A method for preparing 2-methoxy-4-methylphenol from biomass-based vanillin

By loading non-noble metal Co catalysts on nitrogen-doped hollow carbon spheres, the problem of high cost of precious metal catalysts in vanillin hydrodeoxygenation is solved, and efficient and low-cost preparation of 2-methoxy-4-methylphenol is achieved with excellent performance. industrial application prospects.

CN114656337BActive Publication Date: 2024-10-01SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210428077.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-22
Publication Date
2024-10-01
Estimated Expiration
2042-04-22

AI Technical Summary

Technical Problem

In the prior art, the active metal component of the catalyst for hydrodeoxygenation of vanillin to 2-methoxy-4-methylphenol is precious metal, which is costly and unfavorable for industrial production.

Method used

Nitrogen-doped hollow carbon spheres are used to support non-noble metal Co catalysts, and 2-methoxy-4-methylphenol is generated through a hydrogen replacement reaction at 90-180°C. The catalyst is composed of polystyrene nanospheres and cobalt nitrate hexahydrate through ultrasonic treatment and roasted to form a porous structure to improve catalytic activity.

Benefits of technology

It achieves highly selective conversion of vanillin to 2-methoxy-4-methylphenol, reduces the cost of the catalyst, improves the stability and performance of the catalyst, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114656337B_ABST
    Figure CN114656337B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing 2-methoxy-4-methylphenol from biomass-based vanillin. The method adds vanillin, a catalyst and a solvent into a reactor, and after a chemical reaction is carried out in the reactor, the desired 2-methoxy-4-methylphenol is obtained, wherein the catalyst is a nitrogen-doped hollow carbon sphere loaded with a non-precious metal Co catalyst, and the main structure of the catalyst is a hollow carbon sphere, which is used as a carrier on which metal particles are loaded. Since the surface of the hollow carbon sphere has a mesoporous structure, a unique confinement effect can be provided for the hydrodeoxygenation reaction of vanillin, and metal nanoparticles can be stabilized to improve the stability of the catalyst, while a strong metal-carrier interaction can be formed, effectively changing the electronic properties of the metal surface, thereby enhancing the adsorption and activation of vanillin and an intermediate vanillyl alcohol on the catalyst surface, and improving the selectivity of preparing 2-methoxy-4-methylphenol from the hydrodeoxygenation of vanillin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fine chemicals, and particularly relates to a method for preparing 2-methoxy-4-methylphenol from biomass-based vanillin. Background Art

[0002] With the rapid development of modern society, the demand for energy is expected to increase further in the next few decades. At present, the supply of energy still mainly depends on fossil energy, but the excessive exploitation and utilization of fossil energy will not only lead to resource depletion, but also bring a series of environmental problems. Therefore, it is necessary to find a new type of green energy that can replace or reduce the use of fossil energy to solve the problem of energy demand for modern social development. Biomass, as a natural renewable resource, has received widespread attention in recent years because it can be effectively converted into various chemicals and fuels, which can effectively solve current energy and environmental problems. Bio-oil obtained by pyrolysis or liquefaction of biomass has high energy density and convenient storage, and can be used as a liquid fuel to replace fossil fuels. In order to improve the quality of bio-oil, many scholars have focused on the hydrodeoxygenation (HDO) research of bio-oil model compounds, especially the research on phenolic compounds and lignin model compounds. Among them, vanillin has representative functional groups in bio-oil, including phenolic hydroxyl and methoxyl groups. Vanillin can be converted into high-value-added 2-methoxy-4-methylphenol after HDO treatment. It is a potential liquid biofuel and an important intermediate for spices and medicinal materials. However, since vanillin contains multiple functional groups, it is still challenging to control the selectivity of 2-methoxy-4-methylphenol. The process of preparing 2-methoxy-4-methylphenol by hydrogenation and deoxygenation of vanillin is as follows: (1) vanillin is hydrogenated to produce vanillyl alcohol; (2) vanillyl alcohol is deoxygenated to produce the target product 2-methoxy-4-methylphenol. The specific reaction pathway is as follows: Figure 1 As shown, in order to achieve efficient conversion of vanillin to 2-methoxy-4-methylphenol, the preparation and selection of the catalyst are crucial.

[0003] At present, vanillin is hydrodeoxygenated to 2-methoxy-4-methylphenol. Catalysts with noble metals such as Ru, Pd, Au, Pt and Rh supported on activated carbon or other types of carriers have been used for this reaction. However, these noble metal catalytic systems not only have harsh reaction conditions, such as high temperature and high pressure, but also the active metal components of the catalysts are noble metals, which are expensive and not conducive to industrial production. Therefore, it is urgent to develop new non-noble metal nanocatalysts with low price, high efficiency and stability to achieve highly selective conversion of vanillin to 2-methoxy-4-methylphenol. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a method for preparing 2-methoxy-4-methylphenol from biomass-based vanillin, so as to solve the problem that the active metal component of the catalyst in the prior art is a precious metal, which has a high cost and is not conducive to industrial production.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for preparing 2-methoxy-4-methylphenol from biomass-based vanillin comprises the following steps:

[0007] Mixing vanillin, a catalyst and a reaction solvent, replacing the atmosphere in the reaction system with hydrogen, reacting at 90 to 180° C., wherein the reaction atmosphere is hydrogen, and generating 2-methoxy-4-methylphenol after the reaction;

[0008] The catalyst is a hollow carbon sphere doped with nitrogen, and metal Co nanoparticles are loaded on the hollow carbon sphere.

[0009] A further improvement of the present invention is:

[0010] Preferably, the reaction pressure is 1-5 MPa.

[0011] Preferably, the reaction time is 0.5 to 2.4 hours.

[0012] Preferably, the mass ratio of vanillin to catalyst is (3-15):1.

[0013] Preferably, the reaction solvent is any one of dioxane, tetrahydrofuran, methanol, ethanol, propanol, n-butanol, isopropanol, isobutanol, dimethyl sulfoxide, N,N-dimethylformamide and water.

[0014] Preferably, the preparation process of the catalyst is as follows: polystyrene nanospheres and 2-methylimidazole are mixed and then ultrasonically treated to form a mixed system; cobalt nitrate hexahydrate is added to water to form a cobalt nitrate hexahydrate aqueous solution, the cobalt nitrate hexahydrate aqueous solution is added dropwise to the mixed system, the mixed system is stirred and then centrifuged, the centrifuged product is washed with deionized water and methanol, the washed sample is placed in an oven, the baked sample is placed in a tubular furnace for calcining, and the catalyst is obtained after the calcination is completed.

[0015] Preferably, the mixing ratio of the polystyrene nanospheres, 2-methylimidazole and cobalt nitrate hexahydrate is 0.3 g:5.5 g:1.55 mmol.

[0016] Preferably, the preparation process of the polystyrene nanospheres is: adding methyl methacrylate, styrene, acrylic acid and ammonium bicarbonate into water, heating and stirring to react, adding ammonium persulfate and continuing to heat and stir to react, centrifuging and washing the reaction system to obtain polystyrene nanospheres.

[0017] Preferably, the mixing ratio of methyl methacrylate, styrene, acrylic acid and ammonium bicarbonate is: 1.1 mL: 21 mL: 0.92 mL: 0.49 g.

[0018] Preferably, methyl methacrylate, styrene, acrylic acid and ammonium bicarbonate are added to water, heated and stirred to react, and the whole system is heated to 70° C., and then the whole reaction system is heated to 80° C. and stirred for 12 hours to complete the reaction.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The invention provides a method for preparing 2-methoxy-4-methylphenol by hydrodeoxygenation (HDO) reaction of biomass-based vanillin. Vanillin, a catalyst and a solvent are added into a reactor, and after a chemical reaction is carried out in the reactor, the desired 2-methoxy-4-methylphenol is obtained, the catalyst is a nitrogen-doped hollow carbon sphere loaded with a non-precious metal Co catalyst, the main structure of the catalyst is a hollow carbon sphere, the hollow carbon sphere is doped with nitrogen elements, and the nitrogen-doped hollow carbon sphere has a large specific surface area due to the special hollow structure, and is a porous structure with low density and controllable size. The hollow structure is used as a carrier, and metal particles are loaded thereon. Since the surface of the hollow structure has a mesoporous structure, a unique confinement effect can be provided for the hydrodeoxygenation reaction of vanillin, which can not only stabilize metal nanoparticles and improve the stability of the catalyst, but also form a strong metal-carrier interaction, effectively change the electronic properties of the metal surface, and then enhance the adsorption and activation of vanillin and intermediate vanillyl alcohol on the catalyst surface, and improve the selectivity of preparing 2-methoxy-4-methylphenol by hydrodeoxygenation of vanillin. The entire reaction condition is simple, the required cost is greatly reduced, and the catalyst has excellent performance and low price, and has good industrial application prospects.

[0021] Furthermore, the hollow carbon sphere-loaded metal nanocatalyst prepared by the present invention can significantly improve the stability of the metal nanoparticle catalyst, and avoid the situation where the metal nanoparticles are not highly active or deactivated due to agglomeration during the reaction. The catalyst prepared by the present invention has a high carbonization yield, uses non-precious metal Co as a metal source, and has a low preparation cost. The catalyst prepared by the present invention has small and uniformly distributed Co metal nanoparticles. The catalyst prepared by the present invention can meet the standards of green, environmental protection, and sustainable development, and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a reaction pathway diagram of vanillin;

[0023] Figure 2 This is the gas phase diagram of 2-methoxy-4-methylphenol prepared in Example 33;

[0024] Figure 3 A product gas phase diagram was prepared for Example 33. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:

[0026] The invention discloses a method for obtaining 2-methoxy-4-methylphenol by taking vanillin as a substrate, controlling the temperature to be 90-180 DEG C, the reaction pressure to be 1-5MPa, and performing a hydrodeoxygenation reaction for 0.5-24h in the presence of a catalyst, a hydrogen atmosphere and a solvent; the catalyst is a nitrogen-doped hollow carbon sphere loaded with non-precious metal Co, and the expression is Co@NHCS-x, wherein NHCS represents the nitrogen-doped hollow carbon sphere, and x represents the calcination temperature.

[0027] Furthermore, the synthesis steps of the catalyst include: (1) preparation of hard template PS nanospheres; (2) polymerization of carbon source and metal precursor on the template surface; and (3) high temperature carbonization and template removal.

[0028] The specific preparation process of the catalyst required for preparing 2-methoxy-4-methylphenol from the biomass-based platform compound vanillin is as follows:

[0029] 1. Preparation method of catalyst:

[0030] 1.1mL methyl methacrylate, 21mL styrene, 0.92mL acrylic acid and 0.49g ammonium bicarbonate were added to 100mL deionized water, added to a round-bottom flask, placed in an oil bath and heated and stirred, and when the temperature reached 70°C, 0.53g ammonium persulfate was added, and then the temperature was raised to 80°C and stirred for 12h. After stirring, the sample was centrifuged and washed, and the centrifuged sample was obtained to obtain polystyrene nanospheres. The polystyrene nanospheres can not only serve as a hard template for the catalyst, but also are easy to decompose at high temperatures, without the need to specifically remove the template, and the polystyrene nanospheres also have the characteristics of uniform particle size distribution.

[0031] Add polystyrene nanospheres and 2-methylimidazole to a round-bottom flask containing deionized water, and the mixing mass ratio of polystyrene nanospheres and 2-methylimidazole is 0.3:5.5; after ultrasonic treatment for 30 minutes, transfer it to an oil bath and stir; add 1.55mmol of cobalt nitrate hexahydrate to deionized water, and then transfer it to the previous round-bottom flask. Add it dropwise during the transfer process, and stir at room temperature after the addition. After stirring, centrifuge and wash with deionized water and methanol, put the washed sample into an oven, the baking temperature is 110℃, and the baking time is 10-14h. Then put the sample in the oven into a tubular furnace for calcination, the calcination temperature is 500-1100℃, the calcination insulation time is 4h, and the heating rate is 5℃ / min. After calcination, the desired catalyst is obtained.

[0032] 1. The prepared catalyst is applied to the reaction of hydrodeoxygenation of biomass-based platform compound vanillin to generate 2-methoxy-4-methylphenol. The specific method is: vanillin and nitrogen-doped hollow carbon sphere-loaded non-precious metal Co catalyst are added to a closed high-pressure reactor loaded with a certain amount of solvent, wherein the mass ratio of vanillin and nitrogen-doped hollow carbon sphere-loaded non-precious metal Co catalyst is (3-15):1, and the reaction solvent is any one of dioxane, tetrahydrofuran, methanol, ethanol, propanol, n-butanol, isopropanol, isobutanol, dimethyl sulfoxide, N,N-dimethylformamide and water. At a reaction temperature of 90-180°C and a reaction pressure of 0.5-5MPa, the desired target product 2-methoxy-4-methylphenol is obtained by catalytic reduction amination reaction for 0.5-24h. The entire reaction process is carried out in an intermittent tank reactor or in a continuous tubular reactor.

[0033] The technical solution of the present invention will be described in detail below in conjunction with several embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0034] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent stores.

[0035] Example 1 (Co@NHCS-600)

[0036] 0.3g polystyrene nanospheres, 5.5g 2-methylimidazole and 20mL deionized water were added to a round-bottom flask. After ultrasonication for 30 minutes, it was transferred to an oil bath for stirring. 1.55mmol cobalt nitrate hexahydrate was added to 3mL deionized water and then transferred to the previous round-bottom flask. It needs to be added dropwise during the transfer process. After the addition is completed, stir at room temperature for 6h. After stirring, centrifuge and wash with deionized water and methanol (wash twice with water and methanol each). The washed sample was placed in an oven at 110°C overnight. The sample was placed in a tubular furnace for calcination at a temperature of 600°C, kept warm for 4h, and a heating rate of 5°C / min.

[0037] Example 2 (Co@NHCS-900)

[0038] 0.3g polystyrene nanospheres, 5.5g 2-methylimidazole and 20mL deionized water were added to a round-bottom flask, which was ultrasonicated for 30 minutes and then transferred to an oil bath for stirring; 1.55mmol cobalt nitrate hexahydrate was added to 3mL deionized water and then transferred to the previous round-bottom flask. It needs to be added dropwise during the transfer process and stirred at room temperature for 6h after the addition is completed. After stirring, centrifuge and wash with deionized water and methanol (wash twice with water and methanol each), and place the washed sample in an oven at 110°C overnight. The sample was placed in a tubular furnace for calcination at a temperature of 900°C, kept warm for 4h, and a heating rate of 5°C / min.

[0039] Example 3 (Co@NHCS-1000)

[0040] 0.3g polystyrene nanospheres, 5.5g 2-methylimidazole and 20mL deionized water were added to a round-bottom flask, which was ultrasonicated for 30 minutes and then transferred to an oil bath for stirring; 1.55mmol cobalt nitrate hexahydrate was added to 3mL deionized water and then transferred to the previous round-bottom flask. It needs to be added dropwise during the transfer process and stirred at room temperature for 6h after the addition is completed. After stirring, centrifuge and wash with deionized water and methanol (wash twice with water and methanol each), and place the washed sample in an oven at 110°C overnight. The sample was placed in a tubular furnace for calcination at a temperature of 1000°C, kept warm for 4h, and a heating rate of 5°C / min.

[0041] Embodiment 4-14

[0042] 10 mg of Co@NHCS catalyst with different calcination temperatures, 0.5 mmol of vanillin, and 6 mL of isopropanol solvent were added to the lining of a 50 mL stainless steel high-temperature reactor. After high-purity hydrogen was introduced to replace the gas 5 times, the hydrogen was filled to 2 MPa, heated to 120°C, maintained for 6 hours, and the rotation speed was 500 rpm. After the reaction was completed, the reactor was placed in water and cooled to room temperature and then vented. The reaction liquid was then centrifuged and the supernatant was taken for gas chromatography detection.

[0043] After the reaction was completed, the content of furfurylamine in the reaction solution was calculated using the following method.

[0044] The reaction products were quantitatively analyzed by gas chromatography (Agilent 7820, Agilent Co., Ltd., Beijing). The separation column was SE-54 with a specification of 25m×0.25mm×1.0μm. The gas chromatography column was tested by the following method: 50°C for 2 min, heating to 250°C at a rate of 10°C / min, and then kept at 250°C for 2 min, injection port temperature: 250°C, detector temperature: 250°C. FID hydrogen flame ionization detector. The conversion rate of vanillin, selectivity and yield of 2-methoxy-4-methylphenol were calculated according to the following formula.

[0045]

[0046]

[0047]

[0048] The specific experimental temperature, reaction pressure, added substrate, reaction time and test results are shown in Table 1:

[0049] Table 1 Effect of different calcination temperatures on the yield of target products

[0050]

[0051]

[0052] In the above examples 4-10, the effect of catalysts with different calcination temperatures on the yield of the target product 2-methoxy-4-methylphenol was investigated. It can be seen from examples 4-10 that among the seven catalysts with different calcination temperatures, when other reaction conditions remain the same, Co@NHCS-900 has the best catalytic performance because it has the highest yield of 2-methoxy-4-methylphenol.

[0053] In the above examples 4-10, the effects of different calcination temperatures on the yield of the target product 2-methoxy-4-methylphenol were investigated. The results showed that Co@NHCS-900 had the best catalytic performance.

[0054] Examples 11-13

[0055] The effect of different hydrogen pressures on the yield of 2-methoxy-4-methylphenol was further explored. The specific results are shown in Table 2.

[0056] Table 2 Effect of different pressures on the yield of target products

[0057]

[0058] According to the above catalytic reaction results and in combination with Example 8, the hydrogen pressure during the hydrodeoxygenation of vanillin has a great influence on the yield of the target product 2-methoxy-4-methylphenol. In the range of 0.5 to 3 MPa, as the hydrogen pressure increases, the yield of the target product gradually increases. When the hydrogen pressure is subsequently increased, the yield of the target product remains unchanged. The optimal hydrogen pressure is 3 MPa.

[0059] Examples 15-21

[0060] Based on the above examples, the effects of different solvents on the yield of the target product were further determined. The specific results are shown in the table:

[0061] Table 3 Effect of different solvents on the yield of 2-methoxy-4-methylphenol

[0062]

[0063] According to the above catalytic reaction results and in combination with Example 8, it can be seen that during the hydrodeoxygenation of vanillin, the solvent has a great influence on the yield of 2-methoxy-4-methylphenol, among which isopropanol is the optimal reaction solvent.

[0064] Examples 22-30

[0065] The effect of reaction time on the yield of the target product was determined, and the results are shown in Table 4:

[0066] Table 4 Effect of different reaction times on the yield of target products

[0067]

[0068]

[0069] According to the above catalytic reaction results and in combination with Example 8, it can be seen that during the hydrodeoxygenation of vanillin, as the reaction time increases, the yield of the target product 2-methoxy-4-methylphenol gradually increases. When the reaction time is 8 h, the yield of the target product is the highest. Subsequently, as the reaction time is further extended, the yield remains basically unchanged.

[0070] Embodiment 31

[0071] 10 mg Co@NHCS-900 catalyst, 76 mg vanillin, and 6 mL isopropanol as solvent were added to the inner lining of a 50 mL stainless steel high-temperature reactor. After high-purity hydrogen was introduced to replace the gas 5 times, the hydrogen was filled to 2 MPa, heated to 140°C, maintained for 6 h, and the rotation speed was 500 rpm. According to the above method, the amount of 2-methoxy-4-methylphenol in the reaction solution was determined and calculated.

[0072] The results showed that the conversion rate of 2-methoxy-4-methylphenol was 100%, the selectivity was 75%, and the yield was 75%.

[0073] Embodiment 32

[0074] 10 mg Co@NHCS-900 catalyst, 76 mg vanillin, and 6 mL isopropanol as solvent were added to the inner lining of a 50 mL stainless steel high-temperature reactor. After high-purity hydrogen was introduced to replace the gas 5 times, the hydrogen was filled to 2 MPa, heated to 150 ° C, maintained for 6 h, and the rotation speed was 500 rpm. According to the above method, the amount of 2-methoxy-4-methylphenol in the reaction solution was determined and calculated.

[0075] The results showed that the conversion rate of 2-methoxy-4-methylphenol was 100%, the selectivity was 87%, and the yield was 87%.

[0076] Embodiment 33

[0077] 10 mg Co@NHCS-900 catalyst, 76 mg vanillin, and 6 mL isopropanol as solvent were added to the inner lining of a 50 mL stainless steel high-temperature reactor. After high-purity hydrogen was introduced to replace the gas 5 times, the hydrogen was filled to 2 MPa, and the reaction mixture was heated to 160 ° C for 6 h at a speed of 500 rpm. According to the method described above, the amount of 2-methoxy-4-methylphenol in the reaction solution was determined and calculated. Figure 2 It can be seen that the peak position of 2-methoxy-4-methylphenol is 11.0. Figure 3 The measured reaction liquid gas phase diagram shows that 2-methoxy-4-methylphenol also appears at about 11.0, which can prove the formation of 2-methoxy-4-methylphenol. The peak at 14.6 corresponds to vanillyl alcohol, the peak at 7.4 is the internal standard added in the reaction, and the peak at 15.1 corresponds to the by-product 4-hydroxy-3-methoxybenzyl alcohol.

[0078] The results showed that the conversion rate of 2-methoxy-4-methylphenol was 100%, the selectivity was 91%, and the yield was 91%.

[0079] Embodiment 34

[0080] 10 mg Co@-NHCS-900 catalyst, 76 mg vanillin, and 6 mL isopropanol as solvent were added to the inner lining of a 50 mL stainless steel high-temperature reactor. After high-purity hydrogen was introduced to replace the gas 5 times, the hydrogen was filled to 2 MPa, heated to 180°C, maintained for 6 h, and the rotation speed was 500 rpm. According to the above method, the amount of 2-methoxy-4-methylphenol in the reaction solution was determined and calculated.

[0081] The results showed that the conversion rate of 2-methoxy-4-methylphenol was 100%, the selectivity was 90%, and the yield was 90%.

[0082] Embodiment 35

[0083] 2.0g 30-50 mesh Co@NHCS-900 catalyst was loaded into the constant temperature section of the tubular fixed bed reactor, and the rest was filled with quartz sand. After the system was checked and sealed, the catalyst bed was heated to 100°C under a hydrogen atmosphere, and then 20% vanillin (isopropanol as solvent) was pumped into the system at a feed flow rate of 1.5mL / h. After gasification, it was reacted through the catalyst bed. After 24 hours, the reaction mixture was cooled in an ice bath and separated from the gas and liquid, and the gas was emptied. The liquid collected after the reaction was sampled for gas chromatography detection. The test results showed that the yield of 2-methoxy-4-methylphenol was 90%.

[0084] In summary, the present invention uses nitrogen-doped hollow carbon spheres loaded with non-precious metal Co catalysts to effectively produce 2-methoxy-4-methylphenol through a hydrodeoxygenation reaction of vanillin, and the methods for preparing the catalyst and 2-methoxy-4-methylphenol have good industrial prospects.

[0085] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing 2-methoxy-4-methylphenol from biomass-based vanillin, characterized in that: The following steps are involved: Mixing vanillin, a catalyst and a reaction solvent, replacing the atmosphere in the reaction system with hydrogen, reacting at 90-180° C., the reaction atmosphere is hydrogen, and generating 2-methoxy-4-methylphenol after the reaction; The catalyst is a hollow carbon sphere doped with nitrogen, and the hollow carbon sphere is loaded with metal Co nanoparticles; The reaction pressure is 1~5MPa; the reaction time is 0.5~2.4h; The preparation process of the catalyst comprises: mixing polystyrene nanospheres and 2-methylimidazole and then performing ultrasonic treatment to form a mixed system; adding cobalt nitrate hexahydrate into water to form a cobalt nitrate hexahydrate aqueous solution; dropping the cobalt nitrate hexahydrate aqueous solution into the mixed system; stirring the mixed system and then performing centrifugal treatment; washing the centrifugal product with deionized water and methanol; placing the washed sample in an oven; placing the baked sample in a tubular furnace for calcining; and obtaining the catalyst after the calcination. The mass ratio of vanillin to catalyst is (3-15):1; The reaction solvent is any one of dioxane, tetrahydrofuran, methanol, ethanol, propanol, n-butanol, isopropanol, isobutanol, dimethyl sulfoxide, N,N-dimethylformamide and water; The mixing ratio of the polystyrene nanospheres, 2-methylimidazole and cobalt nitrate hexahydrate is 0.3 g: 5.5 g: 1.55 mmol; The preparation process of the polystyrene nanospheres is as follows: methyl methacrylate, styrene, acrylic acid and ammonium bicarbonate are added into water, heated and stirred for reaction, ammonium persulfate is added and heated and stirred for reaction, the reaction system is centrifuged and then washed to obtain polystyrene nanospheres; The mixing ratio of the methyl methacrylate, styrene, acrylic acid and ammonium bicarbonate is: 1.1 mL: 21 mL: 0.92 mL: 0.49 g.