Film for forming protective film, composite sheet for forming protective film, and method for producing small sheet with protective film
By providing a filler distribution with a large particle size difference in the protective film forming film, the vibration of the cutting blade is suppressed, the edge chipping problem is solved, and the strength of the semiconductor chip and the laser marking effect are improved.
Patent Information
- Application Number
- CN202080074351.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-23
- Filing Date
- 2020-10-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-10-22
AI Technical Summary
When cutting semiconductor wafers, the shaking and vibration of the cutting blade cause edge chipping (cracks), which affects the flexural strength and failure rate of the chip. Reducing the filler particle size to suppress shaking will reduce the supportability and laser marking contrast. .
In the protective film forming film, the difference in filler particle size between the first region and the second region is greater than 5%. The particle size in the first region is smaller and the particle size in the second region is larger to suppress the shaking of the cutting blade and maintain the laser Markability.
It effectively reduces the stripe cracks from the back to the surface of the semiconductor chip, improves the strength and appearance quality of the chip, while maintaining the visibility of laser marking.
Smart Images

Figure CN114599517B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a protective film forming film and a protective film forming composite sheet that can form a protective film on a workpiece such as a semiconductor wafer or a processed product obtained by processing these workpieces (for example, a semiconductor chip), and a method for manufacturing small pieces (small pieces) with a protective film, such as a semiconductor chip with a protective film obtained by using these protective film forming films or protective film forming composite sheets. Background Art
[0002] In recent years, a so-called face-down mounting method has been used to manufacture semiconductor devices. In this method, when mounting a semiconductor chip having a circuit surface with electrodes such as bumps, the circuit surface side of the semiconductor chip is bonded to a chip mounting portion such as a lead frame. As a result, a structure is formed in which the back side of the semiconductor chip without a circuit is exposed.
[0003] Therefore, a protective film made of a hard organic material is often formed on the back side of the semiconductor chip to protect the semiconductor chip. The protective film is formed using a dicing sheet including a protective film forming film called a semiconductor backside film as shown in Patent Document 1 or Patent Document 2.
[0004] When a protective film is formed on a semiconductor chip or the like using a dicing sheet including a protective film forming film, the protective film forming film on the dicing sheet is attached to the back of the semiconductor wafer. Next, the semiconductor wafer and the protective film forming film are cut using a dicing knife or the like to obtain a laminate of a semiconductor chip and a protective film forming film having the same shape as the semiconductor chip. In order to control the strength of the protective film and the shrinkage during curing and to impart laser marking properties, a filler is mixed in the protective film forming film that becomes the protective film.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2011-9711
[0008] Patent Document 2: Japanese Patent Application Publication No. 2011-151360 Summary of the invention
[0009] Technical Problems to be Solved by the Invention
[0010] Semiconductor chips obtained by cutting semiconductor wafers may sometimes have cracks during cutting. This is also called edge collapse, which may cause the bending strength of the semiconductor chip to decrease and cause failure. Although the edge collapse has various forms, sometimes a stripe-shaped crack may occur from the back side to the front side of the semiconductor chip.
[0011] The inventor of the present application studied the cause of the stripe cracks and believed that the cause was the shaking of the cutting blade caused by the impact during cutting. When the cutting blade is used to cut the semiconductor wafer and the protective film forming film, the blade enters from the surface side of the semiconductor wafer, and after cutting the wafer, the blade cuts the protective film forming film. Since the protective film forming film contains fillers and resins, the load applied to the blade is different when cutting hard fillers and when cutting soft resins, and the blade shakes and vibrates. It is believed that the result is that the blade hits the cutting surface of the chip, thereby generating cracks.
[0012] In particular, the blade is prone to shaking when cutting large fillers. Therefore, it is believed that by reducing the particle size of the filler mixed in the protective film forming film, the shaking and vibration of the blade can be suppressed. However, if the particle size of the filler mixed in the protective film forming film is reduced, the support of the protective film forming film is reduced, the blade becomes easy to vibrate, and the edge collapse cannot be fully reduced. In addition, if the particle size of the filler mixed in the protective film forming film is reduced, even if the protective film forming film or the protective film as its solidified product is laser marked, sufficient contrast cannot be obtained, and the recognition of the mark is reduced.
[0013] Therefore, an object of the present invention is to suppress the occurrence of edge chipping when a workpiece such as a semiconductor wafer and a protective film-forming film are cut using a dicing blade to produce a small piece with a protective film such as a semiconductor chip with a protective film.
[0014] Technical means to solve technical problems
[0015] In order to achieve the above purpose, after careful research, it was found that by mixing a filler with a smaller particle size in the upper area of the protective film forming film (the bonding part with the workpiece) where the blade entering the protective film forming film first contacts, and mixing a filler with a larger particle size in the lower area of the protective film forming film (the stacking part with the cutting piece), the shaking and vibration of the blade during cutting can be suppressed. In addition, it is believed that by mixing a filler with a larger particle size in the lower part of the protective film forming film (the exposed surface of the protective film), the laser marking performance can be fully maintained.
[0016] Therefore, in order to achieve the above-mentioned object, the present invention includes the following points.
[0017] (1) A protective film-forming film comprising a filler, wherein in cross-sectional observation of the film, when the total thickness of the film is defined as T, and a region from the surface of one side of the film to a depth of 0.2T is defined as a first region, and a region from the surface of the other side of the film to a depth of 0.2T is defined as a second region, a 50% cumulative particle size D of the filler observed in the first region is 50 1 and the 50% cumulative particle size D of the filler observed in the second region50 2 satisfies the following relationship:
[0018] D 50 1 <D 50 2. And
[0019] (D 50 2-D 50 1) / D 50 1×100≥5(%).
[0020] (2) The protective film forming film according to (1), comprising two or more constituent layers.
[0021] (3) The protective film-forming film according to (1) or (2), wherein the filler is an inorganic filler.
[0022] (4) The protective film-forming film according to (3), wherein the inorganic filler is a silica filler.
[0023] (5) The protective film forming film according to any one of (1) to (4), wherein the surface on the first region side is attached to a workpiece.
[0024] (6) A composite sheet for forming a protective film, comprising an adhesive sheet in which a base material and an adhesive layer are laminated, and a protective film forming film according to any one of (1) to (5) laminated on the adhesive layer side of the adhesive sheet.
[0025] The protective film forming composite sheet is formed by laminating the surface of the protective film forming film on the second region side on the adhesive layer.
[0026] (7) A method for producing a small piece with a protective film, comprising the following steps (1) to (4):
[0027] Step (1): a step of attaching the surface of the protective film-forming film of the protective film-forming composite sheet described in (6) above on the first region side to a workpiece;
[0028] Step (2): a step of heating and curing the protective film-forming film to obtain a protective film;
[0029] Step (3): a step of cutting the workpiece and the protective film forming film or the protective film to obtain a laminate of small pieces singulated into the same shape and the protective film forming film or the protective film; and
[0030] Step (4): A step of separating the protective film-forming film or the protective film from the adhesive sheet.
[0031] Effects of the Invention
[0032] According to the protective film forming film and the protective film forming composite sheet of the present invention, the shaking and vibration of the blade when the stack of the workpiece and the protective film forming film is cut with a cutting knife can be suppressed, thereby reducing the stripe-like cracks sometimes generated from the back side to the surface side of the semiconductor chip. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a schematic diagram of a partial cross section of a protective film-forming film according to one embodiment of the present invention.
[0034] Figure 2 This is a cross-sectional view of a composite sheet for forming a protective film according to one embodiment of the present invention.
[0035] Figure 3 This is a cross-sectional view of a composite sheet for forming a protective film according to another embodiment of the present invention.
[0036] Figure 4 This is a cross-sectional view showing an example of use of the composite sheet for forming a protective film according to one embodiment of the present invention. DETAILED DESCRIPTION
[0037] The present invention will be described in detail below. First, main terms used in this specification will be described.
[0038] (Meth)acrylate refers to a term used to represent both "acrylate" and "methacrylate", and the same applies to other similar terms.
[0039] Adhesive sheet refers to a laminate comprising a substrate and an adhesive layer, and it may also include other constituent layers in addition thereto. For example, it may be a composition having an intermediate layer between the substrate and the adhesive layer, or it may be formed on the substrate surface on the adhesive layer side to improve the adhesion of the interface between the substrate surface and the adhesive layer or the interface between the substrate surface and the intermediate layer or to prevent the transfer of low molecular weight components, etc., or it may be laminated on the surface of the adhesive layer until use to protect the release film of the adhesive layer. In addition, the substrate may be a single layer or may be a plurality of layers having functional layers such as a buffer layer.
[0040] The dicing sheet is an adhesive sheet used to hold the wafer and chips when singulating the wafer into chips for each circuit.
[0041] The protective film forming film is a film for forming a protective film on a workpiece or a processed object obtained by processing the workpiece. The protective film may be an uncured protective film forming film, preferably composed of a cured protective film forming film. As a workpiece, for example, a semiconductor wafer can be listed, and as a processed object obtained by processing the workpiece, for example, a small piece such as a semiconductor chip can be listed, however, the present invention is not limited thereto. In addition, when the workpiece is a semiconductor wafer, the protective film is formed on the back side of the semiconductor wafer (the side where electrodes such as bumps are not formed).
[0042] The “front surface” of a semiconductor wafer refers to a surface on which circuits, electrodes, etc. are formed, and the “back surface” refers to a surface on which circuits, etc. are not formed.
[0043] Hereinafter, embodiments of the present invention will be described.
[0044] [Film for forming protective film]
[0045] like Figure 1 As shown, the protective film forming film 1 includes a filler 2, and is characterized in that the particle size of the filler is different near the surface of one side of the film and near the surface of the other side. Specifically, in cross-sectional observation of the protective film forming film 1, when the total thickness of the film is set to T, and the region from the surface of one side of the film (hereinafter, sometimes referred to as the first surface) to a depth of 0.2T is set as the first region, and the region from the surface of the other side of the film (hereinafter, sometimes referred to as the second surface) to a depth of 0.2T is set as the second region, the 50% cumulative particle size D of the filler observed in the first region is 50 1 and the 50% cumulative particle size D of the filler observed in the second region 50 2 satisfies the following relationship:
[0046] D 50 1 <D 50 2, and
[0047] (D 50 2-D 50 1) / D 50 1×100≥5(%). The 50% cumulative particle size refers to the particle size of particles corresponding to 50% cumulatively when particles observed within a specific range are arranged from the smaller particle size side.
[0048] When the protective film-forming film of the present invention is attached to a workpiece, the first surface is attached to the workpiece. When the protective film-forming film or the protective film is laser marked, the laser marking is performed on the second surface.
[0049] (D 50 2-D 50 1) / D 501×100(%) is preferably 10% or more, more preferably 20% or more, and particularly preferably 30% or more. (D 50 2-D 50 1) / D 50 When 1×100 is less than 5% and the difference between the 50% cumulative particle size of the filler in the first region and the 50% cumulative particle size of the filler in the second region is small, the effect of suppressing edge chipping may not be fully obtained. (D 50 2-D 50 1) / D 50 The upper limit of 1×100(%) is not particularly limited, but is preferably less than 10000%, more preferably less than 5000%, and even more preferably less than 3000%.
[0050] In addition, D 50 2 / D 50 1 is preferably less than 100, further preferably less than 50, and particularly preferably less than 30. When the filler particle size of the first region is significantly different from the filler particle size of the second region, for example, if (D 50 2-D 50 1) / D 50 1×100(%) is 10000% or more or D 50 2 / D 50 When 1 is 100 or more, the protective film forming film may peel off from the semiconductor chip during the reflow process. In particular, when the protective film forming film is a two-layer product, when the first film with a small filler particle size and the second film with a large filler particle size are directly laminated, if the difference in filler particle size is too large, the difference in thermal expansion coefficient between the first film and the second film becomes large, and peeling may sometimes occur at the interface between the first film and the second film during the reflow process. Even when the protective film forming film is a single-layer structure, if the difference in filler particle size is too large, the adhesion on the first surface side becomes insufficient, and the protective film forming film may peel off from the semiconductor chip.
[0051] D 50 1 is preferably in the range of 0.01 to 2 μm, more preferably 0.05 to 1 μm, and particularly preferably 0.05 to 0.5 μm. 50 If D is too large, the blade tends to shake and vibrate more when cutting the protective film forming film. 50 If D 1 is too small, the viscosity of the coating liquid for forming the first region increases, and coating may be difficult. 50 2 is preferably in the range of 0.01 to 3 μm, more preferably 0.05 to 2 μm, and particularly preferably 0.1 to 1 μm. 50 2 is too small, the laser marking performance will decrease. 50 2 If it is too large, the surface of the protective film becomes rough.
[0052] In another embodiment of the present invention, the maximum particle size D of the filler observed in the first region is preferably max 1 and the maximum particle size D of the filler observed in the second region max 2 satisfies the following relationship, which is satisfied in another embodiment of the present invention:
[0053] D max 1 <D max 2 and (D max 2-D max 1) / D max 1×100≥5(%).
[0054] (D max 2-D max 1) / D max 1×100(%) is preferably 10% or more, more preferably 20%, and particularly preferably 30% or more. max 2-D max 1) / D max If 1×100 is less than 5%, the effect of suppressing edge chipping cannot be fully obtained. (D max 2-D max 1) / D max The upper limit of 1×100(%) is not particularly limited, but is preferably less than 10000%, more preferably less than 5000%, and even more preferably less than 3000%.
[0055] In addition, D max 2 / D max 1 is preferably less than 100, further preferably less than 50, and particularly preferably less than 30. max 1 and D max When the difference of 2 is too large, the protective film forming film may be peeled off from the semiconductor chip during the reflow process as described above.
[0056] D max 1 is preferably in the range of 0.01 to 5 μm, more preferably 0.05 to 3 μm, and particularly preferably 0.1 to 2 μm. max If D is too large, the blade tends to shake and vibrate more when cutting the protective film forming film. max If D 1 is too small, the viscosity of the coating liquid used to form the first region increases, which may make coating difficult. max 2 is preferably in the range of 0.05 to 8 μm, more preferably in the range of 0.1 to 6 μm, and particularly preferably in the range of 0.3 to 5 μm. max 2 is too small, the laser marking performance will decrease. max 2 If it is too large, the surface of the protective film becomes rough.
[0057] The particle size of the filler in the cross-sectional observation of the protective film-forming film (D max , D 50 ), is obtained by curing the protective film forming film and cutting the cured protective film to observe the cross section, which is determined by the maximum particle size and cumulative particle size of the filler particle size. The cross-sectional observation can be carried out in a field of view where each area contains more than 10 fillers, or multiple fields of view can be observed to measure a total of more than 10 filler particle sizes. The filler particle size obtained by cross-sectional observation is the diameter of the filler cross section. Therefore, sometimes the major diameter is observed due to the cross-sectional position of the filler, or the end of the filler is formed as a cut surface. Therefore, the filler particle size obtained by cross-sectional observation is different from the filler particle size of the powder used as the raw material. The filler particle size obtained by cross-sectional observation is obtained as an equivalent circle diameter. "Equivalent circle diameter" refers to the diameter of a circle having the same area as the area of the filler cross section, also known as the Heywood diameter.
[0058] In addition, the blending amount (mass) of the filler in the protective film forming film of the present embodiment is preferably substantially the same. The blending amount (M1) of the filler in the first region is substantially equal to the blending amount (M2) of the filler in the second region, and the ratio of the two, M1 / M2, is preferably in the range of 0.8 to 1.3, more preferably 0.9 to 1.2, and particularly preferably 0.95 to 1.1. If the difference between M1 and M2 is too large, a difference in shrinkage will occur when the protective film forming film is cured, which may sometimes cause peeling of the protective film or chip warping.
[0059] The average blending amount of the filler in the protective film forming film is preferably 10 to 80% by mass, particularly preferably 20 to 70% by mass, and further preferably 30 to 65% by mass relative to the total mass of the protective film forming film. If the blending amount of the filler is too small, the strength of the protective film is insufficient, and if the blending amount of the filler is too large, the adhesion of the protective film forming film becomes insufficient.
[0060] In order to effectively function as a protective film, the thickness of the protective film-forming film is preferably 3 to 300 μm, particularly preferably 5 to 200 μm, and further preferably 7 to 100 μm. When the protective film-forming film is a multilayer product, it refers to the total thickness.
[0061] The protective film forming film of this embodiment may be composed of a single layer or a plurality of layers. In the case of a single layer film, as long as the filler particle size in the first region and the filler particle size in the second region satisfy the above relationship, it is preferred that the filler particle size increases continuously or in stages from the first region side to the second region side. Therefore, it is preferred that a region in which the filler particle size increases continuously or in stages is formed between the first region and the second region.
[0062] When the protective film forming film is composed of multiple layers, it can be a two-layer product of a first film that satisfies the filler particle size of the first region and a second film that satisfies the filler particle size of the second region. In addition, it can also be a structure containing a third film containing fillers between the first film and the second film. The third film can be a structure in which the filler particle size increases continuously from the contact surface with the first film to the contact surface with the second film. In addition, the third film can be set as a plurality of layers in a manner in which the filler particle size increases in stages from the contact surface with the first film to the contact surface with the second film. When the third film is set, M1 / M2, which is the ratio of the blending amount (M1) of the filler in the first region to the blending amount (M2) of the filler in the second region, can exceed the above-mentioned preferred range.
[0063] From the viewpoint of ease of production, the protective film-forming film is preferably a multilayer product.
[0064] When the protective film-forming film has a plurality of constituent layers, the thickness of each constituent layer is not particularly limited, but is preferably about 1 to 30 μm, more preferably 2 to 20 μm, and particularly preferably about 3 to 15 μm.
[0065] The protective film forming film is preferably composed of an uncured resin composition. At this time, after overlapping a workpiece such as a semiconductor wafer on the protective film forming film, by curing the protective film forming film, the protective film can be firmly bonded to the workpiece, and a durable protective film can be formed on a chip, etc.
[0066] In addition, when the protective film-forming film is composed of an uncured resin composition containing a filler, the dispersion state of the filler in the protective film-forming film after curing is almost unchanged from the dispersion state before curing.
[0067] The protective film forming film preferably has adhesiveness at room temperature or exerts adhesiveness by heating. Thus, as described above, when a workpiece such as a semiconductor wafer is overlapped on the protective film forming film, the two can be bonded. Therefore, the position can be accurately determined before the protective film forming film is cured.
[0068] The resin composition constituting the protective film-forming film having the above-mentioned properties preferably contains a filler, a curable component, and a binder polymer component.
[0069] As a filler, any of an inorganic filler and an organic filler can be used. Among them, an inorganic filler is preferred, and silica such as crystalline silica, fused silica, and synthetic silica, or inorganic fillers such as alumina and glass beads (Glass Balloon) can be used. Among them, silica is preferred, and synthetic silica is more preferred. In particular, the most suitable is a synthetic silica of a type that tries to remove the radiation source of α rays, which is the main cause of failure of semiconductor devices. As the shape of the filler, spherical, needle-shaped, amorphous, etc. can be listed, but a spherical shape is preferred, and a perfect sphere is particularly preferred. If the filler is spherical or a perfect sphere, it can be filled and dispersed smoothly.
[0070] Furthermore, the filler may be surface treated with a coupling agent, preferably a silane coupling agent. Examples of the silane coupling agent include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-(methacryloxypropyl)trimethoxysilane, γ-aminopropyltrimethoxysilane, N-6-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-6-(aminoethyl)-γ-aminopropylmethyldiethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-ureidopropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, bis(3-triethoxysilylpropyl)tetrasulfide, methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriacetoxysilane, and imidazolesilane. These silane coupling agents may be used alone or in combination of two or more.
[0071] Furthermore, the type of filler contained in the first region and the type of filler contained in the second region may be the same or different, and are preferably the same type of filler, preferably silicon dioxide, and more preferably synthetic silicon dioxide.
[0072] If the protective film forming film contains fillers, the hardness of the protective film after curing can be highly maintained, and the moisture resistance can be improved. Furthermore, the thermal expansion coefficient of the protective film after curing can be made close to the thermal expansion coefficient of the semiconductor wafer, thereby suppressing the warping of the semiconductor wafer during processing and suppressing the peeling of the protective film after curing.
[0073] As a curable component, a thermosetting component, an energy ray curable component, or a mixture of the two can be used. When an energy ray curable component is used, it is necessary to control the light transmittance of the protective film forming film, and a filler with a smaller filler particle size is preferred. In a protective film forming film using a thermosetting component, it is not necessary to control the light transmittance, and the range of material selection is wide, so it is more preferred.
[0074] Examples of the thermosetting component include epoxy resins, phenolic resins, melamine resins, urea resins, polyimide resins, benzoxazine resins, and mixtures thereof. Among them, epoxy resins, phenolic resins, and mixtures thereof are preferably used.
[0075] The epoxy resin is three-dimensionally reticulated by heating and has the property of forming a strong coating. As such an epoxy resin, various known epoxy resins can be used, but epoxy resins with a molecular weight of about 300 to 2000 are generally preferred, and epoxy resins with a molecular weight of 300 to 500 are particularly preferred. It is further preferred to use the epoxy resin in the form of blending a molecular weight of 330 to 400, which is liquid at room temperature, and a molecular weight of 400 to 2500, especially a molecular weight of 500 to 2000, which is solid at normal conditions. In addition, the epoxy equivalent of the epoxy resin is preferably 50 to 5000 g / eq.
[0076] Specific examples of such epoxy resins include glycidyl ethers of phenols such as bisphenol A, bisphenol F, resorcinol, phenyl novolac, and cresol novolac; glycidyl ethers of alcohols such as butanediol, polyethylene glycol, and polypropylene glycol; glycidyl ethers of carboxylic acids such as phthalic acid, isophthalic acid, and tetrahydrophthalic acid; glycidyl-type or alkylglycidyl-type epoxy resins obtained by replacing the active hydrogen bonded to the nitrogen atom of aniline isocyanurate with a glycidyl group; so-called alicyclic epoxides such as vinylcyclohexene dioxide, 3,4-epoxycyclohexylmethyl-3,4-dicyclohexanecarboxylate, and 2-(3,4-epoxy)cyclohexyl-5,5-spiro(3,4-epoxy)cyclohexane-m-dioxane, into which an epoxy group is introduced, for example, by oxidizing the carbon-carbon double bond in the molecule. In addition, epoxy resins having a biphenyl skeleton, a dicyclohexadiene skeleton, a naphthalene skeleton, etc. can also be used.
[0077] Among them, bisphenol glycidyl epoxy resins, o-cresol novolac epoxy resins, and phenol novolac epoxy resins are preferably used. These epoxy resins may be used alone or in combination of two or more.
[0078] When using epoxy resin, it is preferred to use a heat-active latent epoxy resin curing agent as an auxiliary agent at the same time. A heat-active latent epoxy resin curing agent refers to a type of curing agent that does not react with epoxy resin at room temperature, but is activated by heating to a certain temperature or above, thereby reacting with epoxy resin. Methods for activating heat-active latent epoxy resin curing agents include: a method of generating active substances (anions, cations) through a chemical reaction based on heating; a method of stably dispersing in the epoxy resin at around room temperature and being compatible and dissolved with the epoxy resin at high temperature, thereby initiating a curing reaction; a method of using a molecular sieve-enclosed curing agent to elute at high temperature to initiate a curing reaction; a method of using microcapsules, etc.
[0079] Specific examples of heat-active latent epoxy resin curing agents include various onium salts, dibasic acid dihydrazide compounds, dicyandiamide, amine adduct curing agents, high melting point active hydrogen compounds such as imidazole compounds, etc. These heat-active latent epoxy resin curing agents can be used alone or in combination of two or more. The heat-active latent epoxy resin curing agent described above is preferably used in a ratio of 0.1 to 20 parts by mass, particularly preferably 0.2 to 10 parts by mass, and further preferably 0.3 to 5 parts by mass relative to 100 parts by mass of epoxy resin.
[0080] As the phenolic resin, condensates of phenols and aldehydes such as alkylphenols, polyphenols, and naphthols can be used without particular limitation. Specifically, phenol novolac resins, o-cresol novolac resins, p-cresol novolac resins, tert-butylphenol novolac resins, dicyclopentadiene cresol resins, poly-p-vinyl phenolic resins, bisphenol A novolac resins, or modified products thereof can be used.
[0081] The phenolic hydroxyl groups contained in these phenolic resins are easily subjected to addition reaction with the epoxy groups of the epoxy resins by heating, thereby forming a cured product with high impact resistance. Therefore, epoxy resins and phenolic resins can be used simultaneously.
[0082] The binder polymer component can impart appropriate tack to the protective film forming film and can improve the operability of the composite sheet 3 for protective film formation. The mass average molecular weight of the binder polymer is generally in the range of 50,000 to 2 million, preferably 100,000 to 1.5 million, and particularly preferably 200,000 to 1 million. If the molecular weight is too low, the formation of the film of the protective film forming film is insufficient. If it is too high, the compatibility with other components deteriorates, resulting in the formation of a uniform film. As such a binder polymer, for example, acrylic polymers, polyester resins, phenoxy resins, urethane resins, silicone resins, rubber polymers, etc. can be used, and acrylic polymers are particularly preferred.
[0083] Examples of acrylic polymers include (meth)acrylate copolymers composed of (meth)acrylate monomers and structural units derived from (meth)acrylic acid derivatives. Among them, as (meth)acrylate monomers, (meth)acrylic acid alkyl esters having an alkyl group with 1 to 18 carbon atoms are preferably used, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, etc. In addition, examples of (meth)acrylic acid derivatives include (meth)acrylic acid, glycidyl (meth)acrylate, hydroxyethyl (meth)acrylate, etc.
[0084] In the above, if glycidyl methacrylate or the like is used as a structural unit to introduce a glycidyl group into the acrylic polymer, the compatibility with the epoxy resin as the above thermosetting component is improved, the glass transition temperature (Tg) of the protective film-forming film after curing is increased, and the heat resistance is improved. In addition, in the above, if hydroxyethyl acrylate or the like is used as a structural unit to introduce a hydroxyl group into the acrylic polymer, the adhesion and adhesive properties to the workpiece can be controlled.
[0085] When an acrylic polymer is used as the binder polymer, the mass average molecular weight of the polymer is preferably 100,000 or more, particularly preferably 150,000 to 1,000,000. The glass transition temperature of the acrylic polymer is usually 20°C or less, preferably about -70 to 0°C, and has adhesiveness at room temperature (23°C).
[0086] The blending ratio of the thermosetting component to the binder polymer component is preferably 50 to 1500 parts by mass, particularly preferably 70 to 1000 parts by mass, and further preferably 80 to 800 parts by mass relative to 100 parts by mass of the binder polymer component. If the thermosetting component and the binder polymer component are blended in such a ratio, appropriate viscosity will be exhibited before curing, and the attachment operation can be stably performed. In addition, a protective film with excellent coating strength can be obtained after curing.
[0087] The protective film-forming film preferably contains a colorant, thereby improving the visibility and design of laser printing.
[0088] As the colorant, for example, known colorants such as inorganic pigments, organic pigments, and organic dyes can be used.
[0089] Examples of the inorganic pigments include carbon black, cobalt pigments, iron pigments, chromium pigments, titanium pigments, vanadium pigments, zirconium pigments, molybdenum pigments, ruthenium pigments, platinum pigments, ITO (indium tin oxide) pigments, and ATO (antimony tin oxide) pigments.
[0090] Examples of organic pigments and organic dyes include amine pigments, cyanine pigments, merocyanine pigments, croconium pigments, squarylium pigments, azulenium pigments, polyacetylene pigments, naphthoquinone pigments, pyrylium pigments, phthalocyanine pigments, naphthalocyanine pigments, naphtholactam pigments, azo pigments, condensed azo pigments, Indigo pigments, perinone pigments, perylene pigments, dioxazine pigments, quinacridone pigments, isoindolinone pigments, quinophthalone pigments, pyrrole pigments, thioindigo pigments, metal complex pigments (metal complex salt dyes), dithiol metal complex pigments, indoxyl pigments, triarylmethane pigments, anthraquinone pigments, dioxazine pigments, naphthol pigments, azomethine pigments, benzimidazolone pigments, pyranthrone pigments and threne pigments, etc. These pigments or dyes can be appropriately mixed and used to adjust to the target transmittance.
[0091] Among the above, black pigments are preferred, and carbon black is particularly preferred. Carbon black can shield electromagnetic waves in a wide wavelength range.
[0092] The amount of colorant (especially carbon black) added in the protective film forming film varies depending on the thickness of the protective film forming film. For example, when the thickness of the protective film forming film is 25 μm, the amount of colorant added is preferably 0.05 to 1% by mass, particularly preferably 0.075 to 0.75% by mass, and more preferably 0.1 to 0.5% by mass relative to the total mass of the protective film forming film. If the amount of colorant added is 0.05% by mass or more, grinding marks on semiconductor chips, etc. can be shielded in a manner that is invisible to the naked eye. On the other hand, even if the amount of colorant added is greater than 1% by mass, the shielding property will almost change. If excessive blending is performed, the adhesion will be impaired. In addition, when the thickness of the protective film forming film becomes thinner, there is a tendency for the transmittance to increase, and when the thickness of the protective film forming film becomes thicker, there is a tendency for the transmittance to decrease, so it is desired to appropriately adjust the amount of colorant added according to the thickness of the protective film forming film. Specifically, it is desirable to adjust the thickness of the protective film-forming film so as to be in inverse proportion to the amount of the colorant blended.
[0093] The average particle size of the colorant (especially carbon black) is preferably 1 to 500 nm, particularly preferably 3 to 100 nm, and further preferably 5 to 50 nm. If the average particle size of the colorant is within the above range, it is easy to control the light transmittance within the desired range. In addition, the average particle size of the colorant in this specification is a value measured by a dynamic light scattering method using a particle size distribution measuring device (manufactured by NIKKISO CO., LTD., NanoTrac Wave-UT151).
[0094] The colorant is relatively soft and has a low hardness, so even if it is cut with a cutter, the shaking and vibration of the blade are small and will not affect the effect of the present invention.
[0095] The protective film forming film may further contain a coupling agent. By containing a coupling agent, after the protective film forming film is cured, the heat resistance of the protective film will not be impaired, and the adhesion-adhesion between the protective film and the workpiece can be improved, and the water resistance (moisture heat resistance) can be improved. From the perspective of versatility and cost-effectiveness, a silane coupling agent is preferably used as the coupling agent.
[0096] Examples of the silane coupling agent include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-(methacryloxypropyl)trimethoxysilane, γ-aminopropyltrimethoxysilane, N-6-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-6-(aminoethyl)-γ-aminopropylmethyldiethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-ureidopropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, bis(3-triethoxysilylpropyl)tetrasulfide, methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriacetoxysilane, and imidazolesilane. These silane coupling agents may be used alone or in combination of two or more.
[0097] In order to adjust the cohesive force before curing, the protective film forming film may also contain a cross-linking agent such as an organic polyisocyanate compound, an organic polyimide compound, and an organic metal chelate compound. In addition, in order to suppress static electricity and improve the reliability of the chip, the protective film forming film may also contain an antistatic agent. Further, in order to improve the flame retardancy of the protective film and improve the reliability as a package, the protective film forming film may also contain a flame retardant such as a phosphoric acid compound, a bromide, and a phosphorus compound.
[0098] The manufacturing method of the protective film forming film is not particularly limited. When the protective film forming film is a two-layer product, a first film satisfying the filler particle size of the first region and a second film satisfying the filler particle size of the second region are laminated. The protective film forming film can be obtained by preparing a resin composition for forming a protective film containing a filler of a specific particle size and a coating liquid further containing a solvent as required, and applying it on the release surface of the release sheet using a coating machine such as a roll coater, a blade coater, a roll knife coater, an air knife coater, a die coater, a rod coater, a gravure coater, a curtain coater, and drying it. Prepare two films with different particle sizes of the contained filler, and laminate them to obtain a protective film forming film with a two-layer structure. When laminating the films, hot pressing can be performed.
[0099] When there are three or more constituent layers, a film containing a filler having a particle size between the filler particle size of the first film and the filler particle size of the second film may be prepared, and the films may be laminated so that the filler particle size changes stepwise.
[0100] For a single-layer protective film-forming film, for example, by using a coating liquid containing a plurality of fillers with different specific gravities and particle sizes, particles with different specific gravities precipitate during the period from coating to drying, thereby forming a gradient of particle sizes in the thickness direction. For example, if a coating liquid is prepared by mixing a filler with a large particle size and specific gravity with a filler with a small particle size and specific gravity, the large filler precipitates on the lower side in the thickness direction during the period from coating to drying, and the small filler tends to exist on the upper side of the coating. As a result, a protective film-forming film can be obtained in which the particle size of the filler changes continuously in the thickness direction.
[0101] [Protective film forming sheet]
[0102] The protective film-forming film may be rolled up and stored in the state of a protective film-forming sheet by protecting one or both sides of the protective film-forming film with a release sheet before use. The release sheet is peeled off when the protective film-forming film is used.
[0103] The composition of the release sheet is arbitrary, and examples thereof include a plastic sheet that is releaseable from the protective film forming film, and a sheet obtained by subjecting the plastic sheet to a release treatment using a release agent or the like. Specific examples of plastic sheets include polyester sheets such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, and polyolefin sheets such as polypropylene and polyethylene. As release agents, silicones, fluorines, and long-chain alkyls can be used, but silicones are preferred because they are inexpensive and can provide stable performance. The thickness of the release sheet is not particularly limited, but is generally about 20 to 250 μm.
[0104] When the protective film forming film has release sheets on both sides, it is preferred that the release force of one release sheet be increased to make it a heavy release sheet, and the release force of the other release sheet be decreased to make it a light release sheet.
[0105] When the protective film-forming sheet is produced, the protective film-forming film is formed on the release surface (surface having release properties; generally, the surface subjected to release treatment, but not limited thereto) of the release sheet by the above-mentioned method.
[0106] As an example of the use of the protective film forming sheet, a method for manufacturing a chip with a protective film from a semiconductor wafer as a workpiece is described below. First, the surface (first surface) on the first region side of the protective film forming film of the protective film forming sheet is attached to the back of a semiconductor wafer on which a circuit is formed and back grinding is performed. At this time, the protective film forming film can be heated as needed to exert its adhesiveness.
[0107] Next, the peeling sheet is peeled off from the protective film forming film. Then, the protective film forming film is cured to form a protective film, thereby obtaining a semiconductor wafer with a protective film. In addition, the protective film forming film can be cured after the dicing step described later.
[0108] After obtaining the semiconductor wafer with the protective film as described above, the protective film is irradiated with laser light as needed to perform laser printing. In addition, the laser printing can be performed before curing the protective film forming film or after the dicing step described later.
[0109] Next, the semiconductor wafer with the protective film is cut using a dicing sheet according to a conventional method to obtain a chip with the protective film (a chip with a protective film). Then, the dicing sheet is expanded in a planar direction as required, and the chip with the protective film is picked up from the dicing sheet.
[0110] The chip with a protective film obtained as described above has a grinding mark caused by the back grinding process which is invisible to the naked eye due to the protective film, so the appearance is excellent. In addition, the strength of the chip with a protective film and the semiconductor wafer with a protective film is improved due to the protective film, so the damage during transportation, storage, and processing can be reduced. Furthermore, since the back of the semiconductor chip with a protective film is shielded, it can shield various electromagnetic waves generated in the electronic device, thereby reducing the failure of the semiconductor device.
[0111] [Composite sheet for forming protective film]
[0112] Figure 2 FIG. 1 is a cross-sectional view of a composite sheet for forming a protective film according to an embodiment of the present invention. Figure 2 As shown, the composite sheet 3 for forming a protective film of the present embodiment includes an adhesive sheet 4 in which an adhesive layer 42 is laminated on one surface of a substrate 41, and a protective film-forming film 1 laminated on the adhesive layer 42 side of the adhesive sheet 4, and, if necessary, includes a jig adhesive layer 5 laminated on the peripheral portion of the protective film-forming film 1 on the side opposite to the adhesive sheet 4. The surface (second surface) on the second region side of the protective film-forming film 1 is laminated on the adhesive layer 41. In addition, the jig adhesive layer 5 is a layer for bonding the composite sheet 3 for forming a protective film to a jig such as a ring frame.
[0113] The composite sheet 3 for forming a protective film of this embodiment is attached to and holds the workpiece when processing the workpiece, and is used to form a protective film on the workpiece or the processed product obtained by processing the workpiece. The protective film can be an uncured protective film forming film 1, and is preferably composed of a cured product of the protective film forming film 1.
[0114] The protective film forming composite sheet 3 of this embodiment is used to hold the semiconductor wafer as a workpiece when dicing the semiconductor wafer and to form a protective film on the semiconductor chip obtained by dicing, but is not limited thereto. The adhesive sheet 4 of the protective film forming composite sheet 3 is usually called a dicing sheet.
[0115] 1. Adhesive sheet
[0116] The adhesive sheet 4 of the composite sheet 3 for forming a protective film according to the present embodiment includes a base material 41 and an adhesive layer 42 laminated on one surface of the base material 41 .
[0117] 1-1. Base material
[0118] The base material 41 of the adhesive sheet 4 is not particularly limited in terms of its constituent material as long as it is suitable for workpiece processing, such as dicing and expanding of semiconductor wafers, and is generally composed of a film mainly made of a resin material (hereinafter referred to as a "resin film").
[0119] Specific examples of resin films include polyethylene films such as low-density polyethylene (LDPE) films, linear low-density polyethylene (LLDPE) films, and high-density polyethylene (HDPE) films, polypropylene films, polybutylene films, polybutadiene films, polymethylpentene films, ethylene-norbornene copolymer films, and norbornene resin films; ethylene copolymer films such as ethylene-vinyl acetate copolymer films, ethylene-(meth)acrylic acid copolymer films, and ethylene-(meth)acrylic acid ester copolymer films; polyvinyl chloride films such as polyvinyl chloride films and vinyl chloride copolymer films; polyester films such as polyethylene terephthalate films and polybutylene terephthalate films; polyurethane films; polyimide films; polystyrene films; polycarbonate films; fluororesin films, etc. In addition, modified films such as cross-linked films and ionomer films of these films can also be used. The substrate 41 can be a film composed of one of these films, or a laminated film formed by combining two or more of these films.
[0120] Among them, from the perspective of environmental safety, cost, etc., polyolefin films are preferred, and polypropylene films with excellent heat resistance are preferred. As long as it is a polypropylene film, the expansion suitability of the adhesive sheet 4 and the chip pickup suitability will not be damaged, and heat resistance can be given to the substrate 41. By giving the substrate 41 such heat resistance, when the protective film forming film 1 is thermally cured in a state where the protective film forming composite sheet 3 is attached to the workpiece, the adhesive sheet 4 can be prevented from being loosened.
[0121] For the resin film, in order to improve the adhesion with the adhesive layer 42 stacked on the surface, one or both sides thereof may be subjected to surface treatment or primer treatment based on oxidation or embossing, etc. as needed. Examples of the oxidation method include corona discharge treatment, plasma discharge treatment, chromium oxidation treatment (wet), flame treatment, hot air treatment, ozone-ultraviolet irradiation treatment, etc., and examples of the embossing method include sandblasting, thermal spraying, etc.
[0122] The base material 41 may contain various additives such as a colorant, a flame retardant, a plasticizer, an antistatic agent, a lubricant, and a filler in the resin film.
[0123] The thickness of the substrate 41 is not particularly limited as long as it can appropriately function in each step using the protective film-forming composite sheet 3. The thickness is preferably in the range of 20 to 450 μm, more preferably 25 to 400 μm, and particularly preferably 50 to 350 μm.
[0124] The elongation at break of the substrate 41 of the adhesive sheet 4 of the present embodiment is preferably 100% or more, particularly preferably 200 to 1000%, measured at 23°C and a relative humidity of 50%. The elongation at break is the elongation of the length of the test piece relative to the original length when the test piece breaks in a tensile test according to J1S K7161:1994 (ISO 527-1 1993). The substrate 41 having an elongation at break of 100% or more is not easy to break during the expansion process, and it is easy to separate the chips formed by cutting the workpiece.
[0125] In addition, the tensile stress of the substrate 41 of the adhesive sheet 4 in the present embodiment when the strain is 25% is preferably 5 to 15 N / 10 mm, and the maximum tensile stress is preferably 15 to 50 MPa. Among them, the tensile stress and the maximum tensile stress when the strain is 25% are measured by a test based on JIS K7161: 1994. If the tensile stress when the strain is 25% is 5 N / 10 mm or more and the maximum tensile stress is 15 MPa or more, after the protective film forming film 1 is attached to the workpiece, when it is fixed on a frame such as a ring frame, the substrate 41 can be prevented from loosening and conveying errors can be prevented. On the other hand, if the tensile stress when the strain is 25% is less than 15 N / 10 mm and the maximum tensile stress is less than 50 MPa, the adhesive sheet 4 itself can be prevented from peeling off from the ring frame during the expansion process. In addition, the above-mentioned elongation at break, tensile stress when the strain is 25%, and maximum tensile stress refer to the values obtained by measuring the length direction of the coil of the substrate 41.
[0126] 1-2. Adhesive layer
[0127] The adhesive layer 42 of the adhesive sheet 4 of the composite sheet 3 for forming a protective film of the present embodiment may be composed of a non-energy ray curable adhesive or an energy ray curable adhesive. As the non-energy ray curable adhesive, a non-energy ray curable adhesive having the required adhesive force and removability is preferred, for example, an acrylic adhesive, a rubber adhesive, a silicone adhesive, a urethane adhesive, a polyester adhesive, a polyvinyl ether adhesive, etc. may be used. Among them, an acrylic adhesive having high adhesion to the protective film forming film 1 and being able to effectively suppress the detachment of a workpiece or a processed object in a cutting process, etc. is preferred.
[0128] On the other hand, since the adhesive strength of the energy-ray-curable adhesive is reduced by irradiation with energy rays, when separating the workpiece or processed object from the adhesive sheet 4 , the separation can be easily performed by irradiation with energy rays.
[0129] When the adhesive layer 42 is composed of an energy-ray-curable adhesive, the adhesive layer 42 directly below the protective film-forming film in the protective film-forming composite sheet 3 can be cured. The material formed by curing the energy-ray-curable adhesive usually has a high elastic coefficient and a high surface smoothness. Therefore, if the protective film-forming film 1 in contact with the cured portion composed of the material is cured to form a protective film, the smoothness and glossiness of the surface of the protective film in contact with the cured portion become high, thereby forming a protective film for a chip with excellent aesthetics. In addition, if laser printing is performed on a protective film with high surface smoothness, the recognizability of its printing is improved. It can also be used in cutting when the adhesive layer 42 is not cured. At this time, the adhesive force is continuously maintained, so it is not easy to cause the chip to fly during cutting.
[0130] The energy-curable adhesive constituting the adhesive layer 42 may contain an energy-curable polymer as a main component, or may contain a mixture of a non-energy-curable polymer and an energy-curable multifunctional monomer and / or oligomer as a main component.
[0131] The following description will focus on the case where the energy-ray-curable adhesive contains a polymer having energy-ray curability as a main component.
[0132] The energy-curable polymer is preferably a (meth)acrylate (copolymer) polymer (A) (hereinafter sometimes referred to as "energy-curable polymer (A)") having an energy-curable functional group (energy-curable group) introduced into the side chain. The energy-curable polymer (A) is preferably a polymer obtained by reacting a (meth)acrylic copolymer (a1) having a monomer unit containing a functional group with an unsaturated group-containing compound (a2) having a substituent bonded to the functional group thereof.
[0133] The acrylic copolymer (a1) is composed of a structural unit derived from a functional group-containing monomer and a structural unit derived from a (meth)acrylic acid ester monomer or a derivative thereof.
[0134] As the functional group-containing monomer of the structural unit of the acrylic copolymer (a1), a monomer having a polymerizable double bond and a functional group such as a hydroxyl group, an amino group, a substituted amino group, or an epoxy group in the molecule is preferred.
[0135] Further specific examples of the functional group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and the like. These monomers may be used alone or in combination of two or more.
[0136] As the (meth)acrylic acid ester monomer constituting the acrylic copolymer (a1), alkyl (meth)acrylates having an alkyl group with carbon atoms of 1 to 20, cycloalkyl (meth)acrylates, and benzyl (meth)acrylates can be used. Among them, alkyl (meth)acrylates having an alkyl group with carbon atoms of 1 to 18 are particularly preferred, and examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.
[0137] The acrylic copolymer (a1) contains structural units derived from the above-mentioned functional group-containing monomers usually at a ratio of 3 to 100% by mass, preferably 5 to 40% by mass, and structural units derived from (meth)acrylate monomers or derivatives thereof usually at a ratio of 0 to 97% by mass, preferably 60 to 95% by mass.
[0138] The acrylic copolymer (a1) can be obtained by copolymerizing the above-mentioned functional group-containing monomers with (meth)acrylate monomers or derivatives thereof by a conventional method. In addition to these monomers, dimethylacrylamide, vinyl formate, vinyl acetate, styrene and the like may also be copolymerized.
[0139] The energy-ray curable polymer (A) can be obtained by reacting the acrylic copolymer (a1) having the above-mentioned functional group-containing monomer unit with the unsaturated group-containing compound (a2) having a substituent bonded to the functional group.
[0140] The substituent of the unsaturated group-containing compound (a2) can be appropriately selected according to the type of the functional group of the functional group-containing monomer unit of the acrylic copolymer (a1). For example, when the functional group is a hydroxyl group, an amino group or a substituted amino group, an isocyanate group or an epoxy group is preferably used as the substituent, and when the functional group is an epoxy group, an amino group, a carboxyl group or an aziridine group is preferably used as the substituent.
[0141] In addition, the unsaturated group-containing compound (a2) contains 1 to 5, preferably 1 to 2, energy-ray-polymerizable carbon-carbon double bonds per molecule. Specific examples of such unsaturated group-containing compounds (a2) include 2-methacryloyloxyethyl isocyanate, m-isopropenyl-α,α-dimethylbenzyl isocyanate, methacryloyl isocyanate, allyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate; acryloyl monoisocyanate compounds obtained by reaction of a diisocyanate compound or a polyisocyanate compound with hydroxyethyl (meth)acrylate; acryloyl monoisocyanate compounds obtained by reaction of a diisocyanate compound or a polyisocyanate compound with a polyol compound and hydroxyethyl (meth)acrylate; glycidyl (meth)acrylate; (meth)acrylic acid, 2-(1-aziridinyl)ethyl (meth)acrylate, 2-vinyl-2-oxazoline, 2-isopropenyl-2-oxazoline, and the like.
[0142] The unsaturated group-containing compound (a2) is usually used in a ratio of 10 to 100 equivalents, preferably 20 to 95 equivalents, per 100 equivalents of the functional group-containing monomer of the acrylic copolymer (a1).
[0143] In the reaction of the acrylic copolymer (a1) and the unsaturated group-containing compound (a2), the reaction temperature, pressure, solvent, time, presence or absence of a catalyst, and the type of catalyst can be appropriately selected according to the combination of the functional group and the substituent. Thus, the functional group present in the acrylic copolymer (a1) reacts with the substituent in the unsaturated group-containing compound (a2), and the unsaturated group is introduced into the side chain of the acrylic copolymer (a1), thereby obtaining the energy-ray-curable polymer (A).
[0144] The mass average molecular weight of the energy-ray curable polymer (A) thus obtained is preferably 10,000 or more, particularly preferably 150,000 to 1,500,000, and further preferably 200,000 to 1,000,000. The mass average molecular weight (Mw) in this specification is a value measured by gel permeation chromatography (GPC) in terms of polystyrene.
[0145] When the energy-ray curable adhesive contains a polymer having energy-ray curability as a main component, the energy-ray curable adhesive may further contain an energy-ray curable monomer and / or oligomer (B).
[0146] As the energy-ray-curable monomer and / or oligomer (B), for example, esters of polyols and (meth)acrylic acid can be used.
[0147] Examples of the energy-ray-curable monomer and / or oligomer (B) include monofunctional acrylates such as cyclohexyl (meth)acrylate and isobornyl (meth)acrylate; polyfunctional acrylates such as trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, and dihydroxymethyltricyclodecane di(meth)acrylate; polyester oligo(meth)acrylates; and polyurethane oligo(meth)acrylates.
[0148] When the energy-ray-curable monomer and / or oligomer (B) is blended, the content of the energy-ray-curable monomer and / or oligomer (B) in the energy-ray-curable adhesive is preferably 5 to 80% by mass, particularly preferably 20 to 60% by mass.
[0149] Among them, when ultraviolet rays are used as the energy ray for curing the energy ray-curable adhesive, it is preferable to add a photopolymerization initiator (C). By using the photopolymerization initiator (C), the polymerization curing time and the light irradiation amount can be reduced.
[0150] Specific examples of the photopolymerization initiator (C) include benzophenone, acetophenone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin methyl benzoate, benzoin dimethyl ketal, 2,4-diethylthioxanthone, 1-hydroxycyclohexyl phenone, benzyl diphenylsulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, benzil, dibenzil, diacetyl, β-chloroanthraquinone, (2,4,6-trimethylbenzyldiphenyl)phosphine oxide, 2-benzothiazolyl diethyldithiocarbamate, oligomeric
[0151] {2-hydroxy-2-methyl-1-[4-(1-propenyl)phenyl]propanone}, 2,2-dimethoxy-1,2-diphenylethane-1-one, etc. These photopolymerization initiators may be used alone or in combination of two or more.
[0152] The photopolymerization initiator (C) is preferably used in an amount ranging from 0.1 to 10 parts by mass, particularly from 0.5 to 6 parts by mass, relative to 100 parts by mass of the energy-ray-curable copolymer (A) (when the energy-ray-curable monomer and / or oligomer (B) is blended, the total amount of the energy-ray-curable copolymer (A) and the energy-ray-curable monomer and / or oligomer (B) is 100 parts by mass).
[0153] In addition to the above components, other appropriate components may be blended into the energy-ray-curable adhesive. Examples of other components include polymer components or oligomer components (D) that do not have energy-ray curability, and crosslinking agents (E).
[0154] Examples of the non-energy-ray-curable polymer component or oligomer component (D) include polyacrylates, polyesters, polyurethanes, polycarbonates, and polyolefins, and polymers or oligomers having a mass average molecular weight (Mw) of 3,000 to 2,500,000 are preferred.
[0155] As the crosslinking agent (E), a polyfunctional compound reactive with the functional group possessed by the energy-ray curable copolymer (A) etc. can be used. Examples of such polyfunctional compounds include isocyanate compounds, epoxy compounds, amine compounds, melamine compounds, aziridine compounds, hydrazine compounds, aldehyde compounds, oxazoline compounds, metal alkoxide compounds, metal chelate compounds, metal salts, ammonium salts, reactive phenolic resins etc.
[0156] By blending these other components (D) and (E) into the energy-ray curable adhesive, it is possible to improve the tackiness and peelability before curing, the strength after curing, the adhesion to other layers, the storage stability, etc. The blending amount of these other components is not particularly limited, and the blending amount of the other components can be appropriately determined within the range of 0 to 40 parts by mass relative to 100 parts by mass of the energy-ray curable copolymer (A).
[0157] Next, the case where the energy-ray curable adhesive contains a mixture of a polymer component not having energy-ray curability and an energy-ray curable multifunctional monomer and / or oligomer as a main component will be described.
[0158] As the non-energy-curable polymer component, for example, the same components as those of the acrylic copolymer (a1) can be used. The content of the non-energy-curable polymer component in the energy-curable adhesive is preferably 20 to 99.9% by mass, particularly preferably 30 to 80% by mass.
[0159] As the energy-ray-curable multifunctional monomer and / or oligomer, the same compound as the above-mentioned component (B) can be selected. Regarding the ratio of the polymer component not having energy-ray curability to the energy-ray-curable multifunctional monomer and / or oligomer, the multifunctional monomer and / or oligomer is preferably 10 to 150 parts by mass, particularly preferably 25 to 100 parts by mass, relative to 100 parts by mass of the polymer component.
[0160] In this case, a photopolymerization initiator (C) and a crosslinking agent (E) may be appropriately blended in the same manner as described above.
[0161] The thickness of the adhesive layer 42 is not particularly limited as long as it can appropriately function in each step using the protective film-forming composite sheet 3. Specifically, it is preferably 1 to 50 μm, particularly preferably 2 to 30 μm, and further preferably 3 to 20 μm.
[0162] As the adhesive constituting the clamp adhesive layer 5, an adhesive having the required adhesive force and removability is preferred, for example, acrylic adhesives, rubber adhesives, silicone adhesives, urethane adhesives, polyester adhesives, polyvinyl ether adhesives, etc. can be used. Among them, acrylic adhesives are preferred, which have high adhesion to clamps such as annular frames and can effectively suppress the peeling of the protective film forming composite sheet 3 from the annular frame, etc. in the cutting process, etc. In addition, a base material as a core material can be sandwiched in the thickness direction of the clamp adhesive layer 5.
[0163] On the other hand, from the viewpoint of adhesion to a jig such as a ring frame, the thickness of the jig adhesive layer 5 is preferably 5 to 200 μm, particularly preferably 10 to 100 μm.
[0164] 2. Method for producing composite sheet for forming protective film
[0165] The composite sheet 3 for forming a protective film is preferably manufactured by the following method: after separately preparing a first laminate including a protective film-forming film 1 and a second laminate including an adhesive sheet 4, the protective film-forming film 1 and the adhesive sheet 4 are laminated using the first laminate and the second laminate, but the present invention is not limited to this method. In addition, as described above, the second surface side of the protective film-forming film 1 is in contact with the adhesive layer of the adhesive sheet and the two are laminated.
[0166] When manufacturing the first laminate, the protective film forming film 1 is formed on the release surface of the release sheet by the above method. If the protective film forming film is a two-layer product, for example, a coating liquid for the protective film forming film is prepared, the coating liquid contains a resin composition constituting the first film and the second film of the protective film forming film 1 and a solvent further contained as required, and is coated on the release surface of the release sheet by a coating machine such as a roll coater, a knife coater, a roll knife coater, an air knife coater, a die coater, a rod coater, a gravure coater, a curtain coater, etc. and dried to form the first film and the second film, which are bonded together to form the protective film forming film 1. A state in which release sheets are laminated on both sides of the protective film forming film 1 is formed (the first laminate). At this time, it is preferred to use a heavy release type release sheet with a larger release force as the release sheet on the first film side, and a light release type release sheet with a smaller release force as the release sheet on the second film side.
[0167] In the first laminate, punching can be performed as required to form the protective film forming film 1 (and the release sheet with light release force) into a desired shape, such as a circle, etc. At this time, the excess parts of the protective film forming film 1 and the light release sheet generated by the punching can be appropriately removed.
[0168] On the other hand, when manufacturing the second laminated body, a coating liquid for an adhesive layer containing an adhesive constituting the adhesive layer 42 and a solvent further contained as required is applied to the release surface of the release sheet and dried to form the adhesive layer 42. Then, the substrate 41 is pressed against the exposed surface of the adhesive layer 42 to obtain a laminated body (second laminated body) consisting of the adhesive sheet 4 and the release sheet. The adhesive sheet 4 is composed of the substrate 41 and the adhesive layer 42.
[0169] Among them, when the adhesive layer 42 is composed of an energy-ray-curable adhesive, the adhesive layer 42 can be cured after the protective film-forming film 1 is stacked on the adhesive layer 42. In addition, when the adhesive layer 42 is cured after being stacked with the protective film-forming film 1, the adhesive layer 42 can be cured before the cutting process, and preferably the adhesive layer 42 is cured after the cutting process.
[0170] As energy rays, ultraviolet rays, electron beams, etc. can be generally used. The irradiation amount of energy rays varies depending on the type of energy rays. For example, in the case of ultraviolet rays, the light amount is preferably 50 to 1000 mJ / cm 2 Preferably, 100 to 500 mJ / cm 2 In the case of an electron beam, the light intensity is preferably about 10 to 1000 krad.
[0171] After obtaining the first laminate and the second laminate as described above, the light release sheet in the first laminate is peeled off to expose the surface (second surface) of the second film side of the protective film forming film 1, and the release sheet in the second laminate is peeled off, and the surface of the second film side of the protective film forming film 1 exposed in the first laminate is overlapped and pressed with the adhesive layer 42 of the adhesive sheet 4 exposed in the second laminate. The adhesive sheet 4 can be stamped as required to form it into a desired shape, such as a circle with a diameter larger than the protective film forming film 1. At this time, the excess portion of the adhesive sheet 4 generated by the stamping process can be appropriately removed.
[0172] Thus, an adhesive sheet 4 formed by laminating an adhesive layer 42 on a substrate 41, a protective film forming film 1 laminated on the adhesive layer 42 side of the adhesive sheet 4, and a protective film forming composite sheet 3 composed of a heavy peeling type peeling sheet laminated on the side opposite to the adhesive sheet 4 of the protective film forming film 1 can be obtained. As needed, a ring-shaped clamp adhesive layer 5 can be formed on the peripheral portion of the protective film forming film 1 exposed after peeling off the heavy peeling sheet. The clamp adhesive layer 5 can also be formed by coating and stamping using the same method as the above-mentioned adhesive layer 42. When the adhesive layer 42 is composed of an energy-ray-curing adhesive, the clamp adhesive layer 5 is not necessary in order to have sufficient adhesion before curing. When the adhesive layer 42 is composed of a non-energy-ray-curing adhesive with low adhesion, in order to fix a clamp such as an annular frame, a clamp adhesive layer 5 is preferably provided.
[0173] 3. Method of using the composite sheet for forming a protective film
[0174] As an example of a method of using the composite sheet 3 for forming a protective film according to the present embodiment, a method of obtaining a small piece with a protective film such as a semiconductor chip with a protective film from a workpiece such as a semiconductor wafer will be described.
[0175] The manufacturing method comprises the following steps (1) to (4);
[0176] Step (1): a step of attaching the surface (first surface) on the first region side of the protective film-forming film 1 of the protective film-forming sheet 3 to the back surface of the workpiece 6;
[0177] Step (2): a step of heating and curing the protective film-forming film 1 to obtain a protective film;
[0178] Step (3): cutting the workpiece 6 and the protective film forming film or the protective film to obtain a stack of small pieces singulated into the same shape and the protective film forming film or the protective film; and step (4): separating the protective film forming film or the protective film from the adhesive sheet.
[0179] In addition, the steps after step (1) may be the order of steps (2), (3), and (4), the order of steps (3), (2), and (4), or the order of steps (3), (4), and (2).
[0180] The method for manufacturing a small piece with a protective film will be described in further detail below. In particular, the case where the workpiece 6 is a semiconductor wafer and the small piece obtained is a semiconductor chip with a protective film will be described below as an example.
[0181] like Figure 4As shown, the protective film forming film 1 of the protective film forming sheet 3 is attached to the back side of the semiconductor wafer 6 (step (1)). At this time, the outer periphery of the protective film forming film 1 can be fixed by the ring frame 7. In addition, when the clamp adhesive layer 5 is provided, the clamp adhesive layer 5 is attached to the ring frame 7. The back side of the semiconductor wafer 6 is attached to the surface (first surface) on the first film side of the protective film forming film 1. When attaching the protective film forming film 1 to the semiconductor wafer 6, the protective film forming film 1 can be heated as needed to exert its adhesiveness.
[0182] Then, the protective film forming film 1 is cured to form a protective film (step (2)), thereby obtaining a semiconductor wafer 6 with a protective film. When the protective film forming film 1 is thermosetting, the protective film forming film 1 can be heated at a predetermined temperature for an appropriate time. In addition, the protective film forming film 1 can be cured after the dicing step, or the protective film can be cured after the semiconductor chip with the protective film forming film is picked up from the adhesive sheet.
[0183] After obtaining the semiconductor wafer 6 with a protective film as described above, the protective film is irradiated with laser through the adhesive sheet 4 as needed to perform laser printing. In addition, the laser printing can be performed before the protective film forming film 1 is cured. The surface (second surface) on the second region side of the protective film forming film or the protective film is laser printed.
[0184] Next, the semiconductor wafer 6 with the protective film is cut by a conventional method to obtain a chip with the protective film (chip with the protective film) (process (3)). Then, the adhesive sheet 4 is expanded in the planar direction as needed, and the chip with the protective film is picked up from the adhesive sheet 4 (process (4)).
[0185] The chip with a protective film obtained as described above has an excellent appearance because the grinding marks caused by the back grinding process are hidden by the protective film and cannot be seen by the naked eye. In addition, the strength of the chip with a protective film and the semiconductor wafer with a protective film is improved by the protective film, so the damage during transportation, storage, and processing can be reduced. Furthermore, because the back of the semiconductor chip with a protective film is shielded, it can shield various electromagnetic waves generated in the electronic device, thereby reducing the failure of the semiconductor device.
[0186] 4. Other embodiments of composite sheets for forming protective films
[0187] Figure 3 FIG. 2 is a cross-sectional view of a composite sheet for forming a protective film according to another embodiment of the present invention. Figure 3As shown, the composite sheet 3A for forming a protective film of the present embodiment is composed of an adhesive sheet 4 having an adhesive layer 42 laminated on one surface of a substrate 41, and a protective film forming film 1 laminated on the adhesive layer 42 side of the adhesive sheet 4. The protective film forming film 1 in the present embodiment is almost the same as the workpiece when viewed from above, or is formed to be slightly larger than the workpiece and smaller than the adhesive sheet 4. The adhesive layer 42 of the portion where the protective film forming film 1 is not laminated can be attached to a fixture such as a ring frame.
[0188] The materials and thicknesses of the components of the composite sheet 3A for forming a protective film of the present embodiment are the same as those of the composite sheet 3 for forming a protective film described above. When the adhesive layer 42 is composed of an energy-ray-curable adhesive, the energy-ray-curable adhesive is preferably cured in the portion of the adhesive layer 42 that contacts the protective film-forming film 1, and the energy-ray-curable adhesive is not cured in the other portions. Thus, the smoothness and glossiness of the protective film after curing the protective film-forming film 1 can be improved, and the adhesion to the clamp such as the ring frame can be highly maintained.
[0189] In addition, a jig adhesive layer similar to the jig adhesive layer 5 of the protective film forming composite sheet 3 may be separately provided on the periphery of the adhesive layer 42 of the adhesive sheet 4 of the protective film forming composite sheet 3A.
[0190] The embodiments described above are described for easy understanding of the present invention, and are not described for limiting the present invention. Therefore, the various elements disclosed in the embodiments described above also cover all design changes and equivalent technical solutions within the technical scope of the present invention.
[0191] For example, in order to protect the protective film-forming film until use, a release sheet may be laminated on the protective film-forming film 1 side of the protective film-forming composite sheet 3 or the protective film-forming composite sheet 3A.
[0192] Example
[0193] Hereinafter, the present invention will be further described using examples and the like, but the scope of the present invention is not limited to these examples and the like.
[0194] [Example 1]
[0195] (Preparation of Film for Protective Film Formation)
[0196] The following components were mixed at the ratios shown in Table 1 (in terms of solid content), and diluted with methyl ethyl ketone so that the solid content concentration was 61% by mass to prepare protective film-forming film coating solutions 1 to 4.
[0197] (a) Binder polymer: a (meth)acrylate copolymer obtained by copolymerizing 9 parts by mass of n-butyl acrylate, 71 parts by mass of methyl acrylate, 6 parts by mass of glycidyl methacrylate and 14 parts by mass of 2-hydroxyethyl acrylate (mass average molecular weight: 800,000, glass transition temperature: -1°C)
[0198] (b) Thermosetting components
[0199] (b-1) Bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, jER828, epoxy equivalent 184 to 194 g / eq)
[0200] (b-2) Bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, jER1055, epoxy equivalent 800 to 900 g / eq)
[0201] (b-3) Dicyclopentadiene type epoxy resin (manufactured by DIC Corporation, EPICLON HP-7200HH, epoxy equivalent 255 to 260 g / eq)
[0202] (c) Thermally active latent epoxy resin curing agent: dicyandiamide (manufactured by ADEKA, ADEKA HARDENER EH-3636AS, active hydrogen content 21 g / eq)
[0203] (d) Curing accelerator: 2-phenyl-4,5-dihydroxymethylimidazole (manufactured by SHIKOKU CHEMICALS CORPORATION, CUREZOL 2PHZ)
[0204] (e) Colorant: Carbon black (manufactured by Mitsubishi Chemical Corporation, MA600B, average particle size 20 nm)
[0205] (f) Silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., KBM403)
[0206] The following four silica fillers were used as silica fillers. Silica filler (g-1) was used in coating liquid 1, silica filler (g-2) was used in coating liquid 2, silica filler (g-3) was used in coating liquid 3, and silica filler (g-4) was used in coating liquid 4. In the following, D max ' represents the maximum particle size of the raw material filler, and D 50 ' represents the 50% cumulative particle size of the raw material filler.
[0207] (g-1) Silica filler (manufactured by Admatechs, SC4050-MMQ, D max ': 5μm, D 50 ': 1.0μm)
[0208] (g-2) Silica filler (manufactured by Admatechs, SC2050-MA, D max ': 2μm, D 50 ': 0.5μm)
[0209] (g-3) Silica filler (manufactured by Admatechs, SC105G-MMQ, D max ': 1.5μm, D 50 ': 0.3μm)
[0210] (g-4) Silica filler (manufactured by Admatechs, YA050C-MJE, D max ': 0.2μm, D 50 ': 0.05μm)
[0211] In addition, for D 50 ' Fillers smaller than 1 μm, the particle size of the raw material filler in this specification (maximum particle size D max ', 50% cumulative particle size D 50 ') is a value measured by a particle size distribution measuring device (manufactured by NIKKISO CO., LTD., NanoTrac Wave-UT151) using a dynamic light scattering method. 50 The particle size of the filler with a particle size of 1 μm or more is a value measured by a laser diffraction scattering method using a particle size distribution measuring device (Microtrac MT3000II manufactured by NIKKISO CO., LTD.).
[0212] The blending ratio (parts by mass) of each component in coating liquids 1 to 4 is shown in the following table.
[0213] [Table 1]
[0214]
[0215] A first release sheet (manufactured by LINTEC Corporation: SP-PET3811, thickness 38 μm) having a silicone release agent layer formed on one surface of a polyethylene terephthalate (PET) film and a second release sheet (manufactured by LINTEC Corporation: SP-PET381031, thickness 38 μm) having a silicone release agent layer formed on one surface of a PET film were prepared.
[0216] The coating liquid was applied to the release surface of the first release sheet using a knife coater so that the thickness of the filler-containing film finally obtained was 7 μm, and then dried in an oven at 120° C. for 2 minutes to prepare a filler-containing film. The filler-containing film obtained using coating liquid 1 was designated as film 1, and the films obtained using coating liquids 2 to 4 were designated as films 2 to 4 in the same manner.
[0217] The second release sheet was peeled off from the obtained film to expose one surface of the film, and the films were thermocompression-bonded to each other at 70° C. to prepare a protective film-forming film having the following two-layer structure.
[0218] Film for forming protective film (1 / 2): laminate of film 1 and film 2
[0219] Film for forming protective film (1 / 3): laminate of film 1 and film 3
[0220] Film for forming protective film (1 / 4): laminate of film 1 and film 4
[0221] Film for forming protective film (2 / 3): laminate of film 2 and film 3
[0222] Film for forming protective film (2 / 4): laminate of film 2 and film 4
[0223] Film for forming a protective film (1 / 1): Laminated body of films 1
[0224] Film for forming a protective film (4 / 4): a laminate of films 4
[0225] The protective film-forming film (1 / 1) and the protective film-forming film (4 / 4) are substantially single-layer films.
[0226] The protective film-forming film was punched out into a shape having a diameter of 200 mm, which was the same as the silicon wafer to be attached.
[0227] (Adhesive Sheet Production)
[0228] The following energy-ray-curable acrylic copolymer was used as a main agent of the adhesive layer.
[0229] An energy-ray-curable acrylic copolymer having a methacryloyloxy group on a side chain, a mass average molecular weight of 800,000 and a glass transition temperature of -10°C, is obtained by reacting 2-methacryloyloxyethyl isocyanate (hereinafter abbreviated as "MOI") with an acrylic polymer copolymerized by 80 parts by mass of 2-ethylhexyl acrylate (2EHA) and 20 parts by mass of 2-hydroxyethyl acrylate (HEA) (the total molar number of isocyanate groups in MOI is 80% relative to the total molar number of hydroxyl groups derived from HEA in the acrylic polymer).
[0230] 100 parts by mass of the energy-ray-curable acrylic copolymer, 3 parts by mass of Irgacure 184 (manufactured by BASF) as a photopolymerization initiator, 3 parts by mass of Irgacure 127 (manufactured by BASF), and 6 parts by mass of CORONATE L (manufactured by TOSOH CORPORATION, toluene diisocyanate crosslinking agent) as a crosslinking agent were mixed in a solvent to obtain a coating solution of an adhesive composition.
[0231] The obtained coating solution of the adhesive composition was applied by a knife coater onto the release-treated surface of a release sheet (manufactured by LINTEC Corporation, product name "SP-PET381031", thickness: 38 μm) having one surface of a polyethylene terephthalate film subjected to release treatment with a silicone release agent, and treated at 100° C. for 1 minute to form an adhesive layer with a thickness of 20 μm.
[0232] The obtained adhesive layer was attached to a polypropylene substrate having a thickness of 80 μm, and the release sheet was peeled off to obtain an adhesive sheet. The obtained adhesive sheet was punched into a circular shape having a diameter of 330 mm to obtain a cut sheet.
[0233] (Measurement of filler particle size in cross section of protective film forming film)
[0234] The protective film-forming film was heated at 130° C. for 2 hours to be cured. The cured protective film was cut and the cross section was polished under the following conditions.
[0235] Polishing conditions
[0236] Device: Polishing device (manufactured by Refine Tec Ltd., product name: Refine Polisher-HV)
[0237] Polishing: Made by Refine Tec Ltd., grinding and polishing, suede cloth
[0238] Abrasive: Musashi Holts Co., Ltd., aluminum oxide particle dispersion MH159
[0239] Polishing speed: 200rpm
[0240] Load for polishing: 1N
[0241] The maximum particle size D of the filler was obtained by observing the polished surface with VE-9800 manufactured by KEYENCE. max And cumulative particle size D 50In addition, the polished surface was observed in each of the following areas until 30 fillers were confirmed.
[0242] Cross-sectional observation was performed in the following first region and second region.
[0243] First region: When the total thickness of the protective film forming film is T, the region from the surface of one side to a depth of 0.2T
[0244] Second region: When the total thickness of the protective film forming film is T, the region from the other surface to a depth of 0.2T
[0245] The filler particle size observed from the cross section is calculated using the equivalent circle diameter. 50 The area on the smaller side is referred to as the "first area".
[0246] The maximum particle size D of the filler particles in each region of the laminated protective film prepared as described above is shown below. max And cumulative particle size D 50 In addition, the protective film forming film (1 / 1) and the protective film forming film (4 / 4) are substantially single-layer films, and the maximum particle size D max And cumulative particle size D 50 The same is true in the first region and the second region.
[0247] [Table 2]
[0248]
[0249] (Example 1)
[0250] The surface of the first region side of the protective film forming film (1 / 2) (the surface of the film 2) was attached to the polished surface of a silicon wafer (diameter 200 mm, thickness 280 μm) after #2000 polishing while being heated to 70°C using a film laminating machine (manufactured by LINTEC Corporation, RAD-3600F / 12).
[0251] Next, the adhesive layer of the dicing sheet prepared above was attached to the surface of the second region side of the protective film-forming film (the surface of the film 1 ). In addition, the outer periphery of the adhesive layer was fixed to a ring frame.
[0252] The stacked body of the silicon wafer, the protective film forming film (1 / 2), and the dicing sheet was heated at 130° C. for 2 hours to cure the protective film forming film, thereby forming a protective film on the polished surface of the silicon wafer.
[0253] The silicon wafer with the protective film attached to the dicing sheet was diced using a dicing device ("DFD6362" manufactured by Disco Corporation) to obtain chips with a size of 5 mm×5 mm with the protective film.
[0254] The cutting conditions are as follows.
[0255] Cutting knife moving speed: 50mm / sec
[0256] Cutting knife speed: 30000rpm
[0257] (Breakdown Evaluation)
[0258] After the cutting process, ultraviolet rays are irradiated from the substrate surface side of the cut sheet to cure the adhesive, and then two chips are picked up from the center of the wafer. In addition, two chips are picked up from two straight lines that are perpendicular to each other through the center point of the wafer and are about 20 mm away from the center of the wafer (a total of 4 places). A digital microscope (manufactured by KEYENCE CORPORATION, VE-9800) is used to confirm the presence or absence of stripe-shaped cracks (collapsed edges) in the thickness direction starting from the polished surface of the chip and the length of the cracks for the total of 10 chips. According to the maximum length of the cracks generated on the 10 chips, the following standards are used for evaluation.
[0259] S: Maximum length less than 10 μm
[0260] A: Maximum length is 10μm or more and less than 15μm
[0261] B: Maximum length is 15μm or more and less than 30μm
[0262] F: Maximum length is 30 μm or more
[0263] (Example 2)
[0264] The same procedure as in Example 1 was performed except that the surface on the first region side (surface of film 3) of the protective film-forming film (1 / 3) was attached to a silicon wafer and the surface on the second region side (surface of film 1) was attached to a dicing sheet.
[0265] (Example 3)
[0266] The same procedure as in Example 1 was performed except that the surface on the first region side (surface of film 4) of the protective film-forming film (1 / 4) was attached to a silicon wafer and the surface on the second region side (surface of film 1) was attached to a dicing sheet.
[0267] (Example 4)
[0268] The same procedure as in Example 1 was performed except that the surface on the first region side (surface of film 3 ) of the protective film-forming film ( 2 / 3 ) was attached to a silicon wafer and the surface on the second region side (surface of film 2 ) was attached to a dicing sheet.
[0269] (Example 5)
[0270] The same procedure as in Example 1 was performed except that the surface on the first region side (surface of film 4) of the protective film-forming film (2 / 4) was attached to a silicon wafer and the surface on the second region side (surface of film 2) was attached to a dicing sheet.
[0271] (Example 6)
[0272] The same as in Example 1 except that the protective film forming film (1 / 2) was attached to the dicing sheet in advance. Specifically, the adhesive layer of the dicing sheet prepared above was attached to the surface of the second region side of the protective film forming film (1 / 2) (the surface of the film 1). Next, a film attaching machine (manufactured by LINTEC Corporation, RAD-3600F / 12) was used to attach the surface of the first region side (the surface of the film 2) to the polished surface of the silicon wafer (diameter 200mm, thickness 280μm) after #2000 polishing while heating to 70°C. The subsequent steps were the same as in Example 1.
[0273] (Comparative Example 1)
[0274] The same procedure as in Example 1 was carried out except that the protective film-forming film (1 / 1) was used.
[0275] (Comparative Example 2)
[0276] The same procedure as in Example 1 was carried out except that the protective film-forming film (4 / 4) was used.
[0277] (Reference Example 1)
[0278] The same procedure as in Example 1 was performed except that the surface on the second region side (surface of film 1) of the protective film-forming film (1 / 4) was attached to a silicon wafer and the surface on the first region side (surface of film 4) was attached to a dicing sheet.
[0279] (Reference Example 2)
[0280] The same procedure as in Example 1 was performed except that the second region side surface (film 2 surface) of the protective film forming film (2 / 3) was attached to a silicon wafer and the first region side surface (film 3 surface) was attached to a dicing sheet.
[0281] [Table 3]
[0282]
[0283] It can be seen from Table 3 that by attaching the first region containing fillers with smaller particle sizes to the semiconductor wafer side and attaching the second region containing fillers with larger particle sizes to the cutting sheet side, when the cutting sheet is used to cut the stack of the semiconductor wafer and the protective film forming film, the shaking and vibration of the blade can be suppressed and the edge chipping can be reduced.
[0284] Industrial Applicability
[0285] The protective film-forming film and the protective film-forming composite sheet of the present invention are particularly suitable for manufacturing small pieces (semiconductor chips, etc.) having a protective film from a workpiece such as a semiconductor wafer, and are particularly useful for reducing edge chipping.
[0286] Description of Reference Numerals
[0287] 1: film for forming a protective film; 2: filler; 3, 3A: composite sheet for forming a protective film; 4: adhesive sheet; 41: substrate; 42: adhesive layer; 5: adhesive layer for a fixture; 6: workpiece (semiconductor wafer); 7: ring frame.
Claims
1. A film for forming a protective film, comprising a filler, wherein: In cross-sectional observation of the film, when the total thickness of the film is defined as T, and the region from the surface of one side of the film to a depth of 0.2T is defined as the first region, and the region from the surface of the other side of the film to a depth of 0.2T is defined as the second region, The 50% cumulative particle size D of the filler observed in the first region 50 1 and the 50% cumulative particle size D of the filler observed in the second region 50 2 satisfies the following relationship: D 50 1 <D 50 2. And 10000%>(D 50 2-D 50 1) / D 50 1×100%≥5%; The D 50 1 In the range of 0.01 to 2 μm, the D 50 2In the range of 0.01 to 3 μm; The filler is a silicon dioxide filler; The surface on the first region side is attached to a workpiece, and the surface on the second region side is attached to a cutting blade. 2 . The protective film-forming film according to claim 1 , comprising two or more constituent layers.
3. A composite sheet for forming a protective film, comprising an adhesive sheet formed by laminating a substrate and an adhesive layer, and the protective film forming film according to claim 1 or 2 laminated on the adhesive layer side of the adhesive sheet, The protective film forming composite sheet is formed by laminating the surface of the protective film forming film on the second region side on the adhesive layer.
4. A method for producing a small piece with a protective film, comprising the following steps (1) to (4): Step (1): a step of attaching the surface of the protective film-forming film of the protective film-forming composite sheet according to claim 3 on the first region side to a workpiece; Step (2): a step of heating and curing the protective film-forming film to obtain a protective film; Step (3): a step of dicing the semiconductor wafer and the protective film forming film or the protective film to obtain a stack of small pieces singulated into the same shape and the protective film forming film or the protective film; and Step (4): A step of separating the protective film-forming film or the protective film from the adhesive sheet.