Method for recovering copper from secondary raw materials
By using redox reaction and oxygen control in the pyrometallurgy process, the problem of insufficient heat input in the secondary copper smelting step is solved, and more stable and economical temperature control is achieved, reducing the complexity of exhaust gas treatment and fuel consumption.
Patent Information
- Application Number
- CN202080076822.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-22
- Filing Date
- 2020-11-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-11-20
AI Technical Summary
In the existing pyrometallurgical process, the heat input in the secondary copper smelting step is insufficiently efficient, resulting in difficulty in temperature control, large fuel consumption, complex waste gas treatment, and high risk of temperature loss.
The redox reaction is used to generate heat by adding excess elemental iron and metals or compounds as inert as iron or zinc into the furnace, and the temperature is adjusted by controlling oxygen injection, avoiding temperature out of control while reducing the amount of exhaust gas.
It improves the control accuracy and responsiveness of furnace temperature, reduces fuel consumption and waste gas treatment costs, reduces the burden of evaporation and waste gas treatment systems of valuable metals, and improves the economic and reliability of the process.
Smart Images

Figure CN114651076B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the recovery of copper (Cu) and other non-ferrous metals such as tin (Sn), lead (Pb), nickel (Ni) and zinc (Zn) mainly from secondary feedstocks by means of pyrometallurgical process steps. The present invention preferably relates to secondary feedstocks, also referred to as recyclable materials. Recyclable materials may be, for example, by-products of metal producers, waste materials and scrap materials. Background Art
[0002] The present invention is primarily concerned with the well-known pyrometallurgical step in copper production, namely the smelting step. Depending on the source of the feed material, the smelting step can be further defined as a primary or secondary smelting step.
[0003] Smelting is a process of applying heat and chemical reagents to metal ores to extract base metals, most often in a single smelting process. In more technical detail, smelting is a process of liquefying a metal-bearing solid by chemical reaction, resulting in the metal. It is used to extract many metals, including silver, iron, copper, and other base metals, from the inert gangue component of the ore. It is a form of extractive metallurgy in which chemical reactions are used to drive off other elements as gases or slag, leaving behind a liquid bath containing the metal, either in its elemental form or in a chemically combined form, such as with sulfur, called "matte". The elemental metal is recovered in a separate molten metal phase. In addition, the matte usually forms a separate liquid phase. Most ores are impure and usually require the use of fluxes such as limestone or silica to remove the accompanying gangue, which forms a typical by-product called "slag" as part of the other separate liquid phase.
[0004] In the process of recovering copper from secondary materials, smelting can also be used as a first step to recover a concentrated copper phase from secondary raw materials, which may be too contaminated and / or have too low a copper content to be suitable for direct use as feedstock for refining to anode copper quality. These secondary raw materials are usually richer in copper than primary copper sources (e.g., copper ore or even copper concentrated intermediates), which are usually first obtained from the ore by, for example, mineral flotation performed upstream of the smelting step. A portion of the copper in the secondary materials may also already be present in elemental form and therefore not chemically bound. For these reasons, the operating conditions of the copper smelting step performed on secondary raw materials are significantly different from the operating conditions of the primary copper smelting step performed on copper concentrates or, occasionally, copper ore.
[0005] In primary copper smelting, the usual starting materials are copper-containing sulfides such as chalcopyrite (CuFeS2), bornite (Cu5FeS4) and chalcocite (Cu2S). Their reaction (oxidation) with oxygen removes S in the form of SO2 in the tail gas and forms a "matte" phase (Cu2S.FeS) and a slag phase (FeO.SiO2), the latter being formed by reaction with added silicon dioxide. In a second step, also usually in the smelting furnace, the FeS is removed by further reaction with oxygen and silicon dioxide to form more slag and more SO2 gas, leaving behind the so-called "white matte" (Cu2S), which usually has less than 1% residual iron. The latter is then oxidized with an oxygen-containing gas, preferably air, according to the following reaction:
[0006] Cu2S+O2→2Cu+SO2,
[0007] Cu2S+3 / 2O2→Cu2O+SO2
[0008] Cu2S+2Cu2O→6Cu+SO2)
[0009] This primary copper smelting process is usually carried out in a so-called "Pierce-Smith" converter to form so-called "blister copper", which includes nickel and precious metals, slag containing most of Fe, Zn and 2-15% Cu, furnace dust (including most of Sb, As, Bi, Cd, Pb) and tail gas (also containing SO2). A large amount of S released in these process steps is removed in the form of SO2 and recovered in the form of sulfuric acid. Therefore, the primary copper smelting step is usually mainly a strong oxidation step. For example, JPS61531 (A) or its authorized version JPH0515769 (B2) describes a primary copper smelting process. The treatment of the copper matte phase is described in, for example, CN101871050A and GB2462481A. US3,954,448 describes a method for further treating the copper matte or slag from the primary copper smelting step.
[0010] JP 2003253349 describes a primary copper smelting process in which the copper matte raw material also contains iron sulfides. In a first step, the iron sulfides are selectively oxidized to iron oxides using oxygen-enriched air. The iron oxides and added silicon dioxide are ultimately present in a separate slag phase, which is removed from the furnace before the copper sulfides are further processed in a second step. The amount of iron sulfides present and their reaction to form FeO may not be sufficient to generate the reaction heat required to maintain the furnace temperature in the first step, especially when cold raw materials are to be processed. In the first step, for each ton of copper matte processed, a certain amount of additional metallic iron is added to offset the further oxidation of iron to magnetite (Fe2O3), which otherwise will increase the viscosity of the slag and impair the subsequent phase separation and slag removal at the end of the first step. Under the oxidation conditions that usually prevail in the primary copper smelting step, the additional metallic iron is oxidized, and this reaction generates additional heat.
[0011] The metal in the usual starting material for the secondary copper smelting step is mainly present in the form of oxides, but a small amount of sulfides may also be present. Therefore, an important difference from the primary copper smelting step is that there is no copper matte as an intermediate. Some of the copper in the raw material may actually already exist in its elemental form, but the concentration is too low, or in a form that is not very suitable for pyrometallurgical copper refining, and even less suitable for hydrometallurgical recovery (leaching + electrolytic deposition). The copper in the form of oxides is then reduced in the smelting step by adding a reducing agent (e.g., a carbon source such as coke, and / or metallic iron, usually in the form of iron scrap). Therefore, another major difference from the primary copper smelting step includes the reducing conditions under which the smelting step of the secondary raw material is carried out.
[0012] US3,682,623 (Ludo Dierckx et al.) describes a copper refining process starting from secondary raw materials, wherein the first step is a smelting step, i.e. a reduction step, which is carried out in a smelting furnace, wherein copper-containing materials are heated together with solid materials containing metallic iron in an oxygen-rich neutral flame, and a molten bath including a slag phase is produced under gentle stirring of the charge. A small amount of alkaline or neutral flux may be added to optimize the specific gravity and viscosity of the slag formed. In addition, additional silica may be added to absorb the iron compounds produced in the reduction reaction. As the temperature of the molten bath in the smelting furnace increases, the chemically bound copper, lead, tin or nickel in the charge is said to be reduced by the solid metallic iron to form a molten metal called "black copper" and a molten slag containing iron silicates. The general process reactions are said to include:
[0013] MeO+Fe→FeO+Me
[0014] (MeO) x SiO2+xFe→(FeO) x SiO2+xMe
[0015] x FeO+SiO2→(FeO) x SiO2
[0016] These reactions confirm that the so-called "smelting" step of US 3,682,623 corresponds to a "smelting" step as referred to herein. These reactions are exothermic and the heat of reaction is said to rapidly raise the temperature of the charge. Once the material is melted to the point where it flows easily along the walls of the vessel, the stirring of the vessel can be increased. At the end of the reduction step, black copper and smelting slag are formed which can be separated from each other by gravity and can be removed from the furnace separately.
[0017] Throughout the reduction operation, the temperature is controlled to be as low as possible, consistent with maintaining a fluid slag temperature. The fuel supply must be adjusted to prevent the temperature of the reaction mass from exceeding about 1300°C at any time during the smelting furnace cycle. Preferably, the temperature should be maintained at no greater than the temperature at which the slag becomes substantially fluid. For ordinary furnace charges, a bath temperature of about 1180°C is reported to be satisfactory, but lower temperatures may be used if borax is used as a flux.
[0018] Low temperature not only minimizes the vaporization of lead and tin, but also limits the dissolution of solid iron in the produced molten copper. It is said that the presence of a large amount of solid iron is necessary to provide rapid and complete reduction of the slag. The dissolution of iron should also be minimized to maintain high solubility of lead and tin in the produced black copper. As the reduction reaction proceeds and the solid iron-containing material gradually dissolves in the molten metal, additional solid material containing metallic iron can be advantageously added after the smelting is completed to achieve the final reduction of copper, tin, lead and zinc remaining in the slag. In general, excess iron is used, which remains in the furnace, at least a portion of which is dissolved in the black copper. Zinc is volatilized out of the furnace, but at the end of the smelting step, a considerable amount of zinc also remains in the black copper.
[0019] At the end of the so-called smelting step, when the final reduction step is complete, as shown by further slag analysis, the smelting slag is poured from the top of the furnace and granulated. After pouring the smelting slag from the furnace, the resulting black copper is subsequently pre-refined in the same furnace together with the addition of more secondary raw materials, which are already quite rich in copper, using a strong oxidizing flame. This pre-refining step is therefore no longer part of the upstream smelting step, which is a reduction step characterized by a reducing environment.
[0020] In Example 1 of US 3,682,623, the charge of the smelting furnace is melted "under a neutral oxygen-enriched flame" (column 15, lines 1-2), which flame is understood to be a neutral flame, using oxygen-enriched air. After adding an additional amount of copper / iron scrap, the slag is further reduced under a slightly reducing flame (column 15, lines 33-35). Most of the zinc present is evaporated and recovered as dust in the exhaust system. Subsequently, the slag is poured from the top and granulated.
[0021] DE 10 2012 005 401 A1 describes a molten bath smelting furnace, in which copper-containing substances, preferably copper-containing secondary raw materials, undergo a smelting process, which is fueled by oil and / or gas together with air and / or oxygen, which is injected into the molten bath by means of an immersion lance. The smelting step produces a primary slag with relatively few impurities discharged from the process, and a secondary slag, which is transferred from the molten bath smelting furnace to a rotary drum furnace for further processing. The rotary drum furnace has a burner at one end, which can be supplied with oil or gas, and optionally also with oxygen from an oxygen reservoir. The further processing is carried out step by step and successively produces anode grade copper, black copper, a raw tin mixture that can be further processed with silicon, and a final slag. In each process step, coal is added to the rotary drum furnace. In each step of the method of DE 10 2012 005 401 A1, the furnace is heated by burning fuel and air and / or oxygen.
[0022] EP 0185004 describes a process in which, in order to increase the yield of valuable metals, an oxidation smelting step of secondary materials forms a liquid bath from which tin and zinc are removed in two steps in succession by fuming, and then the iron-containing slag is removed from the furnace while retaining a copper-containing metallic phase. This metallic phase is further processed to first separate out a lead silicate slag, low-nickel blister copper and a copper-nickel oxide bath which can then be reduced to form a copper-nickel alloy.
[0023] US2017 / 0198371 A1 deals with the large variations that may exist in the organic content of the smelting feed and its impact on the process throughput. The article proposes that the organic components are removed in a batch manner in the first stage, while the so-called "black copper" is already produced, which can be converted into blister copper by further oxidation in a subsequent stage. Another product of the first step is the final metal-poor slag. The article states that "a suitably adjusted amount of oxygen is blown into the process chamber". In this process, "the composition of the slag and the content of valuable metals still present therein are monitored during the smelting process by sampling and rapid analysis".
[0024] A disadvantage of the smelting step of US 3,682,623 is that a significant portion of the heat input is provided by a neutral flame burning in oxygen-enriched air during most of the smelting step. This requires large amounts of fuel, air and pure oxygen, with the associated complexity, additional equipment and operating burden.
[0025] The input of heat from the flame above the furnace into the molten bath presents some requirements, since heat must be transferred from the combustion gases into the liquid molten bath. The heat transfer from the gas to the liquid is rather slow, and the contact area between the burner at the top of the furnace and the liquid molten bath is limited. With submerged burners, gravity forces the gases to rise quickly and leave the liquid phase. Therefore, the contact time between the combustion gases and the molten bath is relatively small. Therefore, the input of heat from the flame into the molten bath is mainly by radiation. Therefore, the input of heat by the flame is not efficient, and possibly a major part of the heat input from the flame ends up leaving the furnace in the exhaust gases, which means an additional burden on the exhaust gas cooling system.
[0026] The large amount of smoke generated by the flames also requires the installation and operation of a large exhaust gas treatment system.
[0027] The inventors have discovered that there exists a need for more convenient and efficient heat input into a secondary copper smelting furnace whilst maintaining or even improving the means for controlling the temperature during the smelting step.
[0028] It is an object of the present invention to obviate or at least alleviate the above described problems and / or to generally provide improvements. Summary of the invention
[0029] According to the present invention, there is provided a method as defined herein.
[0030] In one embodiment, the present invention provides a method for recovering copper from secondary raw materials, comprising the steps of: smelting a feedstock including raw materials in a furnace in at least one feed batch to recover a concentrated copper intermediate from the furnace,
[0031] wherein said feed of raw material is gradually introduced into said furnace, said feed comprising copper and optionally at least one metal which is more noble than copper under the operating conditions of the furnace, said metal being at least partly an oxide,
[0032] wherein the feed material further comprises iron, and optionally at least one metal or compound which is at most as inert as iron or zinc under the conditions of the furnace, the iron and the metal which is at most as inert as iron or zinc being present at least partly in elemental form,
[0033] wherein heat is generated in the furnace by redox reactions which convert elemental iron and metals or compounds up to as inert as iron or zinc into oxides and which convert oxides of copper and metals more inert than copper into elemental metals,
[0034] wherein the elemental metal is at least partially collected in the molten liquid metal phase, and the oxide is at least partially collected in the upper liquid slag phase,
[0035] wherein the liquid phases are separable and at the end of the smelting step at least one liquid phase is at least partially removed from the furnace as smelting slag and / or as a concentrated copper intermediate,
[0036] It is characterized in that
[0037] During said smelting step, an excess of iron in elemental form and a metal or compound which is at most as inert as iron or zinc under said furnace conditions is maintained in said furnace relative to the amount required to complete said redox reaction, and
[0038] During the smelting step, further heat input into the furnace is provided by the injection of an oxygen-containing gas for oxidizing excess iron and metals or compounds up to as inert as iron or zinc present in the furnace, and optionally for burning combustible sources of carbon and / or hydrogen which may otherwise be introduced into the furnace.
[0039] Preferably, an excess of iron and optionally a metal or compound that is at most as inert as iron or zinc under the furnace conditions is maintained by purposefully adding to the furnace as part of the feed at least one additional raw material rich in iron and / or at least one metal or suitable compound.
[0040] Applicants have found that maintaining an excess of iron and optionally other metals and / or compounds that are at most as inert as iron or zinc in the furnace provides a very convenient method for controlling a highly controllable portion of the heat input, and therefore the temperature in the furnace, by controlling the oxygen-containing gas injected into the furnace, since the oxygen in the gas is available for oxidation of the excess elemental iron and / or other metals or compounds that are at most as inert as iron or zinc. Applicants have found that this method enables direct, accurate and correct dosing of the oxygen input to generate a portion of the heat of reaction, more advantageously, to become readily, directly and fully available in the liquid bath in the furnace at the level of the location where it is most needed, namely at the interface between the metal phase and the slag phase, where redox reactions and phase changes should occur.
[0041] The heat from the oxidation of iron and other metals and / or compounds which are at most as inert as iron or zinc by reaction with oxygen from the oxygen-containing gas is generated in the molten bath itself and does not require any additional heat transfer steps. This reaction heat is immediately and fully dissipated to the smelting bath.
[0042] The applicant has found that, thanks to the present invention, temperature control in the smelting furnace becomes easier and more responsive. This is very advantageous because as the temperature in the molten liquid bath increases, more iron dissolves into the molten liquid metal and becomes available for oxidation by the oxygen, which in the presence of oxygen in large quantities will generate more heat and will cause a runaway temperature.
[0043] The present invention makes it possible to avoid this risk of temperature runaway because, in the method according to the invention, the input of oxygen as part of the oxygen-containing gas is very controllable. If the feedstock introduces a relatively large amount of oxygen available for participating in the redox reaction at a certain moment, and if the heat generated by these additional redox reactions will lead to an increase in the temperature of the smelting bath, the temperature of the smelting bath can be easily controlled by reducing the injection rate of the oxygen-containing gas, and any risk of temperature runaway can be easily avoided or at least significantly reduced.
[0044] Another advantage of the invention is that, unlike the combustion of natural gas or other carbon- and / or hydrogen-containing fuels, the oxidation of iron and other metals or compounds that are at most as inert as iron or zinc generally does not generate large quantities of waste gases, and the furnace waste gas treatment system associated with a smelting plant operating the method according to the invention can be designed to be smaller, thus requiring lower capital costs and consuming lower operating costs during operation. Another advantage of lower waste gas volumes is that generally less valuable tin, lead and zinc are evaporated and therefore do not need to be captured in the waste gas treatment system.
[0045] Thus, the applicant has discovered that heat generated by oxidizing excess iron to iron oxides, for example by injecting oxygen into the smelting bath, is more effective and efficient than burning a carbon and / or hydrogen based flame in the furnace. The applicant estimates that approximately 80% of the injected oxygen reacts with compounds in the liquid bath in the furnace, and the heat generated by these reactions remains in the liquid bath, which is a very high yield compared to the heat that can be contributed by the combustion of hydrocarbon fuels such as natural gas, even if such combustion is carried out with pure oxygen or oxygen-enriched air. The applicant believes that this difference is because the conversion of iron to iron oxides occurs in the liquid bath itself, while the combustion of natural gas occurs in the gas phase, and the heat of combustion still has to be transferred to the liquid phase to contribute to the enthalpy content of the liquid bath. In addition, such combustion is not necessarily complete.
[0046] The applicant has also found that suitable sources of elemental iron, as well as sources of metals or compounds that are at most as inert as iron or zinc, are readily available from a wide range of sources and can be readily obtained on economic terms, making this method of heat input economically more advantageous than heat input by means of a neutral flame, even from the standpoint of operating costs alone. Furthermore, the process according to the invention has a lower carbon footprint than the processes described in the above-mentioned prior art.
[0047] Although included within the scope of the present invention, applicants prefer not to operate the option of providing a portion of the total heat input to the furnace by burning a combustible source of carbon and / or hydrogen in the furnace. Applicants have found that, under certain economic conditions, it may be advantageous to operate this option, but applicants always, even when operating this option, prefer to control the furnace temperature by injecting oxygen-containing gas because of its greater convenience, easier control and lower risk of temperature runaway.
[0048] Another advantage of the invention related to the presence of excess iron dissolved in the layer of molten liquid metal in the furnace is that a layer of solid iron and / or iron oxides forms around the submerged tuyere through which the oxygen-containing gas is introduced and forms an additional protection for these tuyere against wear, since these tuyere are cooled by a gas stream which is generally cooler than the smelting bath. The protective layer, which is generally in the shape of a hollow mushroom, is formed because the tuyere itself is cooler, the molten liquid metal around the tuyere becomes cooler, thereby reducing the solubility of iron in the concentrated molten liquid copper phase, and the iron precipitates and adheres to the outer surface of the tuyere except for the port through which the gas is injected.
[0049] A high responsiveness of the temperature control is advantageous because if the temperature of the molten liquid increases, the protective layer may dissolve again and the tuyere may lose its protective layer, resulting in possible serious damage and production losses. The high responsiveness of the temperature control system has the effect that the risk of such tuyere damage and the associated production losses can be greatly reduced and preferably avoided.
[0050] The applicant has found that a beneficial effect of the present invention is to obtain a more stable and reliable smelting step.The smelting step is usually a very early step in a more complex overall pyrometallurgical process.
[0051] The overall process can be such that the product of the smelting step is further processed into derivatives according to the method of the invention.
[0052] The slag from the smelting step preferably may be further processed, such as by fuming, to produce a slag that poses fewer concerns for landfill and / or use in higher value end uses, as further described herein.
[0053] Preferably, after having been separated from the smelting slag formed in the smelting step, the concentrated copper intermediate may be further processed, for example by refining, to produce a more concentrated refined copper product which becomes suitable for higher value end uses, optionally by casting copper anodes as electrolysis feedstock which may ultimately produce high purity copper cathodes which meet many, if not all, current industry standards for more demanding copper end uses.
[0054] Further processing of the concentrated copper intermediate and / or the slag from the smelting step may produce other valuable by-products of refined copper products.
[0055] Such valuable by-products may be, for example, a crude solder stream, which may be obtained from a copper refining slag, which may come from the refining of a concentrated copper intermediate. Such crude solder may be further refined and / or conditioned, i.e., cleaned by removing elements that may affect downstream processing and / or impair or prevent a specific application of the final product obtained from the solder stream. Such valuable by-products may, for example, include at least one product belonging to the list consisting of a soft lead product, a hard lead product, a silver-rich anode mud product, and a high-grade tin product, as further explained herein.
[0056] Applicants believe that the beneficial effects brought about by the present invention do extend to the production of derivatives of the products of the smelting step as listed above. The advantage brought about by the improved stability and reliability of the smelting step is that the downstream processes producing these derivatives are guaranteed a more stable and reliable feed flow from the smelting step, which makes their own operation more stable and reliable. This allows the production of final products with more stable and reliable quality. It also reduces the process monitoring burden and / or operator attention and increases the possibility of electronic monitoring and control of each step in these processes and the entire process. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 A process flow sheet is shown which includes the method according to the present invention as part of an overall process for recovering non-ferrous metals from a secondary feedstock. DETAILED DESCRIPTION
[0058] Below, the present invention will be described in the specific embodiments and possibly with reference to specific drawings, but the present invention is not limited thereto, but only by the claims. Any of the drawings are only schematic and non-restrictive. In the drawings, for the purpose of illustration, the size of some elements may be exaggerated and not drawn to scale. The sizes and relative sizes in the drawings do not necessarily correspond to the actual abbreviations in the practice of the present invention.
[0059] In addition, the terms "first", "second", "third", etc. in the specification and claims are used to distinguish similar elements and do not necessarily indicate a sequential or chronological order. These terms are interchangeable under appropriate circumstances, and embodiments of the present invention may operate in other sequences than those described and / or illustrated herein.
[0060] Furthermore, the terms top, bottom, over, under, etc. in the specification and claims are used for descriptive purposes and not necessarily for describing relative positions. The terms so used are interchangeable under appropriate circumstances, and the embodiments of the invention described herein can operate in other orientations than described or illustrated herein.
[0061] As used in the claims, the term "comprising" should not be considered to be limited to the elements listed with the term in this article. The presence of other elements or steps is not excluded. It should be regarded as providing the presence of these features, integers, steps or components as required, but does not exclude the presence or addition of one or more other features, integers, steps or components or groups thereof. Therefore, the number of "articles including devices A and B" is not limited to objects consisting only of reagents A and B. This means that A and B are only elements related to the subject matter related to the present invention. Accordingly, the terms "including" or "embedded" also include the more restrictive terms "essentially consisting of..." and "consisting of...". Therefore, by replacing "comprise, include" with "consisting of...", these terms represent the basis of preferred but narrower embodiments, which are also provided as part of the content of this document related to the present invention.
[0062] Unless otherwise indicated, all ranges provided herein are inclusive up to and including the given endpoints, and values for compositions or components are expressed as weight percent or wt% of each component in the composition.
[0063] As used herein, "weight percent", "wt-%", "percent weight", "% weight", "ppm wt", "ppm weight", "ppm by weight", or "ppm" and variations thereof refer to the concentration of a substance, i.e., the weight of the substance divided by the total weight of the composition, and multiplied by 100 or 1,000,000 (as applicable), unless otherwise indicated. It should be understood that as used herein, "percent", "%" is intended to be synonymous with "weight percent", "wt-%", etc.
[0064] It should be noted that, as used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the content clearly dictates otherwise. Thus, for example, reference to a composition containing "a compound" includes compositions containing two or more compounds. It should also be noted that the term "or" is generally used in its sense including "and / or" unless the content clearly dictates otherwise.
[0065] Additionally, each compound used herein may be described interchangeably as its chemical formula, chemical name, abbreviation, etc.
[0066] Metals and compounds that are at most as inert as iron or zinc are those that have an affinity for oxygen at least the same as or even higher than that of iron or zinc under furnace conditions, and even higher than that of copper, nickel, tin and lead. This definition relates to "iron or zinc" because the relative positions of zinc and iron in terms of their affinity for oxygen under furnace conditions are very close and can even change depending on the furnace conditions. Therefore, in order to make this definition correct and comprehensive, it is necessary to mention both metals at the same time. Under furnace conditions, these selected metals or compounds very easily participate in the oxidation side of the redox reactions that are part of the present invention. Suitable metals are, for example, elemental zinc and iron themselves, aluminum, silicon and calcium. Suitable compounds can be, for example, metal silicides, preferably silicides of already suitable metals, such as iron silicide (FeSi), but bimetallic or polymetallic compounds can also be suitable, including mixtures, such as SnAl, CuFe, FeSn or alloys such as brass (ZnCu). Suitable compounds may also be metal sulfides, for example FeS, ZnS and / or sulfides of other metals, where the sulfide or the metal is at most as inert as iron or zinc.
[0067] Metals and compounds that are more noble than copper are compounds that have a lower affinity for oxygen than copper under furnace conditions. These raw materials participate very readily on the reduction side of the redox reaction that is part of the present invention and result in the release of the corresponding metal in its elemental form. Suitable examples are, for example, silver, gold, other noble metals including platinum group metals, alloys and mixtures thereof, including those containing other metals.
[0068] In the context of the present invention, the terms "smelting", "to be smelted", "melting" or similar variations of "melting" denote a process that includes more than just a change of the state of matter of the compounds from solid to liquid. In pyrometallurgy, the smelting step takes place with several chemical processes that transform specific chemical substances into other chemical substances. Important among these transformations can be oxidation reactions that may be accompanied by the formation of oxides, or reduction reactions, by which the oxidation state of some atoms changes. In this document, the terms "furnace", "smelting furnace" and "melting furnace" are used interchangeably, and all of these terms refer to the furnace in which this process step takes place.
[0069] In the context of the present invention, the term "scum" or "dregs" refers to a generally pasty material that is formed as a result of an operating step and that separates from a different liquid phase, usually under the action of gravity, and usually floats to the top. The scum or dregs can usually be skimmed or removed from the underlying liquid.
[0070] The term "solder" in the context of the present invention means a metallic composition rich in tin and / or lead, but may also contain other metals. Solder is characterized by a relatively low melting temperature, which makes the composition suitable for forming a metallic connection between two other metal parts, the so-called "soldering", once cooled after being heated to a relatively limited temperature.
[0071] In this article, unless otherwise stated, the amount of metal and oxide is represented according to typical practice in pyrometallurgy. Whether the metal is present in its elemental form (oxidation state = 0) or in any chemically bonded form that is usually an oxidized form (oxidation state> 0), the presence of each metal is usually represented as its total presence. For metals that may be relatively easily reduced to their elemental form and may appear as molten metals in pyrometallurgical processes, their presence is usually represented in their elemental metal form, even when the composition of slag is given, most of these metals may actually exist in an oxidized form. Therefore, the composition of slag (such as the slag obtained according to the method of the present invention) defines the content of Fe, Zn, Pb, Cu, Sb, Bi as elemental metals. Under non-ferrous pyrometallurgical conditions, less inert metals are more difficult to reduce and mainly appear in an oxidized form. These metals are usually represented as their most common oxide forms. Therefore, the slag composition usually gives the content of Si, Ca, Al, Na, which are respectively represented as SiO2, CaO, Al2O3, Na2O.
[0072] Metallurgical slag is usually not a pure substance, but a mixture of many different components. Therefore, metallurgical slag does not have a clear melting temperature. In the prior art, the term "liquidus temperature" is usually used, that is, the temperature at which the slag is completely liquefied.
[0073] In an embodiment of the method according to the present invention, the feedstock further comprises at least one second metal selected from the group consisting of nickel, tin and lead. Raw materials comprising at least one second metal selected from this list are of great interest for recovering copper therefrom, but the presence of the second metal may cause additional burdens or difficulties compared to raw materials not comprising the second metal. The applicant has found that the smelting step is a very suitable process step for introducing raw materials comprising at least one such second metal. The applicant has found that the at least one second metal may also be present in the feedstock in the form of its oxide or in another form of a metal that can participate in a redox reaction under furnace conditions and release its elemental form. In this context, the applicant prefers the oxide form because of its higher availability under favorable conditions, because of the heat of reaction generated by the redox reaction in which it participates, and because it contributes oxygen to the furnace, which reduces the amount of oxygen that needs to be injected. The reduction in the amount of oxygen injected also reduces the gas flow through the smelting step, which is beneficial because the reaction rate is not limited by the external oxygen supply rate, but only by the reaction kinetics. Less gas input also means that there are fewer furnace exhaust gases to be treated, and there is less solid mist entrainment therein.
[0074] In one embodiment of the method according to the present invention, wherein the feedstock comprises at least one second metal, the concentrated copper intermediate further comprises at least one second metal. The applicant has found that the smelting step can be operated so that: by ao driving the redox reaction in the smelting furnace to an appropriate degree, most of the second metal can also be most easily recovered as part of the concentrated copper intermediate. The applicant has found that this feature brings the advantage that the at least one second metal can also be further recovered downstream as part of the desired high quality main product.
[0075] In one embodiment of the method according to the invention, the feedstock comprises scrap iron, scrap silicon, scrap zinc and / or scrap aluminum, more preferably scrap iron. The applicant has found that such waste can be easily dosed accurately enough by mixing an appropriate amount of scrap with other raw materials as part of a feed batch. The applicant can also add such waste to the furnace as an additional raw material stream. The applicant has found that waste such as scrap iron and scrap aluminum, but also to some extent scrap silicon, can be easily obtained in appropriate quantities and under economically favorable conditions. The applicant has also found that adding the waste separately to the furnace as an additional raw material feed stream, preferably scrap iron, provides the advantage of being able to very conveniently control and maintain an excess of iron in elemental form and / or metals and / or compounds that are at most as inert as iron or zinc under furnace conditions.
[0076] In one embodiment of the method according to the invention, the method further comprises the step of at least partially removing the smelting slag from the furnace. The applicant prefers to remove at least part of the smelting slag from the furnace before starting a subsequent feeding batch. If the feed provided at the time of a new feeding batch comprises a relatively fine portion, the applicant prefers to keep a layer of slag in the furnace, because this layer provides a suitable cover layer, under which the fine portion of the feed or the feed comprising a relatively fine portion can be introduced without generating an excessive risk of fine feed particles being entrained by the furnace exhaust gas and forming an additional burden and / or interference with the furnace exhaust gas treatment system. If the available feed comprises a relatively coarse portion, the applicant prefers to remove substantially all of the formed slag from the furnace before starting a subsequent feeding batch. This brings the advantage that more furnace volume can be provided for subsequent feeding batches, and thus facilitates the throughput and / or productivity of the smelting furnace. The applicant has found that the step of removing slag from the furnace can be performed several times in the same furnace feeding batch.
[0077] In one embodiment of the method according to the invention, the method comprises a step of removing at least part, preferably most of the concentrated copper intermediate from the furnace. The applicant prefers to ensure the proper physical presence of molten metal in the furnace when starting a subsequent feed batch or a campaign comprising a series of feed batches. This molten metal is then readily available as a hot liquid at the start of a new feed batch or the entire campaign for receiving and wetting solid feed and possibly additional amounts of iron in elemental form and metals or compounds that are at most as inert as iron or zinc under furnace conditions, which are required or necessary for easily producing and / or maintaining an excess of these additives in the method according to the invention. The iron dissolved in this molten metal reacts easily with oxygen injected into the liquid bath, thereby immediately generating heat of reaction. Another advantage is that the solid iron that can be added to the furnace at the start of a new feed batch is still floating on the molten metal phase, which is the exact position that can fully promote the redox reaction expected in the method. The applicant has found that keeping a portion of the concentrated copper intermediate in the furnace when starting a new furnace charge batch significantly reduces the time before the furnace is again operating at high capacity as part of the next charge batch and thus brings about a significant increase in the productivity of the smelting step. The applicant prefers to remove a portion of the molten metal formed during the previous charge batch before starting a new furnace charge batch. The applicant has found that the step of removing a portion of the concentrated copper intermediate from the furnace can even be performed several times during the same furnace charge batch.
[0078] The applicant prefers to operate the smelting step in an almost semi-continuous mode as far as possible, in which suitable materials can be continuously added to the furnace until the available furnace volume is fully utilized. When the slag and metal phases have reached the desired quality, first at least most of the slag can be removed from the furnace, for example by tilting the furnace to overflow from the feed port, and if all the slag has been removed, then most of the liquid molten metal phase can also be removed in the same way, or through a "bottom discharge hole" appropriately located in the furnace wall. For the above reasons, when the next feed batch is introduced into the smelting furnace, a suitable part of the molten metal is preferably retained in the furnace. The applicant has found that this operation can last for a long time and may only have to be interrupted or stopped due to external reasons or when it is considered necessary to perform maintenance intervention on the smelting furnace. The applicant has found that this operation can be further improved by preparing batches of suitable pre-mixed feed materials according to the composition and size of the solids in the feed batch. The applicant has found that this can bring the advantage of a more stable operation in terms of the timing of the step sequence and the quality of the concentrated copper intermediate removed from the furnace as the main product each time.
[0079] In one embodiment of the method according to the present invention, the iron and at most the same inert compound as iron or zinc introduced with the feed include solid iron, solid silicon, solid zinc and / or solid aluminum, preferably including copper-containing / iron-containing waste, silicon-containing waste, zinc-containing waste and / or aluminum-containing waste. The applicant has found that the sources of these iron, silicon, zinc and aluminum can be easily obtained from various sources. In addition, they can contain a small amount of other metals, which can be recyclable and worth recovering in the smelting step and the downstream of the smelting step in its elemental form. Such other metals can include tin, lead and nickel. They can also include trace amounts of more inert metals or even precious metals (PMs), such as silver or gold, or even platinum group metals (PGMs), such as ruthenium, rhodium, osmium, palladium, iridium and platinum itself, wherein a very small amount can also be worth recovering because of their scarcity and high economic value.
[0080] In one embodiment of the method according to the invention, the feed material is at least partly solid, wherein the solid feed material is fed gradually, preferably continuously, into the furnace, preferably in a large part of the smelting feed batch, more preferably in a large part of the entire smelting campaign, preferably by means of at least one conveyor belt and / or a rocking conveyor. As explained elsewhere herein, the applicant prefers to feed a portion of the coarse fraction of the available feed material in the early stages of the furnace feed batch and / or campaign, until a layer of metallurgical slag of suitable thickness is formed as a covering layer on the molten metal phase in the furnace. If this layer of slag is present from the beginning of the feed batch or once this layer of slag is formed on the coarse fraction of the available feed material by running the furnace, the applicant prefers to also introduce a certain amount of the fine fraction of the available feed material into the furnace, and the applicant prefers to pneumatically introduce this fine fraction by means of a lance immersed in the liquid molten bath and release this fine fraction at the interface between the molten metal phase and the upper molten slag phase, because this brings the advantage of a reduced risk of fine feed particles being lost with the furnace exhaust gases.
[0081] In one embodiment of the method according to the invention, the input rate of the feedstock is maintained below the rate at which the heat generation will be insufficient to melt the solid feedstock and / or to bring the feedstock to the desired furnace temperature. The applicant prefers to avoid as much as possible the risk that the enthalpy balance of the furnace becomes insufficient because the heat generated is insufficient to heat and melt the feedstock being introduced, in which case there is a risk that the temperature in the furnace will drop. The applicant has found that it is advantageous to control the input rate of the raw materials, for example, so that iron can be added at a sufficient rate that a sufficiently high excess of iron in elemental form and of metals and compounds that are at most as inert as iron or zinc under the furnace conditions is maintained, combined with a sufficient oxygen input, to be able to generate sufficient reaction heat to achieve rapid heating and melting of the introduced feedstock.
[0082] In one embodiment of the method according to the invention, at least a portion of the feedstock is in the form of a finely divided portion, and the finely divided feedstock portion has an average particle size of at most 10 mm, preferably, the finely divided feedstock portion material has an average particle size of at most 3.36 mm. The applicant has found that finely divided raw materials including copper and other metals of interest in the method according to the invention are generally difficult to process in other processes, so the raw materials can be found in large quantities under economically attractive conditions. The applicant has found that in the method according to the invention, such materials can be easily and perfectly processed. The applicant tends to introduce such finely divided feedstock portions into the furnace only when there is already a continuous molten slag layer floating on top of the molten metal phase below in the furnace. The applicant tends to introduce the finely divided feedstock portion at the interface between the molten metal and the molten slag, so that the slag layer can act as a covering layer that can capture any small particles before they reach the furnace gas phase and have the risk of being entrained by the exhaust gas and not participating in the process in the furnace.
[0083] In one embodiment of the method according to the invention, in which the feed comprises a finely divided feed fraction, the finely divided feed fraction material is pneumatically conveyed and injected into the furnace. The applicant has found that this is a very convenient method for introducing such a finely divided feed fraction and that the method provides the possibility of introducing the fraction in the most favourable position, i.e. close to a position above the interface between liquid metal and liquid slag, where any elemental iron present (such as scrap iron) also typically floats and where most chemical reactions take place.
[0084] In one embodiment of the method according to the invention, in which the feed comprises a finely divided feedstock fraction, the finely divided feedstock fraction material is injected into the liquid slag phase and above the metal phase of the liquid molten bath. Applicants have found that the slag phase is close to the interface between the liquid metal and the liquid slag and any elemental iron present (such as scrap iron) also typically floats at this location. Most of the chemical reactions take place at this location and most of the heat of reaction is also generated at this location.
[0085] In one embodiment of the method according to the invention, wherein the feed comprises a finely divided feed fraction, the average composition of the finely divided feed fraction of the feed in the entire smelting feed batch in the furnace after heating to 1150° C. satisfies at least one, preferably all, of the following conditions:
[0086] comprising at least 5 wt% of total metals, preferably at least 5 wt% of total metals copper, nickel, tin, lead and zinc, preferably at least 6 wt%, more preferably at least 7 wt%, even more preferably at least 8 wt%, preferably at least 9 wt%, more preferably at least 10 wt% of total metals, preferably total metals copper, nickel, tin, lead and zinc,
[0087] Comprising up to 70.0wt% copper (Cu), preferably up to 65.0wt%, more preferably up to 60.0wt%, even more preferably up to 55.0wt%, still more preferably up to 50wt%, preferably up to 48wt% copper, and optionally at least 10wt% copper, preferably at least 15wt%, more preferably at least 20wt%, even more preferably at least 25wt%, still more preferably at least 30wt%, preferably at least 35wt%, more preferably at least 40wt%, even more preferably at least 42.0wt% copper.
[0088] comprising at most 2.00 wt% nickel (Ni), preferably at most 1.50 wt%, more preferably at most 1.00 wt% nickel,
[0089] The invention comprises at least 0.50 wt% and at most 10.00 wt% lead (Pb), preferably at least 1.00 wt%, more preferably at least 1.50 wt%, and optionally at most 9.00 wt%, preferably at most 8.00 wt% lead, and at most 15.00 wt% tin, preferably at most 14.00 wt%, more preferably at most
[0090] 13.00 wt%, even more preferably up to 12.00 wt% tin.
[0091] The composition comprises at most 2.00 wt% antimony (Sb), preferably at most 1.50 wt%, more preferably at most
[0092] 1.00wt% antimony,
[0093] comprising at most 7.0 wt% iron (Fe), preferably at most 6.0 wt%, more preferably at most 5.0 wt%, even more preferably at most 4.0 wt%, still more preferably at most 3.50 wt% iron, and
[0094] The present invention comprises at most 55 wt% zinc (Zn), preferably at most 50 wt%, more preferably at most 45 wt%, even more preferably at most 43 wt%, even more preferably at most 40 wt%, still more preferably at most
[0095] 35.0 wt% zinc.
[0096] The Applicant has found that the described finely divided feedstock fraction is very suitable for the process according to the invention due to the presence of metals of interest recovered in high quality products downstream of the process and / or due to the presence of metals that may bring about reaction heat as part of the process according to the invention, while at the same time the content of these metals in the finely divided feedstock fraction is sufficiently low that this fraction is not of sufficient economic interest for other processes for recovering metals from primary and / or secondary raw materials, so that this feedstock can be found under economically attractive conditions, which feedstock provides a significant improvement when processed in the process according to the invention. Compliance with the upper limit of the sulfur content as part of one of the conditions in the above list further avoids the formation of a separate copper matte phase and thus clearly distinguishes the process according to the invention comprising this feature from copper smelting processes in which a copper matte phase is formed as one of the products or intermediates.
[0097] In one embodiment of the method according to the invention, the feedstock comprises at least one material returned from the treatment of the molten liquid metal phase and / or the liquid slag phase formed by the method. The applicant has found that the smelting step is a very convenient step for returning by-products that can be formed by further treatment of the molten liquid metal phase and / or the liquid slag phase formed in the smelting step. Such further treatment can be carried out in the same furnace after the smelting step, but is preferably carried out downstream of the smelting step and in a different device. An embodiment of such downstream treatment will be further explained below.
[0098] In one embodiment of the method according to the present invention, wherein the feedstock comprises at least one return material, the at least one return material comprises at least one material selected from spent anodes or other products containing copper, tin and / or lead, metal oxides or sulphides, preferably metal oxides or sulphides of copper, nickel, tin, lead and / or zinc, the at least one material comprising dross containing metals in the form of oxides or sulphides formed and removed from downstream processing steps, metal silicides, preferably silicides of metals selected from the group consisting of copper, zinc, nickel, iron, lead and tin, and crusts or other solids formed along the walls of a crucible or ladle used to transfer molten metal and / or molten slag removed from the furnace. Applicants have found that the smelting step is a very suitable process location for returning by-products which are rather difficult to define in terms of what they contain, such as some of the materials in the above list, or by-products which may contain various metals of interest, such as zinc oxide dust which may be collected by filtering the exhaust gases of furnaces performing various pyrometallurgical process steps, or furnace slag containing recoverable metals, where the content of these recoverable metals burdens or prevents more common exports and / or requires the addition of additional channels through the overall metal recovery process.
[0099] In one embodiment of the method according to the invention, the feedstock is introduced centrally into the liquid bath in the furnace. This has the advantage that the solid feedstock, due to the buoyancy it experiences, when immersed in the molten metal phase, generally floats on top of the molten metal phase without coming into contact with the refractory lining in the furnace. This reduces the wear that the solid feedstock may cause to the refractory lining, thereby increasing the life of the refractory lining and extending the time between two maintenance interventions to repair the refractory lining.
[0100] In one embodiment of the method according to the invention, the feed comprises a coarse feed fraction, the coarse feed fraction preferably having an average particle size of at least 5 mm, preferably at least 10 mm, even more preferably at least 15 mm, and the average composition of the coarse feed fraction of the feed in the entire smelting feed batch in the furnace after heating to 1150° C. meets at least one of the following conditions, and preferably meets all of the conditions:
[0101] comprising at least 20 wt% of total metals, preferably at least 20 wt% of total metals copper, nickel, tin, lead and zinc, preferably at least 30 wt%, more preferably at least 40 wt%, even more preferably at least 50 wt%, preferably at least 60 wt%, more preferably at least 70 wt%, and optionally up to 95 wt% of total metals, preferably total metals copper, nickel, tin, lead and zinc,
[0102] comprising at least 10.0 wt% and at most 70.0 wt% copper (Cu), preferably at least 15.0 wt%, more preferably at least 17.0 wt%, even more preferably at least 18.0 wt%, still more preferably at least 19.0 wt%, and optionally at most 65.0 wt%, preferably at most 60.0 wt%, more preferably at most 55.0 wt%, even more preferably at most 50.0 wt%, yet more preferably at most 45.0 wt% copper,
[0103] comprising at least 0.50 wt% and at most 2.00 wt% nickel (Ni), preferably at least 0.60 wt%, more preferably at least 0.70 wt%, even more preferably at least 0.80 wt%, still more preferably at least 0.90 wt%, and optionally at most 1.90 wt%, preferably at most 1.80 wt%, more preferably at most 1.70 wt%, even more preferably at most 1.60 wt%, yet more preferably at most 1.50 wt% nickel,
[0104] comprising at least 1.00 wt% and at most 8.00 wt% lead (Pb), preferably at least 1.10 wt%, more preferably at least 1.25 wt%, even more preferably at least 1.50 wt%, still more preferably at least 1.60 wt%, and optionally at most 7.50 wt%, preferably at most 7.00 wt%, more preferably at most 6.50 wt%, even more preferably at most 6.00 wt%, and yet more preferably at most 5.50 wt% lead,
[0105] comprising at least 0.50 wt% and at most 2.50 wt% tin (Sn), preferably at least 0.60 wt%, more preferably at least 0.70 wt%, even more preferably at least 1.00 wt%, still more preferably at least 1.20 wt%, and optionally at most 2.40 wt%, preferably at most 2.30 wt%, more preferably at most 2.20 wt%, even more preferably at most 2.00 wt%, yet more preferably at most 1.90 wt% Sn,
[0106] comprising at most 0.10 wt% antimony (Sb), preferably at most 0.08 wt%, more preferably at most 0.06 wt% antimony,
[0107] comprising at least 10.0 wt% and at most 35.00 wt% iron (Fe), preferably at least 11.0 wt%, more preferably at least 12.0 wt%, even more preferably at least 13.0 wt%, still more preferably at least 14.0 wt%, and optionally at most 34.5 wt%, preferably at most 34.0 wt%, more preferably at most 33.0 wt%, even more preferably at most 32.0 wt%, yet more preferably at most 31.0 wt% iron, and
[0108] comprising at least 2.00 wt% and at most 15.00 wt% of zinc (Zn), preferably at least 2.50 wt%, more preferably at least 3.00 wt%, even more preferably at least 3.50 wt%, still more preferably at least 4.00 wt%,
[0109] and optionally at most 14.00 wt%, preferably at most 12.00 wt%, more preferably at most 11.00 wt%,
[0110] Even more preferred is up to 10.00 wt%, still more preferred up to 9.00 wt% zinc.
[0111] The applicant has found that the coarse feed fraction is very suitable as feed for the method according to the invention. The fraction comprises a sufficient amount of the metals of interest to make the fraction interesting as a whole, but the content of valuable metals is not high enough to make the coarse feed fraction the object of interest of other methods for recovering some of the metals. The applicant has found that the coarse feed fraction is not sufficiently rich in copper and / or tin plus lead to make it a suitable feed for fire refining of copper, as described, for example, in WO 2019 / 115533A1. Compliance with the upper limit of the sulfur content as part of one of the conditions in the above list further helps to avoid the formation of a separate copper matte phase and therefore clearly distinguishes the method according to the invention including this feature from copper smelting methods in which a copper matte phase is formed as one of the products or intermediates.
[0112] Applicants have also found that relatively low levels of sulphur can be readily accepted in the coarse fraction of the feedstock. This has the advantage that a wider selection of raw materials can be accepted in the smelting step, including raw materials that are unacceptable or less desirable in other processes for processing such raw materials.
[0113] In one embodiment of the method according to the invention, the content of iron and / or metals and compounds as inert as iron or zinc dissolved in the molten metal in the furnace is maintained at at least 1.0 wt%, preferably at least 1.5 wt%, wherein the concentration of the metals and compounds as inert as iron or zinc is converted to an equivalent iron concentration, wherein the equivalent iron concentration is an iron concentration that can contribute the same amount of reaction heat as the metal or compound as inert as iron or zinc when reacting with oxygen under furnace conditions. The applicant has found that compliance with this condition is very convenient for monitoring and maintenance, and it is easy to ensure that the iron in elemental form and the metal or compound as inert as iron or zinc under furnace conditions are sufficiently excessive. Compliance with this condition also ensures that there is always a sufficient excess of iron and / or metals or compounds as inert as iron or zinc in the furnace, so that the temperature in the furnace can be easily maintained under sufficient oxygen injection. Another advantage is that this condition ensures protection of the tuyere by solid iron and / or iron oxides described elsewhere herein.
[0114] In one embodiment of the method according to the invention, the content of iron and / or metals and compounds that are at most as inert as iron or zinc at furnace conditions dissolved in the molten metal in the furnace is maintained at at most 10.0 wt%, preferably at most 9.0 wt%, more preferably at most 8.0 wt%, even more preferably at most 7.0 wt%, still more preferably at most 6.0 wt%, preferably at most 5.0 wt%, more preferably at most 4.0 wt%, even more preferably at most 3.5 wt%, yet more preferably at most 3.0 wt%, preferably at most 2.5 wt%, wherein the concentration of metals and compounds that are at most as inert as iron or zinc is converted into an equivalent iron concentration, wherein the equivalent iron concentration is the iron concentration that is able to contribute the same amount of reaction heat as the metal or compound that is at most as inert as iron or zinc when reacting with oxygen at furnace conditions. Compliance with this condition reduces the risk of iron coming out of solution at cooler locations in the furnace, for example against the furnace walls, in which case it may reduce the available furnace volume and impair the stirring of the liquid bath in the furnace.
[0115] In one embodiment of the process according to the invention, elemental iron is introduced into the smelting step at a rate at which excess iron in the process, exceeding its solubility in the molten metal bath under furnace conditions, is retained in the smelting bath. Applicants have found that this is a very convenient method for providing sufficient iron in the furnace to ensure the required excess iron.
[0116] In one embodiment of the method according to the invention, the amount of excess iron present in the furnace is maintained by at least periodically sampling the molten metal phase in the furnace and analyzing the samples for iron. Preferably, the amount of excess iron is limited to keep the amount of solid iron parts freely moving in the liquid bath of the furnace limited to limit the damage, wear and tear that these free-floating parts may cause to the refractory lining in the furnace.
[0117] In one embodiment of the method according to the invention, the combustible source of carbon and / or hydrogen is selected from the group consisting of coke, charcoal, carbon black, hydrocarbons, natural gas, methane, ethane, propane, butane, hydrocarbons that are liquid under standard conditions, hydrocarbon-containing polymers, plastics, waste plastics, grease, oil, paint, varnish, rubber, preferably wastes thereof and combinations thereof. The applicant has found that a wide range of sources are suitable, some of which are very readily available under very attractive conditions of supply.
[0118] In one embodiment of the method according to the invention, the amount of combustible sources of carbon and / or hydrogen is kept below a level at which slag foaming would impair the operation of the smelting step, preferably significantly below that level, so that the risk of slag foaming is also kept at an acceptably low level. The applicant has found that the acceptable upper limit depends on the combustible source selected, but can be easily determined by repeated trials. Another benefit of observing this precaution is that the temperature of the furnace off-gas and the carbon monoxide content in the off-gas are kept within acceptable ranges. Alternatively, the amount of combustible sources of carbon and / or hydrogen is limited to a level below which the temperature of the furnace off-gas is kept at an acceptably low temperature, or to a level below which the carbon monoxide content of the off-gas is kept at an acceptably low content.
[0119] In one embodiment of the method according to the invention, at least a portion of the oxygen-containing gas is introduced into the upper slag phase, preferably as close as possible to the interface between the metal phase and the upper slag phase. The applicant prefers to introduce at least a portion of the oxygen-containing gas at the target location where oxygen is most easily consumed by oxidizing elemental metals such as iron dissolved in the metal phase and from which the oxides formed by the oxidation reaction can easily move to the upper slag phase with a minimum diffusion distance for coverage.
[0120] In one embodiment of the method according to the invention, at least part of the oxygen-containing gas is introduced through at least one metal lance, the tip of which is immersed in the liquid slag phase. The applicant has found that this is a very convenient way to introduce the oxygen-containing gas at the target location. The lance can be introduced through a dedicated opening in the furnace wall or can be introduced through a filling port of the furnace, through which the feed material can also be introduced.
[0121] In one embodiment of the method according to the invention using at least one metal lance, the gas injected by the metal lance comprises at least 30 vol% oxygen, preferably at least 40 vol%, more preferably at least 50 vol%, still more preferably at least 75 vol%, and even more preferably the gas is high purity oxygen. This has the advantage of reducing and preferably avoiding the generation of additional furnace exhaust gas compared to using air as the oxygen-containing gas. As a result, the exhaust gas treatment system can become smaller or can be operated more efficiently. Another advantage is that the furnace exhaust gas contains less nitrogen oxides and is therefore more environmentally acceptable.
[0122] In one embodiment of the method according to the invention using at least one metal lance, the gas flow through the metal lance provides sufficient cooling to avoid corrosion and / or melting of the lance under the conditions of immersion in a liquid bath of molten slag. The applicant prefers to introduce the gas lance into the furnace from above the liquid bath and immerse the lance only in the upper slag phase without immersing the lance as far as the molten metal bath. The applicant has observed that the lance can remain exposed to the hot slag phase for a long time, but will quickly dissolve in the underlying molten metal phase, because the gas flowing through the lance has a sufficient cooling effect as specified.
[0123] In one embodiment of the method according to the invention, at least part of the oxygen-containing gas is introduced into the bottom of the furnace through at least one tuyeres, preferably a plurality of tuyeres, more preferably the plurality of tuyeres are evenly distributed in the bottom of the furnace. This brings the advantage of highly agitating the liquid bath in the furnace.
[0124] In one embodiment of the method according to the invention using tuyere, the gas introduced through at least one tuyere is an oxygen-containing gas comprising at most 50 vol% oxygen, preferably at most 40 vol%, more preferably at most 30 vol%, even more preferably at most 25 vol%, still more preferably the gas introduced through the tuyere is air. The gas needs to overcome the hydrostatic pressure exerted by the height of the liquid furnace contents. Therefore, the gas needs to be compressed in order to be able to be introduced through the tuyere. If the gas comprises air, the air is compressed before introduction.
[0125] In one embodiment of the method according to the invention using tuyere, the gas introduced through at least one tuyere is cooler than the molten liquid metal phase surrounding the tuyere. Thereby, the molten liquid metal phase around the tuyere is cooled, its solubility for iron is thus reduced, and when the molten liquid metal phase reaches iron saturation at a higher temperature, iron and / or iron-containing compounds such as iron oxides precipitate and form deposits around the tuyere, typically in the form of hollow mushrooms, which provides good protection of the tuyere from corrosion caused by the high heat of oxidation of the iron close to the tuyere.
[0126] In one embodiment of the method according to the invention, the smelting slag produced by the method comprises at least 20 wt% iron (Fe), preferably at least 22.5 wt%, more preferably at least 25.0 wt%, even more preferably at least 27.50 wt%, still more preferably at least 30.00 wt% iron. Herein, the iron content is the total amount of iron present in all its valence states, thus the total amount of all iron present as elemental iron and in chemically bound form (usually in the form of oxides). This brings the advantage of blast furnace slag fluidity, i.e. lower viscosity at the same temperature.
[0127] In one embodiment of the method according to the present invention, the composition of the produced smelting slag meets at least one of the following conditions, preferably meets all of the following conditions:
[0128] The invention relates to an alloy of at most 1.00 wt% copper (Cu), preferably at most 0.90 wt%, more preferably at most 0.80 wt%, even more preferably at most 0.70 wt%, still more preferably at most 0.60 wt% copper, at most 0.20 wt% nickel (Ni), preferably at most 0.17 wt%, more preferably at most 0.15 wt%, even more preferably at most 0.12 wt%, still more preferably at most 0.10 wt% nickel, at most 2.00 wt% lead (Pb), preferably at most 1.50 wt%, more preferably at most
[0129] 1.00 wt %, even more preferably at most 0.95 wt %, still more preferably at most 0.90 wt % of lead, containing at most 1.00 wt % of tin (Sn), preferably at most 0.80 wt %, more preferably at most 0.60 wt %, even more preferably at most 0.40 wt %, still more preferably at most 0.25 wt % of Sn, containing at most 22.50 wt % of zinc (Zn), preferably at most 20.00 wt %, more preferably at most
[0130] 17.50 wt%, even more preferably at most 15.00 wt%, still more preferably at most 12.50 wt% zinc.
[0131] Compliance with the upper limits of copper, nickel, tin and lead regulations brings the advantage of low losses of valuable metals in the process.The present invention relates to a process for recovering copper which brings the advantage of high copper recovery from available raw materials due to limiting the loss of copper in the smelting slag.
[0132] Applicants have found that many copper-containing raw materials, and particularly secondary materials within such materials, also contain mainly significant amounts of tin, but may also contain lead, nickel and zinc. Applicants have found that most of these metals, with the exception of copper, can be recovered from the same raw materials by pyrometallurgical process steps, provided that these metals are not allowed to be lost in the smelting slag. Observing upper limits for the other metals, primarily for tin and nickel, but also for lead and, to some extent, also for zinc, brings the benefit of recovering these metals at high recovery rates from the available raw materials.
[0133] The presence of zinc in the smelting slag may be allowed to be higher if an additional slag fuming step is provided, in which the smelting slag is fumed to reduce its zinc content, and optionally also its lead content. The applicant prefers to add such an additional fuming step to remove more zinc from the smelting slag, preferably also further remove trace amounts of lead, preferably as described in WO 2016 / 156394 A1.
[0134] The applicant has discovered that the above-mentioned characteristics of low valuable metal loss rate in the smelting furnace slag can be controlled and obtained by appropriate operation of the smelting step, which involves the furnace temperature, furnace stirring and oxygen, the addition of reducing agents and their selection, and flux materials (or also called slag forming agents) and their selection.
[0135] In one embodiment of the method according to the invention, the composition of the concentrated copper intermediate as the main product from the smelting step meets at least one of the following conditions, preferably all of the conditions:
[0136] comprising at least 50.0wt% copper (Cu), preferably at least 55.0wt%, more preferably at least 60.0wt%, even more preferably at least 65.0wt%, still more preferably at least 70wt%, preferably at least 72.5wt%, more preferably at least 75.0wt%, even more preferably at least 77.0wt%, still preferably at least 78wt% or even 79.0wt% copper (Cu), and optionally at most 97.0wt%, preferably at most 95wt%, more preferably at most 90.0wt%, even more preferably at most 85wt%, still more preferably at most 82.0wt%, preferably at most 80wt%, more preferably at most 79.0wt%, even more preferably at most 78.0wt%, still preferably at most 77.0wt% copper (Cu),
[0137] comprising at least 0.01 wt% nickel (Ni), preferably at least 0.05 wt%, more preferably at least 0.10 wt%, even more preferably at least 0.50 wt%, still more preferably at least 1.00 wt%, preferably at least 1.10 wt%, more preferably at least 1.25 wt%, even more preferably at least 1.40 wt%, still more preferably at least 1.50 wt% or even 1.70 wt% nickel (Ni), and optionally at most 15.00 wt%, preferably at most 12.50 wt%, more preferably at most 10.00 wt%, more preferably at most 7.50 wt%, still more preferably at most 5.00 wt%, preferably at most 4.00 wt%, more preferably at most 3.00 wt%, even more preferably at most 2.50 wt%, still preferably at most 2.40 wt% nickel (Ni),
[0138] comprising at least 0.10 wt% lead (Pb), preferably at least 0.50 wt%, more preferably at least 1.00 wt%, even more preferably at least 2.00 wt%, still more preferably at least 3.00 wt%, preferably at least 3.50 wt%, more preferably at least 4.00 wt%, even more preferably at least 4.50 wt%, still preferably at least 5.00 wt% or even 5.50 wt% lead, and optionally at most 15.00 wt%, preferably at most 14.50 wt% , more preferably at most 14.00wt%, even more preferably at most 13.50wt%, still more preferably at most 13.00wt%, preferably at most 12.50wt%, more preferably at most 12.00wt%, even more preferably at most 11.50wt%, still more preferably at most 11.00wt%, preferably at most 10.50wt%, more preferably at most 10.00wt%, even more preferably at most 9.50wt%, yet preferably at most 9.00wt% of lead (Pb),
[0139] comprising at least 1.00wt% tin (Sn), preferably at least 1.25wt%, more preferably at least 1.50wt%, even more preferably at least 1.75wt%, still more preferably at least 2.00wt%, preferably at least 2.25wt%, more preferably at least 2.50wt%, even more preferably at least 2.75wt%, still preferably at least 3.00wt% or even 3.25wt% tin (Sn), and optionally at most 12.00wt%, preferably at most 10.00wt%, more preferably at most 8.00wt%, even more preferably at most 7.00wt%, still more preferably at most 6.00wt%, preferably at most 5.50wt%, more preferably at most 5.00wt%, even more preferably at most 4.50wt%, still preferably at most 4.00wt% tin (Sn),
[0140] comprising at least 0.05 wt% iron (Fe), preferably at least 0.10 wt%, more preferably at least 0.30 wt%, even more preferably at least 0.50 wt%, still more preferably at least 0.60 wt%, preferably at least 0.70 wt%, more preferably at least 0.80 wt%, even more preferably at least 0.90 wt%, yet more preferably at least 1.00 wt% or even 1.10 wt% iron (Fe), and optionally at most 5.00 wt%, preferably at most 4.00 wt%, more preferably at most 3.00 wt%, even more preferably at most 2.50 wt%, yet more preferably at most 2.00 wt%, preferably at most 1.75 wt%, more preferably at most 1.50 wt%, even more preferably at most 1.25 wt%, yet preferably at most 1.00 wt% iron (Fe),
[0141] comprising at least 0.10 wt% zinc (Zn), preferably at least 0.50 wt%, more preferably at least 1.00 wt%, even more preferably at least 2.00 wt%, still more preferably at least 2.50 wt%, preferably at least 3.00 wt%, more preferably at least 3.50 wt%, even more preferably at least 4.00 wt% zinc (Zn), and optionally at most 10.00 wt%, preferably at most 9.50 wt%, more preferably at most 9.00 wt%, even more preferably at most 8.50 wt%, still more preferably at most 8.00 wt%, preferably at most 7.50 wt%, more preferably at most 7.00 wt%, even more preferably at most 6.50 wt%, still more preferably at most 6.00 wt%, preferably at most 5.50 wt%, more preferably at most 5.00 wt% zinc (Zn),
[0142] comprising at most 5 wt% sulfur (S), preferably at most 4.5 wt%, more preferably at most 4.0 wt%, even more preferably at most 3.5 wt%, still more preferably at most 3.0 wt%, preferably at most 2.5 wt%, more preferably at most 2.0 wt%, preferably at most 1.5 wt%, more preferably at most 1.0 wt%, even more preferably at most 0.5 wt%, yet more preferably at most 0.1 wt% sulfur, and optionally at least
[0143] 5 ppm by weight, preferably at least 50 ppm by weight, more preferably at least 100 ppm by weight, even more preferably at least 500 ppm by weight, still more preferably at least 1000 ppm by weight, preferably at least 0.5 wt%, more preferably at least 1.0 wt% sulfur.
[0144] The applicant has found that the above-mentioned features of the present invention can also be controlled and obtained by appropriate operation of the smelting steps, as described above, including the selection of the raw materials. Complying with the upper limit of the sulfur content as part of one of the conditions in the above list further avoids the formation of a separate copper matte phase and thus clearly distinguishes the process according to the present invention including this feature from copper smelting processes in which a copper matte phase is formed as one of the products or intermediates. The applicant has further found that the above-mentioned metal phase is very suitable for the recovery of the valuable metals listed in the pyrometallurgical process steps described herein below.
[0145] Applicants have further discovered that the large amount of copper in the metal phase can act as an extractant for other valuable metals such as nickel, tin and lead from the slag phase, thereby contributing to high recovery rates itself and also to high recovery rates of these metals other than copper.
[0146] Applicants have further discovered that compliance with regulated lead levels provides advantages in recovering more economically favorable metallic tin, since tin and lead can be recovered as a solder-type by-product stream which, due to the lead content, can be appropriately adjusted and subsequently distilled to recover a high purity tin main product, as well as equally valuable lead-containing by-products of varying qualities.
[0147] In one embodiment of the method according to the invention, the liquid molten bath in the furnace has a temperature of 1100-1300°C, preferably at least 1120°C, more preferably at least 1140°C or even 1150°C, and optionally at most 1250°C, preferably at most 1200°C, more preferably at most 1180°C. The applicant has found that this temperature range can bring the advantages of sufficient slag fluidity and sufficient fuming of the zinc already obtained from the smelting step, while maintaining a low fuming rate of the tin and / or lead obtained from the smelting step, thus contributing to a high recovery rate of tin and / or lead and / or zinc and a high operability of the smelting step. The applicant prefers to let the contents of the furnace cool to at most 1140°C before removing the metal from the furnace. The applicant has found that this precaution helps to extend the service life of the container that receives the molten metal and transfers it to the subsequent process steps.
[0148] In one embodiment of the method according to the invention, the off-gases from the smelting furnace are collected and treated by cooling and / or filtering. The applicant has found that the off-gases from the smelting step contain valuable metals worth recovering and said treatment also reduces the environmental problems associated with the discharge of the off-gases from the smelting step into the atmosphere.
[0149] In one embodiment of the method according to the invention, secondary exhaust gases from the furnace surroundings are also collected and treated by filtering, optionally combined with cooling. The Applicant has found that this feature further reduces the environmental problems associated with the operation of the furnace according to the invention.
[0150] In one embodiment of the method according to the invention, the smelting is carried out in a smelting furnace.
[0151] The smelting furnace has the advantages of being simple to operate and simple in equipment, and thus economically advantageous. The smelting furnace brings the further advantage of being tolerant in terms of raw material quality. The smelting furnace is able to accept raw materials that are highly diluted and / or contaminated with a wide variety of components, such as a wide variety of organics. In the smelting furnace, the metal is melted and the organics and other combustible materials are burned. Since these mixed and / or contaminated raw materials have almost no other end use, they can be supplied at very economically attractive conditions. Therefore, the ability to process these raw materials and upgrade the valuable metals contained therein is of interest to the operator of the method according to the invention.
[0152] The smelting furnace is a relatively simple and inexpensive apparatus consisting of a large cylindrical furnace which need only be capable of tilting about its longitudinal axis over a portion of a full circle. This discovery brings with it the advantages of low capital investment and / or low operating costs for carrying out the smelting step.
[0153] In one embodiment of the method according to the invention, the wall of the furnace is cooled at least partially on the furnace wall surface. This brings the advantage of reducing wear and tear on the furnace wall, in particular for movable parts provided as part of the device for moving the furnace in order to agitate the liquid bath and for enhancing and / or controlling the agitation of the bath.
[0154] In an embodiment of the invention, the method further comprises a step of fuming the slag phase formed in the smelting step to obtain fumed slag, preferably the fuming is carried out in a fuming furnace. The fuming step produces fumed slag, as well as dust containing at least most of the metals fumed from the smelting slag, which metals are usually present in their oxidized form. The applicant has found that it is advantageous to provide this additional process step, which broadens the acceptance criteria for raw materials for the smelting step, because raw materials containing more zinc and optionally also lead can be included. These raw materials are often difficult to process in other processes, where they may be a process and / or economic burden, so they can be provided with higher abundance and more attractive economic conditions. The zinc fuming step can be based on, for example, Michael Borell in Sweden in 2005. The process is described in “Slag-a resource in the sustainable society”, in the proceedings of the International Conference on Mining and the Environmental Metals and Energy Recovery, which took place in Sweden in 2005, pp 130-138 of the proceedings). However, the applicant prefers to perform such an additional fuming step as disclosed in WO 2016 / 156394 A1.
[0155] In one embodiment of the method according to the invention, when the slag is removed from the smelting step or from the fuming step, the slag is granulated. Preferably, the slag from the smelting slag and / or the slag from the fuming step is removed from the respective furnace in a liquid state. This has the advantage that when the slag obtained cools, the furnace can be freed for further production and / or slag treatment. The slag can be cooled and / or solidified by contacting the slag with a cooling medium such as air, possibly ambient air.
[0156] In one embodiment of the method according to the invention, cooling of the slag is performed by contacting the liquid slag with water. The applicant has found that cooling with water is very effective and can be implemented in a variety of ways, resulting in a relatively well controlled cooling rate.
[0157] In one embodiment of the method according to the present invention, the method further comprises the step of using the produced slag for an end use selected from the group consisting of providing a wear layer and / or coating for roofing tiles or roofing shingles, as a blasting sand or blasting grit component, as a foamed tile component used as a black colorant, preferably for building products, more preferably for black tiles, as a black block, preferably for decorative purposes, and as high density ballast, preferably for underwater applications, more preferably for hydraulic engineering, and combinations thereof.
[0158] In one embodiment of the method according to the invention for producing an object for the construction industry, the method further comprises the step of adding the produced slag as aggregate and / or binder, preferably as a binder for aggregates, preferably as an active binder, more preferably as a binder with pozzolanic activity, even more preferably as a substitute for Portland cement, even more preferably as a partial substitute for Portland cement, during the production of the object for the construction industry.
[0159] In one embodiment of the method according to the invention the produced slag is added as a binder to the inorganic polymer composition, preferably in combination with a base, more preferably as the main binder in the inorganic polymer composition, even more preferably as the only binder in the inorganic polymer composition.
[0160] In one embodiment of the method according to the invention, in which the slag produced is added during the production of an object for the building industry, the method further comprises a step of foaming the inorganic polymer composition.
[0161] In one embodiment of the method according to the invention for producing an object for the construction industry, the object for the construction industry is a building element, preferably the building element is selected from the list of bricks, pavers, blocks, concrete blocks and combinations thereof.
[0162] In one embodiment of the method according to the invention for producing an object for the building industry, the object for the building industry has a foamed structure.
[0163] In one embodiment of the method according to the invention for producing an object for the building industry, the method further comprises the step of using the object for improved thermal and / or acoustic insulation, shielding against X-rays and combinations thereof.
[0164] In one embodiment of the method according to the present invention, the method further comprises a step of refining the concentrated copper intermediate to obtain a refined copper product and at least one copper refining slag. The applicant has found that the refining step can be appropriately carried out as described in WO2019 / 115543 A1.
[0165] In one embodiment of the method according to the present invention, wherein the concentrated copper intermediate further comprises tin and lead, the method further comprises recovering the crude solder metal composition from the concentrated copper intermediate. Such recovery of the crude solder metal may be suitably carried out as described in WO 2019 / 115524A1.
[0166] In one embodiment of the method according to the invention comprising recovering a crude solder metal composition, the method further comprises the step of recovering at least one of a purified soft lead product, a purified hard lead product and a purified tin product from the crude solder metal composition. Applicants have found that the crude solder metal composition is a highly suitable feedstock for recovering at least one of the listed products, preferably at least a purified tin product, more preferably also one of the purified lead products, and even more preferably both purified lead products.
[0167] In one embodiment of the method according to the invention comprising recovering the crude solder metal composition, the method further comprises the step of pre-refining the crude solder metal composition to produce a pre-refined solder metal composition.
[0168] The crude solder metal composition obtained as a by-product of refining the concentrated copper intermediate obtained from the method according to the present invention can be further pre-refined or treated to remove more contaminants therein, especially copper. This can be carried out by contacting the crude solder metal composition as a molten liquid with elemental silicon and / or aluminum, which silicon and / or aluminum elements combine with Cu, Ni and / or Fe under operating conditions and form separate silicide and / or aluminide alloy phases. The applicant prefers to use waste containing silicon and / or aluminum. Preferably, the added material also includes Sn and / or Pb, because these metals are easily upgraded to the corresponding main products when introduced into this process stage. Since Sb and As are usually present in the crude solder metal composition, the applicant prefers to use silicon and avoid aluminum, although aluminum is generally more readily available and more reactive. This avoids the generation of H2S, toxic gases, and more exothermic reactions in the processing container, and also avoids the possibility of the highly toxic gases antimonide and / or arsine generated by the alloy phase byproduct when it comes into contact with water. Applicants have found that the silicon feedstock for this processing step can contain limited amounts of iron (Fe), easily exceeding 1 wt%, easily up to 5 wt%, and even up to 10 wt% Fe. Thus, the process can be operated using silicon products that are not acceptable to other silicon consumers, such as rejects from production lines, and which can therefore be more readily available. Applicants have found that the burden of handling this additional iron, which is also combined with the silicon, is generally easily compensated by favorable conditions for the supply of silicon sources.
[0169] The pre-refining can suitably be carried out as described in WO 2019 / 115524A1 and produces a so-called "cupro phase" by-product, which can advantageously be recycled to the smelting step of the method according to the invention, preferably after the "washing" described.
[0170] In one embodiment of the method according to the invention comprising recycling the crude solder metal composition, the method further comprises a step of conditioning the crude solder metal composition or pre-refining the solder metal composition to produce a conditioned solder metal composition. The conditioning step enables further preparation of the solder to make it suitable for vacuum distillation, a technically demanding process step that is sensitive to the excessive presence of specific metal contaminants. Such conditioning and distillation may suitably be performed as described in WO 2018 / 060202 A1.
[0171] In one embodiment of the method according to the invention for producing a modified solder metal composition, the method further comprises a first distillation step for distilling the modified solder composition, wherein lead is removed from the solder by evaporation and a first distillation overhead product and a first distillation bottom product are obtained. This first distillation can be suitably carried out as described in WO 2018 / 060202 A1.
[0172] In one embodiment of the method according to the invention for producing a first distillation overhead product, the method further comprises a step of removing at least one contaminant selected from metallic arsenic, antimony and tin from the first distillation overhead product to obtain a purified soft lead product. Preferably, the purified soft lead product is produced as described in WO 2020 / 157165A1.
[0173] In one embodiment of the process according to the invention comprising a first distillation step, the first distillation bottoms product of the first distillation step contains lead and silver, and the process further comprises a step of separating the bottoms product of the first distillation step into a first silver-rich liquid discharge product at the liquid end of the crystallization step and a first tin-rich product at the crystallization end of the crystallization step by fractional crystallization. The applicant prefers to perform this separation as described in WO 2020 / 157167 A1.
[0174] In one embodiment of the method according to the invention comprising a fractional crystallization step, the method further comprises the step of separating the first silver-rich liquid discharge product into a lead and tin-rich product and a silver-rich product, preferably by electrolysis, wherein the anode mud represents the silver-rich product. The applicant prefers to perform this separation as described in WO 2020 / 157167A1.
[0175] In one embodiment of the method according to the present invention for producing a first tin-rich product and the first tin-rich product also contains lead and antimony, the method further comprises a second distillation step for distilling the first tin-rich product, wherein the step mainly evaporates lead and antimony and obtains a second distillation tower top product and a second distillation tower bottom product.
[0176] In one embodiment of the process according to the invention comprising a second distillation step, the process further comprises a third distillation step for distilling the second distillation top product, wherein this step evaporates lead and obtains a third distillation top product and a third distillation bottom product, preferably the third distillation bottom product is at least partly recycled to the feed of the second distillation step and / or to the feed of the fractional crystallization step.
[0177] In one embodiment of the method according to the invention comprising a third distillation step, the method further comprises a step of removing at least one contaminant selected from metallic arsenic and tin from the third distillation top product to obtain a purified hard lead product. The applicant prefers to carry out this step as described in WO 2020 / 157168 A1.
[0178] In one embodiment of the method according to the invention comprising a second distillation step, the method further comprises a step of refining the second distillation bottom product to obtain a purified tin product. The applicant prefers to carry out this step as described in WO 2020 / 157168A1.
[0179] In one embodiment of the method according to the invention comprising refining the concentrated copper intermediate to obtain a refined copper product, the method further comprises the step of casting the refined copper product to produce refined copper anodes. The applicant has found that the refined copper product in the form of copper anodes makes the product highly suitable for a further electrolytic process step for producing high purity copper cathodes and anode mud that can be further processed to recover the valuable metals contained therein. The applicant prefers to carry out this electrolytic purification process step as described in WO 2019 / 219821 A1.
[0180] In an embodiment of the method of the invention, at least a part of the method is electronically monitored and / or controlled. The applicant has found that the advantage of electronically controlling the method according to the invention, preferably by means of a computer program, is better processing, so that the results are more predictable and closer to the processing target. For example, on the basis of temperature measurements, if necessary, also on the basis of pressure measurements and / or liquid level measurements and / or in combination with the results of chemical analysis of samples taken from the process flow and / or the results of analysis obtained online, the control program can control the following related equipment: the supply or removal of electrical energy, the supply of heating or cooling medium, flow and / or pressure control. The applicant has found that such monitoring or control is particularly advantageous for steps operated in continuous mode, and it is also advantageous for steps operated in batch or semi-batch. In addition and preferably, the monitoring results obtained during or after the steps of the method according to the invention can also be used to monitor and / or control other steps as part of the method according to the invention, and / or processes adopted upstream or downstream of the method according to the invention, which are part of the overall process of which the method according to the invention is only a part. Preferably, the overall process is all monitored electronically, more preferably by at least one computer program. Preferably, the overall process is controlled electronically as much as possible.
[0181] Applicants intend that computer control also provides for the transfer of data and instructions from one computer or computer program to at least one other computer or computer program or module of the same computer program to monitor and / or control other processes, including but not limited to the processes described herein.
[0182] Figure 1 Further illustrating the claimed invention, a process flow chart of the overall process is shown as a preferred embodiment, which includes process steps for recovering a concentrated copper intermediate according to the present invention.
[0183] exist Figure 1 In the present invention, the following reference numerals represent the following process steps or process flows:
[0184] 100 Melting Step or Smelting
[0185] 200 Copper Refining
[0186] 300 Copper Anode Casting
[0187] 400 Slag Fuming Step 500 Lead / Tin Recovery
[0188] 1 Coarse feed section
[0189] 2 Finely divided feed fraction or dust
[0190] 3 Black copper as an intermediate for concentrated copper
[0191] 4Smelting dust byproduct from smelting furnace
[0192] 5Smelting slag
[0193] 6Refining slag
[0194] 7Crude solder by-product from copper refining
[0195] 8 Refined Copper
[0196] 9Copper anode products
[0197] 10Soft lead products
[0198] 11Hard Lead Products
[0199] 12Refined tin products
[0200] 13 Fumed slag
[0201] 14 Fume dust byproducts from fuming furnaces
[0202] Figure 1 A coarse feed portion 1 and a fine feed portion 2 are shown being fed into a smelting furnace 100 into which an oxygen-containing gas (not shown) is injected to control the reaction and thus the temperature in the furnace. The smelting furnace exhaust gases are cooled and filtered, thereby collecting smelting dust 4. Smelting slag 5 is removed from the furnace and fed to a fuming step 400 to recover the fuming dust 14 and produce an end slag or so-called "clean slag" 13 as a second slag.
[0203] Black copper 3 as a concentrated copper intermediate is fed to a copper refining step 200, which produces a refined copper product 8, a crude solder byproduct 7, and a refined slag 6. The refined slag 6 may be transferred to a fuming step 400 to increase the amount of terminal slag 13 and fumed dust 14. Refined copper 8 is fed to a copper anode casting step 300 to produce copper anodes 9. The crude solder 7 is transferred to a lead / tin recovery step 500, where a soft lead product 10, a refined tin product 12, and an optional hard lead product 11 are produced.
[0204] Applicants have found that the beneficial technical effects of the present invention, not only but especially the more stable and reliable operation of the smelting step 100, are easily transferred downstream and all the way down to Figure 1 In the production of derivatives 9, 10, 11, 12, 13 and 14 shown. Due to the present invention, the derivatization step enjoys a more stable and reliable feed flow from the smelting step and is therefore able to produce a final product with a more stable and reliable quality. Another benefit is that the present invention reduces the monitoring burden and operator attention of operating downstream process steps and the entire process.
[0205] Example
[0206] In the rotary drum furnace with an inner diameter of 3 meters, liquid black copper at a height of about 1,00 meters is retained as a concentrated copper intermediate from the previous feed batch, the amount of which is about 113 metric tons.
[0207] The furnace was operated in semi-continuous mode during a continuous 16-month operation period using a repetitive sequence of the following operating patterns, during which each cycle involved a different pre-mixed feed batch composed and collected from parcels selected from a large inventory of available raw materials:
[0208] Mode 1: Starting with a suitable feed batch, coarse solid raw materials are gradually fed into the furnace. If necessary, this mode is included until a continuous slag layer floating on top of the liquid metal phase is obtained.
[0209] Mode 1+2: If a continuous slag layer is present in the furnace, a finely divided feed material, also called "dust", is pneumatically conveyed from another suitable premixed feed batch constituted for this purpose and injected into the liquid slag phase and above the metal phase of the liquid molten bath, usually also gradually over time, while a gradual feed of coarse solid material is preferably also continued,
[0210] Mode 3: Typically, but only when required, as part of the operation, once a feed batch has been completed and / or the furnace is deemed full, the furnace conditions are maintained for a period of time and chemical reactions are allowed to proceed until the desired slag and metal composition is achieved.
[0211] Mode 4: The slag is poured out of the furnace by tilting the drum until the upper slag phase is at least partially poured out through the feed opening of the furnace. The slag is preferably transferred in liquid form in a suitable container to a fuming furnace for further recovery of zinc by fuming, and optionally also lead, and possibly also copper as part of the metallic phase as a by-product of the fuming step. The slag obtained from this fuming step, but if there is no fuming step, the slag obtained from the smelting step is cooled, solidified and granulated by contacting the hot liquid slag with a large amount of water.
[0212] Mode 5: The metal is partially removed from the furnace, if convenient, until there is still at least about 1,00 m of liquid metal in the furnace plus possibly some liquid slag. The removal step is carried out if the slag is completely removed by also allowing the metal phase to overflow through the feed opening, and if only a portion of the slag phase is removed, the metal is removed through tapping holes at appropriate locations in the furnace wall.
[0213] After the slag and / or metal are removed in mode 4 and / or mode 5, i.e. when the furnace has more space again, the feeding of raw materials is restarted as shown in the above-mentioned mode 1 or mode 1+2, depending on the presence of slag in the furnace, and if the previous feeding batch has ended, it starts from the next feeding batch.
[0214] If downstream processing of the concentrated copper intermediate requires more feed, a portion of the liquid metal phase is intermittently removed from the furnace before or without removing any overlying slag phase, which is performed before or immediately after metal removal.
[0215] Additional flux material, sometimes also referred to as "slag former" as a translation of the common term in German, is usually sand, which is added to the furnace on a necessary basis to ensure adequate slag fluidity. Before granulating the slag from the furnace or from the downstream fuming furnace, additional silica is added if necessary to ensure the correct ratio of Fe / Si so that the risk of hydrogen generation during slag pouring and granulation and the associated explosion risk is under control. An average total amount of 11.5 tons of sand is added to the furnace per feed batch during the time required to process the feed batch.
[0216] During modes 1, 1+2 and 3, pure oxygen is injected when necessary to maintain the furnace temperature by means of lances introduced through the feed port. During these operating modes, the rotary drum furnace is shaken, if possible, to agitate the liquid contents therein.
[0217] During all operating modes, compressed air at a pressure of 10 barg is fed into four tuyeres arranged at appropriate positions on the furnace wall below the liquid level, and this air is injected into the furnace primarily to agitate the molten bath, but also to introduce additional oxygen into the bath to participate in the predetermined chemical reactions.
[0218] In the stage considered, a total amount of about 92.4 tons of coarse solid raw material (including some return material) was introduced into the furnace on average per feed batch, and a total amount of about 23.2 tons of finely divided raw material was introduced into the furnace. The coarse solid raw material and the finely divided raw material had the average composition shown in Table 1. Sufficient additional solid scrap iron was fed into the furnace as part of the premixed feed batch of the coarse solid raw material and as part of the feed batch to maintain the presence of solid iron floating on the metal phase. Therefore, the amount of additional scrap iron introduced is included in the composition of the coarse solid raw material in Table 1.
[0219] Table I
[0220]
[0221]
[0222] Throughout the entire operating period under consideration, an average total of about 6.6 tons of oxygen per feed batch is injected into the bottom of the furnace in the form of compressed air at about ambient temperature through four tuyeres, and as oxygen through lances located close to the interface between the metal phase and its upper slag phase. The furnace temperature can be maintained very conveniently and accurately within a narrow range of 1150-1180°C. Most importantly, control of the oxygen injection makes it possible to avoid temperature excursions above this range, thereby minimizing the evaporation of tin and / or lead. Control of the feed rate of the raw materials, including the injection of coarse solid material and dust, makes it possible to avoid the temperature from falling below the desired level, and if such a drop occurs, the injection of oxygen makes it easy to recover from temporary temperature drops. In order to remove metal from the furnace, the temperature can be reduced to about 1140°C to reduce the risk of damaging the containers transferring the molten metal.
[0223] The exhaust gases from the furnace are cooled and filtered to recover the solids in the cooled gases as smelting dust.
[0224] During the entire operating period under consideration, the average product quantities and compositions shown in Table II were obtained and removed from the smelting furnace for each feed batch.
[0225] Table II
[0226] Components (wt%) Smelting slag Metal dust Cu 0.60 77.41 6.18 Pb 0.30 9.40 10.99 Sn 0.11 4.25 1.03 Ni 0.04 1.74 0.03 Fe 35.85 1.12 0.50 Si 0.00 0.00 0.00 Al 0.00 0.00 0.00 Zn 11.48 4.98 48.90 Bi 0.00 0.04 0.00 As 0.00 0.04 0.03 Sb 0.00 0.07 0.04 CaO 2.20 0.00 0.00 <![CDATA[SiO2]]> 31.40 0.02 0.60 <![CDATA[Al2O3]]> 3.58 0.00 0.01 total 85.56 99.07 68.31 mt 70.1 61.1 2.5
[0227] The sulfur level of the metal phase obtained as the concentrated copper intermediate from the process in the example was determined and found to be well below 2 wt% for each feed batch and in the range of up to 0.25 wt%. For each feed batch, the sulfur content in the slag was up to 0.33 wt%, while the sulfur content in the dust was up to 0.21 wt%.
[0228] Having now fully described the invention, those skilled in the art will appreciate that the invention can be carried out within a wide range of parameters within the claimed scope without departing from the scope of the invention defined by the claims.
Claims
1. A method for recovering copper from secondary raw materials, comprising the following steps: smelting a feedstock comprising said raw material in a furnace in at least one feed batch to recover a concentrated copper intermediate from said furnace, wherein said feedstock of raw material is gradually introduced into said furnace, said feedstock comprising copper, at least partly present as an oxide, wherein the feedstock further comprises iron, the iron being present at least partially in its elemental form, wherein heat is generated inside the furnace by redox reactions which convert elemental iron and, if present, metals or compounds no more noble than iron or zinc into oxides, and convert oxides of copper and, if present, oxides of metals more noble than tin into elemental metals, wherein the elemental metal is at least partially collected in the molten liquid metal phase, and the oxide is at least partially collected in the upper liquid slag phase, wherein the liquid phases are separable and at least one of the liquid phases is at least partially removed from the furnace at the end of the smelting step, wherein the slag phase is removed as smelting slag (5) and the metal phase is removed as a concentrated copper intermediate, wherein during the smelting step, an excess of iron in elemental form and a metal or compound which is at most as inert as iron or zinc under furnace conditions is maintained in the furnace relative to the amount required to complete the redox reaction, and During the smelting step, further heat input into the furnace is provided by the injection of an oxygen-containing gas for oxidizing excess iron and metals or compounds up to as inert as iron or zinc present in the furnace, and for burning a combustible source containing at least one of carbon and hydrogen which may additionally be introduced into the furnace, if present.
2. The method according to claim 1, wherein: The feedstock also includes at least one second metal selected from the group consisting of nickel, tin, and lead.
3. The method according to claim 2, wherein: The concentrated copper intermediate also includes the at least one second metal.
4. The method according to claim 1, wherein: The feed material is at least partially in a solid state, and wherein the solid feed material is gradually fed into the furnace.
5. The method according to claim 1, wherein: At least a portion of the feedstock is in the form of a finely divided feedstock portion (2), and the finely divided feedstock portion (2) has an average particle size of at most 10 mm.
6. The method according to claim 1, wherein: The content of iron and metals or compounds up to as inert as iron or zinc dissolved in the molten metal in the furnace is maintained at at least 1.0 wt %, wherein the concentration of the metals and compounds up to as inert as iron or zinc is converted to an equivalent iron concentration, wherein the equivalent iron concentration is the iron concentration capable of contributing the same amount of heat of reaction as the metals or compounds up to as inert as iron or zinc when reacting with oxygen under furnace conditions.
7. The method according to claim 1, wherein: At least a portion of the oxygen-containing gas is introduced through at least one metal lance, the tip of which is immersed in the liquid slag phase.
8. The method according to claim 1, wherein: At least a portion of the oxygen-containing gas is introduced into the bottom of the furnace through at least one tuyeres.
9. The method according to claim 1, wherein: The composition of the concentrated copper intermediate, which is the main product from the smelting step, meets at least one of the following conditions: comprising at least 50.0 wt% copper (Cu), including at least 0.01 wt% nickel (Ni), including at least 0.10 wt% lead (Pb), including at least 1.00 wt% of tin (Sn), including at least 0.05 wt% iron (Fe), including at least 0.10 wt% zinc (Zn), and • Includes up to 5 wt% sulphur (S).
10. The method according to claim 1, further comprising the step of fuming the slag phase formed in the smelting step to obtain fumed slag (13).
11. The method according to claim 1, further comprising adding the produced slag as a component selected from the group consisting of aggregate and binder during the manufacture of an object for the construction industry.
12. The method of claim 1, further comprising the step of refining the concentrated copper intermediate to obtain a refined copper product and at least one copper refining slag.
13. The method according to claim 12, wherein: The concentrated copper intermediate also includes tin and lead, and the method further includes recovering a crude solder metal composition from the concentrated copper intermediate.
14. The method of claim 13, further comprising the step of recovering at least one product selected from the group consisting of a purified soft lead product, a purified hard lead product, and a purified tin product from the crude solder metal composition.
15. The method of claim 12, further comprising the step of casting the refined copper product to produce a refined copper anode.