Methods for preparing controlled peptide-based polymers and copolymers in aqueous solutions

By using polymerization-induced self-assembly method in aqueous media, an amphiphilic polypeptide copolymer is prepared in a single step, solving the problem of multi-step and toxic solvent use in the prior art, and achieving rapid, simple, biocompatible nanoparticles Preparation, suitable for medicines and cosmetics.

CN114585664BActive Publication Date: 2024-11-19UNIVERSITE DE BORDEAUX +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080072425.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-03
Filing Date
2020-09-03
Publication Date
2024-11-19
Estimated Expiration
2040-09-03

AI Technical Summary

Technical Problem

The prior art has problems of multiple steps, the use of toxic organic solvents, sensitivity to water and humidity, and scale changes in the preparation of amphiphilic polypeptide nanomaterials, resulting in complex preparation and unfavorable regulatory approval.

Method used

Using a single step polymerization-induced self-assembly method (PISA) in aqueous media, two-dimensional solvent-free two-dimensional polymers containing amine functional groups are combined with hydrophobic α-amino acid N-carboxylic acid anhydride monomers. Preparation of virulent polypeptide copolymers to form stable nanoparticles.

Benefits of technology

Achieve rapid, simple, bioassimilable, biocompatible amphiphilic polypeptide copolymers, reduces the complexity of known methods, improves dry extraction rate, reduces the use of organic solvents, and is suitable for drugs and Cosmetic preparations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003596896620000031
    Figure BDA0003596896620000031
  • Figure BDA0003596896620000032
    Figure BDA0003596896620000032
  • Figure BDA0003596896620000041
    Figure BDA0003596896620000041
Patent Text Reader

Abstract

The present invention relates to a "one-pot" method for preparing an aqueous solution of nanoparticles of an amphiphilic block copolymer containing polypeptide units, the method comprising at least one step (E1), in an aqueous solvent, combining at least one hydrophilic polymer (P1) and at least one hydrophobic α-amino acid N-carboxyl intracyclic anhydride monomer, wherein the at least one hydrophilic polymer comprises at least one amine functional group.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The subject matter of the present invention relates to a process for the preparation of controlled peptidyl polymers and copolymers in aqueous solution, and to the products obtained. Background Art

[0002] Self-assembly of amphiphilic copolymers is a promising strategy to design advanced nanomaterials with unique properties. Among amphiphilic copolymers, peptides constitute an emerging class of biomaterials used as active carriers in pharmaceutical and cosmetic applications. To date, the most economical and efficient methods for preparing nanomaterials based on amphiphilic peptides are those that require several steps, including, inter alia, the ring-opening polymerization of N-carboxy intracyclic anhydride monomers (ROP or ROPISA).

[0003] This controlled polymerization uses the simplest reagents, but still has serious limitations, especially 1) tedious purification steps of N-carboxylic anhydride monomers; 2) significant sensitivity to water and humidity; and 3) implementation in toxic organic solvents (such as DMF), which must be removed later. The preparation of nanoparticles from amphiphilic polypeptides requires at least one second formation step, namely nanoprecipitation, which is the addition of a non-solvent for the hydrophobic segment to a copolymer solution in a common solvent for the two blocks. The nanoprecipitation step is usually carried out under relatively dilute conditions (<1 wt%) using toxic or volatile organic solvents and is sensitive to problems related to scale changes, which is usually not conducive to regulatory approval of this method.

[0004] Polymerization induced self-assembly (PISA) is a simple and reliable way to obtain amphiphilic polymers, with the advantage of obtaining nanoparticles of these same polymers simultaneously. The PISA method refers to the spontaneous self-assembly of active amphiphilic polymer chains in situ growth in nanostructures. So far, the PISA method has been implemented using free radical polymerization processes (RAFT, ATRP, NMP, CMP, TERP) in dispersions or emulsions. Summary of the invention

[0005] The present invention aims to provide functionalized nano-objects in a single preparation step.

[0006] Another object of the present invention is to provide a simple, rapid "one-pot" method to obtain amphiphilic peptide copolymers in an aqueous medium in a single step without the need for subsequent purification.

[0007] Another object of the present invention is to provide a polymerization process having very fast polymerization kinetics, thereby making it possible to obtain functionalized, bioassimilable, biocompatible and biodegradable polymers.

[0008] Therefore, the present invention relates to a "one-pot" method for preparing an aqueous solution of nanoparticles of an amphiphilic block copolymer comprising polypeptide units, said method comprising at least one step (E1) of combining together in an aqueous solvent free of organic solvents:

[0009] at least one hydrophilic polymer (P1) containing at least one amine functional group; and

[0010] At least one hydrophobic α-amino acid N-carboxyl cyclic anhydride monomer (NCA).

[0011] Thus, by the method of the present invention, an aqueous solution of nanoparticles of amphiphilic block copolymers based on polypeptides can be obtained or is obtained in an aqueous medium.

[0012] The method of the present invention is based on a polymerization-induced self-assembly method (referred to as PISA). By applying the PISA method to NCA monomers, the inventors unexpectedly determined that the spontaneous self-assembly of the PISA method protects NCA monomers from hydrolysis.

[0013] Thus, the present invention relates to the preparation of amphiphilic polypeptides by ring-opening polymerization in aqueous solution.

[0014] The method of the present invention is a method that does not require the use of an organic solvent. In the present invention, the method is carried out without any organic solvent.

[0015] In the present invention, the aqueous solvent does not include an organic solvent.

[0016] The present invention thus relates to a method for the preparation of controllable peptidyl polymers and copolymers in aqueous solution, as well as their spontaneous self-formation when carrying out the same method, thereby enabling the formation in a single preparation step of stable functionalized nanoparticles, which can be included, for example, in the preparation of pharmaceutical or cosmetic preparations, but is not limited thereto.

[0017] The method of the present invention is to prepare an amphiphilic polypeptide copolymer without an organic solvent, which is fast and controllable, and can also simultaneously form nanoparticles, and a dry extraction rate of more than 10% by weight, thereby reducing the complexity of the known methods. In particular, the present invention relates to a method for preparing an amphiphilic polypeptide copolymer with faster spontaneous self-formation by simultaneously carrying out these two steps in an aqueous medium without purification.

[0018] As stated above, the methods of the present invention involve the use of at least one hydrophobic NCA monomer.

[0019] Any hydrophobic NCA monomer may be used. Depending on the type of NCA monomer used, it may be modified to render it hydrophobic, inter alia, by means of hydrophobic protecting groups.

[0020] In one embodiment, the hydrophobic α-amino acid N-carboxyl intracyclic anhydride monomer has the following formula (I):

[0021]

[0022] wherein R is an optionally protected, natural or modified hydrophobic α-amino acid side chain.

[0023] When the NCA monomer used is an NCA of a hydrophilic α-amino acid (especially containing OH, COOH or NH2 functional groups), the above R group contains a hydrophobic protecting group to make the monomer hydrophobic.

[0024] When the NCA used is that of an α-amino acid which is hydrophobic in nature, such protection is not necessary.

[0025] As hydrophobic α-amino acid N-carboxyl intracyclic anhydride monomers, the following compounds are used in particular:

[0026]

[0027] Preferred examples may be NCA monomers of γ-benzyl-L-glutamic acid, ε-Boc-L-lysine, L-leucine or L-phenylalanine.

[0028] As mentioned above, the process of the present invention comprises the use of at least one hydrophilic polymer (P1) containing at least one amine function. The hydrophilic polymer acts as a macroinitiator.

[0029] In one embodiment, the polymer (P1) is selected from the group consisting of polyethers, polyesters, poly(meth)acrylates, polysaccharides, polypeptides, polypeptides, DNA and protein derivatives, in particular elastin-like polypeptides (ELPs) containing at least one amine functional group, and is preferably selected from poly(ethylene oxide) having at least one amine functional group.

[0030] Preferably, polymer (P1 ) is PEG.

[0031] Preferably, the hydrophilic polymer (P1) has a molecular weight higher than 500 g / mol, more preferably a molecular weight between 2000 g / mol and 10000 g / mol.

[0032] Preferably, polymer (P1) has the following formula:

[0033]

[0034] where x is from 16 to 500.

[0035] In the method of the present invention, the starting product may be similar to a suspension, ie, an opaque, heterogeneous medium, while the final product obtained is preferably in the form of a homogeneous, transparent solution.

[0036] Thus, by the process of the present invention, highly heterogeneous media, in particular solids dispersed in water, can be advantageously converted into solutions of well-defined nanoparticles based on amphiphilic copolymers of controlled macromolecular structure.

[0037] The process of the present invention is a "one-pot" process, ie, the reagents undergo one or more sequential or simultaneous reactions in a single reaction mixture.

[0038] In one embodiment, in the methods of the present invention, the aqueous solvent is water or a buffer.

[0039] For example, an aqueous solvent is water to which a buffer solution has been added.

[0040] In one embodiment, the aqueous solvent further comprises a buffer solution comprising a salt in a concentration range of 0.01 M to 1 M, in particular selected from the group formed by sodium bicarbonate solution and phosphate buffer solution.

[0041] Preferably, the method of the present invention uses an aqueous solution of NaHCO3.

[0042] Preferably, the pH value of the aqueous solvent is between 2 and 12, in particular between 7 and 10.

[0043] In one embodiment, the temperature of step (E1) is from -10°C to 80°C, preferably from 0°C to 4°C.

[0044] In one embodiment, step (E1) is carried out with stirring from a dispersion of hydrophobic α-amino acid N-carboxyl intracyclic anhydride monomers.

[0045] The process of the present invention can also be applied to obtain multi-block copolymers.

[0046] Therefore, in one embodiment, the aqueous solution of nanoparticles of the amphiphilic block copolymer obtained after step (E1) is subsequently contacted with a second hydrophobic α-amino acid N-carboxyl ring anhydride monomer, thereby obtaining an aqueous solution of modified nanoparticles of the modified amphiphilic block copolymer, wherein the second hydrophobic α-amino acid N-carboxyl ring anhydride monomer is the same as or different from the monomer in step (E1).

[0047] Therefore, in this embodiment, when the at least one second hydrophobic α-amino acid N-carboxyl intracyclic anhydride monomer added is different from the monomer used in step (E1), a gradient or statistical multi-block copolymer can be obtained.

[0048] The method of the invention can be used to obtain nanoparticles, preferably core-corona shaped, preferably elongated, preferably rigid, preferably having a size ranging from 2 nm to 1 μm. Thus, in this embodiment, nanoparticles having anisotropic optical properties can be obtained.

[0049] The present invention also relates to nanoparticles of amphiphilic block copolymers and comprising polypeptide units obtainable by a process such as defined above.

[0050] Therefore, the present invention also relates to nanoparticles of amphiphilic block copolymers comprising polypeptide units obtained by a process such as defined above, said nanoparticles having a core-shell structure and a particle size ranging from 2 nm to 1 μm.

[0051] Therefore, the invention also relates to an aqueous composition comprising nanoparticles such as defined above in an amount of at least 2% by weight relative to the weight of the aqueous composition, preferably between 2% and 15% by weight relative to the weight of the aqueous composition.

[0052] The solid content was measured after polymerization and after purification of the salts by dialysis by lyophilization (comparison of the weight of the residue with the weight before lyophilization). BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 It involves the PEG in Example 1 5k Size exclusion chromatogram of DMF (+1 mg / mL LiBr) of -b-PBLG copolymer. Left: RI detection. Right: Absorbance detection.

[0054] Figure 2 It is shown that the PEG in Example 1 5k -b-PBLG copolymer obtained by CDCl3 + 15% TFA 1 H NMR spectrum.

[0055] Figure 3 The PEG in Example 1 is shown 5k - Distribution of hydrodynamic diameter (Dh) of b-PBLG nanoparticles expressed as diffusion intensity (in ultrapure water).

[0056] Figure 4 The nanoparticle images taken by cryo-transmission electron microscopy (Cryo-TEM) are given: PEG in Example 1 5k -b-PBLG copolymer nanoparticles.

[0057] Figure 5 It is shown that the PEG in Example 2 5kSize exclusion chromatogram of DMF (+1 mg / mL LiBr) of -b-PBLG copolymer. Left: RI detection. Right: Absorbance detection.

[0058] Figure 6 It is shown that the PEG in Example 2 5k -b-PBLG copolymer obtained by CDCl3 + 15% TFA 1 H NMR spectrum.

[0059] Figure 7 The PEG in Example 2 is given 5k Cryo-TEM image of nanoparticles of -b-PBLG copolymer.

[0060] Figure 8 It is shown that the PEG in Example 3 5k Size exclusion chromatogram of DMF (+1 mg / mL LiBr) of -b-PBLG copolymer. Left: RI detection. Right: Absorbance detection.

[0061] Fig. 9 It is shown that the PEG in Example 3 5k -b-PBLG copolymer obtained by CDCl3 + 15% TFA 1 H NMR spectrum.

[0062] Fig.10 The PEG in Example 3 is given 5k - Distribution of hydrodynamic diameters (Dh) of b-PBLG nanoparticles (in ultrapure water) (expressed as diffusion intensity).

[0063] Fig.11 It is shown that the PEG in Example 4 5k Size exclusion chromatogram of DMF (+1 mg / mL LiBr) of -b-PBLG copolymer. Left: RI detection. Right: Absorbance detection.

[0064] Fig.12 Given the PEG in Example 4 5k -b-PBLG copolymer obtained by CDCl3 + 15% TFA 1 H NMR spectrum.

[0065] Fig.13 The PEG in Example 4 is given 5k - Distribution of hydrodynamic diameters (Dh) of b-PBLG nanoparticles (in ultrapure water) (expressed as diffusion intensity).

[0066] Fig.14 The PEG in Example 4 is given 5kCryo-TEM image of nanoparticles of -b-PBLG copolymer.

[0067] Fig.15 It is shown that the PEG in Example 5 5k Size exclusion chromatogram of a -b-PBLG copolymer in DMF (+1 mg / mL LiBr). RI detection is shown in black and gray, and absorbance detection is shown in gray dashed line.

[0068] Fig.16 Given the PEG in Example 5 5k - Distribution of hydrodynamic diameter (Dh) of b-PBLG nanoparticles (in ultrapure water) (expressed as diffusion intensity).

[0069] Fig.17 It is shown that the PEG in Example 6 5k Size exclusion chromatogram of DMF (+1 mg / mL LiBr) of -b-PBLG copolymer. Left: RI detection. Right: Absorbance detection.

[0070] Fig.18 Given the PEG in Example 6 5k -b-PBLG copolymer obtained by CDCl3 + 15% TFA 1 H NMR spectrum.

[0071] Fig.19 The PEG in Example 6 is given 5k Cryo-TEM image of nanoparticles of -b-PBLG copolymer.

[0072] Fig. 20 Shown are: A) size exclusion chromatogram (RI detection) obtained from a DMF (+1 mg / mL LiBr) solution of the ELPM40-b-PBLG copolymer in Example 7; B) TEM image of nanoparticles of the ELPN40-b-PBLG copolymer in Example 7 (stained with uranyl acetate).

[0073] Fig.21 It is shown that the PEG in Example 8 5k Size exclusion chromatogram of DMF (+1 mg / mL LiBr) of -b-PLys copolymer. Refractive index (RI) detection.

[0074] Fig. 22 Given the PEG in Example 8 5k -b-PLys copolymer obtained in DMF-d6 1 H NMR spectrum.

[0075] Fig.23 The PEG in Example 8 is given5k -b-Distribution of the hydrodynamic diameter (Dh) of PLys nanoparticles (in ultrapure water) (expressed as diffusion intensity).

[0076] Fig.24 The PEG in Example 8 is given 5k Cryo-TEM image of nanoparticles of -b-PLys copolymer.

[0077] Fig.25 It is shown that the PEG in Example 9 5k Size exclusion chromatogram of DMF (+1 mg / mL LiBr) of -b-PLys-b-PBLG copolymer. RI detection.

[0078] Fig.26 Shown are: A) the size exclusion chromatogram (RI detection) obtained from DMF (+1 mg / mL LiBr) of the PLeu-b-PBLG copolymer in Example 10; B) the TEM image of the nanoparticles of the PLeu-b-PBLG copolymer in Example 10 (stained with uranyl acetate).

[0079] Fig. 27 Shown are: A) size exclusion chromatogram (RI detection) obtained from DMF (+1 mg / mL LiBr) of the PPhe-b-PBLG copolymer in Example 11; B) TEM image of nanoparticles of the PPhe-b-PBLG copolymer in Example 11 (stained with uranyl acetate).

[0080] Fig.28 Shown: A) by PEG in Example 12 5k -b-PBLG-b-PEG 5k Size exclusion chromatogram (RI detection) of DMF (+1 mg / mL LiBr) of copolymer; B) PEG in Example 12 5k -b-PBLG-b-PEG 5k TEM image of copolymer nanoparticles (stained with uranyl acetate).

[0081] Fig.29 Shown are: A) size exclusion chromatogram (RI detection) obtained from DMF (+1 mg / mL LiBr) of the PEG-4-arm-b-(PBLG)4 copolymer in Example 13; B) TEM image of nanoparticles of the PEG-4-arm-b-(PBLG)4 copolymer in Example 13 (stained with uranyl acetate).

[0082] Fig.30Shown are: A) size exclusion chromatogram (RI detection) obtained from DMF (+1 mg / mL LiBr) of the PSar-b-PBLG copolymer in Example 14; B) TEM image of nanoparticles of the PSar-b-PBLG copolymer in Example 14 (stained with uranyl acetate).

[0083] Fig.31 Shown are: A) the size exclusion chromatogram (RI detection) obtained from the PGA-b-PBLG copolymer in Example 15 in H2O (Juanito buffer); B) the TEM image of the nanoparticles of the PGA-b-PBLG copolymer in Example 15 (uranyl acetate staining).

[0084] Fig.32 Shown are: A) infrared analysis of Example 16 (powder); B) TEM image of nanoparticles of the copolymer in Example 16 (stained with uranyl acetate).

[0085] Fig.33 It is shown that the PEG in Example 17 5k -Exclusion chromatogram (RI detection) of DMF (+1 mg / mL LiBr) of b-PBLG copolymer.

[0086] Figure 34 shows: A) TEM image of nanoparticles of the copolymer in Example 18 (stained with uranyl acetate); B) distribution of hydrodynamic diameter (Dh) of the nanoparticles in Example 18 (in ultrapure water) (expressed as diffusion intensity); C) electrophoresis gel showing the formation of the copolymer in Example 18. DETAILED DESCRIPTION

[0087] Example

[0088] Example 1: Amphiphilic Peptide Diblock Copolymer Poly(ethylene glycol) 5k Concomitant Synthesis of -block-poly(γ-benzyl-L-glutamic acid) and Its Corresponding Nanoparticles

[0089] γ-Benzyl-L-glutamic acid N-carboxyl ring anhydride monomer (BLG-NCA) is a commercial chemical reagent sold by ISOCHEM. 5k -NH2 (Mp = 5516Da, ) was sold by RAPP Polymer, Inc. Other reagents were sold by Sigma-Aldrich.

[0090] Under an inert atmosphere, NCA monomer of γ-benzyl-L-glutamic acid (300 mg, 1.14 mmol) was placed in a Schlenk tube containing a magnetic stir bar. The Schlenk tube was cooled in an ice bath for at least 10 minutes. Meanwhile, a PEG-containing macroinitiator was prepared. 5k -NH2 (8mL, 300mg, 0.06mmol) was added to a 0.05M aqueous solution of NaHCO3 and cooled in an ice bath for at least 10 minutes. While keeping the aqueous solution in an ice bath, it was added to the NCA powder under vigorous stirring. A milky dispersion was obtained due to the immiscibility of the monomers in the aqueous phase. The reaction was stirred 1) first in an ice water bath for about 2 hours, and 2) then at ambient temperature for 16 hours. The milky dispersion became an aqueous milky white colloidal solution, which was then transferred to a dialysis tube (3.5kDa dialysis membrane) and dialyzed with ultrapure water for 2 days. A white powder was obtained after lyophilization with a yield of 85±3% ( Figures 1 to 4 ).

[0091] Example 2: Amphiphilic peptide diblock copolymer poly(ethylene glycol) under salt-free conditions 5k Concomitant Synthesis of -block-poly(γ-benzyl-L-glutamic acid) and Its Corresponding Nanoparticles

[0092] γ-Benzyl-L-glutamic acid N-carboxyl ring anhydride monomer (BLG-NCA) is a commercial chemical reagent sold by ISOCHEM. 5k -NH2 (Mp = 5516Da, ) was sold by RAPP Polymer, Inc. Other reagents were sold by Sigma-Aldrich.

[0093] Under an inert atmosphere, NCA monomer of γ-benzyl-L-glutamic acid (300 mg, 1.14 mmol) was placed in a Schlenk tube containing a magnetic stir bar. The Schlenk tube was cooled in an ice bath for at least 10 minutes. 5k -NH2 (8mL, 300mg, 0.06mmol) was diluted in ultrapure water and cooled in an ice bath for at least 10 minutes. While the aqueous solution was kept in an ice bath, it was added to the NCA powder under vigorous stirring. A milky dispersion was obtained due to the immiscibility of the monomers in the aqueous phase. The reaction was stirred 1) first in an ice-water bath for about 2 hours, 2) then at ambient temperature for 16 hours. The milky dispersion became an aqueous milky white colloidal solution, which was then transferred to a dialysis tube (dialysis membrane of 3.5kDa) and dialyzed with ultrapure water for 2 days. A white powder ( Figures 5 to 7 ).

[0094] Example 3: High solids content amphiphilic peptide diblock copolymer poly(ethylene glycol) 5k Concomitant Synthesis of -block-poly(γ-benzyl-L-glutamic acid) and Its Corresponding Nanoparticles

[0095] γ-Benzyl-L-glutamic acid N-carboxyl ring anhydride monomer (BLG-NCA) is a commercial chemical reagent sold by ISOCHEM. 5k -NH2 (Mp = 5516Da, ) is sold by RAPP Polymer, Inc. Other reagents are sold by Sigma-Aldrich.

[0096] Under an inert atmosphere, NCA monomer of γ-benzyl-L-glutamic acid (600 mg, 2.28 mmol) was placed in a Schlenk tube containing a magnetic stir bar. The Schlenk tube was cooled in an ice bath for at least 10 minutes. Meanwhile, a 5% PEG-containing macroinitiator was prepared. 5k -NH2 (8mL, 600mg, 0.12mmol) was added to a 0.05M aqueous solution of NaHCO3 and cooled in an ice bath for at least 10 minutes. While the aqueous solution was kept in an ice bath, it was added to the NCA powder under vigorous stirring. A milky dispersion was obtained due to the immiscibility of the monomers in the aqueous phase. The reaction was stirred 1) first in an ice water bath for about 2 hours, and 2) then at ambient temperature for 16 hours. The milky dispersion became an aqueous milky white colloidal solution, which was then transferred to a dialysis tube (3.5kDa dialysis membrane) and dialyzed with ultrapure water for 2 days. A white powder was obtained after lyophilization with a yield of 77% ( Figures 8 to 10 ).

[0097] Example 4: Extended Amphiphilic Peptide Diblock Copolymer Poly(ethylene glycol) 5k -block-poly(γ-benzyl-L-glutamic acid) chain scheme

[0098] γ-Benzyl-L-glutamic acid N-carboxyl ring anhydride monomer (BLG-NCA) is a commercial chemical reagent sold by ISOCHEM. 5k -NH2 (Mp = 5516Da, ) is sold by RAPP Polymer, Inc. Other reagents are sold by Sigma-Aldrich.

[0099] Under an inert atmosphere, NCA monomer of γ-benzyl-L-glutamic acid (300 mg, 1.14 mmol) was placed in a Schlenk tube containing a magnetic stir bar. The Schlenk tube was cooled in an ice bath for at least 10 minutes. Meanwhile, a PEG-containing macroinitiator was prepared. 5k -NH2 (8mL, 300mg, 0.06mmol) in a 0.05M aqueous solution of NaHCO3 and cooled in an ice bath for at least 10 minutes. While keeping the aqueous solution in an ice bath, it was added to the NCA powder under vigorous stirring. A milky dispersion was obtained due to the immiscibility of the monomers in the aqueous phase. After 90 minutes, NCA (300mg, 1.14mmol) of γ-benzyl-L-glutamate was added for the second time. The reaction was stirred 1) first in an ice water bath for about 2 hours, and 2) then stirred at ambient temperature for 16 hours. The milky dispersion became an aqueous milky white colloidal solution, which was then transferred to a dialysis tube (3.5kDa dialysis membrane) and dialyzed with ultrapure water for 2 days. A white powder was obtained after lyophilization with a yield of 85% ( Figures 11 to 14 ).

[0100] Example 5: Amphiphilic Peptide Diblock Copolymer Poly(ethylene glycol) 2k Concomitant Synthesis of -block-poly(γ-benzyl-L-glutamic acid) and Its Corresponding Nanoparticles

[0101] γ-Benzyl-L-glutamic acid N-carboxyl ring anhydride monomer (BLG-NCA) is a commercial chemical reagent sold by ISOCHEM. 2k -NH2 (Mp = 2022Da, ) is sold by RAPP Polymer, Inc. Other reagents are sold by Sigma-Aldrich.

[0102] Under an inert atmosphere, NCA monomer of γ-benzyl-L-glutamic acid (30 mg, 0.11 mmol) was placed in a Schlenk tube containing a magnetic stir bar. The Schlenk tube was cooled in an ice bath for at least 10 minutes. 2k-NH2 (800 μ L, 30 mg, 0.015 mmol) 0.2 M NaHCO3 aqueous solution and cooled in an ice bath for at least 10 minutes. While keeping the aqueous solution in an ice bath, add it to the NCA powder under vigorous stirring. Obtain a milky dispersion due to the immiscibility of the monomers in the aqueous phase. The reaction was stirred 1) first in an ice-water bath for about 2 hours, 2) then at ambient temperature for 16 hours. The milky dispersion becomes an aqueous colloidal solution, which is then transferred to a dialysis tube (dialysis membrane of 3.5 kDa) and dialyzed with ultrapure water for 2 days. A white powder ( Fig.15 and Fig.16 ).

[0103] Example 6: Amphiphilic Peptide Diblock Copolymer Poly(ethylene glycol) 10k Concomitant Synthesis of -block-poly(γ-benzyl-L-glutamic acid) and Its Corresponding Nanoparticles

[0104] γ-Benzyl-L-glutamic acid N-carboxyl ring anhydride monomer (BLG-NCA) is a commercial chemical reagent sold by ISOCHEM. 10k -NH2 (Mp = 11153Da, ) is sold by RAPP Polymer, Inc. Other reagents are sold by Sigma-Aldrich.

[0105] Under an inert atmosphere, NCA monomer of γ-benzyl-L-glutamic acid (300 mg, 1.14 mmol) was placed in a Schlenk tube containing a magnetic stir bar. The Schlenk tube was cooled in an ice bath for at least 10 minutes. Meanwhile, a PEG-containing macroinitiator was prepared. 10k -NH2 (8mL, 300mg, 0.03mmol) 0.05M NaHCO3 aqueous solution and cooled in an ice bath for at least 10 minutes. While the aqueous solution is kept in an ice bath, it is added to the NCA powder under vigorous stirring. A milky dispersion is obtained due to the immiscibility of the monomers in the aqueous phase. The reaction is stirred 1) first in an ice-water bath for about 2 hours, 2) then at ambient temperature for 16 hours. The milky dispersion becomes a gel, which is then transferred to a dialysis tubing (dialysis membrane of 3.5kDa) and dialyzed with ultrapure water for 2 days. A white powder ( Figures 17 to 19 ).

[0106] Example 7: Concomitant Synthesis of Amphiphilic Peptide Diblock Copolymers (Elastin-Like Polypeptides)-block-Poly(γ-Benzyl-L-Glutamic Acid) and Their Corresponding Nanoparticles

[0107] γ-Benzyl-L-glutamic acid N-carboxycyclic anhydride monomer (BLG-NCA) is a commercial chemical sold by ISOCHEM. Elastin-like polypeptide (ELP) is a recombinant protein produced by Escherichia coli (E.Coli) in the laboratory: Laboratoire de Chimie des Polymères Organiques de Bordeaux, France. The ELP used has a primary amine at its N-terminus. Its structure is MW (VPGVPVPGMG VPGVG VPGVG) 10 And the molecular weight is 17035 Da. Other unconventional reagents are sold by Sigma-Aldrich.

[0108] Under an inert atmosphere, the NCA monomer (10 mg, 0.04 mmol) of γ-benzyl-L-glutamic acid was placed in a test tube containing a magnetic stirring bar. The test tube was cooled in an ice bath for at least 10 minutes. At the same time, a 0.05M aqueous solution of NaHCO3 containing a macroinitiator ELP (2.7 mL, 10 mg, 0.001 mmol) was prepared and cooled in an ice bath for at least 10 minutes. While the aqueous solution was kept in an ice bath, it was added to the NCA powder under vigorous stirring. A milky dispersion was obtained due to the immiscibility of the monomers in the aqueous phase. The reaction was allowed to proceed at 4 ° C under magnetic stirring for 20 hours. At ambient temperature, the milky dispersion became a turbid dispersion and was transferred to a dialysis tube (dialysis membrane of 3.5 kDa) and dialyzed with ultrapure water at 4 ° C for 2 days. A white powder ( Fig. 20 ).

[0109] Example 8: Concomitant Synthesis of Amphiphilic Peptide Diblock Copolymer Poly(ethylene glycol)-block-Poly(ε-Boc-L-lysine) and Its Corresponding Nanoparticles

[0110] The monomer of ε-tert-butyloxycarbonyl-L-lysine N-carboxyl intracyclic anhydride (LysBOC-NCA) is a commercial product sold by ISOCHEM. 5k -NH2 (Mp = 5516Da, ) is sold by RAPP Polymer, Inc. Other unconventional reagents are sold by Sigma-Aldrich.

[0111] Under an inert atmosphere, NCA monomer of ε-Boc-L-lysine (310 mg, 1.14 mmol) was placed in a Schlenk tube containing a magnetic stir bar. The Schlenk tube was cooled in an ice bath for at least 10 minutes. 5k-NH2 (8mL, 300mg, 0.06mmol) in a 0.05M aqueous solution of NaHCO3 and cooled it in an ice bath for at least 10 minutes. While keeping the aqueous solution in an ice bath, add it to the NCA powder under vigorous stirring. A milky dispersion is obtained due to the immiscibility of the monomers in the aqueous phase. The reaction is kept under stirring 1) first in an ice water bath for about 2 hours, and 2) then at ambient temperature for 16 hours. The milky dispersion becomes an aqueous milky white colloidal solution, which is then transferred to a dialysis tube (3.5kDa dialysis membrane) and dialyzed with ultrapure water for 2 days. A white powder is obtained after lyophilization with a yield of 79% ( Figure 21 to Figure 24 ).

[0112] Example 9: Concomitant Synthesis of Amphiphilic Peptide Triblock Copolymer Poly(ethylene glycol)-block-Poly(ε-Boc-L-lysine)-block-Poly(γ-benzyl-L-glutamic acid) and Its Corresponding Nanoparticles

[0113] γ-Benzyl-L-glutamic acid N-carboxylic anhydride (BLG-NCA) and ε-tert-butyloxycarbonyl-L-lysine N-carboxylic anhydride (LysBOC-NCA) monomers are commercial products sold by ISOCHEM. 5k -NH2 (Mp = 5516Da, ) is sold by RAPP Polymer, Inc. Other unconventional reagents are sold by Sigma-Aldrich.

[0114] Under an inert atmosphere, NCA monomer of ε-Boc-L-lysine (300 mg, 1.10 mmol) was placed in a Schlenk tube containing a magnetic stir bar. The Schlenk tube was cooled in an ice bath for at least 10 minutes. 5k-NH2 (8mL, 300mg, 0.06mmol) 0.2M NaHCO3 aqueous solution and cooled it in an ice bath for at least 10 minutes. While the aqueous solution is kept in an ice bath, it is added to the NCA powder under vigorous stirring. A milky dispersion is obtained due to the immiscibility of the monomer in the aqueous phase. The reaction is kept in an ice-water bath for about 15 minutes under stirring. Meanwhile, under an inert atmosphere, the NCA monomer (BLG-NCA, 300mg, 1.14mmol) of γ-benzyl-L-glutamic acid is placed in a Schlenk tube comprising a magnetic stirring bar. The Schlenk tube is cooled in an ice bath for at least 10 minutes. While the aqueous milky colloidal solution is kept in an ice bath, it is mixed with the BLG-NCA powder under vigorous stirring. A milky dispersion is obtained due to the immiscibility of the monomer in the aqueous phase. The reaction was stirred 1) first in an ice-water bath for about 2 hours and 2) then at ambient temperature for 16 hours. The milky dispersion became an aqueous milky colloidal solution, which was then transferred to a dialysis tube (dialysis membrane of 3.5 kDa) and dialyzed against ultrapure water for 2 days. A white powder was obtained after freeze-drying with a yield of 75 ± 3% ( Fig.25 ).

[0115] Example 10: Amphiphilic Peptide Diblock Copolymer Poly(ethylene glycol) 5k Simultaneous synthesis of -block-poly(L-leucine) and its corresponding nanoparticles

[0116] L-Leucine N-carboxycyclic anhydride monomer (LEU-NCA) is a commercial chemical reagent sold by ISOCHEM. 5k -NH2 (Mp = 5516Da, ) is sold by RAPP Polymer, Inc. Other reagents are sold by Sigma-Aldrich.

[0117] Under an inert atmosphere, NCA monomer of leucine (300 mg, 1.9 mmol) was placed in a Schlenk tube containing a magnetic stir bar. The Schlenk tube was cooled in an ice bath for at least 10 minutes. 5k-NH2 (8mL, 300mg, 0.06mmol) in a 0.05M aqueous solution of NaHCO3 and cooled it in an ice bath for at least 10 minutes. While keeping the aqueous solution in an ice bath, add it to the NCA powder under vigorous stirring. A milky dispersion is obtained due to the immiscibility of the monomers in the aqueous phase. The reaction is kept under stirring 1) first in an ice water bath for about 2 hours, and 2) then at room temperature for 16 hours. The milky dispersion becomes an aqueous milky white colloidal solution, which is then transferred to a dialysis tube (3.5kDa dialysis membrane) and dialyzed with ultrapure water for 2 days. A white powder is obtained after lyophilization with a yield of 77% ( Fig.26 ).

[0118] Example 11: Amphiphilic Peptide Diblock Copolymer Poly(ethylene glycol) 5k Concomitant Synthesis of -block-Poly(L-phenylalanine) and Its Corresponding Nanoparticles

[0119] L-phenylalanine N-carboxycyclic anhydride monomer (PHE-NCA) is a commercial chemical reagent sold by ISOCHEM. 5k -NH2 (Mp = 5516Da, ) is sold by RAPP Polymer, Inc. Other reagents are sold by Sigma-Aldrich.

[0120] Under an inert atmosphere, NCA monomer of phenylalanine (150 mg, 0.8 mmol) was placed in a Schlenk tube containing a magnetic stir bar. The Schlenk tube was cooled in an ice bath for at least 10 minutes. 5k -NH2 (8mL, 300mg, 0.06mmol) in a 0.05M aqueous solution of NaHCO3 and cooled it in an ice bath for at least 10 minutes. While keeping the aqueous solution in an ice bath, add it to the NCA powder under vigorous stirring. A milky dispersion is obtained due to the immiscibility of the monomers in the aqueous phase. The reaction is kept under stirring 1) first in an ice water bath for about 2 hours, and 2) then at ambient temperature for 16 hours. The milky dispersion becomes an aqueous milky white colloidal solution, which is then transferred to a dialysis tube (3.5kDa dialysis membrane) and dialyzed with ultrapure water for 2 days. A white powder is obtained after lyophilization with a yield of 72% ( Fig. 27 ).

[0121] Example 12: Amphiphilic peptide triblock copolymer poly(γ-benzyl-L-glutamic acid-block-poly(ethylene glycol) 5k -block-poly(γ-benzyl-L-glutamic acid)) and its corresponding nanoparticles

[0122] γ-Benzyl-L-glutamic acid N-carboxyl ring anhydride monomer (BLG-NCA) is a commercial chemical reagent sold by ISOCHEM. NH2-PEG 5k -NH2 (PEG-2 arm) was sold by RAPP Polymer, Inc. Other reagents were sold by Sigma-Aldrich.

[0123] Under an inert atmosphere, γ-benzyl-L-glutamic acid N-carboxyl ring anhydride NCA monomer (BLG-NCA) (29 mg, 0.11 mmol) was placed in a test tube containing a magnetic stirring bar. The test tube was cooled in an ice bath for at least 10 minutes. At the same time, a 5% ethanol solution containing a macroinitiator NH2-PEG was prepared. 5k -NH2 (0.85mL, 35mg) 0.05M NaHCO3 aqueous solution and cooled it in an ice bath for at least 10 minutes. While keeping the aqueous solution in an ice bath, add it to the NCA powder under vigorous stirring. Obtain a milky dispersion due to the immiscibility of the monomers in the aqueous phase. The reaction was stirred 1) first in an ice-water bath for about 2 hours, 2) then at ambient temperature for 16 hours. The milky dispersion becomes an aqueous milky white colloidal solution, which is transferred to a dialysis tubing (dialysis membrane of 3.5kDa) and dialyzed with ultrapure water for 2 days. A white powder ( Fig.28 ).

[0124] Example 13: Amphiphilic peptide star copolymer poly(γ-benzyl-L-glutamic acid) 4-block-poly(ethylene glycol) 5k Concomitant synthesis of its corresponding nanoparticles

[0125] γ-Benzyl-L-glutamic acid N-carboxyl ring anhydride monomer (BLG-NCA) is a commercial chemical reagent sold by ISOCHEM. PEG-4 arms are sold by RAPP Polymer (star shape: 4 NH2 ends). Other reagents are sold by Sigma-Aldrich.

[0126] Under an inert atmosphere, γ-benzyl-L-glutamic acid N-carboxyl ring anhydride NCA monomer (BLG-NCA) (18 mg, 0.07 mmol) was placed in a test tube containing a magnetic stirring bar. The test tube was cooled in an ice bath for at least 10 minutes. At the same time, a PEG-containing macroinitiator was prepared. 5k -4-arm (PEG 5k-4arm) (0.70mL, 35mg) of 0.05M NaHCO3 aqueous solution and cooled it in an ice bath for at least 10 minutes. While keeping the aqueous solution in an ice bath, add it to the NCA powder under vigorous stirring. A milky dispersion is obtained due to the immiscibility of the monomers in the aqueous phase. The reaction is kept under stirring 1) first in an ice-water bath for about 2 hours, 2) then at ambient temperature for 16 hours. The milky dispersion becomes an aqueous milky white colloidal solution, which is transferred to a dialysis tube (dialysis membrane of 3.5kDa) and dialyzed with ultrapure water for 2 days. A white powder ( Fig.29 ).

[0127] Example 14: Concomitant Synthesis of Amphiphilic Peptide Diblock Copolymer Poly(sarcosine)-block-(γ-benzyl-L-glutamate) and Its Corresponding Nanoparticles

[0128] γ-Benzyl-L-glutamic acid N-carboxyl ring anhydride monomer (BLG-NCA) is a commercial chemical reagent sold by ISOCHEM. Poly(sarcosine) PSar (Mp = 2100 Da, ) was synthesized in the laboratory by conventional ring-opening polymerization. Other reagents were sold by Sigma-Aldrich.

[0129] Under an inert atmosphere, the NCA monomer of γ-benzyl-L-glutamic acid (120 mg, 0.46 mmol) was placed in a Schlenk tube containing a magnetic stirring bar. The Schlenk tube was cooled in an ice bath for at least 10 minutes. At the same time, a 0.05M aqueous solution of NaHCO3 containing a macromolecular initiator (4 mL, 50 mg, 0.02 mmol) was prepared and cooled in an ice bath for at least 10 minutes. While the aqueous solution was kept in an ice bath, it was added to the NCA powder under vigorous stirring. A milky dispersion was obtained due to the immiscibility of the monomers in the aqueous phase. The reaction was stirred 1) first in an ice water bath for about 2 hours, 2) then at ambient temperature for 16 hours. The milky dispersion became an aqueous milky white colloidal solution, which was transferred to a dialysis tube (dialysis membrane of 3.5 kDa) and dialyzed with ultrapure water for 2 days. A white powder was obtained after lyophilization with a yield of 55% ( Fig.30 ).

[0130] Example 15: Concomitant Synthesis of Amphiphilic Peptide Diblock Copolymers Poly(L-Glutamic Acid)-block-Poly(γ-Benzyl-L-Glutamic Acid) and Their Corresponding Nanoparticles

[0131] γ-Benzyl-L-glutamic acid N-carboxyl ring anhydride monomer (BLG-NCA) is a commercial chemical reagent sold by ISOCHEM. Poly(L-glutamic acid) PGA (Mw=6600 g / mol) was synthesized in the laboratory by conventional ring-opening polymerization. Other reagents were sold by Sigma-Aldrich.

[0132] Under an inert atmosphere, the NCA monomer (300 mg, 1.14 mmol) of γ-benzyl-L-glutamic acid was placed in a Schlenk tube containing a magnetic stirring bar. The Schlenk tube was cooled in an ice bath for at least 10 minutes. At the same time, a 0.20 M aqueous solution of NaHCO3 containing a macromolecular initiator (8 mL, 300 mg, 0.45 mmol) was prepared and cooled in an ice bath for at least 10 minutes. While the aqueous solution was kept in an ice bath, it was added to the NCA powder under vigorous stirring. A milky dispersion was obtained due to the immiscibility of the monomer in the aqueous phase. The reaction was first kept in an ice water bath for about 2 hours under stirring, and then kept at ambient temperature for 16 hours. The milky dispersion becomes an aqueous milky colloidal solution, which is transferred to a dialysis tube (dialysis membrane of 3.5 kDa) and dialyzed with ultrapure water for 2 days (TEM images, Fig.31 After lyophilization, the PBLG block was deprotected under mild acidic conditions (MSA, TFA) to obtain a white powder that could be analyzed in aqueous SEC (Juanito buffer) ( Fig.31 ).

[0133] Example 16: Concomitant Synthesis of Amphiphilic Peptide Diblock Copolymer Polysaccharide-block-Poly(γ-Benzyl-L-Glutamic Acid) and Its Corresponding Nanoparticles

[0134] γ-Benzyl-L-glutamic acid N-carboxyl cyclic anhydride monomer (BLG-NCA) is a commercial chemical reagent sold by ISOCHEM. Polyamino sugar (Polysacc., Mw=7750 g / mol) was synthesized in the laboratory by anionic polymerization of β-lactam monomers. Other reagents were sold by Sigma-Aldrich.

[0135] Under an inert atmosphere, the NCA monomer (13mg, 0.05mmol) of γ-benzyl-L-glutamic acid is placed in a test tube containing a magnetic stirring bar. The test tube is cooled in an ice bath for at least 10 minutes. At the same time, a 0.05M NaHCO3 aqueous solution containing a macromolecular initiator (2mL, 20mg, 0.003mmol) is prepared and cooled in an ice bath for at least 10 minutes. While the aqueous solution is kept in an ice bath, it is added to the NCA powder under vigorous stirring. A milky dispersion is obtained due to the immiscibility of the monomer in the aqueous phase. The reaction is stirred 1) first in an ice-water bath for about 2 hours, 2) then at ambient temperature for 16 hours. The milky dispersion becomes an aqueous whitish colloidal solution, which is transferred to a dialysis tube (dialysis membrane of 3.5kDa) and dialyzed for 2 days with ultrapure water. A white powder ( Fig.32 ).

[0136] Example 17: Very Small Scale Amphiphilic Peptide Diblock Copolymer Poly(ethylene glycol) 5k Concomitant Synthesis of -block-poly(γ-benzyl-L-glutamic acid) and Its Corresponding Nanoparticles

[0137] γ-Benzyl-L-glutamic acid N-carboxyl ring anhydride monomer (BLG-NCA) is a commercial chemical reagent sold by ISOCHEM. 5k -NH2 (Mp = 5516Da, ) is sold by RAPP Polymer, Inc. Other reagents are sold by Sigma-Aldrich.

[0138] Under an inert atmosphere, NCA monomer of γ-benzyl-L-glutamic acid (3 mg, 0.01 mmol) was placed in an Eppendorf tube containing a small magnetic stir bar and the tube was cooled in an ice bath for at least 10 minutes. 5k -NH2 (80 μ L, 3 mg) 0.05 M NaHCO3 aqueous solution and cooled it in an ice bath for at least 10 minutes. While keeping the aqueous solution in an ice bath, add it to the NCA powder under vigorous magnetic stirring. Obtain a milky dispersion due to the immiscibility of the monomers in the aqueous phase. The reaction was stirred 1) first in an ice-water bath for about 2 hours, 2) then at ambient temperature for 16 hours. The milky dispersion becomes an aqueous milky white colloidal solution, which is transferred to a dialysis tube (dialysis membrane of 3.5 kDa) and dialyzed with ultrapure water for 2 days. A white powder ( Fig.33 ).

[0139] Example 18: Very Small Scale Simultaneous Synthesis of Amphiphilic Peptide Diblock Copolymers DNA-block-Poly(γ-Benzyl-L-Glutamic Acid) and Their Corresponding Nanoparticles

[0140] γ-Benzyl-L-glutamic acid N-carboxyl ring anhydride monomer (BLG-NCA) is a commercial chemical reagent sold by ISOCHEM. Deoxyribonucleic acid DNA (TTT) 15 (Mw = 4680 g / mol) is sold by IDT Technology. Other reagents are sold by Sigma-Aldrich.

[0141] Under inert atmosphere, the NCA monomer (5mg) of γ-benzyl-L-glutamic acid is placed in an Ai Bende tube, and the tube is cooled in an ice bath for at least 10 minutes. Meanwhile, an aqueous solution of 0.05M NaHCO3 containing a DNA macromolecular initiator (1mL, 5mg) is prepared and cooled in an ice bath for at least 10 minutes. While the aqueous solution is maintained in an ice bath, it is added to the NCA powder under violent magnetic agitation. The milky dispersion produced due to the immiscibility of the monomer in the aqueous phase is obtained. The reaction is stirred 1) first kept in an ice-water bath for about 2 hours, 2) then kept at ambient temperature for 16 hours. The milky dispersion becomes an aqueous milky colloidal solution, which is transferred to a dialysis tubing (dialysis membrane of 3.5kDa), and dialyzed for 2 days in ultrapure water. White powder (Figure 34) is obtained after freeze drying.

[0142] Tables 1 and 2 below give the molecular and physicochemical properties of the copolymers and nanoparticles thereof synthesized by ROPISA according to the above examples.

[0143] Table 1

[0144]

[0145]

[0146] *Number average molecular weight (M) was determined by SEC in DMF (+LiBr) solution using a polystyrene calibration curve. n ) and dispersion

[0147] Table 2

[0148]

Claims

1. A "one-pot" method for preparing an aqueous solution of nanoparticles of an amphiphilic block copolymer comprising polypeptide units, the method comprising at least one step (E1) carried out at a temperature of -10°C to 80°C, in an aqueous solvent free of organic solvents, combining the following: at least one hydrophilic polymer (P1), said at least one hydrophilic polymer (P1) comprising at least one amine functional group, wherein The hydrophilic polymer (P1) is selected from the group consisting of polyethers, polyesters, poly(meth)acrylates, polysaccharides, polypeptides, polypeptides, DNA and protein derivatives, and At least one hydrophobic α-amino acid N-carboxyl intracyclic anhydride monomer, wherein the hydrophobic α-amino acid N-carboxyl intracyclic anhydride monomer has the following formula (I): wherein R is an optionally protected, natural or modified hydrophobic α-amino acid side chain, Wherein, the aqueous solvent comprises a buffer solution, the buffer solution comprises an inorganic salt with a concentration ranging from 0.01M to 1M, and the pH of the aqueous solvent is 2 to 12.

2. The method according to claim 1, wherein: The hydrophilic polymer (P1) is chosen from elastin-like polypeptides (ELP) comprising at least one amine functional group.

3. The method according to claim 1, wherein: The hydrophilic polymer (P1) is selected from poly(ethylene oxide) having at least one amine functional group.

4. The method according to claim 1, wherein: The hydrophilic polymer (P1) has the following formula: where x is from 16 to 500.

5. The method according to claim 1, wherein: The temperature of step (E1) is 0°C to 4°C.

6. The method according to claim 1, wherein: Step (E1) is carried out from a dispersion of a hydrophobic α-amino acid N-carboxyl intracyclic anhydride monomer under stirring.

7. The method according to claim 1, wherein: The aqueous solution of the amphiphilic block copolymer nanoparticles obtained after step (E1) is subsequently contacted with a second hydrophobic α-amino acid N-carboxyl ring anhydride monomer, thereby obtaining an aqueous solution of modified nanoparticles of the modified amphiphilic block copolymer, wherein the second hydrophobic α-amino acid N-carboxyl ring anhydride monomer is the same as or different from the hydrophobic α-amino acid N-carboxyl ring anhydride monomer in step (E1).

8. An aqueous composition comprising amphiphilic block copolymer nanoparticles comprising polypeptide units obtained according to the method of claim 1, wherein the nanoparticles have a core-shell structure and a particle size of 2 nm to 1 μm, and the weight content of the nanoparticles is at least 2 weight % relative to the weight of the aqueous composition.