A method for preparing a polymer field effect transistor based on magnetron sputtering
The silver source drain electrodes are prepared in a vacuum environment through magnetron sputtering technology, which solves the problems of high-temperature damage and metal oxidation in the vacuum thermal evaporation method, significantly improves the electrical performance of organic transistors, and achieves better metal-semiconductor contact Effect.
Patent Information
- Application Number
- CN202210292904.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-03-24
AI Technical Summary
The existing vacuum thermal evaporation method When manufacturing metal electrodes of organic transistors, high temperatures lead to thermal damage to the semiconductor layer and metal oxidation, affecting device performance, and high contact resistance, making it difficult to meet the needs of modern high-performance polymer devices.
Magneto-controlled sputtering technology is used to prepare silver-source drain electrodes in vacuum environments using low-energy ion sputtering to avoid high-temperature damage and metal oxidation, and optimize the contact between semiconductors and metal electrodes.
The electrical performance of P-type polymer field effect transistors is improved, the carrier mobility and output current are significantly improved, the threshold voltage is reduced, and the contact resistance is reduced, and the device performance is better than the traditional thermal evaporation method.
Smart Images

Figure CN114665019B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the fields of microelectronic materials and device technologies, and in particular to a method for preparing a polymer field effect transistor based on magnetron sputtering. Background Art
[0002] In recent years, rising material and manufacturing costs and public interest in more environmentally friendly electronic materials have supported the development of organic electronic products. Organic field-effect transistors (OFETs) are transistors composed of organic semiconductors. Since Tsumura et al. first prepared organic field-effect transistors using semiconductor materials as active layers in 1986, their research has developed rapidly and achieved many breakthroughs. Decades later, their characteristics such as on-off ratio and carrier mobility have been greatly improved. In addition, from a material point of view, organic semiconductor materials are more diverse and cheaper than inorganic semiconductor materials. They have better flexibility and can be used in flexible substrates and circuits, and we can relatively easily control their performance through molecular design and synthesis. At present, the development direction of OFET is to replace inorganic transistors in simple circuits, thereby realizing flexible and stretchable circuits. Therefore, it has great application prospects in radio frequency trademarks, electronic paper, sensors and organic display matrix drivers. In addition, in daily life, it also has certain potential value for wearable devices, medical monitoring, electronic skin, etc.
[0003] However, organic transistors are affected by the interface properties, and the impact of contact resistance cannot be ignored, so optimization is urgently needed in device manufacturing. Although there have been many different manufacturing processes before, they are basically for small molecule polymers or some early materials. The microstructure of the materials used now has changed a lot, so the previous processes can no longer meet the subsequent device application development. The process of manufacturing the source and drain electrodes involved in the electrical contact of modern high-performance polymers is crucial, and it also needs to be characterized and its electrical properties continuously optimized after manufacturing.
[0004] Regarding the manufacture of metal electrodes, most of them are completed by vacuum thermal evaporation (such as reference [1]: Zhu Dalong, Xie Yingtao, Xu Xin, et al. Research on the performance of organic thin film transistors based on the preparation process of metal electrodes and organic semiconductor layers [J]. 2015, 36 (1): 88-91.). As described in reference [1], this technology uses Ag as the electrode and uses vacuum evaporation to prepare the electrode. The final contact resistance reaches 107Ω. The high contact resistance indicates that there are some problems in the preparation method of vacuum evaporation, which seriously affects the formation of its interface. First of all, from a physical point of view, the temperature in the chamber is too high during evaporation, which will cause serious thermal damage to the semiconductor layer film, especially the top contact device, and will also enhance the diffusion effect and affect the contact effect; from a chemical point of view, absolute vacuum cannot be guaranteed in the experiment. At such a high temperature, even in a very low water oxygen environment, metals such as silver will undergo chemical reactions such as oxidation to form silver oxide; and silver oxide is not a very good semiconductor material, which has a great impact on the performance of the device.
[0005] Therefore, it is necessary to propose a method for electrode fabrication that can reduce the influence of high temperature and improve the performance of organic transistors. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and to propose a method for preparing a polymer field effect transistor based on magnetron sputtering. The P-type polymer field effect transistor applicable to the method has a bottom gate top contact structure, and the transistor is composed of a source-drain electrode, a semiconductor active layer, a silicon dioxide insulating layer and a silicon gate from top to bottom. In the process of manufacturing the source-drain electrode, the method does not use a vacuum evaporation method, but uses a vacuum magnetron sputtering apparatus to prepare silver source-drain electrodes on the semiconductor layer by ion sputtering, thereby optimizing the contact between the semiconductor active layer and the silver electrode and improving the electrical performance of the P-type polymer transistor.
[0007] The specific technical scheme for achieving the purpose of the present invention is as follows:
[0008] A method for preparing a polymer field effect transistor based on magnetron sputtering, wherein the polymer field effect transistor has a bottom gate top contact structure, the method comprising: firstly oxidizing and growing a layer of silicon dioxide as an insulating layer on the surface of a silicon wafer, then spin coating an organic semiconductor active layer on the surface of the silicon dioxide, then using a mask to use a magnetron sputtering method to prepare a layer of silver as a source and a drain on top of the active layer, and finally isolating each transistor on the silicon wafer and using copper foil and conductive silver glue for gate processing.
[0009] Furthermore, the preparation method comprises the following steps:
[0010] 1) Substrate preparation: Take a silicon wafer with a 300nm silicon dioxide oxide layer on the surface and cut it into 1.5cm±0.2cm square pieces, in which the silicon dioxide oxide layer is directly used as an insulating layer; you can choose the silicon wafer produced by Suzhou Yancai Micro-Nano Technology Co., Ltd., which has a 300nm silicon dioxide oxide layer on its surface when it leaves the factory.
[0011] 2) Cleaning of substrate;
[0012] 3) Preparation of semiconductor film: Spread the semiconductor solution on the surface of the silicon wafer and spin coat it using a spin coater; anneal after the spin coating and then cool for 30 minutes;
[0013] 4) Preparation of source and drain electrodes: Using magnetron sputtering technology, first place the silver target on the A target of the vacuum sputtering instrument, then clean the stainless steel source and drain mask, cover it on the semiconductor film of the silicon wafer and send it into the cavity of the sputtering instrument, and use a mechanical pump and a molecular pump to evacuate the cavity of the sputtering instrument to a vacuum of 10 -5 ~10 -3 Pa condition; then keep the argon gas in to keep the gas pressure at 0.8Pa, and after ignition, sputter the silver source and drain at a power of 10W for 15 minutes;
[0014] 5) Gate preparation: Use a diamond pen to scrape the silicon dioxide layer at a corner of the silicon wafer to expose the silicon. Use conductive silver glue to stick a small piece of copper foil on the exposed silicon to make a gate. All transistors on the entire silicon wafer share this gate.
[0015] Furthermore, in the step 2), the specific steps of cleaning the substrate are as follows: the oxidized silicon wafer is placed in deionized water and alcohol in turn, cleaned with an ultrasonic cleaner for 15 minutes respectively, then blown dry with a nitrogen gun, heated on a 100°C heating table for 15 minutes, and finally cleaned with UV ozone for 30 minutes.
[0016] Furthermore, in the step 3), the semiconductor solution is prepared as follows: the organic semiconductor material and the organic solvent are prepared at a mass volume ratio of 5 mg / mL; the prepared semiconductor solution is placed on a heating table at 80°C and heated for more than 12 hours. The semiconductor material is a polymer IDT-BT; and the organic solvent is o-dichlorobenzene, i.e., DCB solution.
[0017] Furthermore, in the step 3), the spin coating method is as follows: pre-spin coating at a speed of 500 rpm for 3 seconds, and then spin coating at a speed of 2000 rpm for 60 seconds.
[0018] Furthermore, in the step 3), the annealing method is as follows: pre-annealing at 80° C. for 5 minutes, and then annealing at 150° C. for 30 minutes.
[0019] The invention also provides a P-type polymer field effect transistor prepared by the preparation method.
[0020] Magnetron sputtering is a conventional metal deposition process, which is widely used in the manufacture of inorganic semiconductor devices such as silicon-based and oxides, but it is rarely used in organic semiconductor devices. This is mainly due to the fact that most of the early high-performance organic semiconductors are small molecule materials, which are single crystal or polycrystalline, and are easily damaged by high-energy physics during magnetron sputtering, resulting in poor electrical contact and device performance. Therefore, the electrode preparation of most organic devices to date has adopted low-rate thermal evaporation. The donor-acceptor conjugated polymer used in the present invention is a new type of high-performance polymer semiconductor, which is very sensitive to electrical contact. Conventional low-speed thermal evaporation will cause a large amount of metal body diffusion and interface metal oxidation, and the device performance is not optimal. The inventors noticed that the annealing temperature of this type of semiconductor after film formation is above 150 degrees Celsius, and the microstructure is close to amorphous, so the physical microstructure damage caused by magnetron sputtering is not obvious, and magnetron sputtering avoids metal oxidation caused by high-temperature heating, which is very beneficial to gold-semiconductor contact. The experimental results of the present invention prove this idea. By optimizing the process parameters, the performance of the final manufactured device has obvious advantages over that of conventional thermal evaporation devices. So far, there has been no relevant literature report on such devices, so it has certain superiority and innovation.
[0021] The present invention has the following technical effects:
[0022] 1) The present invention uses a magnetron sputtering electrode preparation process to prepare silver source and drain electrodes on the upper surface of the semiconductor active layer under the self-alignment of the mask. Since magnetron sputtering usually uses low-pressure inert gas glow discharge to generate incident ions. The cathode target is made of silver, a coating material, and a silicon wafer sample is used as an anode. 0.8Pa of argon or other inert gas is introduced into the vacuum chamber, and a glow discharge is generated under the action of 1-3KV DC negative high voltage or 13.56MHz radio frequency voltage of the cathode (target). The ionized argon ions bombard the target surface, causing the target silver atoms to sputter out and deposit on the silicon wafer covered with the mask to form a thin film. Since the sputtered atoms are sputtered out after exchanging kinetic energy with positive ions with an energy of tens of electron volts, the sputtered atoms have high energy, which is beneficial to improve the diffusion ability of atoms during deposition, improve the density of the deposited structure, and make the produced film have strong adhesion to the surface of the silicon wafer. Unlike traditional vacuum evaporation, it does not require very high temperatures to form metal vapor, so the temperature in the cavity is very low, which makes the temperature rise of the silicon wafer surface very small, and will not cause serious thermal damage to the semiconductor film. In addition, the low temperature also makes it difficult for silver metal to oxidize to form silver oxide, reducing the impact on the charge transfer between the source and drain and the active layer. Therefore, the present invention can improve the electrical performance of the P-type polymer field effect transistor.
[0023] 2) The polymer field effect transistor prepared by the present invention has a better contact effect between the metal electrode and the semiconductor active layer. The carrier mobility and output current of the device are significantly improved, and the threshold voltage of the device is also reduced. It can be seen that the present invention improves the electrical performance of the bottom-gate top-contact polymer transistor, has the characteristics of simple process steps, convenient operation, and easy to be widely used. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the cross-sectional structure of the polymer field effect transistor of Comparative Example 1 and Example 1;
[0025] Figure 2 It is a comparison diagram of the transfer characteristic curves of the P-type polymer field effect transistor prepared in comparative example 1 and example 1, wherein the solid line represents the transfer characteristic curve of the P-type polymer field effect transistor prepared in example 1, and the dotted line represents the transfer characteristic curve of the P-type polymer field effect transistor prepared in comparative example 1. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0027] The present invention provides embodiments and comparative examples below. Figure 1 1 is a cross-sectional schematic diagram of Example 1 of the present invention and Comparative Example 1. Each layer in the figure is represented by a rectangle. This table is for illustrative purposes only and is not intended to limit the scope of the present invention.
[0028] The sources of materials involved in this invention are described as follows:
[0029] Reagents and Materials Manufacturer IDT-BT Sigma-Aldrich DCB Sigma-Aldrich
[0030] The sources of the equipment involved in the present invention are described as follows:
[0031] Experimental Instruments Manufacturer Ultrasonic cleaning machine Fuxiang Ultrasonic Cleaning Equipment Co., Ltd. UV ozone cleaning machine Novascan Spin Coater Jiangsu Leibo Scientific Instrument Co., Ltd. Vacuum Evaporation Equipment Shenyang Chuangyi Vacuum Technology Co., Ltd. Magnetron sputtering Shenyang Pengcheng Vacuum Technology Co., Ltd.
[0032] Comparative Example 1
[0033] Fabrication of contact electrodes for polymer field effect transistors using vacuum evaporation
[0034] Step 1: Solution preparation
[0035] A1: Preparation of semiconductor solution
[0036] The organic semiconductor material and the organic solvent are prepared at a mass volume ratio of 5 mg / mL; wherein the semiconductor material is a polymer IDT-BT; and the organic solvent is o-dichlorobenzene, i.e., DCB solution;
[0037] A2: Dissolution of solution
[0038] Place the prepared semiconductor solution on a heating table at 80°C and heat for more than 12 hours;
[0039] Step 2: Device preparation
[0040] B1: Substrate preparation
[0041] Choose silicon wafers produced by Suzhou Yancai Micro-Nano Technology Co., Ltd., which have a 300nm silicon dioxide oxide layer on their surface when they leave the factory, and can be directly used as an insulating layer. Cut them into 1.5cm±0.2cm square pieces;
[0042] B2: Substrate cleaning
[0043] Place the oxidized silicon wafer in deionized water and alcohol in turn, clean it with an ultrasonic cleaner for 15 minutes respectively, blow it dry with a nitrogen gun, heat it on a 100℃ heating table for 15 minutes, and finally clean it with UV ozone for 30 minutes;
[0044] B3: Preparation of semiconductor thin films
[0045] Use air blowing to clean the surface of the silicon wafer, and use a pipette to spread the prepared semiconductor solution, i.e., IDT-BT solution, on the surface of the silicon wafer. Use a spin coater to pre-spin coat at a speed of 500 rpm for 3 seconds, and then spin coat at a speed of 2000 rpm for 60 seconds. After the spin coating is completed, pre-anneal at 80°C for 5 minutes, and then anneal at 150°C for 30 minutes. After the time is up, cool for about 30 minutes.
[0046] B4: Preparation of source and drain electrodes
[0047] Using vacuum evaporation technology, silver particles were first placed on the No. 1 evaporation boat of the vacuum evaporator, and then the stainless steel source and drain mask was cleaned and placed on the semiconductor film of the silicon wafer and sent into the chamber of the evaporator. The mechanical pump and molecular pump were used to evacuate the chamber of the evaporator to a vacuum degree of 5×10 -4 Pa; turn on the evaporation boat, adjust the power control knob to gradually increase the evaporation power; finally, the thermal evaporation current reaches 95A, and a silver source and drain electrode with a thickness of about 50nm is prepared at a rate of 0.1nm / s; finally, slowly reduce the power, wait for the cavity to cool for about 20 minutes, fill it with nitrogen, open the cavity and take out the silicon wafer;
[0048] B5: Gate Preparation
[0049] At one corner of the silicon wafer, a diamond pen is used to scrape the silicon dioxide layer to expose the silicon. A small piece of copper foil is glued to the exposed silicon using conductive silver glue to form a gate. All transistors on the entire silicon wafer share this one gate.
[0050] Example 1
[0051] Step 1: Solution preparation
[0052] A1: Preparation of semiconductor solution
[0053] The organic semiconductor material and the organic solvent are prepared at a mass volume ratio of 5 mg / mL; wherein the semiconductor material is a polymer IDT-BT; and the organic solvent is o-dichlorobenzene, i.e., DCB solution;
[0054] A2: Dissolution of solution
[0055] Place the prepared semiconductor solution on a heating table at 80°C and heat for more than 12 hours;
[0056] Step 2: Device preparation
[0057] B1: Substrate preparation
[0058] Choose silicon wafers produced by Suzhou Yancai Micro-Nano Technology Co., Ltd., which have a 300nm silicon dioxide oxide layer on their surface when they leave the factory, and can be directly used as an insulating layer. Cut them into 1.5cm±0.2cm square pieces;
[0059] B2: Substrate cleaning
[0060] Place the oxidized silicon wafer in deionized water and alcohol in turn, clean it with an ultrasonic cleaner for 15 minutes respectively, blow it dry with a nitrogen gun, heat it on a 100℃ heating table for 15 minutes, and finally clean it with UV ozone for 30 minutes;
[0061] B3: Preparation of semiconductor thin films
[0062] Use air blowing to clean the surface of the silicon wafer, and use a pipette to spread the prepared semiconductor solution, i.e., IDT-BT solution, on the surface of the silicon wafer. Use a spin coater to pre-spin coat at a speed of 500 rpm for 3 seconds, and then spin coat at a speed of 2000 rpm for 60 seconds. After the spin coating is completed, pre-anneal at 80°C for 5 minutes, and then anneal at 150°C for 30 minutes. After the time is up, cool for about 30 minutes.
[0063] B4: Preparation of source and drain electrodes
[0064] Using magnetron sputtering technology, the silver target is first placed on the A target of the vacuum sputtering instrument, and then the stainless steel source and drain mask is cleaned and placed on the semiconductor film of the silicon wafer and sent into the cavity of the sputtering instrument. The mechanical pump and molecular pump are used to evacuate the sputtering chamber to a vacuum degree of 5×10 -4 Pa; then keep the argon gas in to keep the gas pressure at about 0.8Pa, and after ignition, sputter the silver source and drain at a power of 10W for about 15 minutes;
[0065] B5: Gate Preparation
[0066] At one corner of the silicon wafer, a diamond pen is used to scrape the silicon dioxide layer to expose the silicon. A small piece of copper foil is glued to the exposed silicon using conductive silver glue to form a gate. All transistors on the entire silicon wafer share this one gate.
[0067] like Figure 1 As shown, Figure 1 Schematic diagram of the cross-sectional structure of the P-type polymer field effect transistor prepared in this embodiment and comparative example 1; the P-type polymer field effect transistor has a bottom gate top contact structure, and the transistor comprises source and drain electrodes, a semiconductor active layer, a silicon dioxide insulating layer and a silicon gate from top to bottom.
[0068] Figure 2 The figure is a comparison of the transfer characteristic curves of the polymer field effect transistor obtained in comparative example 1 and example 1. Figure 2 It can be seen that the transfer characteristic curve of the transistor in Example 1 using the contact electrode manufactured by the magnetron sputtering method has a significant improvement over the transistor performance using the electrode prepared by evaporation. As shown in Table 1, the electrical parameters such as mobility, subthreshold swing, threshold voltage and contact resistance of the two devices are listed. For the polymer field effect transistor in the comparative example, its mobility is 0.021 cm 2 / V·s, subthreshold swing is 4.77V / dec, threshold voltage reaches 18.25V, and contact resistance reaches 8.45×10 2 Ω·cm; while for the polymer field effect transistor of Example 1 of the present invention, its mobility is 0.100cm 2 / V·s, subthreshold swing is 3.35V / dec, threshold voltage is 8.40V, and contact resistance is 2.08×10 2 Therefore, from the above electrical parameter indicators, it can be seen that the electrical performance of the polymer field effect transistor prepared by the present invention has been significantly improved.
[0069] Table 1
[0070] Electrical parameters Vacuum evaporation Magnetron sputtering Threshold voltage (V) 18.25 8.40 Subthreshold swing (V / dec) 4.77 3.35 <![CDATA[Mobility (cm 2 / V·s)]]> 0.021 0.100 Contact resistance (Ω·cm) <![CDATA[8.45×10 2 ]]> <![CDATA[2.08×10 2 ]]>
[0071] The magnetron sputtering method does not require a high temperature environment to prepare contact electrodes. Its principle is to use energetic particles to bombard the target surface in a vacuum, so that the bombarded particles are deposited on the substrate. Therefore, this method will not cause thermal damage to the semiconductor active layer when preparing the source and drain, reduce the effects of diffusion and penetration, and make the film more flat and compact, and the interface smoother. In addition, high temperature can easily cause metal materials to oxidize, and the conductivity of their oxides will be greatly reduced. The sputtering method avoids the occurrence of these chemical reactions, reduces the injection barrier, and makes the electrical contact closer to theoretical speculation. The results show that the performance of devices using sputtering electrical contacts is significantly improved compared to that of devices using thermal evaporation electrical contacts, such as a 5-fold increase in mobility, a reduction of about 10V in threshold voltage, and a reduction of more than 70% in contact resistance; this is mainly due to the optimization of metal-semiconductor contacts, which improves charge injection and subsequent charge transport, thereby improving device performance overall.
[0072] Therefore, the preparation method of the present invention can improve the electrical performance of the P-type polymer field effect transistor and solve the related problems in the preparation of the contact electrode. Moreover, since the preparation method of the transistor is simple, it has a very profound significance for realizing the application of the polymer field effect transistor.
Claims
1. A method for preparing a polymer field effect transistor based on magnetron sputtering, It is characterized in that The polymer field effect transistor has a bottom gate top contact structure, and the preparation method comprises the following steps: firstly, a layer of silicon dioxide is oxidized on the surface of a silicon wafer as an insulating layer, then an organic semiconductor active layer is spin-coated on the surface of the silicon dioxide, then a layer of silver is prepared on the active layer by a magnetron sputtering method through a mask plate as a source and a drain, and finally each transistor on the silicon wafer is isolated and a copper foil and a conductive silver paste are used for gate treatment; The specific steps include: 1) Substrate preparation: Take a silicon wafer with a 300nm silicon dioxide oxide layer on the surface and cut it into 1.5cm±0.2cm square pieces, in which the silicon dioxide oxide layer is directly used as an insulating layer; 2) Cleaning of substrate; 3) Preparation of semiconductor film: Spread the semiconductor solution on the surface of the silicon wafer and spin coat it using a spin coater; anneal after the spin coating and then cool for 30 minutes; 4) Preparation of source and drain electrodes: Using magnetron sputtering technology, first place the silver target on the A target of the vacuum sputtering instrument, then clean the stainless steel source and drain mask, cover it on the semiconductor film of the silicon wafer and send it into the cavity of the sputtering instrument, and use a mechanical pump and a molecular pump to pump the sputtering instrument cavity to 10 -5 ~10 -3 Pa; then keep the argon gas flowing in to keep the gas pressure at 0.8Pa, and after ignition, sputter the silver source and drain at a power of 10W for 15 minutes; 5) Gate preparation: Use a diamond pen to scrape the silicon dioxide layer at one corner of the silicon wafer to expose the silicon, and use conductive silver glue to stick a small piece of copper foil on the exposed silicon to make a gate. All transistors on the entire silicon wafer share this gate; In the step 2), the specific steps of cleaning the substrate are as follows: the oxidized silicon wafer is placed in deionized water and alcohol in turn, and cleaned with an ultrasonic cleaner for 15 minutes respectively, then blown dry with a nitrogen gun, placed on a heating table at 100°C for 15 minutes, and finally cleaned with UV ozone for 30 minutes; In the step 3), the semiconductor solution is prepared as follows: the organic semiconductor material and the organic solvent are prepared at a mass volume ratio of 5 mg / mL; the prepared semiconductor solution is placed on a heating table at 80° C. and heated for more than 12 hours; The semiconductor material is a polymer IDT-BT; the organic solvent is o-dichlorobenzene, namely, DCB solution.
2. The preparation method according to claim 1, It is characterized in that In the step 3), the spin coating method is as follows: pre-spin coating at a speed of 500 rpm for 3 seconds, and then spin coating at a speed of 2000 rpm for 60 seconds.
3. The preparation method according to claim 1, It is characterized in that In the step 3), the annealing method is as follows: pre-annealing at 80° C. for 5 minutes, and then annealing at 150° C. for 30 minutes.
4. A P-type polymer field effect transistor prepared by the preparation method as described in any one of claims 1 to 3.