Polymer gels in polymer brush formation
By using a swellable and removable polymer gel during polymer brush formation, the problems of uneven distribution of reactants and solvent evaporation during polymer brush formation are solved, and a uniform polymer brush on complex surfaces is achieved Form and mass production of high-quality effects.
Patent Information
- Application Number
- CN202080072355.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-15
- Filing Date
- 2020-10-09
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-10-09
AI Technical Summary
The prior art has problems with product inhomogeneity caused by uneven distribution of reactants and solvent evaporation when forming polymer brushes, especially in large-scale production and complex surfaces, which are difficult to achieve complete polymer brush formation.
Using a swellable and removable polymer gel as the polymeric medium, the oxygen migration is slowed down and the polymeric brushes are ensured uniform formation and control of the polymeric brushes by forming polymer brushes on the surface and providing a uniformly distributed reaction environment during the polymerization reaction.
The polymer brush formation on all geometric shapes and complex surfaces is achieved, ensuring uniformity and high quality of the product, simplifying the mass production process, and avoiding undesirable polymer brush formation.
Smart Images

Figure HDA0003596495060000011 
Figure HDA0003596495060000021 
Figure HDA0003596495060000022
Abstract
Description
Technical Field
[0001] The present invention relates to the use of a polymer gel in forming a polymer brush. In particular, the present invention relates to a polymer gel swollen in a polymeric medium, said swollen polymer gel being applied to form a polymer brush. The present invention further relates to the use of a polymer gel in forming a polymer brush on a surface. In particular, the polymer gel used in the present invention is a polymer gel swellable in a polymeric medium and further removable after forming a polymer brush on a surface. The present invention provides an improved method for forming a polymer brush on a surface, thereby enabling easy mass production of polymer brush-coated surfaces as well as the formation of specific polymer brushes. In particular, the present invention enables the application of a polymeric medium on surfaces of all geometries. Background Art
[0002] The formation of polymer brushes is well known. A polymer brush is a polymer structure tethered at one end to a substrate such as a metal, plastic or ceramic material. Using specific preparation techniques and specific monomers, polymer brushes with specific properties such as chemical composition, thickness, grafting density and architecture can be designed and synthesized.
[0003] In particular, polymer brushes are used to join otherwise incompatible materials, i.e. materials that cannot be easily joined by gluing or conventional interlocking methods. A powerful feature of polymer brushes is that materials can be joined in an almost invisible manner.
[0004] A variety of methods for forming polymer brushes on surfaces are known. When forming a polymer brush, a polymerization initiator is first formed on the surface on which the polymer brush is to be formed. Secondly, the surface is contacted with a suitable monomer, catalyst, ligand and optional solvent, or with a suitable monomer, catalyst, ligand, oxygen scavenger and optional solvent, whereby the polymer brush can be formed using specific reaction conditions. The polymerization initiator and monomer are selected to suit the purpose and properties of the resulting polymer brush. The polymer brush can also be formed into a layer of polymer brushes by repeating the formation of the polymer brush, for example using another starting monomer. This can be achieved due to the controlled nature of the polymerization, which leaves an initiation site at the end of the polymer brush.
[0005] Nevertheless, the preparation of polymer brushes and the handling of reagents remain specialized tasks. In addition, the production of large-scale polymer brush-coated surfaces presents various difficulties, such as obtaining a uniform distribution of the reactants on the surface on which the polymer brush is to be formed, and avoiding the formation of depressions of the reactants on the surface or flat areas where the reactants are not present. Another difficulty is dealing with the evaporation of the solvent during the formation process, which obviously results in a product with an uneven distribution of polymer brushes. Similarly, areas without any polymer brush at all can be a problem, which results in poor quality polymer brush products. In order to ensure complete formation of the polymer brush on the surface, the surface can be completely immersed in the reactants, however, this approach may not be feasible for larger surfaces or substrates.
[0006] Therefore, there remains a need to improve and ensure uniform distribution of reactants for forming polymer brushes.
[0007] Polymer gel is a well-known substance. Polymer gel can be used for many applications from diapers to contact lenses and implants and can be used for tissue engineering. Polymer gel is a three-dimensional polymer network that can absorb large amounts of water (hydrogel) or organic solvents (organogel), up to 500 times its own weight. Polymer gel is obtained by cross-linking polymers into a cross-linked polymer matrix. These cross-linking sites can be divided into reversible cross-linking and irreversible cross-linking. Reversibly cross-linked polymer gels can be obtained by different interactions or bonds, including ion attraction, H-bonding or metal coordination. Subjecting reversible polymer gels to certain stimuli causes cross-linking fractures. Irreversible cross-linked polymer gels have a network of covalent bonds and produce a permanent gel network.
[0008] Polymer gels have many valuable characteristics, particularly viscoelastic responses to mechanical deformation. In particular, polymer gels have been proposed for use in a variety of applications, such as artificial muscles, purification or separation systems, regenerative medicine, biosensors, shape memory materials, transport systems, and molecular recognition systems. Thus, polymer gels are able to absorb or respond to other compounds.
[0009] Recently, hydrogels (polymer gels that swell in water) have been proposed for drug delivery due to their affinity for water and the potential for sustained drug release through, for example, diffusion, swelling, chemical or environmental control. However, although promising, very few products have entered the market, which may be attributed to the difficulty in releasing drugs from hydrogels without degrading the hydrogels, thereby causing the risk of introducing toxic effects due to the potential harm of degraded hydrogels to human health. One approach is to synthesize drug delivery hydrogels that can be enzymatically degraded to avoid accumulation of the hydrogel in the body.
[0010] Hydrogels have been combined with polymer brushes in the form of polymer brush-gels, see S. Demirci, Polymers 2018, 10, 956. Crosslinkers react or combine with brush-forming monomers to form brush-gels (or crosslinked polymer brush networks) from which other compounds can be released (taking methylene blue as an example). In S. Demirci, cyclodextrin is incorporated as a crosslinker into a polymer such as poly (2-N-morpholinoethyl methacrylate) to produce crosslinked cyclodextrin methacrylate (CDMA) polymers on silicon wafers. The CDMA polymer is then used to reversibly capture / release methylene blue from the brush-gel.
[0011] Therefore, although hydrogels are widely used in many applications, and polymer gels may also find similar applications, they have some disadvantages as a medium for producing polymer brushes. For example, depending on the polymer gel, the polymer brush reactants can be absorbed by the polymer gel, thereby preventing the reactants from migrating to the interphase, which leads to poor formation of polymer brushes. In addition, the cross-linking sites on the polymer gel can react with the polymer brush reactants and adversely affect the polymer brush formation. In addition, some cross-linking sites can act as free radical scavengers and thus affect the polymer brush formation. In addition, some cross-linking sites can act as metal ligands, which means that the metal catalyst used in the polymerization may be absorbed, thereby disrupting the polymerization process.
[0012] Nevertheless, hydrogels have been used together with polymer brushes. A coating of a hydrogel layer of a polysaccharide and a polymer brush layer is known from EP 3 385 340 A1. The coating is prepared as follows: a) a hydrogel layer is provided on a substrate, b) an initiator having a radically transferable atom is attached to the hydrogel layer, and c) a monomer is reacted with the initiator to form a polymer brush attached to the hydrogel layer. Thus, the hydrogel becomes an integral part of the polymer brush and the hydrogel is functionalized by the polymer brush.
[0013] The inventors of the present invention have surprisingly found that certain polymer gels can promote uniform distribution of the polymerization reactants and even promote the formation of polymer brushes. Summary of the invention
[0014] The present invention relates to the formation of polymer brushes. In particular, the present invention relates to the use of polymer gels in the formation of polymer brushes. The polymer gel used in the present invention is swellable in a polymerization medium and is removable after the polymer brush is formed on a surface. Therefore, the polymer gel acts as a "container" for the polymerization medium containing the reactants required for the formation (or growth) of the polymer brush. The polymer gel provides many advantages, including the ease of applying the reactants required for the formation of the polymer brush. When swollen in the polymerization medium, the polymer gel has a dense structure, which allows better contact between the polymerization medium and the surface on which the polymer brush is to be formed. In addition, after the polymer brush is formed, the polymer gel as well as the excess polymerization medium can be easily removed from the surface. Therefore, the polymer gel does not react with optional functional groups fixed to the surface or components of the polymerization medium, thereby leaving a pure polymer brush after removing the polymer gel.
[0015] Thus, in a first aspect, the present invention relates to a method for forming polymer brushes on a surface whereby a surface having a polymerization initiator immobilized thereon is contacted with a polymerization medium, in which method a swellable and removable polymer gel is used in the formation of the polymer brushes. The main advantage of using the polymerization medium in combination with the polymer gel is that the polymer gel swells in the polymerization medium and thus the polymer gel provides a semi-solid or dense support for the polymerization medium and thus provides a support for the polymer brush forming components of the polymerization medium. This enables the formation of polymer brushes on surfaces of all geometries and orientations, as the swollen polymerization medium adheres to the surface during the polymerization reaction. Another advantage is that the polymer gel slows down the migration of oxygen from the surrounding atmosphere to the polymer gel-surface interphase, which gives a higher degree of control over the polymerization reaction that produces the polymer brushes.
[0016] Thus, the present invention particularly relates to a method wherein the polymer gel is swellable in a polymerizing medium and wherein the polymer gel is removable after forming a polymer brush on a surface.
[0017] Traditionally, polymer brushes are formed in a dip coating method, thus limiting the formation of polymer brushes on larger or more complex structures. In the present invention, the polymerization reaction can be easily carried out without the need to fully immerse the surface / structure in the polymerization medium. Another advantage of the present invention is that if the immobilized initiator is present at all sites on the surface / structure, the formation of polymer brushes can be targeted to only specific sites, while traditional dip coating may result in undesirable polymer brush formation.
[0018] In a second aspect, the present invention relates to the use of a swellable and removable polymer gel in forming a polymer brush. Likewise, the polymer gel is swellable in a polymerization medium and is removable after forming the polymer brush. The use of the polymer gel provides a uniform distribution of the polymerization medium on the surface on which the polymerization initiator is fixed. The use of the polymer gel has the following advantageous effects: the polymer gel swells in the polymerization medium because the swollen polymerization medium (swollen gel) adheres better to the surface, whereby the swollen polymerization medium (swollen gel) can be easily applied to surfaces with complex geometries and various orientations.
[0019] Surprisingly it was found that swelling of the polymer gel in the polymerization medium does not hinder the polymerization reaction (ie the formation of polymer brushes on the surface).
[0020] Description of the drawings
[0021] The present invention will be more fully understood from the detailed description given herein. The accompanying drawings are given by way of illustration only and therefore do not limit the present invention. In the drawings:
[0022] Figure 1 The method of the present invention is shown, wherein a surface having a polymerization initiator immobilized thereon (first step) is brought into contact with a polymer gel swollen in a polymerization medium (second step), and a polymer brush is progressed and formed by the polymerization initiator (third step).
[0023] Figure 2 The method of the invention is shown in which a surface is contacted with a polymer gel swollen in a polymerization medium (see Example 4) and furthermore the medium is able to adhere to the surface even when tilted vertically during a 1 hour polymerization.
[0024] Figure 3 Visually, a uniform polymer brush film was shown only where the polymer gel swollen in the polymerization medium was placed on the surface (after 1 hour). Figure 2 Along the edges, the aluminum sample still has only immobilized initiator and no polymer brushes are formed.
[0025] Figure 4 Shown is the swollen polymer gel of Example 5 smeared on a 10 cm x 10 cm stainless steel plate.
[0026] Figure 5 The sample is shown after it has been polymerized and cleaned, see Example 5.
[0027] Figure 6 The swollen polymer gel of Example 6 is shown.
[0028] Figure 7The polymer brushes formed in the areas where the swollen polymer gel has come into contact with the polymerization initiator are shown, see Example 6.
[0029] Figure 8 The swollen polymer gel of Example 7 is shown.
[0030] Fig. 9 The swollen polymer gel of Example 8 is shown.
[0031] Fig.10 Shown are a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right), see Example 10.
[0032] Fig.11 The IRRAS spectrum after formation of PMMA polymer brushes is shown, see Example 10.
[0033] Fig.12 Shown are a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right), see Example 11.
[0034] Fig.13 The IRRAS spectrum after formation of PMMA polymer brushes is shown, see Example 11.
[0035] Fig.14 Shown are a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right), see Example 12.
[0036] Fig.15 The IRRAS spectrum after formation of PMMA polymer brushes is shown, see Example 12.
[0037] Fig.16 Shown are a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right), see Example 13.
[0038] Fig.17 The IRRAS spectrum after formation of PMMA polymer brushes is shown, see Example 13.
[0039] Fig.18 Shown are a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right), see Example 14.
[0040] Fig.19 The IRRAS spectrum after formation of PMMA polymer brushes is shown, see Example 14.
[0041] Fig. 20Shown are a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right), see Example 15.
[0042] Fig.21 Shown are a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right), see Example 16.
[0043] Fig. 22 The water contact angle between the plate with the formed polymer brush and a water drop is shown, see Example 16.
[0044] Fig.23 Shown are a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right), see Example 17.
[0045] Fig.24 The water contact angle between the plate with the formed polymer brush and a water drop is shown, see Example 17.
[0046] Fig.25 Shown are a polymer gel swollen in a polymerization medium (left) and a visually uniform polymer brush film only where a polymer gel swollen in a polymerization medium is placed on the surface (right), see Example 18.
[0047] Fig.26 The IRRAS spectrum after formation of PGMA polymer brushes is shown, see Example 18.
[0048] Fig. 27 The XPS inspection spectrum of the PMMA polymer brush is shown, see Example 21.
[0049] Fig.28 A high resolution spectrum of the carbon peaks of a PMMA polymer brush is shown, see Example 21.
[0050] Fig.29 The XPS inspection spectrum of the PS polymer brush is shown, see Example 25.
[0051] Fig.30 A high-resolution spectrum of the carbon peaks of a PS polymer brush is shown, see Example 25.
[0052] Fig.31 The XPS inspection spectrum of PHEMA polymer brushes is shown, see Example 26.
[0053] Fig.32 A high resolution spectrum of the carbon peaks of a PHEMA polymer brush is shown, see Example 26. DETAILED DESCRIPTION
[0054] The present invention and its various aspects are described in more detail below.
[0055] The present invention relates to a method for forming a polymer brush on a surface, wherein the surface having a polymerization initiator immobilized thereon is contacted with a polymerization medium, wherein during the formation of the polymer brush, a polymer gel is swollen in the polymerization medium. After the polymer brush is formed, the polymer gel can be removed from the surface.
[0056] In the context of the present invention, the expressions "polymer gel" and "the polymer gel" are intended to include one or more polymer gels. The more than one polymer gel may suitably be two, three, four or five polymer gels.
[0057] The polymer gel to be used in the present invention is suitably swellable in water, in a mixture of water and an alcohol, in a mixture of water and an aprotic solvent, or in an aprotic solvent other than the polymerization medium.
[0058] In a preferred embodiment of the present invention, the polymer gel is a polymer gel in which the crosslinking of the polymer gel is reversible. Thus, the swelling of the polymer gel in the polymerizing medium (swollen gel) can be reversed by an external stimulus.
[0059] The polymer gel to be used in the present invention is a polymer gel that can absorb the organic / aqueous solvent system used in the polymer medium. The polymer gel to be used in the present invention is suitably a reversible polymer gel, i.e. a polymer gel that can be changed between a gelled form and a liquid form. In particular, the polymer gel to be used in the method of the present invention can be a hydrogel. Suitable polymer gels have a single network (one type of polymer and crosslinking) or a double network (two types of polymers and crosslinking), and are reversibly crosslinked polymer gels. Examples of suitable polymer gels include, but are not limited to, polyallylamine (PAH), poly (methacrylic acid 2-hydroxyethyl ester phosphate), polyvinyl imidazole, polyacrylic acid, PEG, collagen, gelatin, agarose and polysaccharides such as chitosan, cyclodextrin (combination of for example β-CD polymer and PEG-cholesterol polymer), alginate, sodium alginate and xanthan gum and polymer gels based on cysteine. It is expected that xanthan gum is a polysaccharide that is very suitable for use as a polymer gel for the purpose of the present invention. The crosslinking agent used to form a crosslinked polymer gel can be introduced as a part of the polymer gel or added to the system as an additive.
[0060] In one embodiment, the polymer gel has metal chelating sites whereby metal coordination is possible. Introducing molecules containing metal chelating moieties, such as tannic acid (TA), can provide crosslinking of the polymer by coordination of metal ions such as Cu(II), Fe(III) and Al(III).
[0061] In another embodiment, crosslinking of the polymer gel relies on hydrophobic interactions. Crosslinking is achieved, for example, through guest-host interactions (eg, cyclodextrin with small hydrophobic molecules).
[0062] In another embodiment, the crosslinking of the polymer gel relies on sulphur bridges. The crosslinking is carried out via disulfide bonds generated internally in a polymer (eg polycysteine).
[0063] In another embodiment, the polymer gel has hydrogen bond acceptors and / or donors, thereby promoting cross-linking by hydrogen bonding. Examples are gelatin and agarose, which are also conveniently thermosensitive polymer gels.
[0064] The polymer gel to be used in the present invention is preferably reversibly cross-linked. Reversibility is obtained by responding to external senses such as pH, temperature, exposure, sonication, solvent polarity or oxidation potential. The example of pH responsive polymer gel is PAH / TA / Fe (III) polymer gel (hydrogel). At lower pH (lower than 7), the polymer gel is in liquid form, and at higher pH (7 or higher), the polymer gel is compact or semisolid. Another example is a hydrogel of poly (2-hydroxyethyl methacrylate phosphate), which gels at high pH, but liquefies when sonicated in water (or at low pH). In particular, the swollen polymer gel can be removed by adjusting pH or temperature, by exposure or by changing the polarity of the solvent mixture. In some methods, sonication is carried out in a suitable solvent, optionally as a series of rinsing steps.
[0065] An example where cross-linking is promoted by hydrophobic interactions is cyclodextrin, which is introduced into the site chain of one polymer. The other polymer is then designed to have a hydrophobic moiety. Gelation is obtained by mixing the two polymers in a hydrophilic environment. Due to energy considerations, the hydrophobic moiety will be attracted to the hydrophobic interior of the cyclodextrin and thereby promote cross-linking. This bond reversal can be achieved by changing to a solvent of the other polarity.
[0066] After the polymer gel is swollen in the polymerization medium, the resulting medium (gel) is transferred to the surface on which the polymer brush is to be formed.
[0067] Typically, the formation of the polymer brushes occurs at room temperature, however, it will be appreciated that other temperatures may also be applied. The temperature may be particularly related to the method used to form the polymer brushes. Furthermore, after the polymer brushes are formed, elevated temperatures may be utilized as a stimulus for liquefaction and thereby easy removal of the polymer gel.
[0068] Typically, polymer brushes are synthesized by SIP (surface initiated polymerization). Examples of suitable methods for forming polymer brushes include ARGET ATRP (activator regenerated by electron transfer atom transfer radical polymerization) method, conventional ATRP method, SARA ATRP (supplementary activated reducing agent atom transfer radical polymerization) method and SET LRP (single electron transfer living radical polymerization) method. These methods are well known in the art. Several methods are described in WO 2019 196999 A1.
[0069] The ATRP method generally employs a transition metal complex as a catalyst, an alkyl halide as a polymerization initiator (RX), and free radicals are generated via an atom transfer process. At the same time, the transition metal is oxidized to a higher oxidation state. The result is the growth of polymer chains from monomers. The ATRP method requires the following reactants: monomer, (solvent), initiator (immobilized on the surface where the polymer brush grows), catalyst, and ligand. In the Arget ATRP method, the activator is regenerated by electron transfer using a reducing agent, such as hydrazine, phenol, sugar, and ascorbic acid for Cu(I) regeneration. In SARA ATRP, Cu(0) is used as a supplementary activator and reducing agent, wherein Cu(0) directly activates the alkyl halide, and Cu(0) additionally reduces Cu(II) to Cu(I), thereby regenerating the Cu(I) activator. In the SIP method, the immobilized polymerization initiator is activated by a catalyst in the presence of monomers, and a polymer brush is formed on the surface. SET-LRP is similar to ATRP, ARGET ATRP, and SARA ATRP, utilizing alkyl halides as initiators. In the presence of monomers, (solvents) and ligands, the polymerization is catalyzed by a catalyst originating from a large amount of Cu(0) that continuously supplies Cu(0) as a catalyst.
[0070] All of the above methods are suitable for preparing polymer brushes on surfaces. These and other (not specifically mentioned herein) methods for forming polymer brushes on surfaces may be equally suitable for the purposes of the present invention.
[0071] Reaction conditions such as temperature, reaction time, washing, etc. are generally known to those skilled in the art. Likewise, depending on the polymer brush formation method, those skilled in the art will know how to select the polymerization medium, i.e., monomers, catalysts / ligands, solvents, etc., required to form the polymer brushes.
[0072] Typically, the polymerization medium to be used in the method of the present invention comprises a combination of solvent or solvent, monomer, part, catalyst and / or activator. In some cases, before the polymer gel and the polymerization medium swell, it may be advantageous to add an activator to the polymer gel. Therefore, when the polymer gel and the polymerization medium are combined, only the reactants of the polymerization medium are activated. In some cases, anti-caking agents such as sodium bicarbonate or silicon dioxide can be used to ensure uniform gelation of the polymerization medium. In some cases, surfactants such as anions, zwitterions or nonionic surfactants can be used to make the distribution of the polymerization medium and the polymer gel easy.
[0073] In the present invention, suitable solvents include alcohols, such as methanol, ethanol and isopropanol. Aprotic solvents such as dimethyl sulfoxide (DMSO), acetone, dimethylformamide, tetrahydrofuran, propylene carbonate, methylene carbonate, ethylene carbonate, ethyl lactate alcohol and ionic liquids (salts dissolved in liquids) can also be used in the method of the present invention. The alcohol and / or aprotic solvent are suitably mixed with water in a suitable ratio, for example water and alcohol are suitably mixed in a ratio of 5 vol%:95 vol%, 10 vol%:90 vol%, 15 vol%:85 vol%, 20 vol%:80 vol%, 25 vol%:75 vol%, 30 vol%:70 vol%, 35 vol%:65 vol%, 40 vol%:60 vol%, 45 vol%:55 vol%, 50 vol%:50 vol%, 55 vol%:45 vol%, 60 vol%:40 vol%, 65 vol%:35 vol%, 70 vol%:30 vol%, 75 vol%:25 vol%, 80 vol%:20 vol%, 85 vol%:15 vol%, 90 vol%:10 vol% or 5 vol%:95 vol% alcohol / aprotic solvent:water. In a preferred embodiment, the ratio is 50 vol%:50 vol% alcohol / aprotic solvent:water.
[0074] Examples of suitable monomers include, but are not limited to, acrylates, methacrylates, halogen-substituted olefins, acrylamides, methacrylamides and styrenes, and mixtures thereof. Specific acrylate monomers include, but are not limited to, methyl acrylate and ethyl acrylate, lauryl acrylate. Specific methacrylate monomers include, but are not limited to, methyl methacrylate (MMA), 2-hydroxyethyl methacrylate (HEMA), glycidyl methacrylate (GMA), ethyl methacrylate and butyl methacrylate, lauryl methacrylate. Specific halogen-substituted olefin monomers include, but are not limited to, vinyl chloride, vinylidene fluoride, tetrafluoroethylene, trifluorochloroethylene and hexafluoropropylene. Specific acrylamide monomers include, but are not limited to, acrylamide, N-isopropyl acrylamide, N-tert-butyl acrylamide and N-hydroxyethyl acrylamide. Specific methacrylamide monomers include, but are not limited to, N-isopropyl methacrylamide, methacrylamide, N-tert-butyl methacrylate and N-hydroxyethyl methacrylate. Specific styrene monomers include, but are not limited to, styrene, 4-methylstyrene, 2,3,4,5,6-pentafluorostyrene, p-divinylbenzene and 4-chlorostyrene.
[0075] Examples of suitable ligands include, but are not limited to, nitrogen-containing ligands such as N,N,N',N",N"'-pentamethyldiethylenetriamine (PMDETA), tris-[2-(dimethylamino)ethyl]amine (MeEtREN), tris(2-aminoethyl)amine (TREN), tris(2-pyridylmethyl)amine (TPMA) and 2,2'-bipyridine (bipy).
[0076] Examples of suitable catalysts include, but are not limited to, metal catalysts derived from copper (Cu), iron (Fe), and nickel (Ni). In particular, Cu may be suitable.
[0077] Examples of suitable activators include, but are not limited to, sodium ascorbate (NaAsc), ascorbic acid (Asc), hydrazine, hydrazine hydrate, sodium hypophosphite, a mixture of iron powder and sodium chloride, bicarbonate, citric acid and pyrogallic acid, and mixtures thereof. In particular, NaAsC, AsC and hydrazine are suitable for the purposes of the present invention.
[0078] In the method of the present invention, a polymer brush is formed on a surface, typically on the surface of a solid material. Such a surface may be suitably made of metal (e.g., aluminum, steel, titanium, nickel, gold, silver, platinum, chromium, copper, iron and alloys of various metals), glass, carbon, carbon fiber, graphene or graphite, ceramics, composite materials or plastics, rubber or other materials including outer coatings of these materials. The surface may be conductive or non-conductive. A polymerization initiator is fixed to the surface. Methods for fixing polymerization initiators are well known in the art. The polymerization initiator can be made to have a predetermined surface chemical property so that it can be fixed to the surface, which depends on the material from which the surface is made, but also on the characteristics of the polymer brush to be formed.
[0079] The concentration of each component (monomer, ligand, catalyst, activator) is generally 0.1nM-35M. Specific examples include, but are not limited to, 1nM, 5nM, 10nM, 50nM, 1M, 5M, 10M, 20M and 30M. It should be understood that the concentration of each component may be the same or may be different. In certain embodiments, the monomer concentration may be 0.01M to 5M. In certain embodiments, the concentration of the activator may be 0.010 to 0.045M. In certain embodiments, the concentration of the ligand is 0.05mM to 0.1M. In certain embodiments, the concentration of the solvent is 0.1 to 35M. In certain embodiments, the concentration of the catalyst is 1.0ppb to 500.0ppm.
[0080] In a preferred embodiment of the present invention, the polymer gel is a reversibly cross-linked polymer gel. Such a reversible polymer gel may suitably be mainly composed of a polymer having a certain cross-linking agent, which is introduced into the polymer side chains or added to the polymer gel solution as an additive (e.g., tannic acid). These cross-linking agents may suitably be metal coordinated and may be implemented using, for example, a pyrogallol (tannic acid) structure. The choice of metal coordination is important because undesirable coordination of metals to metal coordination sites may distort the polymerization reaction and thus distort the formation of polymer brushes. A suitable polymer gel is a polymer gel that swells in a polymerization medium.
[0081] In another embodiment of the present invention, the polymer gel is thixotropic. Xanthan gum is a suitable example of a thixotropic polymer gel.
[0082] In the method of the present invention, the polymer gel is swollen in a polymerization medium. After swelling, the final polymerization medium typically contains 0.1-20% by weight of polymer. The swollen gel is then applied to a surface on which a polymerization initiator is immobilized. The swollen gel can be appropriately brushed / painted, laid or poured on the surface. Then, polymerization and formation of the polymer brush are allowed to proceed.
[0083] The surface and the swollen gel (combined polymer gel and polymerization medium) are generally kept in contact with each other for a suitable period of time, such as 0.1 seconds to 5 hours. Suitable time periods include, but are not limited to, 1 second, 2 seconds, 30 seconds, 1 minute, 5 minutes, 30 minutes, 1 hour, 2 hours, 3 hours, 4 hours, and 5 hours. Polymer brush formation can be carried out at ambient temperature (room temperature) or under cooling or heating. Suitable reaction temperatures are -20°C to 120°C, such as room temperature (about 20°C) to 120°C. Specific temperatures include, but are not limited to -20°C, 0°C, room temperature (about 20°C), 30°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, and 120°C.
[0084] After the polymer brush is formed, the swollen gel is removed from the surface. This can be suitably done by optionally sonicating the surface in an acidic environment. An example of a pH responsive polymer gel is PAH / TA / Fe(III), which is in a liquid phase around pH 7 and below, and in a gel state above pH 7. Immersing the polymer gel in an acidic solution, such as HCl solution, changes the metal coordination and thereby the viscosity of the gel to produce a liquid. When the gel is in a liquid state, it can be easily removed from the polymer brush by, for example, sonication.
[0085] It has been shown that the use of polymer gels to form polymer brushes achieves a number of advantages. The polymer gel provides a stable environment for polymer brush formation because the polymer gel acts as a container for the polymerization medium, and therefore, the polymerization medium can diffuse freely within the polymer gel and promote polymer brush formation at the surface. In addition, the polymer gel provides a viscous environment, thereby enabling the formation of polymer brushes on surfaces with non-planar orientation (non-horizontally positioned) during polymer brush formation, or enabling the formation of polymer brushes on surfaces where specific polymer brush formation is desired. In addition, the use of polymer gels during polymer brush formation minimizes the supply of oxygen during polymer brush formation, thereby ensuring controlled polymerization. These advantages further enable large-scale production of polymer brush coated surfaces.
[0086] Therefore, the present invention also relates to the use of a polymer gel in forming a polymer brush for uniformly distributing the polymerisation medium over a surface on which a polymerisation initiator is immobilised. Above a polymer gel is described and how it can be used to form a polymer brush.
[0087] The use according to the invention involves the swelling of the polymer gel in a polymerization medium.
[0088] Polymer brushes are valuable in many applications, including the bonding of rubber, composites and plastics to metals and glass, and between each other for sealing applications, the bonding of functional thermoplastics to glass for sensor applications, and the effective bonding of polymer brush-coated composite fillers (such as carbon fibers, graphene, particles, etc.) into a matrix of polymers (such as thermoplastic materials) for creating functional surfaces on glass, metals, plastics, etc., such as antibacterial surfaces, low friction surfaces, or superhydrophobic self-cleaning surfaces.
[0089] The present invention is further illustrated by the following non-limiting examples.
[0090] Example
[0091] Example 1
[0092] Preparation of Catalyst / Me6TREN Solution for Polymerization Medium.
[0093] The catalyst / Me6TREN solution (polymerization medium without oxygen scavenger activator and monomer) was prepared as follows:
[0094] 250ml DI-water (deionized water) and 2.40ml N three [2- (dimethylamino) ethyl] amine (Me6TREN-acting as ligand) are mixed in a round-bottomed flask with a Teflon magnet wound with a Cu wire. The solution is stirred for 8 days, thereby Cu (0) is released into the solution. Cu (0) acts as a dormant / inactive catalyst, which can be activated after adding an activator. Ultraviolet visible (UV-Vis) spectroscopy is used to measure Cu (0)-catalyst concentration. The Cu catalyst / Me6TREN stock solution is diluted with water to obtain a catalyst concentration of 73mg / l, 93.8mg / l, 333mg / l or 427mg / l.
[0095] Example 2
[0096] Preparation of Catalyst / PMDETA Solution for Polymerization Medium.
[0097] Prepare the catalyst / PMDETA stock solution (polymerization medium without polymerization activator) as follows:
[0098] 2000 ml DI-water (deionized water) and 44 ml N,N,N',N",N"-pentamethyl-diethylenetriamine (PMDETA-acting as a ligand) were mixed in a conical flask. Using a peristaltic pump and a silicon tube, the solution was passed through a Cu tube (length 10 m, inner diameter 2.8 mm, outer diameter: 4 mm) at a flow rate of 10 ml / min. Thus, Cu(0) was released into the solution. Cu(0) acts as a dormant / inactive catalyst, which can be activated after the addition of an activator. The Cu(0)-catalyst concentration was determined using UV-visible spectroscopy. Thereafter, the Cu-catalyst / PMDETA stock solution was diluted with DI water to obtain a catalyst concentration of about 30 mg / l.
[0099] Example 3
[0100] Preparation of pH-responsive polymer gel: poly(2-hydroxyethyl methacrylate phosphate).
[0101] 2.27 g of 2-hydroxyethyl methacrylate phosphate (monomer) was combined with 8 ml of the catalyst / PMDETA stock solution from Example 2 and 10 μL of α-bromoethyl isobutyrate (initiator). The solution was purged with argon for 5 minutes. 32.7 mg of sodium ascorbate (NaAsc, activator) was added and the solution was purged for another 5 minutes. The reactants were allowed to react overnight. The polymer was separated by suction filtration and washed with water and then with ethanol. This cleaning process, for example, removes excess NaAsC. Unswollen polymer gels, poly (2-hydroxyethyl methacrylate phosphate) were thus obtained.
[0102] Example 4
[0103] The polymer brushes were formed using a polymer gel poly(2-hydroxyethyl methacrylate phosphate).
[0104] The polyacrylamide brushes were formed by swelling the poly(2-hydroxyethyl methacrylate phosphate) gel (prepared in Example 3) in the polymerization medium used to produce the polyacrylamide brushes and applying the resulting gel to a surface having a polymerization initiator immobilized thereon, see below.
[0105] First, a polymerization medium (without oxygen scavenger as activator) was prepared by mixing 4 ml DI-water, 50 μl Me6TREN / catalyst stock solution (prepared in Example 1) and 0.29 g acrylamide. Secondly, 195.5 mg of the poly (2-hydroxyethyl methacrylate phosphate) of Example 3 was dissolved in 1 ml of the polymerization medium by ultrasonic treatment for 5 minutes to swell the polymer gel in the polymerization medium. At this stage, the polymer gel solution combined with the polymerization medium is acidic and is therefore in its liquid form. In order to gel the polymer gel, the pH value of the solution was increased to a pH value of 7 or higher by adding a NaOH solution. It is noteworthy that the polymerization medium was activated simultaneously to enable polymer brush formation by adding an oxygen scavenger activator NaAsc (sodium ascorbate) combined with a NaOH solution. Therefore, 10.2 mg NaAsc was added to 1 ml 1M NaOH, and this solution was added to a solution of the polymer gel in the polymerization medium.
[0106] The polymer gel (mixed with the polymerization medium) started to gel within 3 minutes. A pea-sized piece of gel was placed on a 25×25 mm aluminum plate that had the polymerization initiator (3-(trimethoxysilyl)propyl 2-bromo-2-methylpropionate deposited on aluminum) immobilized on it. The swollen polymerization medium (combination of polymerization medium and polymer gel) was spread on the plate. This Figure 2 As shown in Figure 2 As can be seen, the adhesion of the swollen gel (swollen polymeric medium) to the plate is excellent and the gel remains in place even when tilted vertically as shown.
[0107] The polymer gel swollen in the polymerization medium was left at room temperature for 1 hour to produce polymer brushes on the surface. The polymer gel / polymerization medium was then removed by sonicating the plate in water for 10 minutes. The sonication caused the swollen polymer gel to "dissolve", i.e., become liquid (the swollen gel is reversible). The plate was then cleaned by sonicating in acetone for 10 minutes to remove any physically adsorbed material.
[0108] The formation of a uniform polymer brush coating was observed only in the areas where the polymer gel / polymerization medium was in contact with the surface (visually confirmed and Figure 3 The distinction between the two different regions was also confirmed by water contact angle measurements.
[0109] Example 5
[0110] The polymer gel poly(2-hydroxyethyl methacrylate phosphate) was used to form polymer brushes on a large stainless steel substrate.
[0111] This example is similar to the previous example 4 in that the polyacrylamide brushes were formed by swelling a poly(2-hydroxyethyl methacrylate phosphate) gel (polymer gel, prepared in example 3) in the polymerization medium used to produce the polyacrylamide brushes and applying the resulting gel to a surface having a polymerization initiator immobilized thereon, see below. However, in this example, the process was applied to a large stainless steel plate to demonstrate the scalability of the process.
[0112] First, a polymerization medium (without oxygen scavenger as activator) was prepared by mixing 4 ml DI-water, 50 μl Me6TREN / catalyst stock solution (prepared in Example 1) and 0.31 g acrylamide. Secondly, 603 mg of the poly (2-hydroxyethyl methacrylate phosphate) of Example 3 was dissolved in 2 ml of the polymerization medium by ultrasonic treatment for 5 minutes to swell the polymer gel in the polymerization medium. At this stage, the polymer gel solution combined with the polymerization medium is acidic and is therefore in its liquid form. In order to gel the polymer gel, the pH value of the solution is increased to a pH value of 7 or higher by adding a NaOH solution. It is noteworthy that the polymerization medium is activated simultaneously to enable polymer brush formation by adding an oxygen scavenger activator NaAsc combined with a NaOH solution. Therefore, 11.9 mg NaAsc is added to 2 ml 1 M NaOH, and this solution is added to a solution of the polymer gel in the polymerization medium.
[0113] The polymer gel (mixed with the polymerization medium) started to gel within 3 minutes. The gel was placed on a 100×100 mm stainless steel plate on which a polymerization initiator (2-bromo-2-methyl-propionic acid 3-(trimethoxysilyl)propyl ester deposited on stainless steel) was fixed. The polymer gel swollen in the polymerization medium was smeared on a portion of the plate. This is shown in Figure 4 middle.
[0114] The swollen polymeric medium / polymer gel was allowed to react at room temperature for 1 hour. The polymer gel / polymeric medium was then removed by sonicating the plate in water for 10 minutes. The sonication caused the swollen polymer gel to "dissolve", i.e., become liquid (the swollen gel is reversible). The plate was then cleaned by sonicating in acetone for 10 minutes to remove any physically adsorbed material.
[0115] The formation of a uniform polymer brush coating was seen only in the areas where the swollen polymeric medium was in contact with the surface. This was confirmed by applying water to the surface and observing that the surface was wetted only in the coated areas, as shown in Figure 5 The distinction between the two different regions was also confirmed by water contact angle measurements.
[0116] Example 6
[0117] The polymer gel PAH / TA / Fe(III) was used to form polymer brushes.
[0118] The poly(glycidyl methacrylate) brushes were formed by swelling a PAH / TA / Fe(III) polymer gel in the polymerization medium used to produce the poly(glycidyl methacrylate) brushes. The PAH was purchased (as opposed to the poly(2-hydroxyethyl methacrylate phosphate) used in Examples 3 and 4, which was synthesized).
[0119] First, the polymerization medium was prepared by mixing 172 μl DI-water, 172 μl EtOH, 100 μl PMDETA / catalyst stock solution (prepared in Example 2) and 52 μl glycidyl methacrylate. Secondly, the PAH / TA / Fe(III) polymer gel was prepared by mixing 0.5 ml of 40% PAH aqueous solution, 15.9 mg of tannic acid and 0.17 ml of 0.00865 M FeCl3 in DI aqueous solution. Thirdly, the polymerization medium and the polymer gel were combined to obtain a dark blue solution. At this stage, the polymer gel combined with the polymerization medium was acidic and therefore in its liquid form.
[0120] In order to gel the polymerization medium combined with the polymer gel (i.e. the swollen polymerization medium / polymer gel), the pH of the solution was increased to above pH 7 by adding a NaOH solution. The polymerization medium was simultaneously activated to enable polymer brush formation by adding an oxygen scavenger polymerization activator NaAsc combined with the NaOH solution. Thus, 5.5 mg of NaAsc was added to 0.33 ml of 1 M NaOH and this solution was added to the combined polymer gel and polymerization medium. When the polymer gel swelled in the polymerization medium, this produced a dark red dense solution, thereby forming a polymer gel containing the polymerization medium.
[0121] The swollen polymer gel / polymerization medium was placed on a 25×25 mm aluminum plate on which a polymerization initiator (3-(trimethoxysilyl)propyl 2-bromo-2-methylpropionate deposited on aluminum) was immobilized. Figure 6 middle.
[0122] After 1 hour of polymerization, the plate with the swollen polymer gel was immersed in 0.01 M HCl and sonicated for 10 minutes. The acidic pH is a stimulus to "dissolve" the swollen polymer gel, i.e. the medium becomes liquid (swelling is reversible). The plate was then sonicated for 10 minutes, first in water and then in acetone, to remove any physically adsorbed material.
[0123] The formation of a uniform polymer brush coating was seen only in the area where the polymerization medium and the polymer gel were in contact with the surface (confirmed by optical microscopy, Figure 7 The distinction between the two different regions was also confirmed by water contact angle measurements.
[0124] exist Figure 7 In the images, a clear boundary is seen between the polymer brush-coated areas, where the polymerization medium and polymer gel have come into contact with the surface, and the blank aluminum substrate, where only the initiator is immobilized.
[0125] Example 7
[0126] The polymer gel PAH / TA / Fe(III) was used to form polymer brushes in a denser form.
[0127] This example is similar to the aforementioned Example 6 in that the poly(glycidyl methacrylate) polymer brushes are formed by swelling the PAH / TA / F(III) polymer gel in the polymerization medium used to produce the poly(glycidyl methacrylate) polymer brushes. In this example, a denser swollen gel (polymer gel and polymerization medium) is obtained by adding less polymerization medium.
[0128] First, a polymerization medium was prepared by mixing 104 μl DI-water, 104 μl EtOH, 60 μl PMDETA / catalyst stock solution (prepared in Example 2) and 31 μl glycidyl methacrylate (still without oxygen scavenger as polymerization activator). Second, a PAH / TA / Fe(III) polymer gel was prepared by mixing 0.5 ml of a 40% PAH aqueous solution, 14.8 mg of tannic acid and 0.17 ml of a DI aqueous solution of 0.00865 M FeCl. Third, the polymerization medium and the polymer gel were combined to obtain a dark blue solution in which the polymer gel swelled in the polymerization medium. At this stage, the polymer gel combined with the polymerization medium was acidic and therefore in its liquid form.
[0129] To gel the mixture, the pH of the solution was increased to above pH 7 by adding NaOH solution. It is noteworthy that the polymerization medium was simultaneously activated to enable polymer brush formation by adding an oxygen scavenger activator NaAsc in combination with the NaOH solution. Thus, 4.3 mg of NaAsc was added to 0.33 ml of 1 M NaOH and the solution was added to the mixture of polymer gel and polymerization medium. This produced a dark red, dense solution of polymerization medium contained in the polymer gel.
[0130] The swollen gel (combination of polymer gel and polymerization medium) was placed on a 25×25 mm aluminum plate on which a polymerization initiator (3-(trimethoxysilyl)propyl 2-bromo-2-methylpropionate deposited on aluminum) was fixed. The medium was so dense that the sample could be placed vertically while the medium remained in place. This is shown in Figure 8 middle.
[0131] After 1 hour of polymerization, the plate with the swollen polymer gel / polymerization medium was immersed in 0.01 M HCl and sonicated for 10 minutes. The acidic pH is a stimulus to "dissolve" the gel medium, i.e., it becomes liquid. The plate was then sonicated for 10 minutes, first in water and then in acetone, to remove any physically adsorbed material.
[0132] The formation of a uniform polymer brush coating was seen only in the area where the swollen dense polymeric gel was in contact with the surface (confirmed by optical microscopy). The distinction between the two different areas was also confirmed by water contact angle measurements.
[0133] Furthermore, it can be concluded that even with very dense swollen gels of the polymerization medium and polymer gel, the components of the medium are indeed able to react with the polymerization initiator immobilized on the surface. Therefore, the key components for polymer brush formation are freely accessible for polymer brush formation.
[0134] Example 8
[0135] The polymer gel PAH / TA / Fe(III) was used to form polymer brushes in an even denser form.
[0136] This example is similar to Examples 6 and 7 in that the poly(glycidyl methacrylate) brushes are formed by swelling the PAH / TA / F(III) polymer gel in the polymerization medium used to produce the poly(glycidyl methacrylate) polymer brushes. However, in this example, an even denser swollen gel (polymer gel and polymerization medium) is obtained by adding even less polymerization medium.
[0137] First, the polymerization medium was prepared by mixing 35 μl DI-water, 35 μl EtOH, 20 μl PMDETA / catalyst stock solution (prepared in Example 2) and 10 μl glycidyl methacrylate (still without polymerization activator, however). Secondly, the PAH / TA / Fe(III) polymer gel was prepared by mixing 0.5 ml 40% PAH DI-water solution, 14.1 mg tannic acid and 0.17 ml 0.00865 M FeCl3 DI-water solution. Thirdly, the polymerization medium and the polymer gel were combined to obtain a dark blue solution. At this stage, the polymer gel combined with the polymerization medium was acidic and therefore in its liquid form.
[0138] To gel the polymer gel and polymerization medium, the pH of the solution was increased to above pH 7 by adding NaOH solution. Of note, the medium was simultaneously activated to enable polymer brush formation by adding an oxygen scavenger polymerization activator NaAsc in combination with the NaOH solution. Thus, 4.6 mg of NaAsc was added to 0.33 ml of 1 M NaOH and this solution was added to the combination of polymer gel and polymerization medium. This produced a dark red dense solution when a semi-solid form of the swollen polymer gel was formed.
[0139] The swollen polymerization medium / polymer gel was placed on a 25×25 mm aluminum plate on which the polymerization initiator (3-(trimethoxysilyl)propyl 2-bromo-2-methylpropionate deposited on aluminum) was immobilized. The medium was so dense that the sample could be placed vertically while the medium remained in place. This is shown in Fig. 9 middle.
[0140] After 1 hour of polymerization, the plate was immersed in 0.01 M HCl and sonicated for 10 minutes. The acidic pH is a stimulus to "dissolve" the swollen polymerization medium / polymer gel, i.e. it becomes liquid. The plate was then sonicated for 10 minutes, first in water and then in acetone, to remove any physically adsorbed material.
[0141] The formation of a uniform polymer brush coating was seen only in the area where the gelled polymer gel (polymerization medium and polymer gel) was in contact with the surface (confirmed by optical microscopy). The distinction between the two different areas was also confirmed by water contact angle measurements.
[0142] Furthermore, it can be concluded that even with the denser swollen gel, the components of the medium are indeed able to react with the polymerization initiator immobilized on the surface. Therefore, the key components for polymer brush formation are freely accessible for polymer brush formation.
[0143] Example 9
[0144] Preparation of Sodium Alginate Polymer Gel
[0145] Various polymer gels of sodium alginate were prepared by mixing 4g, 5g, 6g and 8g of sodium alginate in 100mL DI-water, respectively, to form 4w% / v%, 5w% / v%, 6w% / v% and 8w% / v% sodium alginate polymer gels, respectively. The resulting polymer gels were viscous liquids in all cases.
[0146] Example 10
[0147] Polymer brushes were formed using sodium alginate polymer gel in a 14% ethanol solvent system.
[0148] First, a polymer gel was prepared by dissolving 150.1 mg of sodium ascorbate (NaAsc, activator) in 17 ml of a sodium alginate solution (4 w% / v%) prepared according to Example 9. The mixture became a light brown viscous liquid. The polymer gel with the activator was stored in a container.
[0149] In another container, 1.6 ml of methyl methacrylate (MMA) was mixed with 7.1 ml of Cu-catalyst / Me6TREN solution ([Cu]=93.8 mg / l) and 4.3 ml of ethanol to form a polymerization medium.
[0150] The polymerization medium was poured into the sodium alginate polymer gel under stirring. After mixing, the solution turned light blue, and after about 5 minutes, the mixture turned white. Thus, the polymer gel swelled in the polymerization medium.
[0151] The obtained polymer gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized. The polymer gel swollen in the polymerization medium was very dense and covered the plate evenly and well. The plate was left for 10 minutes, allowing a polymer brush to form on the plate. The plate was then placed in a beaker with DI-water. The change in the polarity of the solvent was the stimulus to "dissolve" the swollen polymer gel / polymerization medium and remove it from the plate. It was also rinsed by sonication in water for 5 minutes and then further rinsed by sonication in acetone for 5 minutes.
[0152] The formed polymer brushes had a thickness of 57±7 nm as determined by ellipsometry.The polymer structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0153] exist Fig.10 In FIG. 5 , a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right) are shown. Fig.11 The IRRAS spectra after the formation of the polymer brush are shown in Figure 2. Importantly, the peaks at 2974, 1739, 1273, 1244, 1195, and 1153 cm -1 The peaks at and respectively confirm the presence of sp3 hybridized carbon-hydrogen bonds, carbonyl groups, and carbon-oxygen bonds, which are consistent with what is expected for PMMA polymer brushes.
[0154] Embodiment 11
[0155] Polymer brushes were formed using sodium alginate polymer gel in a 63% ethanol solvent system.
[0156] The procedure was carried out as described in Example 10 using 150 mg sodium ascorbate (activator) and 17 ml sodium alginate solution (4 w% / v%) prepared according to Example 9. The mixture turned into a light brown thick liquid. The polymer gel with the activator was kept in a container.
[0157] In another container, 1.6 ml of methyl methacrylate (MMA) was mixed with 2 ml of Cu-catalyst / Me6TREN solution ([Cu]=333 mg / l) and 9.4 ml of ethanol to form a polymerization medium.
[0158] The polymerization medium was poured into the sodium alginate polymer gel under stirring. After mixing, the solution turned light blue, and after about 5 minutes, the mixture turned light yellow. Thus, the polymer gel swelled in the polymerization medium.
[0159] The obtained polymer gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized. The polymer gel swollen in the polymerization medium was very dense and covered the plate evenly and well. The plate was left for 10 minutes, allowing a polymer brush to form on the plate. The plate was then placed in a beaker with DI water. The change in the polarity of the solvent was the stimulus to "dissolve" the swollen polymer gel and remove it from the plate. It was also rinsed by sonication in water for 5 minutes and then further rinsed by sonication in acetone for 5 minutes.
[0160] The formed polymer brushes had a thickness of 78±7 nm as determined by ellipsometry.The polymer structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0161] exist Fig.12 In FIG. 5 , a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right) are shown. Fig.13 The IRRAS spectra after the formation of the polymer brush are shown in Figure 2. Importantly, the peaks at 2974, 1741, 1271, 1243, 1197, and 1154 cm -1 The peaks at and respectively confirm the presence of sp3 hybridized carbon-hydrogen bonds, carbonyl groups, and carbon-oxygen bonds, which are consistent with what is expected for PMMA polymer brushes.
[0162] Example 12
[0163] Polymer brushes were formed using sodium alginate polymer gel and an aprotic solvent in the polymerization medium.
[0164] The procedure was carried out as in Example 10 using 150.3 mg of sodium ascorbate (activator) dissolved in 17 ml of sodium alginate polymer gel (5 w% / v%). The mixture was stirred to produce a light brown thick liquid.
[0165] The polymerization medium was a mixture of 1.6 ml of methyl methacrylate (MMA) mixed with 1.5 ml of Cu-catalyst / Me6TREN solution ([Cu]=427 mg / l), 0.5 ml of DI-water and 9.4 ml of DMSO solvent.
[0166] Pour the polymerization medium into the polymer gel / activator liquid and stir. After mixing, the combined solution turns light blue and after about 5 minutes, the combined solution is thick and clear.
[0167] The obtained polymer gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized and left for 10 minutes to transform the polymer brush. The plate was rinsed as described in Example 10.
[0168] The formed polymer brushes had a thickness of 64±32 nm as determined by ellipsometry.The polymer structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0169] exist Fig.14 In FIG. 5 , a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right) are shown. Fig.15 The IRRAS spectra after the formation of the polymer brush are shown in Figure 2. Importantly, the peaks at 2967, 1741, 1273, 1243, 1197, and 1154 cm -1 The peaks at and respectively confirm the presence of sp3 hybridized carbon-hydrogen bonds, carbonyl groups, and carbon-oxygen bonds, which are consistent with what is expected for PMMA polymer brushes.
[0170] Embodiment 13
[0171] The polymer brushes were formed using 5 w% / v% sodium alginate polymer gel in ethanol solvent.
[0172] The procedure was carried out as in Example 10 using 150 mg of sodium ascorbate (activator) dissolved in 17 ml of sodium alginate polymer gel (5 w% / v%). The mixture was stirred to produce a light brown thick liquid.
[0173] The polymerization medium was a mixture of 1.6 ml of methyl methacrylate (MMA) mixed with 1.5 ml of Cu-catalyst / Me6TREN solution ([Cu]=427 mg / l), 0.5 ml of DI-water and 9.4 ml of ethanol solvent.
[0174] The polymerization medium was poured into the polymer gel / activator liquid and stirred. After mixing, the combined solution turned light blue, and after about 5 minutes, the combined solution turned into a bright white dense gel. The polymer gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed and left for 10 minutes to convert the polymer brush. The plate was rinsed as described in Example 10.
[0175] The formed polymer brushes had a thickness of 64±6 nm as determined by ellipsometry.The polymer structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0176] exist Fig.16 In FIG. 5 , a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right) are shown. Fig.17 The IRRAS spectra after the formation of the polymer brush are shown in Figure 2. Importantly, the peaks at 2974, 1739, 1273, 1243, 1197, and 1154 cm -1 The peaks at and respectively confirm the presence of sp3 hybridized carbon-hydrogen bonds, carbonyl groups, and carbon-oxygen bonds, which are consistent with what is expected for PMMA polymer brushes.
[0177] Embodiment 14
[0178] Polymer brushes were formed using 6 w% / v% sodium alginate polymer gel in ethanol solvent.
[0179] The procedure was carried out as in Example 10 using 150 mg of sodium ascorbate (activator) dissolved in 17 ml of sodium alginate polymer gel (6 w% / v%). The mixture was stirred to produce a light brown thick liquid.
[0180] The polymerization medium was a mixture of 1.6 ml of methyl methacrylate (MMA) mixed with 1.5 ml of Cu-catalyst / Me6TREN solution ([Cu]=427 mg / l), 0.5 ml of DI-water and 9.4 ml of ethanol solvent.
[0181] The polymerization medium was poured into the polymer gel / activator liquid and stirred. After mixing, the combined solution turned light blue and after about 5 minutes, the combined solution turned into a bright white dense gel. The obtained polymer gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was fixed and left for 10 minutes to form a polymer brush. The plate was rinsed as described in Example 10.
[0182] The formed polymer brushes had a thickness of 56±10 nm as determined by ellipsometry.The polymer structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0183] exist Fig.18 In FIG. 5 , a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right) are shown. Fig.19 The IRRAS spectra after the formation of the polymer brush are shown in Figure 2. Importantly, the peaks at 2974, 1739, 1273, 1243, 1197, and 1154 cm -1 The peaks at and respectively confirm the presence of sp3 hybridized carbon-hydrogen bonds, carbonyl groups, and carbon-oxygen bonds, which are consistent with what is expected for PMMA brushes.
[0184] Embodiment 15
[0185] The polymer brushes were formed using 8 w% / v% sodium alginate polymer gel in ethanol solvent.
[0186] The procedure was carried out as in Example 10 using 150 mg of sodium ascorbate (activator) dissolved in 17 ml of sodium alginate polymer gel (8 w% / v%). The mixture was stirred to produce a light brown thick liquid.
[0187] The polymerization medium was a mixture of 1.6 ml of methyl methacrylate (MMA) mixed with 1.5 ml of Cu-catalyst / Me6TREN solution ([Cu]=427 mg / l), 0.5 ml of DI-water and 9.4 ml of ethanol solvent.
[0188] Pour the polymerization medium into the polymer gel / activator liquid and stir. After mixing, the combined solution turns light blue and after about 5 minutes, the combined solution is a white dense gel.
[0189] The polymer gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized and left for 10 minutes to form a polymer brush. The plate was rinsed as described in Example 10.
[0190] The formed polymer brushes had a thickness of 37±10 nm as determined by ellipsometry.The polymer structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0191] exist Fig. 20 , a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right) are shown.
[0192] Example 16
[0193] Sodium alginate polymer gel was used to form poly(styrene) polymer brushes.
[0194] The procedure was carried out as in Example 10 using 150.2 mg of sodium ascorbate (activator) dissolved in 17 ml of sodium alginate polymer gel (5 w% / v%). The mixture was stirred to produce a light brown thick liquid.
[0195] The polymerization medium is a mixture of 1.6 ml of styrene (monomer) mixed with 1.5 ml of Cu-catalyst / Me6TREN solution ([Cu]=427 mg / l), 0.5 ml of DI-water and 9.4 ml of ethanol solvent. The polymerization medium is poured into the polymer gel / activator liquid and stirred. After mixing, the combined solution becomes light blue, and after about 5 minutes, the combined solution is a white dense gel.
[0196] The polymer gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized and left for 10 minutes to form a polymer brush. The plate was rinsed as described in Example 10.
[0197] The formed polymer brushes had a thickness of 10 ± 2 nm as determined by ellipsometry. Water contact angle measurements after polymerization gave a water contact angle of 84°, confirming that the surface of the plate with the polymer brushes was hydrophobic, consistent with PS.
[0198] exist Fig.21 In FIG. 5 , a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right) are shown. Fig. 22 , the water contact angles of the plate and the water drop are shown.
[0199] Embodiment 17
[0200] Sodium alginate polymer gel was used to form PHEMA polymer brushes.
[0201] The procedure was carried out as in Example 10 using 150.2 mg of sodium ascorbate (activator) dissolved in 17 ml of sodium alginate polymer gel (5 w% / v%). The mixture was stirred to produce a light brown thick liquid.
[0202] The polymerization medium is a mixture of 1.6 ml of 2-(hydroxyethyl) methacrylate (HEMA) (monomer) mixed with 1.5 ml of Cu-catalyst / Me6TREN solution ([Cu]=427 mg / l), 0.5 ml of DI-water and 9.4 ml of ethanol solvent. The polymerization medium is poured into the polymer gel / activator liquid and stirred. After mixing, the combined solution becomes light blue, and after about 5 minutes, the combined solution becomes a white dense gel.
[0203] The polymer gel swollen in the polymerization medium was transferred to a 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized and left for 10 minutes to form a polymer brush. The plate was rinsed as described in Example 10.
[0204] The polymer brushes formed had a thickness of 5 ± 7 nm as determined by ellipsometry.Water contact angle measurements after polymerization gave a water contact angle of 29°, confirming that the surface of the plate with the polymer brushes was hydrophobic, consistent with PHEMA.
[0205] exist Fig.23 In FIG. 5 , a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right) are shown. Fig.24 , the water contact angles of the plate and the water drop are shown.
[0206] Embodiment 18
[0207] Sodium alginate polymer gel was used to form PGMA polymer brushes.
[0208] 18 mg of sodium ascorbate (activator) was dissolved in 2 ml of sodium alginate polymer gel (4 w% / v%). The mixture was stirred.
[0209] The polymerization medium is a mixture of 104 μl glycidyl methacrylate (GMA) (monomer) and 135 μl Cu-catalyst / Me6TREN solution ([Cu]=427 mg / l) and 624 μl ethanol solvent. 1136 μl of the polymer gel / sodium ascorbate solution merged is transferred to the polymerization solution and stirred. After mixing, the merged solution becomes light blue, and after about 5 minutes, the merged solution is a white dense gel.
[0210] The polymer gel swollen in the polymerization medium was transferred to a 25×25 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized and left for 30 minutes to form a polymer brush. The plate was rinsed as described in Example 10.
[0211] The formed polymer brushes had a thickness of 99±17 nm as determined by ellipsometry.The polymer structure of the formed polymer brushes was further confirmed by infrared reflection absorption spectroscopy (IRRAS).
[0212] exist Fig.25 In FIG. 5 , a polymer gel swollen in a polymerization medium (left) and a swollen polymer gel transferred to a plate (right) are shown. Fig.26 The IRRAS spectra after the formation of the polymer brush are shown in Figure 2. Importantly, the 2974, 1737, 1269, 1243, 1173, and 1152 cm -1 The peaks at 908 cm- 1 Glycidyl epoxy groups were observed at 1400 nm and 1400 nm, respectively. All these peaks were consistent with those expected for PGMA polymer brushes.
[0213] Embodiment 19
[0214] Preparation of xanthan gum polymer gel.
[0215] Various polymer gels of xanthan gum were prepared by mixing 2g, 3g, 4g, 4.5g and 6g of xanthan gum in 100mL DI-water, respectively, to form 2w% / v%, 3w% / v%, 4w% / v%, 4.5w% / v% and 6w% / v% xanthan gum polymer gels, respectively. The resulting polymer gels were viscous liquids in all cases.
[0216] Embodiment 20
[0217] 2 w% / v% xanthan gum was used to form PMMA polymer brushes.
[0218] 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum polymer gel (2 w% / v%) and stirred to obtain a light brown dense liquid.
[0219] In another container, 1.6 ml of methyl methacrylate (MMA monomer) was mixed with 1.5 ml of Cu-catalyst / Me6TREN-stock solution ([Cu]=427 mg / l), 0.5 ml of water and 9.4 ml of ethanol (polymerization medium), and poured into the xanthan gum solution under stirring. After mixing, the solution (polymer gel swollen in the polymerization medium) became a transparent gel.
[0220] The formed polymer gel was transferred to a sample plate 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker with DI-water. The change in the polarity of the solvent was a stimulus to "dissolve" the swollen polymer gel and remove it from the plate. It was also rinsed by sonication in water for 5 minutes and then further rinsed by sonication in acetone for 5 minutes.
[0221] The formed polymer brushes had a thickness of 64 ± 6 nm as determined by ellipsometry.
[0222] Embodiment 21
[0223] Xanthan gum (3 w% / v%) was used to form PMMA polymer brushes.
[0224] 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum solution (3 w% / v%) and stirred to obtain a light brown dense liquid.
[0225] In another container, 1.6 ml of methyl methacrylate (MMA monomer) was mixed with 1.5 ml of Cu catalyst / Me6TREN-stock solution ([Cu]=427 mg / l), 0.5 ml of water and 9.4 ml of ethanol (polymerization medium), and poured into the xanthan gum polymer gel under stirring. After mixing, the solution (polymer gel swollen in the polymerization medium) became a transparent gel.
[0226] The formed gel was transferred to a sample plate 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker with DI water. The change in solvent polarity was a stimulus to "dissolve" the swollen polymer gel and remove it from the plate. It was also rinsed by sonication in water for 5 minutes and then further rinsed by sonication in acetone for 5 minutes.
[0227] The formed polymer brushes had a thickness of 54 ± 10 nm as determined by ellipsometry. The chemical composition of the PMMA polymer brushes was confirmed by XPS ( Fig. 27 ). Importantly, the peaks at 535 eV and 287 eV confirm the presence of oxygen and carbon, respectively. The atomic percentages of 24.3% for oxygen and 75.7% for carbon are consistent with the theoretical values for PMMA polymer. Fig.28 , a high-resolution spectrum of the carbon peaks is shown, verifying the chemical structure of the PMMA polymer brushes.
[0228] Embodiment 22
[0229] Xanthan gum polymer gel (4 w% / v%) was used to form PMMA polymer brushes.
[0230] 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum polymer gel (4 w% / v%) and stirred to obtain a light brown dense liquid.
[0231] In another container, 1.6 ml of methyl methacrylate (MMA monomer) was mixed with 1.5 ml of Cu-catalyst / Me6TREN-stock solution ([Cu]=427 mg / l), 0.5 ml of water and 9.4 ml of ethanol (polymerization medium), and poured into the xanthan gum solution under stirring. After mixing, the solution (polymer gel swollen in the polymerization medium) became a transparent gel.
[0232] The formed gel was transferred to a sample plate 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker with DI-water. The change in the polarity of the solvent was a stimulus to "dissolve" the swollen polymer gel and remove it from the plate. It was also rinsed by sonication in water for 5 minutes and then further rinsed by sonication in acetone for 5 minutes.
[0233] The formed polymer brushes had a thickness of 63 ± 21 nm as determined by ellipsometry.
[0234] Embodiment 23
[0235] Xanthan gum polymer gel (4.5 w% / v%) was used to form PMMA polymer brushes.
[0236] 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum polymer gel (4.5 w% / v%) and stirred to obtain a light brown dense liquid.
[0237] In another container, 1.6ml methyl methacrylate (MMA monomer) is mixed with 1.5mL Cu-catalyst / Me6TREN-stock solution ([Cu]=427mg / l), 0.5ml water and 9.4ml ethanol (polymerization medium), and poured into the xanthan gum polymer gel under stirring. After mixing, the solution becomes a transparent gel.
[0238] The formed polymer gel was transferred to a sample plate 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker with DI-water. The change in the polarity of the solvent was a stimulus to "dissolve" the swollen polymer gel and remove it from the plate. It was also rinsed by sonication in water for 5 minutes, and then further rinsed by sonication in acetone for 5 minutes.
[0239] The PMMA polymer brushes formed had a thickness of 7 ± 2 nm as determined by ellipsometry.
[0240] Embodiment 24
[0241] Xanthan gum polymer gel (6 w% / v%) was used to form PMMA polymer brushes.
[0242] 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum polymer gel (6 w% / v%) and stirred to obtain a light brown dense liquid.
[0243] In another container, 1.6 ml of methyl methacrylate (MMA monomer) was mixed with 1.5 ml of Cu-catalyst / Me6TREN-stock solution ([Cu]=427 mg / l), 0.5 ml of water and 9.4 ml of ethanol (polymerization medium), and poured into the xanthan gum polymer gel under stirring. After mixing, the solution (polymer gel swollen in the polymerization medium) became a transparent gel.
[0244] The formed gel was transferred to a sample plate 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker with DI-water. The change in the polarity of the solvent was a stimulus to "dissolve" the swollen polymer gel and remove it from the plate. It was also rinsed by sonication in water for 5 minutes, and then further rinsed by sonication in acetone for 5 minutes.
[0245] The PMMA polymer brushes formed had a thickness of 50 ± 34 nm as determined by ellipsometry.
[0246] Embodiment 25
[0247] Xanthan gum polymer gel (4 w% / v%) was used to form poly(styrene) polymer brushes.
[0248] 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum polymer gel (4 w% / v%) and stirred to obtain a light brown dense liquid.
[0249] In another container, 1.6 ml of styrene (monomer) was mixed with 1.5 ml of Cu catalyst / Me6TREN-stock solution ([Cu]=427 mg / l), 0.5 ml of water and 9.4 ml of ethanol (polymerization medium), and poured into the xanthan gum polymer gel under stirring. After mixing, the solution became a transparent gel.
[0250] The formed polymer gel was transferred to a sample plate 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker with DI-water. The change in the polarity of the solvent was a stimulus to "dissolve" the swollen polymer gel and remove it from the plate. It was also rinsed by sonication in water for 5 minutes, and then further rinsed by sonication in acetone for 5 minutes.
[0251] exist Fig.29 , XPS inspection analysis is shown. No peaks from the sample substrate were observed, inferring that a polymer brush thickness of more than 10 nm was achieved (10 nm is the detection limit of XPS). The chemical composition of the poly(styrene) polymer brush was confirmed by XPS ( Fig.31 ). Importantly, the peaks at 535 eV and 287 eV confirm the presence of oxygen and carbon, respectively. The 93.5% atomic percentage of carbon is consistent with PS (pure carbon-based polymer) and only minor oxygen contamination (6.5%). Fig.30 , a high-resolution spectrum of the carbon peaks is shown, verifying the chemical structure of the poly(styrene) polymer brushes.
[0252] Embodiment 26
[0253] Xanthan gum polymer gel (4 w% / v%) was used to form 2-hydroxyethyl methacrylate polymer brushes.
[0254] 150 mg of sodium ascorbate was dissolved in 17 ml of xanthan gum polymer gel (4 w% / v%) and stirred to obtain a light brown dense liquid.
[0255] In another container, 1.6 ml of 2-hydroxyethyl methacrylate (HEMA monomer) was mixed with 1.5 ml of Cu catalyst / Me6TREN-stock solution ([Cu]=427 mg / l), 0.5 ml of water and 9.4 ml of ethanol (polymerization medium), and poured into the xanthan gum polymer gel under stirring. After mixing, the solution (polymer gel swollen in the polymerization medium) became a transparent gel.
[0256] The formed gel was transferred to a sample plate 10×10 mm stainless steel plate (304 steel alloy) on which a polymerization initiator (4-(chloromethyl)phenyltrimethoxysilane deposited on stainless steel) was immobilized, and polymerization was carried out for 10 minutes. The plate was then placed in a beaker with DI-water. The change in the polarity of the solvent was a stimulus to "dissolve" the swollen polymer gel and remove it from the plate. It was also rinsed by sonication in water for 5 minutes and then further rinsed by sonication in acetone for 5 minutes.
[0257] exist Fig.31 , XPS analysis is shown. No peaks from the sample substrate were observed, inferring that a polymer brush thickness of more than 10 nm was achieved (10 nm is the detection limit of XPS). The chemical composition of the PHEMA polymer brush was confirmed by XPS ( Fig.31 ). Importantly, the peaks at 535 eV and 287 eV confirm the presence of oxygen and carbon, respectively. The atomic percentages of 69.0% for oxygen and 31.0% for carbon are consistent with the theoretical values. Fig.32 , a high-resolution spectrum of the carbon peaks is shown, verifying the chemical structure of the PHEMA polymer brushes.
Claims
1. A method for forming a polymer brush on a surface, wherein the surface having a polymerization initiator immobilized thereon is brought into contact with a polymerization medium, characterized in that A swellable and removable polymer gel is used during formation of the polymer brush, wherein the polymer gel is swellable in the polymerization medium, and wherein the polymer gel is removable after forming the polymer brush on the surface.
2. The method according to claim 1, characterized in that The polymer gel is swellable in water, in a mixture of water and an alcohol, in a mixture of water and an aprotic solvent, or in an aprotic solvent.
3. The method according to claim 1 or 2, characterized in that: The cross-linking of the polymer gel is reversible.
4. The method according to claim 1 or 2, characterized in that: The polymer gel has hydrogen bond acceptors and / or donors to facilitate cross-linking.
5. The method according to claim 1 or 2, characterized in that The polymer gel is a hydrogel.
6. The method according to claim 5, characterized in that The polymer gel is selected from the group consisting of polyallylamine, poly(2-hydroxyethyl methacrylate phosphate), polyvinyl imidazole, polyacrylic acid, PEG, collagen, gelatin, agarose, cyclodextrin, sodium alginate and xanthan gum.
7. The method according to claim 5, characterized in that The polymer gel is selected from chitosan and a combination of β-CD polymer and PEG-cholesterol polymer.
8. The method according to claim 5, characterized in that The polymer gel is selected from polysaccharides.
9. The method according to claim 5, characterized in that The polymer gel is selected from alginate.
10. The method according to claim 5, characterized in that The polymer gel is a cysteine-based polymer gel.
11. The method according to claim 1 or 2, characterized in that: The polymer gel swells to form a semisolid, and the polymer gel is removed by an external stimulus.
12. The method according to claim 1 or 2, characterized in that: The polymer gel is removed by adjusting the pH or temperature, by exposure to light, by sonication or by changing the polarity of the solvent, or by oxidation.
13. The method according to claim 1 or 2, characterized in that: The polymer gel is polyallylamine / tannic acid / Fe(III), chitosan / tannic acid / Fe(III), collagen / tannic acid / Fe(III), polyvinyl imidazole, poly(methacrylate-2-hydroxyethyl phosphate), or sugar.
14. The method according to claim 1 or 2, characterized in that: The polymer gel is sodium alginate, xanthan gum or cyclodextrin.
15. The method according to claim 1 or 2, characterized in that: The polymer gel has metal chelating sites.
16. The method according to claim 15, characterized in that The metal chelating sites coordinate to Cu(II), Fe(III) or Al(III).
17. The method according to claim 1 or 2, characterized in that: The polymer gel swollen in the polymerization medium is applied to the surface.
18. Use of a swellable and removable polymer gel in forming a polymer brush for uniformly distributing a polymerizing medium over a surface on which a polymerization initiator is immobilized, wherein: The polymer gel is swollen in the polymerization medium, and wherein the polymer gel is removable after forming the polymer brush on the surface.
19. The use according to claim 18, characterized in that The polymer gel is selected from the group consisting of polyallylamine, poly(2-hydroxyethyl methacrylate phosphate), polyvinyl imidazole, polyacrylic acid, PEG, collagen, gelatin, agarose, cyclodextrin, sodium alginate and xanthan gum.
20. The use according to claim 18, characterized in that The polymer gel is selected from chitosan and a combination of β-CD polymer and PEG-cholesterol polymer.
21. The use according to claim 18, characterized in that The polymer gel is selected from polysaccharides.
22. The use according to claim 18, characterized in that The polymer gel is selected from alginate.
23. The use according to claim 18, characterized in that The polymer gel is a cysteine-based polymer gel.
24. The use according to claim 18, characterized in that The polymer gel is polyallylamine / tannic acid / Fe(III), chitosan / tannic acid / Fe(III), collagen / tannic acid / Fe(III), polyvinyl imidazole, poly(methacrylate-2-hydroxyethyl phosphate), or sugar.
25. The use according to claim 18, characterized in that The polymer gel is sodium alginate, xanthan gum or cyclodextrin.