Multi-layer single-face plain fabric with three-dimensional effect and production method thereof

Through specific weaving and dyeing and finishing processes, combined with the new three-hole yarn design and two-bath dyeing, the problem of insufficient pattern retention and skin-friendliness of existing cotton cotton three-layer structural fabrics is solved, and a three-dimensional effect is prepared The multi-layer single-sided plain fabric achieves the improvement of the fabric's shape retention, skin-friendliness and smoothness.

CN114645370BActive Publication Date: 2024-11-22DONGGUAN TEXWINCA HLDG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210153274.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-18
Publication Date
2024-11-22
Estimated Expiration
2042-02-18

AI Technical Summary

Technical Problem

The existing cotton cotton fabrics have weak shape protection and poor skin-friendliness in T-shirt clothing, and the hygroscopicity, breathability and heat resistance of spandex fabrics have poor hygroscopicity, breathability and heat resistance, which have certain defects.

Method used

Using specific weaving and dyeing and finishing processing technology, through the new three-hole yarn design and yarn angle adjustment, combined with two-bath dyeing and polishing treatment, a multi-layer single-sided plain fabric with three-dimensional effect is prepared to improve the fabric. stylistically retention, skin-friendly and smooth.

Benefits of technology

It achieves good pattern retention, good skin-friendliness and high flatness, solves the problem of fabric prone to crease in dyeing, improves dyeing rate and color fastness, and is suitable for industrial implementation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114645370B_ABST
    Figure CN114645370B_ABST
Patent Text Reader

Abstract

The present invention specifically relates to a multi-layer single-sided plain fabric with a three-dimensional effect and a production method thereof, the production method comprising selecting yarns and weaving them according to a certain structure to form a grey cloth, pre-shaping and singeing the grey cloth, then scalding, bleaching, dyeing and fixing, and then softening and finalizing the finished product to obtain the fabric. Among them, the angle of the inlay yarn is adjusted by the structural design of a three-hole yarn nozzle to weave a three-layer single-sided plain fabric with a strong three-dimensional effect. The fabric has good shape retention, is skin-friendly and soft, and has high flatness. At the same time, by adjusting the dyeing and finishing process, the problem that such fabrics are prone to creases during dyeing is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of knitted fabrics, and in particular to a multi-layer single-face plain fabric with a three-dimensional effect and a production method thereof. Background Art

[0002] Plain fabric is one of the most common types of knitted fabrics, mainly used in T-shirts. At present, fashion brands are becoming more and more popular among young people, and most of the T-shirts are double-layered structures of cotton and cotton. The fabrics of this type of structure are crisp and stylish, but due to the small changes in the structure, the woven fabrics have weak shape retention and poor skin-friendliness. Therefore, the three-layer structure of cotton and cotton and cotton was developed, and it can well solve the above-mentioned defects of the double-layer structure. Cotton and silk spandex are usually used on the market to present a three-layer effect. In the weaving process, cotton and silk spandex plain fabrics only need two cotton yarn nozzles and two conveyor discs when supplying yarn. In addition, the spandex bypasses the cotton yarn nozzle from the special yarn guide wheel and is fed through the semi-active roller yarn feeder. In addition, the spandex itself has the shrinkage characteristics and is located between the veil and the bottom yarn, thus presenting a three-layer effect. However, the hygroscopicity, air permeability and heat resistance of spandex fabrics are relatively poor, and there are certain defects when used for T-shirts. Therefore, the present invention obtains a three-layer single-sided plain fabric of cotton-cotton-cotton through a specific weaving process and dyeing and finishing process, which has good market prospects and application value. Summary of the invention

[0003] The purpose of the present invention is to solve the deficiencies of the above-mentioned prior art and to provide a multi-layer single-sided plain fabric with a three-dimensional effect and a production method thereof. The production method has a short process, low energy consumption and is suitable for industrial implementation. The prepared fabric has good shape retention, is skin-friendly and comfortable, and has high flatness.

[0004] The purpose of the present invention is achieved through the following technical solutions:

[0005] A method for producing a multi-layer single-sided plain fabric with a three-dimensional effect comprises the following steps:

[0006] S1: Select raw yarn and weave the yarn into single-sided plain grey fabric using a single-sided knitting machine;

[0007] S2: using a pre-forming machine to pre-form the grey cloth obtained in step S1;

[0008] S3: singeing the grey cloth after the treatment in step S2 by using a singeing machine;

[0009] S4: placing the embryonic fabric processed in step S3 in an open-width scouring and bleaching machine for scouring and bleaching, and transferring the scouring and bleaching embryonic fabric to a dyeing vat for dyeing and color fixing treatment;

[0010] S5: softening the fabric after dyeing in step S4, and then drying the softened fabric;

[0011] S6: shaping the fabric obtained in step S5 into a finished product, so as to obtain the single-sided plain fabric.

[0012] Preferably, the single-sided plain fabric consists of a surface layer, a middle layer and a bottom layer, the surface layer is woven by the first yarn using two AB needle stitches, and both are loop-forming units, the middle layer is woven by the second yarn using two AB needle stitches, and both are loop-forming units, the bottom layer is woven by the third yarn using two AB needle stitches, and both are loop-forming units, wherein the first yarn, the second yarn and the third yarn are fed into the warp nozzle simultaneously for weaving.

[0013] Preferably, the first yarn and the third yarn are both cotton yarn or cotton-polyester blended yarn, and the second yarn is any one of polyester filament, cotton yarn or cotton-polyester blended yarn.

[0014] Preferably, in the above step S1, a Japanese Fuyuan high-speed single-sided knitting machine is used, the model is VXC-S3.2RE, and the machine speed of the knitting machine is 25 rpm. In order to realize the yarn feeding function of the surface layer, the middle layer and the bottom layer yarn and adjust the yarn padding angle of the yarn, the traditional two-hole yarn nozzle is structurally upgraded to obtain a new three-hole yarn nozzle.

[0015] The three-hole yarn nozzle includes a yarn nozzle fixing seat, the upper end of which is provided with a yarn guide plate, and an end face of the yarn guide plate away from the yarn nozzle fixing seat is provided with a yarn guide eye group. Specifically, the yarn guide plate includes a connecting portion and a yarn guide portion, the yarn guide portion is vertically arranged at the upper end of the connecting portion, and the connecting portion is fixedly connected to the yarn nozzle fixing seat by screws. The yarn guide portion includes a first yarn guide plate and a second yarn guide plate, the first yarn guide plate is integrally connected to the connecting portion, and the second yarn guide is vertically arranged with the first yarn guide plate. The yarn guide eye group includes a first yarn guide eye, a second yarn guide eye and a third yarn guide eye, the first yarn guide eye and the third yarn guide eye are both arranged on the first yarn guide plate, and the second yarn guide eye is arranged on the second yarn guide plate.

[0016] Furthermore, a yarn nozzle rod is provided at the lower end of the yarn nozzle fixed seat, and a yarn feeding protrusion protruding outward from the yarn nozzle rod is provided on one side of the lower end of the yarn nozzle rod, and the yarn feeding protrusion is provided with a yarn feeding hole group corresponding to the yarn guide eye group, and the yarn feeding protrusion and the yarn nozzle rod are an integrally formed structure, and the yarn guide plate and the yarn nozzle rod are both detachably connected to the yarn nozzle fixed seat. Specifically, the side surface of the yarn feeding protrusion close to the yarn nozzle rod is concave inward and has an arc surface shape. The yarn feeding hole group includes a first yarn feeding hole, which is arranged on the yarn feeding protrusion and longitudinally penetrates the upper and lower end surfaces of the yarn feeding protrusion. The yarn feeding hole group includes a second yarn feeding hole, which is arranged on the recessed portion and longitudinally penetrates the upper and lower end surfaces of the recessed portion. The yarn feeding hole group includes a third yarn feeding hole, which is arranged on the yarn feeding protrusion and transversely penetrates the front and rear end surfaces of the yarn feeding protrusion. When in use, the first yarn passes through the first yarn feeding hole through the first yarn guide eye to be fed as the bottom yarn for weaving operation, the second yarn passes through the second yarn feeding hole through the second yarn guide eye to be fed as the surface yarn for weaving operation, and the third yarn passes through the third yarn feeding hole through the third yarn guide eye to be fed as the middle layer yarn for weaving operation. The setting of the first yarn feeding hole, the second yarn feeding hole and the third yarn feeding hole enables the surface layer, the middle layer and the bottom layer yarns to be fed at different yarn padding angles, and the above-mentioned weaving structure is used for weaving, thereby obtaining a three-layer single-sided plain fabric with a strong three-dimensional effect.

[0017] According to the structural design of the three-hole yarn nozzle component, the yarn inlay angle of each layer of the feeding yarn is specifically adjusted. As a preferred solution of the present invention, the yarn inlay angle of the first yarn is 40 degrees, the yarn inlay angle of the second yarn is 25 degrees, and the yarn inlay angle of the third yarn is 50 degrees. The yarn inlay angle refers to the angle between the yarn and the vertical direction.

[0018] Furthermore, the yarn tension of the first yarn is 13-15CN; when the second yarn is polyester filament, the yarn tension is preferably 4-6CN, and when the second yarn is cotton yarn or cotton-polyester blended yarn, the yarn tension is preferably 9-12CN; the yarn tension of the third yarn is 16-18CN.

[0019] The present invention adjusts the inlay yarn angle and the yarn tension, so that the yarn position and angle are stably controlled, the yarn is not easily reversed, the woven fabric has a strong three-dimensional sense and clear texture, and a three-layer three-dimensional effect is achieved.

[0020] Preferably, in step S2, the specific steps of the pre-setting treatment are: passing the grey cloth through a hot water slurry tank at 80-90°C, and then setting the cloth at a temperature of 180-190°C, and at the same time, the edge of the grey cloth is sizing with a setting slurry. More preferably, the setting slurry is polyacrylate. In the present invention, the grey cloth is firstly set to prevent creases from appearing in the subsequent dyeing process. While setting the cloth, the setting slurry is used to fix the cloth edge to prevent the grey cloth from curling due to excessive vertical tension when passing through the boiling and bleaching machine.

[0021] Preferably, in step S4, the scouring and bleaching process uses a mixture of 4-6 g / L caustic soda and 4-6 g / L hydrogen peroxide as the scouring and bleaching liquid, the scouring and bleaching temperature is 95-105° C., and the time is 1-2 min.

[0022] Preferably, in step S4, a two-bath dyeing process is adopted, and the specific steps are: (1) adding high-temperature disperse dyes to dye polyester, the bath ratio is 1:4-6, the temperature is 120-135°C, and the time is 30-60min; (2) after cooling, the liquid in the tank is discharged and reduction cleaning is performed; (3) after the liquid in the tank is discharged, polishing treatment is performed; (4) reactive dyes are added to dye cotton, the bath ratio is 1:4-6, the temperature is 50-80°C, and the time is 60-90min; (5) after the liquid in the tank is discharged, multiple cleanings are performed.

[0023] Preferably, the polishing treatment uses cellulose hydrolase as a polishing liquid, the pH of the polishing liquid is 6.5-7, the temperature of the polishing liquid is 30-50° C., and the polishing time is 20-40 min.

[0024] Preferably, in step S4, the bath ratio of the color fixing treatment is 1:4-6, the temperature is 40-70°C, and the time is 10-40 min.

[0025] The scouring and bleaching stage in the present invention is completed in an open-width scouring and bleaching device, which reduces the running time of the grey cloth in the dyeing vat and reduces the risk of creases. When dyeing the grey cloth, the present invention first uses high-temperature disperse dyes to dye polyester, then uses insurance powder to wash away the floating color, and then polishes the surface finish of the fabric to make the subsequent dyeing uniform and easy to color, while reducing pilling. After dyeing cotton with reactive dyes, a color fixation treatment is performed to improve the color fastness of the fabric. The present invention uses a two-bath dyeing process to effectively avoid mutual interference between the two dyes, so that the fabric achieves the best dyeing rate and color fastness. The color fixation treatment can improve the dry and wet friction fastness and water washing fastness of the fabric and reduce the fading of the fabric.

[0026] Preferably, in step S6, a finished product setting machine is used for setting treatment, the setting temperature is 140-160°C, and the machine speed is 17-23m / min; and then sent to a heavy pressure pre-shrinking machine for flattening, and the pressure of the pressure roller of the pre-shrinking machine is set to 4Bar. The flatness of the fabric is improved by heavy pressure flattening, and the texture of the fabric is improved.

[0027] A multi-layer single-sided plain fabric with a three-dimensional effect is produced by the above production method. The fabric adopts the above-mentioned unique weaving process of the present invention to obtain a three-layer single-sided structural fabric with a strong three-dimensional effect. The fabric has good shape retention and elasticity, and the bottom layer is a cotton layer with good skin-friendliness. At the same time, through the above-mentioned dyeing and finishing process, the problem of creases that are most likely to occur when dyeing this type of fabric is solved, and the dyeing rate and color fastness of the fabric are improved.

[0028] The beneficial effects of the present invention are as follows: the present invention discloses a method for preparing a multi-layer single-sided plain fabric with a three-dimensional effect. The production method has a short process, low energy consumption, and is suitable for industrial implementation. A new three-hole yarn nozzle is obtained by modifying and designing the traditional yarn nozzle of a single-sided knitting machine, and the yarn padding angle of each layer of yarn is adjusted, which is not easy to reverse the yarn. A single-layer single-sided structure plain fabric with a three-dimensional effect is woven through a specific weaving structure. The fabric has good shape retention, comfortable hand feel and good skin-friendliness, and fabrics with various effects are obtained by matching different yarns. At the same time, the dyeing and finishing process of the present invention solves the problem that creases are easy to appear when dyeing such fabrics, and the fabric has high flatness and good fabric texture. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic structural diagram of the three-hole yarn nozzle of the present invention.

[0030] Figure 2 This is an enlarged image of the fabric obtained in Example 2 placed under a microscope.

[0031] Figure markings: A-surface layer, B-middle layer, C-bottom layer, 1-yarn nozzle fixing seat, 2-yarn guide plate, 3-yarn nozzle rod, 4-yarn feeding protrusion, 5-connecting part, 6-yarn guiding part, 61-first yarn guiding piece, 62-second yarn guiding piece, 63-first yarn guiding eye, 64-second yarn guiding eye, 65-third yarn guiding eye, 41-recessed part, 42-first yarn feeding hole, 43-second yarn feeding hole, 44-third yarn feeding hole, 7-extension part. DETAILED DESCRIPTION

[0032] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.

[0033] As a preferred embodiment, Figure 1As shown, the present invention adopts a Japanese Fuyuan high-speed single-sided knitting machine, model VXC-S3.2RE. In order to realize the yarn feeding function of the surface layer, the middle layer and the bottom layer yarn and adjust the yarn padding angle of the yarn, the traditional two-hole yarn nozzle is structurally upgraded and designed to obtain a new type of three-hole yarn nozzle. The three-hole yarn nozzle includes a yarn nozzle fixing seat 1, and a yarn guide plate 2 is provided at the upper end of the yarn nozzle fixing seat 1. The yarn guide plate 2 is provided with a yarn guide eye group at one end face away from the yarn nozzle fixing seat 1. Specifically, the yarn guide plate 2 includes a connecting portion 5 and a yarn guide portion 6, and the yarn guide portion 6 is vertically arranged at the upper end of the connecting portion 5. The connecting portion 5 is fixedly connected to the yarn nozzle fixing seat 1 by screws. The yarn guide portion 6 includes a first yarn guide piece 61 and a second yarn guide piece 62. The first yarn guide piece 61 is integrally connected to the connecting portion 5, and the second yarn guide 62 is vertically arranged to the first yarn guide piece 61. The yarn guide eye group includes a first yarn guide eye 63 , a second yarn guide eye 64 and a third yarn guide eye 65 . The first yarn guide eye 63 and the third yarn guide eye 65 are both arranged on the first yarn guide piece 61 , and the second yarn guide eye 64 is arranged on the second yarn guide piece 62 .

[0034] Furthermore, a yarn nozzle rod 3 is provided at the lower end of the yarn nozzle fixed seat 1, and a yarn feeding protrusion 4 protruding outward from the yarn nozzle rod 3 is provided on one side of the lower end of the yarn nozzle rod 3, and the yarn feeding protrusion 4 is provided with a yarn feeding hole group corresponding to the yarn guide eye group, and the yarn feeding protrusion 4 and the yarn nozzle rod 3 are an integrally formed structure, and the yarn guide plate 2 and the yarn nozzle rod 3 are both detachably connected to the yarn nozzle fixed seat 1. Specifically, the side surface of the yarn feeding protrusion 4 close to the yarn nozzle rod 3 is inwardly concave and has an arc surface shape. The yarn feeding hole group includes a first yarn feeding hole 42, which is provided on the yarn feeding protrusion 4 and longitudinally penetrates the upper and lower end surfaces of the yarn feeding protrusion 4. The yarn feeding hole group includes a second yarn feeding hole 43, which is provided on the recessed portion 41 and longitudinally penetrates the upper and lower end surfaces of the recessed portion 41. The yarn feeding hole group includes a third yarn feeding hole 44, which is arranged on the yarn feeding protrusion 4 and transversely penetrates the front and rear end surfaces of the yarn feeding protrusion 4. When in use, the first yarn passes through the first yarn feeding hole 42 through the first yarn guide eye 63 as the bottom yarn feeding knitting operation, the second yarn passes through the second yarn feeding hole 43 through the second yarn guide eye 64 as the surface yarn feeding knitting operation, and the third yarn passes through the third yarn feeding hole 44 through the third yarn guide eye 65 as the middle layer yarn feeding knitting operation. The arrangement of the first yarn feeding hole 42, the second yarn feeding hole 43 and the third yarn feeding hole 44 enables the surface layer, the middle layer and the bottom layer yarn to be fed at different inlay angles, and the knitting is performed through the knitting structure of the present invention, thereby obtaining a three-layer single-faced plain fabric with a strong three-dimensional effect.

[0035] Specifically, the inlay angle of the first yarn is 40 degrees; the inlay angle of the second yarn is 25 degrees; the inlay angle of the third yarn is 50 degrees. The yarn tension of the first yarn is 13-15CN; when the second yarn is polyester filament, the yarn tension is preferably 4-6CN, when the second yarn is cotton yarn or cotton-polyester blended yarn, the yarn tension is preferably 9-12CN; the yarn tension of the third yarn is 16-18CN.

[0036] Example 1

[0037] A method for producing a multi-layer single-sided plain fabric with a three-dimensional effect comprises the following steps:

[0038] S1: Select raw yarn and weave the yarn into single-sided plain grey fabric using a single-sided knitting machine;

[0039] S2: using a pre-forming machine to pre-form the grey cloth obtained in step S1;

[0040] S3: singeing the grey cloth after the treatment in step S2 by using a singeing machine;

[0041] S4: placing the embryonic fabric processed in step S3 in an open-width scouring and bleaching machine for scouring and bleaching, and transferring the scouring and bleaching embryonic fabric to a dyeing vat for dyeing and color fixing treatment;

[0042] S5: softening the fabric after dyeing in step S4, and then drying the softened fabric;

[0043] S6: shaping the fabric obtained in step S5 into a finished product, so as to obtain the single-sided plain fabric.

[0044] In this embodiment, the single-sided plain fabric is composed of a surface layer, an intermediate layer and a bottom layer, wherein the surface layer is knitted by the first yarn using two AB needle cylinder stitches, and both are loop forming units, the intermediate layer is knitted by the second yarn using two AB needle cylinder stitches, and both are loop forming units, and the bottom layer is knitted by the third yarn using two AB needle cylinder stitches, and both are loop forming units, wherein the first yarn, the second yarn and the third yarn are fed into the warp nozzle at the same time for knitting. Specifically, the density of the surface layer is 35cm / 100 needles, the density of the intermediate layer is 31cm / 100 needles, and the density of the bottom layer is 32cm / 100 needles.

[0045] In this embodiment, the first yarn and the third yarn are both 50S / 1 long-staple fine cotton / fine cotton 30 / 70 SIRO (AA) compactly spun yarns, and the second yarn is 50D / 32F SORONA polyester composite yarn.

[0046] In this embodiment, the inlay angle of the first yarn is 40 degrees, the inlay angle of the second yarn is 25 degrees, and the inlay angle of the third yarn is 50 degrees. The yarn tension of the first yarn is 13CN, the yarn tension of the second yarn when it is polyester filament is preferably 4CN, and the yarn tension of the third yarn is 17CN.

[0047] In the above step S2, the specific steps of the pre-setting treatment are: passing the grey cloth through a 80°C hot water sizing tank, and then setting the cloth at 180°C, while the edge of the grey cloth is sized with a setting slurry, wherein the setting slurry is polyacrylate.

[0048] In the above step S4, the scouring and bleaching process uses a mixture of 6 g / L caustic soda and 4 g / L hydrogen peroxide as the scouring and bleaching liquid, the scouring and bleaching temperature is 95° C., and the scouring and bleaching time is 2 minutes.

[0049] In the above step S4, a two-bath dyeing process is adopted, and the dyeing vat adopts an air flow machine. The specific steps are: (1) adding high-temperature disperse dyes to dye polyester, the bath ratio is 1:5, the temperature is 125°C, and the time is 50 minutes; (2) after cooling, the liquid in the vat is discharged, and the insurance powder is used for reduction cleaning; (3) after the liquid in the vat is discharged, polishing treatment is performed; (4) then adding reactive dyes to dye cotton, the bath ratio is 1:5, the temperature is 55°C, and the time is 80 minutes; (5) after the liquid in the vat is discharged, soap oil is added to the water for cleaning, and then 80°C hot water is used for cleaning.

[0050] The high temperature disperse dye is anthraquinone and its derivatives, the reactive dye is halogenated triazine, the polishing treatment uses cellulose hydrolase as polishing liquid, the pH of the polishing liquid is 6.5, the temperature of the polishing liquid is 50°C, and the polishing time is 20 minutes.

[0051] In the above step S4, the color fixing treatment uses a polyamine color fixing agent, the bath ratio is 1:4, the temperature is 60° C., and the time is 30 minutes.

[0052] In the above step S5, the softening process uses sodium of higher saturated fatty acid as a softening agent.

[0053] In the above step S6, a finished product setting machine is used for setting treatment, the setting temperature is 160° C., and the machine speed is 20 m / min; and then it is sent to a heavy pressure pre-shrinking machine for flattening, and the pressure of the pressure roller of the pre-shrinking machine is set to 4 Bar.

[0054] Example 2

[0055] A method for producing a multi-layer single-sided plain fabric with a three-dimensional effect comprises the following steps:

[0056] S1: Select raw yarn and weave the yarn into single-sided plain grey fabric using a single-sided knitting machine;

[0057] S2: using a pre-forming machine to pre-form the grey cloth obtained in step S1;

[0058] S3: singeing the grey cloth after the treatment in step S2 by using a singeing machine;

[0059] S4: placing the embryonic fabric processed in step S3 in an open-width scouring and bleaching machine for scouring and bleaching, and transferring the scouring and bleaching embryonic fabric to a dyeing vat for dyeing and color fixing treatment;

[0060] S5: softening the fabric after dyeing in step S4, and then drying the softened fabric;

[0061] S6: shaping the fabric obtained in step S5 into a finished product, so as to obtain the single-sided plain fabric.

[0062] In this embodiment, the single-sided plain fabric is composed of a surface layer, an intermediate layer and a bottom layer, wherein the surface layer is knitted by the first yarn using two AB needle cylinder stitches, and both are loop forming units, the intermediate layer is knitted by the second yarn using two AB needle cylinder stitches, and both are loop forming units, and the bottom layer is knitted by the third yarn using two AB needle cylinder stitches, and both are loop forming units, wherein the first yarn, the second yarn and the third yarn are fed into the warp nozzle at the same time for knitting. Specifically, the density of the surface layer is 34cm / 100 needles, the density of the intermediate layer is 30cm / 100 needles, and the density of the bottom layer is 31cm / 100 needles.

[0063] In this embodiment, the first yarn and the third yarn are both 50S / 1 long-staple fine cotton / fine cotton 30 / 70 SIRO (AA) compactly spun yarns, and the second yarn is 50D / 32F SORONA polyester composite yarn.

[0064] In this embodiment, the inlay angle of the first yarn is 40 degrees, the inlay angle of the second yarn is 25 degrees, and the inlay angle of the third yarn is 50 degrees. The yarn tension of the first yarn is 14CN, the yarn tension of the second yarn is 5CN, and the yarn tension of the third yarn is 16CN.

[0065] In the above step S2, the specific steps of the pre-setting treatment are: passing the grey cloth through a 85°C hot water sizing tank, and then setting the cloth at a temperature of 185°C, while the edge of the grey cloth is sized with a setting slurry, wherein the setting slurry is polyacrylate.

[0066] In the above step S4, the scouring and bleaching process uses a mixture of 5 g / L caustic soda and 5 g / L hydrogen peroxide as the scouring and bleaching liquid, the scouring and bleaching temperature is 100° C., and the scouring and bleaching time is 2 minutes.

[0067] In the above step S4, a two-bath dyeing process is adopted, and the dyeing vat adopts an air flow machine. The specific steps are: (1) adding high-temperature disperse dyes to dye polyester, the bath ratio is 1:6, the temperature is 125°C, and the time is 40 minutes; (2) after cooling, the liquid in the vat is discharged, and the insurance powder is used for reduction cleaning; (3) after the liquid in the vat is discharged, polishing treatment is performed; (4) then adding reactive dyes to dye cotton, the bath ratio is 1:6, the temperature is 60°C, and the time is 60 minutes; (5) after the liquid in the vat is discharged, soap oil is added to the water for cleaning, and then 80°C hot water is used for cleaning.

[0068] Wherein, the high temperature disperse dye is anthraquinone and its derivatives, the reactive dye is halogenated tri-iso-azines, the polishing treatment uses cellulose hydrolase as polishing liquid, the pH of the polishing liquid is 6.8, the temperature of the polishing liquid is 40°C, and the polishing time is 30 minutes.

[0069] In the above step S4, the color fixing treatment uses a polyamine color fixing agent, the bath ratio is 1:5, the temperature is 50° C., and the time is 20 minutes.

[0070] In the above step S5, the softening process uses sodium of higher saturated fatty acid as a softening agent.

[0071] In the above step S6, a finished product setting machine is used for setting treatment, the setting temperature is 150° C., and the machine speed is 18 m / min; and then it is sent to a heavy pressure pre-shrinking machine for flattening, and the pressure of the pressure roller of the pre-shrinking machine is set to 4 Bar.

[0072] Example 3

[0073] A method for producing a multi-layer single-sided plain fabric with a three-dimensional effect comprises the following steps:

[0074] S1: Select raw yarn and weave the yarn into single-sided plain grey fabric using a single-sided knitting machine;

[0075] S2: using a pre-forming machine to pre-form the grey cloth obtained in step S1;

[0076] S3: singeing the grey cloth after the treatment in step S2 by using a singeing machine;

[0077] S4: placing the embryonic fabric processed in step S3 in an open-width scouring and bleaching machine for scouring and bleaching, and transferring the scouring and bleaching embryonic fabric to a dyeing vat for dyeing and color fixing treatment;

[0078] S5: softening the fabric after dyeing in step S4, and then drying the softened fabric;

[0079] S6: shaping the fabric obtained in step S5 into a finished product, so as to obtain the single-sided plain fabric.

[0080] In this embodiment, the single-sided plain fabric is composed of a surface layer, an intermediate layer and a bottom layer, wherein the surface layer is knitted by the first yarn using two AB needle cylinder stitches, and both are loop forming units, the intermediate layer is knitted by the second yarn using two AB needle cylinder stitches, and both are loop forming units, and the bottom layer is knitted by the third yarn using two AB needle cylinder stitches, and both are loop forming units, wherein the first yarn, the second yarn and the third yarn are fed into the warp nozzle at the same time for knitting. Specifically, the density of the surface layer is 34cm / 100 needles, the density of the intermediate layer is 30cm / 100 needles, and the density of the bottom layer is 31cm / 100 needles.

[0081] In this embodiment, the first yarn and the third yarn are both 50S / 1 long-staple fine cotton / fine cotton 30 / 70 SIRO (AA) compactly spun yarns, and the second yarn is 50D / 32F SORONA polyester composite yarn.

[0082] In this embodiment, the inlay angle of the first yarn is 40 degrees, the inlay angle of the second yarn is 25 degrees, and the inlay angle of the third yarn is 50 degrees. The yarn tension of the first yarn is 15CN, the yarn tension of the second yarn is 6CN, and the yarn tension of the third yarn is 18CN.

[0083] In the above step S2, the specific steps of the pre-setting treatment are: passing the grey cloth through a 90°C hot water sizing tank, and then setting the cloth at 190°C, while the edge of the grey cloth is sized with a setting slurry, wherein the setting slurry is polyacrylate.

[0084] In the above step S4, the scouring and bleaching process uses a mixture of 6 g / L caustic soda and 5 g / L hydrogen peroxide as the scouring and bleaching liquid, the scouring and bleaching temperature is 105° C., and the scouring and bleaching time is 1 min.

[0085] In the above step S4, a two-bath dyeing process is adopted, and the dyeing vat adopts an air flow machine. The specific steps are: (1) adding high-temperature disperse dyes to dye polyester, the bath ratio is 1:4, the temperature is 125°C, and the time is 30 minutes; (2) after cooling, the liquid in the vat is discharged, and the insurance powder is used for reduction cleaning; (3) after the liquid in the vat is discharged, polishing treatment is performed; (4) then adding reactive dyes to dye cotton, the bath ratio is 1:4, the temperature is 80°C, and the time is 60 minutes; (5) after the liquid in the vat is discharged, soap oil is added to the water for cleaning, and then 80°C hot water is used for cleaning.

[0086] The high temperature disperse dye is anthraquinone and its derivatives, the reactive dye is halogenated tri-iso-azines, the polishing treatment uses cellulose hydrolase as the polishing liquid, the pH of the polishing liquid is 7, the temperature of the polishing liquid is 50° C., and the polishing time is 20 min.

[0087] In the above step S4, the color fixing treatment uses a polyamine color fixing agent, the bath ratio is 1:6, the temperature is 60° C., and the time is 30 minutes.

[0088] In the above step S5, the softening process uses sodium of higher saturated fatty acid as a softening agent.

[0089] In the above step S6, a finished product setting machine is used for setting treatment, the setting temperature is 160° C., and the machine speed is 20 m / min; and then it is sent to a heavy pressure pre-shrinking machine for flattening, and the pressure of the pressure roller of the pre-shrinking machine is set to 4 Bar.

[0090] Example 4

[0091] A method for producing a multi-layer single-sided plain fabric with a three-dimensional effect comprises the following steps:

[0092] S1: Select raw yarn and weave the yarn into single-sided plain grey fabric using a single-sided knitting machine;

[0093] S2: using a pre-forming machine to pre-form the grey cloth obtained in step S1;

[0094] S3: singeing the grey cloth after the treatment in step S2 by using a singeing machine;

[0095] S4: placing the embryonic fabric processed in step S3 in an open-width scouring and bleaching machine for scouring and bleaching, and transferring the scouring and bleaching embryonic fabric to a dyeing vat for dyeing and color fixing treatment;

[0096] S5: softening the fabric after dyeing in step S4, and then drying the softened fabric;

[0097] S6: shaping the fabric obtained in step S5 into a finished product, so as to obtain the single-sided plain fabric.

[0098] In this embodiment, the single-sided plain fabric is composed of a surface layer, an intermediate layer and a bottom layer, wherein the surface layer is knitted with the first yarn using two AB needles, and both are loop-forming units, the intermediate layer is knitted with the second yarn using two AB needles, and both are loop-forming units, and the bottom layer is knitted with the third yarn using two AB needles, and both are loop-forming units, wherein the first yarn, the second yarn and the third yarn are fed into the warp nozzle at the same time for knitting. Specifically, the density of the surface layer (here, the density refers to the yarn length measured based on 100 coil wales) is 35cm / 100 needles, the density of the intermediate layer is 34cm / 100 needles, and the density of the bottom layer is 33cm / 100 needles.

[0099] In this embodiment, the first yarn, the second yarn and the third yarn are all 40S / 1 long-staple refined cotton / refined cotton 30 / 70 SIRO (AA) compactly spun yarns.

[0100] In this embodiment, the inlay angle of the first yarn is 40 degrees, the inlay angle of the second yarn is 25 degrees, and the inlay angle of the third yarn is 50 degrees. The yarn tension of the first yarn is 15CN, the yarn tension of the second yarn is 10CN, and the yarn tension of the third yarn is 18CN.

[0101] In the above step S2, the specific steps of the pre-setting treatment are: passing the grey cloth through a 85°C hot water sizing tank, and then setting the cloth at a temperature of 190°C, while the edge of the grey cloth is sized with a setting slurry, wherein the setting slurry is polyacrylate.

[0102] In the above step S4, the scouring and bleaching process uses a mixture of 6 g / L caustic soda and 5 g / L hydrogen peroxide as the scouring and bleaching liquid, the scouring and bleaching temperature is 100° C., and the scouring and bleaching time is 1 min.

[0103] In the above step S4, the dyeing vat uses an airflow machine, the polishing treatment uses cellulose hydrolase as a polishing liquid, the pH of the polishing liquid is 6.8, the temperature of the polishing liquid is 40°C, and the polishing time is 30 minutes; then add reactive dyes to dye cotton, the bath ratio is 1:5, the temperature is 60°C, and the time is 60 minutes. After dyeing, the liquid in the vat is discharged, soap oil is added to the water for washing, and then washed with hot water at 80°C. Wherein, the reactive dye is a halogenated triiso-azine.

[0104] In the above step S4, the color fixing treatment uses a polyamine color fixing agent, the bath ratio is 1:5, the temperature is 50° C., and the time is 12 minutes.

[0105] In the above step S5, the softening process uses sodium of higher saturated fatty acid as a softening agent.

[0106] In the above step S6, a finished product setting machine is used for setting treatment, the setting temperature is 150° C., and the machine speed is 28 m / min; and then it is sent to a heavy pressure pre-shrinking machine for flattening, and the pressure of the pressure roller of the pre-shrinking machine is set to 4 Bar.

[0107] The fabric prepared in the embodiment is placed under a microscope and observed as follows: Figure 2As shown, the fabrics prepared in Examples 2 and 4 were subjected to relevant performance tests, wherein the rubbing color fastness test was performed with reference to the GB / T 3920-2008 rubbing color fastness test standard; the anti-pilling performance test was tested according to the requirements of the Anta brand, wherein Example 2 was tested with reference to GB / T 4802.2-2008 using the Martindale method (condition of 2500 revolutions), and Example 4 was tested using the GB / T 4802.1-2008 circular locus E method (condition of 600 pilling times and a pressure of 780CN); the elastic recovery performance test was performed in accordance with the "Determination of the constant force elongation" in FZ / T70006-2004 "Test method for tensile elastic recovery of knitted fabrics". The specific test conditions are as follows: randomly select 3 specimens in the vertical direction and 3 specimens in the horizontal direction, the effective size of the specimen is 100mm×50mm, the fixed force is 40N, the constant speed is 100mm / min, the return speed is 50mm / min, the pre-tension is 1N, the fixed length is controlled for 2 hours, and the elongation is 4 times. Without adding cooling agent, the contact cooling coefficient test is carried out in accordance with the standard GB / T35263-2017 "Testing and Evaluation of the Instantaneous Cooling Performance of Textiles at Contact", the test instrument model is Roaches Q-Max, the test conditions are: temperature is 20.1℃, humidity is 65.1%, hot plate temperature is 35.0℃, cold plate temperature is 20.0℃, washed three times by the 4N program in GB / T 8629-2017, and hung to dry.

[0108]

[0109] It can be seen from the data in the above table that the fabric prepared in Example 2 has high color fastness, is not easy to fade, has high anti-pilling performance, and is not easy to pilling. At the same time, the tensile recovery rate of the fabric before and after washing changes little, indicating that the fabric has good shape retention, good elasticity, washability, durability, softness, and is very suitable for use as a fabric for skin-friendly clothing such as T-shirts.

[0110]

[0111]

[0112] The test data in the above table show that the fabric prepared in Example 4 has high friction color fastness, good anti-pilling performance and high flatness, a large surface area in contact with the skin, and without adding a cooling agent, the contact cooling coefficient of the fabric is greater than the national standard (0.15 J / (cm·s)) before and after washing. It feels cool to the touch, has a straight and stylish texture, and is very suitable for use as a fabric for currently popular trendy style clothing.

[0113] The test results of the fabric thickness obtained in Examples 2 and 4 are shown in the following table:

[0114] First test results Second test results The third test results Example 2 0.83mm 0.85mm 0.83mm Example 4 0.92mm 0.89mm 0.90mm

[0115] Compared with the traditional single-sided plain fabric of the same weight, the fabrics prepared in Examples 2 and 4 of the present invention are thicker, indicating that the 3D stereoscopic effect of the three-layer single-sided plain fabric of the present invention is more obvious.

[0116] The above specific embodiments are further explanations of the technical solutions and beneficial effects of the present invention, and are not limitations of the implementation methods. For those skilled in the art, any obvious replacements that do not depart from the concept of the present invention are within the protection scope of the present invention.

Claims

1. A method for producing a multi-layer single-sided plain fabric with a three-dimensional effect, Features: The steps include: S1: Select raw yarn and weave the yarn into single-sided plain grey fabric using a knitting machine; S2: performing a pre-setting process on the grey cloth obtained in step S1; S3: Singeing the grey cloth after being processed in step S2; S4: placing the embryonic fabric processed in step S3 in an open-width scouring and bleaching machine for scouring and bleaching, and transferring the scouring and bleaching embryonic fabric to a dyeing vat for dyeing and color fixing treatment; S5: softening the fabric after dyeing in step S4, and then drying the softened fabric; S6: shaping the fabric obtained in step S5 into a finished product, so as to obtain the single-sided plain fabric; The single-sided plain fabric consists of a surface layer, an intermediate layer and a bottom layer, wherein the surface layer is knitted with a first yarn using two AB needle cylinder stitches, and both are loop forming units, the intermediate layer is knitted with a second yarn using two AB needle cylinder stitches, and both are loop forming units, and the bottom layer is knitted with a third yarn using two AB needle cylinder stitches, and both are loop forming units, wherein the first yarn, the second yarn and the third yarn are fed into the warp nozzle simultaneously for knitting; The yarn nozzle is a three-hole yarn nozzle; the three-hole yarn nozzle comprises a yarn nozzle fixing seat, the upper end of the yarn nozzle fixing seat is provided with a yarn guide plate, and the end surface of the yarn guide plate away from the yarn nozzle fixing seat is provided with a yarn guide eye group; the lower end of the yarn nozzle fixing seat is provided with a yarn nozzle rod, and one side of the lower end of the yarn nozzle rod is provided with a yarn feeding protrusion protruding outward from the yarn nozzle rod, the yarn feeding protrusion is provided with a yarn feeding hole group corresponding to the yarn guide eye group, the yarn feeding protrusion and the yarn nozzle rod are an integrally formed structure, and the yarn guide plate and the yarn nozzle rod are detachably connected to the yarn nozzle fixing seat; The inlay angle of the first yarn is 40 degrees, the inlay angle of the second yarn is 25 degrees, and the inlay angle of the third yarn is 50 degrees; In step S2, the specific steps of the pre-setting treatment are: passing the grey cloth through a hot water sizing tank at 80-90°C, and then setting the cloth at a temperature of 180-190°C, while the edge of the grey cloth is sizing with a setting slurry; the setting slurry is polyacrylate; In step S4, a two-bath dyeing process is adopted, and the specific steps are as follows: (1) adding high-temperature disperse dyes to dye polyester, the bath ratio is 1:4-6, the temperature is 120-135°C, and the time is 30-60 min; (2) after cooling, the liquid in the tank is discharged and reduction cleaning is performed; (3) After draining the liquid in the tank, polishing is performed; the polishing process uses cellulose hydrolase as the polishing liquid, the pH of the polishing liquid is 6.5-7, the temperature of the polishing liquid is 30-50°C, and the polishing time is 20-40min; (4) Reactive dyes are added to dye the cotton, the bath ratio is 1:4-6, the temperature is 50-80°C, and the time is 60-90min; (5) After draining the liquid in the tank, washing is performed multiple times; In step S4, the bath ratio of the color fixing treatment is 1:4-6, the temperature is 40-70°C, and the time is 10-40 minutes.

2. A method for producing a multi-layer single-face plain fabric with a three-dimensional effect according to claim 1, Features: The first yarn and the third yarn are both cotton yarn or cotton-polyester blended yarn, and the second yarn is any one of polyester filament, cotton yarn or cotton-polyester blended yarn.

3. The method for producing a multi-layer single-face plain fabric with a three-dimensional effect according to claim 1, Features: In step S6, a finished product setting machine is used for setting treatment, the setting temperature is 140-160°C, and the machine speed is 17-23m / min; and then it is sent to a heavy pressure pre-shrinking machine for flattening, and the pressure of the pressure roller of the heavy pressure pre-shrinking machine is set to 4Bar.

4. A multi-layer single-sided plain fabric with a three-dimensional effect, Features: The multi-layer single-face plain fabric with three-dimensional effect is produced by the production method of any one of claims 1 to 3.