations
Fine-pitch anisotropic conductive adhesive
JP2002519473A
Anisotropically conductive adhesive sheet and fine connecting structure
JP2006335910A
Projection grain, conductive grain, conductive material and connection structure
JP2015008129A
Film adhesives and anisotropic conductive adhesives
CN102264853A
Conductive tape and method of connection with the tape
JP1996134417A