A test method for self-healing performance of self-repairing concrete cracks

By prefabricating cracks on concrete specimens and applying water pressure to measure the anti-seepage pressure ratio, the problem in the existing technology of being unable to quantitatively evaluate the self-healing performance of self-healing concrete cracks is solved, and the quantitative evaluation and engineering of self-healing concrete are realized. Normative guidance for application.

CN114689827BActive Publication Date: 2024-10-15BEIJING BUILDING MATERIAL INSPECTION RES INST CO LT
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202210188136.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-28
Publication Date
2024-10-15
Estimated Expiration
2042-02-28

AI Technical Summary

Technical Problem

The existing technology lacks a reasonable and effective testing method to quantitatively evaluate the crack self-healing performance of self-healing concrete. It cannot detect and evaluate the ability of concrete to repair different crack widths, which affects its anti-crack and waterproof performance in engineering applications.

Method used

The self-healing specimens of concrete with cracks and the self-healing specimens of benchmark concrete were used to conduct impermeability pressure tests. The self-healing performance of self-healing concrete was evaluated by applying water pressure step by step and measuring the impermeability pressure ratio. Precast concrete with different widths Cracks and self-healing properties are represented by the impermeability pressure ratio.

Benefits of technology

It has achieved a quantitative evaluation of the self-healing performance of cracks of different widths in self-healing concrete, standardized the preparation and engineering application of crystalline self-healing concrete, and ensured the crack-resistant and waterproof performance of the concrete structure.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of self-repairing concrete detection, and in particular to a method for testing the self-healing performance of self-repairing concrete cracks, the method comprising: performing an anti-seepage pressure test on a self-healing concrete specimen with cracks and a reference concrete specimen with self-healing to obtain the anti-seepage pressure of the self-healing concrete specimen with cracks and the anti-seepage pressure of the reference concrete specimen with self-healing, and evaluating the self-healing performance of the self-repairing concrete cracks by the anti-seepage pressure ratio of the self-healing concrete specimen with cracks to the reference concrete specimen with self-healing. The testing method provided by the present invention can reasonably and effectively evaluate the self-healing performance of self-repairing concrete, so as to standardize and guide the preparation and application of new self-repairing materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of self-repairing concrete detection, and in particular to a method for testing the self-healing performance of self-repairing concrete cracks. Background Art

[0002] Self-repairing concrete is a new type of composite material that imitates the regeneration and recovery mechanism of animal bone tissue structure after trauma. It uses a composite method of repairing adhesives and concrete materials to have the function of self-repairing and regenerating damaged materials, and can restore or even improve material performance. At present, there are three main types of self-healing concrete. The first type is to add hollow capsules or glass fibers containing adhesives into concrete materials, and use water glass, diluted water glass and epoxy resin as repair agents respectively, which are injected into hollow capsules or hollow glass fibers. Once the concrete cracks under the action of external force, some capsules or hollow fibers will rupture, and the adhesive will flow out and penetrate deep into the cracks. The adhesive can heal the concrete cracks again; the second type of microbial self-healing method refers to the use of silica gel, polyurethane or porous clay particles to encapsulate active microbial bacteria and the raw materials required for their growth, which are added to the concrete at the initial mixing stage. When cracks appear in the concrete, under suitable environmental conditions, the carrier ruptures, and the active microorganisms metabolize under the cement-based material to produce calcite (CaCO3) precipitation, thereby achieving the purpose of healing the cracks; the third type is to add special active inorganic materials and organic compounds into the concrete, relying on their own further hydration reaction and the characteristics of slow hardening of organic matter under alkaline conditions to produce new crystals, so that the concrete cracks can achieve the purpose of self-healing and self-passivation.

[0003] Concrete structures are often inevitably cracked in engineering applications due to their high brittleness. This cracking leads to reduced water tightness and leakage in concrete structures, affecting the service life of the project and even making it impossible to use it normally. This is a common problem in the construction industry. Self-healing concrete can solve technical problems that are difficult or impossible to solve with traditional methods. It has great potential in many aspects, such as timely repair of major civil infrastructure and mitigation of the impact of typhoons and earthquakes. It is extremely important to ensure the safety and durability of buildings, and it also poses a strong challenge to traditional building material research, manufacturing, defect prevention and repair.

[0004] At present, the domestic standard GB1845-201 "Cement-based Penetrating Crystalline Waterproof Coating" has a test method for the anti-seepage performance of concrete mixed with waterproofing agents, but this method cannot detect and quantitatively evaluate the width of cracks that can be repaired and healed in concrete. Therefore, there is an urgent need for a reasonable test method to quantitatively evaluate the width of self-healing cracks in self-repairing concrete, to consider the ability of concrete to repair cracks of different widths, so as to standardize and guide the preparation of crystalline self-repairing concrete and its anti-cracking and waterproofing applications in different concrete structure projects. Summary of the invention

[0005] In order to solve the above technical problems, in view of the lack of a reasonable and effective testing method for the self-healing performance of self-repairing concrete cracks in the prior art, the present invention provides a testing method for the self-healing performance of self-repairing concrete cracks.

[0006] Specifically, the testing method for the self-healing performance of self-repairing concrete cracks provided by the present invention includes: performing an anti-seepage pressure test on a self-healing concrete specimen with cracks and a reference concrete self-healing specimen to obtain the anti-seepage pressure of the self-healing concrete specimen with cracks and the anti-seepage pressure of the reference concrete self-healing specimen, and evaluating the self-healing performance of the self-repairing concrete cracks based on the anti-seepage pressure ratio of the self-healing concrete specimen with cracks to the reference concrete self-healing specimen.

[0007] The self-healing performance testing method of self-repairing concrete of the present invention prefabricates cracks on concrete specimens and measures the concrete's impermeability pressure by applying water pressure step by step. The self-healing performance of the concrete is expressed as the impermeability pressure ratio. The testing method provided by the present invention can reasonably and effectively quantify and evaluate the self-healing performance of cracks of different widths in self-repairing concrete, so as to standardize and guide the preparation of crystalline self-repairing concrete and its anti-crack and waterproofing applications in different concrete structure projects.

[0008] Preferably, the cracked concrete self-healing specimen is a concrete self-healing specimen with a crack width of 0.2 to 1.2 mm, preferably, the cross section of the crack is cross-shaped; and / or, the crack is obtained by preferably a cross-shaped plug, preferably a cross-shaped stainless steel plug, preferably, the thickness of the cross-shaped plug is 0.2 to 1.2 mm, preferably 0.3 ± 0.05 mm, 0.4 ± 0.05 mm, 0.5 ± 0.05 mm, 0.6 ± 0.05 mm, 0.8 ± 0.05 mm, 1.0 ± 0.05 mm. More preferably, the thickness of the cross-shaped plug is 0.5 ± 0.05 mm.

[0009] Further preferably, the long side of the cross plug is 70-90mm, the wide side is 50-70mm, and the height is 145-155mm; the long side of the cross crack is 70-90mm, the short side is 50-70mm, and the crack depth is 95-105mm; preferably, the long side of the cross plug is 80±1mm, the wide side is 60±1mm, and the height is 150±5mm; the long side of the cross crack is 80±1mm, the short side is 60±1mm, and the crack depth is 100±5mm; the material of the cross plug is preferably stainless steel 304, and the surface is sprayed with a PTFE coating with a thickness of 20-30μm. In the present invention, the cross plug using this material and coating has better rigidity, corrosion resistance and easy demoulding.

[0010] In experimental research, the present invention found that by using cracked concrete self-healing specimens with specific crack parameters, the width of cracks that the concrete can self-repair can be intuitively and simply detected, which can enable quantitative evaluation of the ability of crystalline self-repairing concrete to self-heal cracks of different widths, better guarantee the quality of different crack-resistant and anti-seepage concrete structure projects, thereby better standardizing and guiding the mix design and preparation of crystalline self-repairing concrete, as well as the crack-resistant and waterproof applications of different concrete structure projects.

[0011] Further preferably, the cracked concrete self-healing specimen and the reference concrete self-healing specimen are both truncated cones; preferably, the first bottom surface diameter of the truncated cone is 175±5 mm, the second bottom surface diameter is 185±5 mm, and the height is 150±5 mm; preferably, the cracks of the cracked concrete self-healing specimen are formed on the second bottom surface of the truncated cone, that is, the specimen is formed by an inverted molding method, which is convenient for the production of cracks.

[0012] Further preferably, the preparation of the cracked concrete self-healing specimen comprises: inserting a cross-shaped plug into the specimen before the initial setting of the concrete, and pulling out the plug after the final setting of the concrete.

[0013] Further preferably, when the cracked concrete self-healing specimen is formed, two layers of material are loaded, and the surface is smoothed with a spatula by manual tamping. Before the initial setting of the concrete, a cross-shaped plug is inserted into the specimen, and the intersection of the cross coincides with the second bottom surface point of the truncated cone. After the final setting of the concrete (curing for 7 to 9 hours), the cross-shaped plug is pulled out.

[0014] Preferably, the anti-seepage pressure test conditions include: the water pressure range applied in the anti-seepage pressure test is 0.1 to 2.0 MPa; preferably, the initial water pressure of the test is 0.1 MPa, and then the water pressure is increased by 0.1 MPa every 7 to 9 hours.

[0015] Further preferably, during the anti-seepage pressure test, when water is found to be seeping out from the periphery of the cracked concrete self-healing specimen or the reference concrete self-healing specimen, the reagent sealing is performed again.

[0016] Preferably, the cracked concrete self-healing specimens and the reference concrete self-healing specimens are each in 1 to 4 groups. During the anti-seepage pressure test, each group of specimens consists of 6±1 specimens. The average water pressure when 3 to 4 specimens in each group have no water seepage is taken as the anti-seepage pressure.

[0017] Further preferably, the self-healing performance of cracks of different widths of the self-repairing concrete is evaluated according to the anti-seepage pressure ratio and the crack width of the self-healing specimen of cracked concrete without water seepage; preferably, the larger the anti-seepage pressure ratio, the better the self-healing performance of the self-repairing concrete cracks; the larger the crack width, that is, the thickness of the plug, the better the self-healing performance of the self-repairing concrete cracks; preferably, the crack width is not less than 0.5 mm, and the anti-seepage pressure ratio is not less than 0.9.

[0018] Further preferably, the anti-seepage pressure is obtained according to the end face water seepage of the cracked concrete self-healing specimen or the reference concrete self-healing specimen; specifically, when water seepage appears on the surfaces of three specimens in a group of specimens, or when less than three of the six specimens have end face water seepage within 8 hours after the specified pressure is applied, the test is stopped and the water pressure at this time is recorded as the anti-seepage pressure.

[0019] Further preferably, the preparation of the reference concrete self-healing specimen comprises: according to the self-repairing concrete dry powder and water addition amount; or the self-repairing concrete mixture, preferably the mixture used for each group of reference concrete self-healing specimens is sampled from the same plate of concrete or the same truck of concrete, the concrete is poured into an inverted truncated cone mold, preferably the truncated cone mold has an inner diameter of 185 mm with the lower opening on the top and an inner diameter of 175 mm on the bottom, and the reference concrete self-healing specimen is formed according to GB / T50082; three groups of reference concrete self-healing specimens are formed simultaneously for each test, with six specimens in each group; the material is loaded in two layers during molding, and the surface is manually inserted and rammed; Scrape it flat with a spatula, place it in a standard curing room, and let it stand for 1 day to demould; after demoulding, immerse the specimen in water with a depth of three-quarters of the specimen height for curing at a water temperature of 20±2℃ and an ambient humidity of more than 95% for water curing for 27 days; one day before reaching the test age, take out the specimen from the curing tank and wipe it clean; after the surface of the specimen is dried, seal the specimen with paraffin wax, and apply a layer of melted paraffin wax with rosin on the side of the specimen; then use a spiral press to press the specimen into a test mold preheated in an oven or an electric furnace, so that the specimen is flush with the bottom of the test mold, and release the pressure after the test mold cools down; the preheating temperature of the test mold is based on the paraffin wax slowly melting in contact with the test mold but not flowing.

[0020] Further preferably, the preparation of the self-healing concrete specimen with cracks includes: according to the self-repairing concrete dry powder and water addition amount; or the self-repairing concrete mixture, preferably the mixture used for each group of reference concrete self-healing specimens is sampled from the same plate of concrete or the same truck of concrete, the concrete is poured into an inverted truncated cone mold, preferably the lower opening of the truncated cone with an internal diameter of 185 mm is on the top, and the upper opening of the internal diameter of 175 mm is on the bottom, and the reference concrete self-healing specimen is formed according to GB / T50082; three groups of reference concrete self-healing specimens are formed simultaneously for each test, with six specimens in each group; the materials are loaded in two layers during molding, and a manual tamping method is adopted; the surface is scraped flat with a spatula, and a "cross" stainless steel plug is inserted into the specimen before the concrete is initially set. After the specimen is cured for 8h and finally set, the stainless steel plug is pulled out to make concrete self-healing specimens with cracks of different widths, which are placed in a standard curing room and demoulded after standing for 1 day; the demoulding specimens are immersed in water with a depth of three-quarters of the specimen height for curing at a water temperature of 20±2℃ and an ambient humidity of more than 95% for water curing for 27 days; one day before reaching the test age, the specimen is taken out of the curing water tank and wiped clean; after the surface of the specimen is dried, the specimen is sealed with paraffin wax, and a layer of melted paraffin wax with rosin is coated on the side of the specimen; then a spiral press is used to press the specimen into a test mold preheated in an oven or an electric furnace so that the specimen is flush with the bottom of the test mold, and the pressure is released after the test mold becomes cold; the preheating temperature of the test mold is based on the paraffin wax slowly melting in contact with the test mold but not flowing.

[0021] Preferably, the self-repairing concrete is crystalline self-repairing concrete.

[0022] The beneficial effects of the present invention are at least as follows: the present invention adopts a method of prefabricating cracks of different widths on concrete specimens, adopts a step-by-step pressurization method, tests the self-healing performance of self-repairing concrete cracks, and the self-healing performance of concrete represented by the impermeability pressure ratio can quantitatively evaluate the width of cracks repaired by crystalline self-repairing concrete; the detection method in the current standard is to first detect the first impermeability pressure for 28 days, then maintain it with the mold for another 56 days, and then detect the second impermeability pressure, that is, after the first impermeability pressure is measured, the specimen is penetrated, but this method does not clearly know the crack conditions and width of the breakdown, and cannot quantitatively evaluate the width and self-healing ability of the repairable cracks. The self-healing performance test method of the self-repairing concrete of the present invention can quantitatively evaluate the self-healing ability of crystalline self-repairing concrete through crack width and impermeability pressure ratio. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described below. The following examples are used to illustrate the present invention, but are not used to limit the scope of the present invention. If the specific technology or conditions are not specified in the embodiments, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased through regular channels.

[0024] The test materials in the embodiments of the present invention are self-repairing concrete dry powder or self-repairing concrete mixture provided by the manufacturer. The test mold has an upper inner diameter of 175 mm, a lower inner diameter of 185 mm and a height of 150 mm. The plug piece is a "cross" stainless steel sheet with a long side of 80 mm, a wide side of 60 mm, and a height of 100 mm. The thickness of the stainless steel sheet in the present invention is 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.8 mm, 1.0 mm, etc. Specifically, a 0.5 mm thick "cross" stainless steel sheet is used in the following embodiments.

[0025] The following test instruments are used in the embodiments of the present invention: Concrete mixing adopts a single-horizontal shaft forced mixer or other types of forced mixers, and the concrete mixing should be ensured to be uniform. The mixer and vibration table used should comply with the provisions of the current industry standards "Mixer for Concrete Test" JG244 and "Vibration Table for Concrete Test" JG / T245 respectively. The concrete impermeability tester complies with the provisions of the current industry standard "Concrete Impermeability Tester" JG / T249, and can make the water pressure act on the test piece stably according to the prescribed system. The water pressure range of the impermeability tester is 0.1~2.0MPa.

[0026] In the standard curing conditions adopted in the embodiments of the present invention, the ambient temperature is (20±2)° C. and the humidity is greater than 95%.

[0027] The test piece in the embodiment of the present invention is prepared as follows:

[0028] 1. Preparation of benchmark concrete self-healing specimens

[0029] According to the self-healing concrete dry powder and water addition provided by the manufacturer; or the self-healing concrete mixture, the mixture used for each group of specimens should be sampled from the same plate of concrete or the same truck of concrete, and the concrete is poured into an inverted truncated cone mold, that is, the lower opening of the truncated cone with an internal diameter of 185mm is on the top, and the upper opening with an internal diameter of 175mm is on the bottom, and the benchmark concrete self-healing specimens are formed according to GB / T50082; three groups of benchmark concrete self-healing specimens are formed simultaneously for each test, with six specimens in each group; the materials are loaded in two layers during molding, and the manual tamping method is adopted; the surface is scraped flat with a spatula, placed in a standard curing room, and left to stand for 1 day Demoulding; then the reference specimen is immersed in water with a depth of three-quarters of the specimen height for curing, the water temperature is (20±2)℃, and the environmental humidity is greater than 95% for water curing for 27 days; one day before reaching the test age, the specimen is taken out from the curing tank and wiped clean; after the surface of the specimen is dried, the specimen is sealed with paraffin wax, and a layer of melted paraffin wax with rosin is coated on the side of the specimen; then the screw press is used to press the specimen into the test mold preheated in an oven or electric furnace, so that the specimen is flush with the bottom of the test mold, and the pressure should be released after the test mold becomes cold; the preheating temperature of the test mold should be based on the paraffin wax contacting the test mold, that is, slowly melting but not flowing.

[0030] 2. Preparation of cracked concrete self-healing specimens

[0031] According to the self-repairing concrete dry powder and water addition provided by the manufacturer; or the self-repairing concrete mixture, the mixture used for each group of specimens should be sampled from the same plate of concrete or the same truck of concrete, and the concrete is poured into an inverted truncated cone mold, that is, the lower opening with an internal diameter of 185mm of the truncated cone is on the top, and the upper opening with an internal diameter of 175mm is on the bottom. The benchmark concrete self-healing specimens are formed according to GB / T50082. Three groups of benchmark concrete self-healing specimens are formed simultaneously for each test, with six specimens in each group; the molding is divided into two layers of loading, and the surface is smoothed with a spatula by manual tamping; before the initial setting of the concrete, a "cross" shaped stainless steel plug is inserted into the specimen, and the intersection of the cross coincides with the second bottom surface point of the truncated cone. The concrete specimen is cured for 8 hours and finally set. After that, the stainless steel plug is pulled out to make concrete self-healing specimens with cracks of different widths, which are placed in a standard curing room and left to stand for 1 day before demoulding; then the reference specimen is immersed in water with a depth of three-quarters of the specimen height for curing, the water temperature is (20±2)℃, and the ambient humidity is greater than 95% for water curing for 27 days; one day before reaching the test age, the specimen is taken out from the curing water tank and wiped clean; after the surface of the specimen is dried, the specimen is sealed with paraffin, and a layer of melted paraffin with rosin is coated on the side of the specimen; then the screw press is used to press the specimen into a test mold preheated in an oven or an electric furnace, so that the specimen is flush with the bottom of the test mold, and the pressure should be released after the test mold becomes cold; the preheating temperature of the test mold should be based on the paraffin contacting the test mold, that is, slowly melting but not flowing.

[0032] The specific test in this embodiment adopts the step-by-step pressurization method, which measures the anti-seepage pressure of the self-healing concrete specimen with cracks and the reference concrete self-healing specimen by applying water pressure step by step, and the self-healing performance of the concrete is expressed by the anti-seepage pressure ratio. The specific test steps are as follows:

[0033] 1) During the test, the water pressure starts from 0.1MPa, and then increases by 0.1MPa every 8 hours, and the water seepage of the specimen end face is observed at any time; when 3 out of 6 specimens have surface seepage, or when less than 3 out of 6 specimens have surface seepage within 8 hours after the specified pressure is applied, the test is stopped and the water pressure at this time is recorded; during the test, if water is found to seep out from the periphery of the specimen, it is re-sealed with paraffin; the anti-seepage pressure of concrete is the water pressure when 3 out of 6 specimens in each group do not have water seepage.

[0034] 2) The anti-seepage pressure ratio is the ratio of the anti-seepage pressure of the cracked concrete self-healing specimen to the anti-seepage pressure of the reference concrete self-healing specimen under the same conditions (same molding, same curing, same age, same test). The larger the anti-seepage pressure ratio, the better the self-healing performance of the self-healing concrete; the larger the crack width of the non-water-seepage specimen, the better the self-healing performance of the self-healing concrete.

[0035] Example 1

[0036] 1. Preparation of benchmark concrete self-healing specimens

[0037] According to the self-healing concrete dry powder and water addition provided by the manufacturer; or the self-healing concrete mixture, the mixture used for each group of specimens should be sampled from the same plate of concrete or the same truck of concrete, and the concrete is poured into an inverted truncated cone mold, that is, the lower opening of the truncated cone with an internal diameter of 185mm is on the top, and the upper opening with an internal diameter of 175mm is on the bottom, and the benchmark concrete self-healing specimens are formed according to GB / T50082; three groups of benchmark concrete self-healing specimens are formed simultaneously for each test, with six specimens in each group; the materials are loaded in two layers during molding, and the manual tamping method is adopted; the surface is scraped flat with a spatula, placed in a standard curing room, and left to stand for 1 day Demoulding; then the reference specimen is immersed in water with a depth of three-quarters of the specimen height for curing, the water temperature is (20±2)℃, and the environmental humidity is greater than 95% for water curing for 27 days; one day before reaching the test age, the specimen is taken out from the curing tank and wiped clean; after the surface of the specimen is dried, the specimen is sealed with paraffin wax, and a layer of melted paraffin wax with rosin is coated on the side of the specimen; then the screw press is used to press the specimen into the test mold preheated in an oven or electric furnace, so that the specimen is flush with the bottom of the test mold, and the pressure should be released after the test mold becomes cold; the preheating temperature of the test mold should be based on the paraffin wax contacting the test mold, that is, slowly melting but not flowing.

[0038] 2. Preparation of cracked concrete self-healing specimens

[0039] According to the self-repairing concrete dry powder and water addition provided by the manufacturer; or the self-repairing concrete mixture, the mixture used for each group of specimens should be sampled from the same pan of concrete or the same truck of concrete, and the concrete is poured into an inverted truncated cone mold, that is, the lower opening with an internal diameter of 185mm of the truncated cone is on the top, and the upper opening with an internal diameter of 175mm is on the bottom. The benchmark concrete self-healing specimens are formed according to GB / T50082. Three groups of benchmark concrete self-healing specimens are formed simultaneously for each test, with six specimens in each group; the molding is divided into two layers of loading, and the surface is smoothed with a spatula by manual tamping; before the initial setting of the concrete, a "cross" shaped stainless steel plug is inserted into the specimen, and the intersection of the cross does not coincide with the second bottom surface point of the truncated cone. The concrete specimen is cured for 8 hours. After solidification, the stainless steel plug is pulled out to make concrete self-healing specimens with cracks of different widths, which are placed in a standard curing room and demoulded after standing for 1 day. The reference specimen is then immersed in water with a depth of three-quarters of the specimen height for curing at a water temperature of (20±2)°C and an ambient humidity of more than 95% for water curing for 27 days. One day before reaching the test age, the specimen is taken out of the curing water tank and wiped clean. After the surface of the specimen is dried, it is sealed with paraffin wax, and a layer of melted paraffin wax with rosin is coated on the side of the specimen. Then, a spiral press is used to press the specimen into a test mold preheated in an oven or an electric furnace so that the specimen is flush with the bottom of the test mold, and the pressure should be released after the test mold becomes cold. The preheating temperature of the test mold should be such that the paraffin wax contacts the test mold, that is, it melts slowly but does not flow.

[0040] The specific test in this embodiment adopts the step-by-step pressurization method, which measures the anti-seepage pressure of the self-healing concrete specimen with cracks and the reference concrete self-healing specimen by applying water pressure step by step, and the self-healing performance of the concrete is expressed by the anti-seepage pressure ratio. The specific test steps are as follows:

[0041] 1) During the test, the water pressure starts from 0.1MPa, and then increases by 0.1MPa every 8 hours, and the water seepage of the specimen end face is observed at any time; when 3 out of 6 specimens have surface seepage, or when less than 3 out of 6 specimens have surface seepage within 8 hours after the specified pressure is applied, the test is stopped and the water pressure at this time is recorded; during the test, if water is found to seep out from the periphery of the specimen, it is re-sealed with paraffin; the anti-seepage pressure of concrete is the water pressure when 3 out of 6 specimens in each group do not have water seepage.

[0042] 2) The anti-seepage pressure ratio is the ratio of the anti-seepage pressure of the cracked concrete self-healing specimen to the anti-seepage pressure of the reference concrete self-healing specimen under the same conditions (same molding, same curing, same age, same test). The larger the anti-seepage pressure ratio, the better the self-healing performance of the self-healing concrete; the larger the crack width of the non-water-seepage specimen, the better the self-healing performance of the self-healing concrete.

[0043] The main problem in this example is that the cross intersection of the cross plug does not coincide with the second bottom point of the truncated cone. After repeated experiments, it was found that the data of the impermeability pressure and the impermeability pressure ratio of the cracked concrete specimen were highly discrete.

[0044] Example 2

[0045] 1. Preparation of benchmark concrete self-healing specimens

[0046] According to the self-healing concrete dry powder and water addition provided by the manufacturer; or the self-healing concrete mixture, the mixture used for each group of specimens should be sampled from the same plate of concrete or the same truck of concrete, and the concrete is poured into a frustum mold placed upright, that is, the lower opening of the frustum with an internal diameter of 175mm is on the top, and the upper opening with an internal diameter of 185mm is on the bottom, and the reference concrete self-healing specimens are formed according to GB / T50082; three groups of reference concrete self-healing specimens are formed simultaneously for each test, with six specimens in each group; the materials are loaded in two layers during molding, and the manual tamping method is adopted; the surface is scraped flat with a spatula, placed in a standard curing room, and left to stand for 1 day Demoulding; then the reference specimen is immersed in water with a depth of three-quarters of the specimen height for curing, the water temperature is (20±2)℃, and the environmental humidity is greater than 95% for water curing for 27 days; one day before reaching the test age, the specimen is taken out from the curing tank and wiped clean; after the surface of the specimen is dried, the specimen is sealed with paraffin wax, and a layer of melted paraffin wax with rosin is coated on the side of the specimen; then the screw press is used to press the specimen into the test mold preheated in an oven or electric furnace, so that the specimen is flush with the bottom of the test mold, and the pressure should be released after the test mold becomes cold; the preheating temperature of the test mold should be based on the paraffin wax contacting the test mold, that is, slowly melting but not flowing.

[0047] 2. Preparation of cracked concrete self-healing specimens

[0048] According to the self-healing concrete dry powder and water addition provided by the manufacturer; or the self-healing concrete mixture, the mixture used for each group of specimens should be sampled from the same plate of concrete or the same truck of concrete, and the concrete is poured into an upright truncated cone mold, that is, the lower opening with an internal diameter of 175mm of the truncated cone is on the top, and the upper opening with an internal diameter of 185mm is on the bottom. The benchmark concrete self-healing specimens are formed according to GB / T50082. Three groups of benchmark concrete self-healing specimens are formed simultaneously for each test, with six specimens in each group; the material is loaded in two layers during molding, and the surface is flattened with a spatula by manual tamping; before the initial setting of the concrete, a "cross" stainless steel plug is inserted into the specimen, and the intersection of the cross coincides with the first bottom surface point of the truncated cone. The concrete specimen is cured for 8 hours and finally set. After that, the stainless steel plug is pulled out to make concrete self-healing specimens with cracks of different widths, which are placed in a standard curing room and left to stand for 1 day before demoulding; then the reference specimen is immersed in water with a depth of three-quarters of the specimen height for curing, the water temperature is (20±2)℃, and the ambient humidity is greater than 95% for water curing for 27 days; one day before reaching the test age, the specimen is taken out from the curing water tank and wiped clean; after the surface of the specimen is dried, the specimen is sealed with paraffin, and a layer of melted paraffin with rosin is coated on the side of the specimen; then the screw press is used to press the specimen into a test mold preheated in an oven or an electric furnace, so that the specimen is flush with the bottom of the test mold, and the pressure should be released after the test mold becomes cold; the preheating temperature of the test mold should be based on the paraffin contacting the test mold, that is, slowly melting but not flowing.

[0049] The specific test in this embodiment adopts the step-by-step pressurization method, which measures the anti-seepage pressure of the self-healing concrete specimen with cracks and the reference concrete self-healing specimen by applying water pressure step by step, and the self-healing performance of the concrete is expressed by the anti-seepage pressure ratio. The specific test steps are as follows:

[0050] 1) During the test, the water pressure starts from 0.1MPa, and then increases by 0.1MPa every 8 hours, and the water seepage of the specimen end face is observed at any time; when 3 out of 6 specimens have surface seepage, or when less than 3 out of 6 specimens have surface seepage within 8 hours after the specified pressure is applied, the test is stopped and the water pressure at this time is recorded; during the test, if water is found to seep out from the periphery of the specimen, it is re-sealed with paraffin; the anti-seepage pressure of concrete is the water pressure when 3 out of 6 specimens in each group do not have water seepage.

[0051] 2) The anti-seepage pressure ratio is the ratio of the anti-seepage pressure of the cracked concrete self-healing specimen to the anti-seepage pressure of the reference concrete self-healing specimen under the same conditions (same molding, same curing, same age, same test). The larger the anti-seepage pressure ratio, the better the self-healing performance of the self-healing concrete; the larger the crack width of the non-water-seepage specimen, the better the self-healing performance of the self-healing concrete.

[0052] The main problem in this example is that the cross intersection of the cross plug does not coincide with the second bottom point of the truncated cone. After repeated experiments, it was found that the data of the impermeability pressure and the impermeability pressure ratio of the cracked concrete specimen were highly discrete.

[0053] This example mainly adopts the method of placing the truncated cone mold upright and pouring concrete to form the specimen. The "cross" stainless steel plug is inserted into the first bottom surface of the specimen, and the intersection of the cross coincides with the first bottom surface of the truncated cone. After repeated experiments, it was found that the data of the impermeability pressure and the impermeability pressure ratio of this cracked concrete specimen are relatively discrete.

[0054] Example 3

[0055] 1. Preparation of benchmark concrete self-healing specimens

[0056] According to the self-healing concrete dry powder and water addition provided by the manufacturer; or the self-healing concrete mixture, the mixture used for each group of specimens should be sampled from the same plate of concrete or the same truck of concrete, and the concrete is poured into an inverted truncated cone mold, that is, the lower opening of the truncated cone with an internal diameter of 185mm is on the top, and the upper opening with an internal diameter of 175mm is on the bottom, and the benchmark concrete self-healing specimens are formed according to GB / T50082; three groups of benchmark concrete self-healing specimens are formed simultaneously for each test, with six specimens in each group; the materials are loaded in two layers during molding, and the manual tamping method is adopted; the surface is scraped flat with a spatula, placed in a standard curing room, and left to stand for 1 day Demoulding; then the reference specimen is immersed in water with a depth of three-quarters of the specimen height for curing, the water temperature is (20±2)℃, and the environmental humidity is greater than 95% for water curing for 27 days; one day before reaching the test age, the specimen is taken out from the curing tank and wiped clean; after the surface of the specimen is dried, the specimen is sealed with paraffin wax, and a layer of melted paraffin wax with rosin is coated on the side of the specimen; then the screw press is used to press the specimen into the test mold preheated in an oven or electric furnace, so that the specimen is flush with the bottom of the test mold, and the pressure should be released after the test mold becomes cold; the preheating temperature of the test mold should be based on the paraffin wax contacting the test mold, that is, slowly melting but not flowing.

[0057] 2. Preparation of cracked concrete self-healing specimens

[0058] According to the self-repairing concrete dry powder and water addition provided by the manufacturer; or the self-repairing concrete mixture, the mixture used for each group of specimens should be sampled from the same plate of concrete or the same truck of concrete, and the concrete is poured into an inverted truncated cone mold, that is, the lower opening with an internal diameter of 185mm of the truncated cone is on the top, and the upper opening with an internal diameter of 175mm is on the bottom. The benchmark concrete self-healing specimens are formed according to GB / T50082. Three groups of benchmark concrete self-healing specimens are formed simultaneously for each test, with six specimens in each group; the molding is divided into two layers of loading, and the surface is smoothed with a spatula by manual tamping; before the initial setting of the concrete, a "cross"-shaped metal plug is inserted into the specimen, and the intersection of the cross coincides with the second bottom surface point of the truncated cone. The concrete specimen is cured for 8 hours and finally set. After that, the metal plug is pulled out to make concrete self-healing specimens with cracks of different widths, which are placed in a standard curing room and demoulded after standing for 1 day. The reference specimen is then immersed in water with a depth of three-quarters of the specimen height for curing at a water temperature of (20±2)℃ and an ambient humidity of more than 95% for water curing for 27 days. One day before reaching the test age, the specimen is taken out from the curing water tank and wiped clean. After the surface of the specimen is dried, it is sealed with paraffin wax, and a layer of melted paraffin wax with rosin is coated on the side of the specimen. Then, a spiral press is used to press the specimen into a test mold preheated in an oven or an electric furnace so that the specimen is flush with the bottom of the test mold, and the pressure should be released after the test mold becomes cold. The preheating temperature of the test mold should be such that the paraffin wax contacts the test mold, that is, it melts slowly but does not flow.

[0059] The specific test in this embodiment adopts the step-by-step pressurization method, which measures the anti-seepage pressure of the self-healing concrete specimen with cracks and the reference concrete self-healing specimen by applying water pressure step by step, and the self-healing performance of the concrete is expressed by the anti-seepage pressure ratio. The specific test steps are as follows:

[0060] 1) During the test, the water pressure starts from 0.1MPa, and then increases by 0.1MPa every 8 hours, and the water seepage of the specimen end face is observed at any time; when 3 out of 6 specimens have surface seepage, or when less than 3 out of 6 specimens have surface seepage within 8 hours after the specified pressure is applied, the test is stopped and the water pressure at this time is recorded; during the test, if water is found to seep out from the periphery of the specimen, it is re-sealed with paraffin; the anti-seepage pressure of concrete is the water pressure when 3 out of 6 specimens in each group do not have water seepage.

[0061] 2) The anti-seepage pressure ratio is the ratio of the anti-seepage pressure of the cracked concrete self-healing specimen to the anti-seepage pressure of the reference concrete self-healing specimen under the same conditions (same molding, same curing, same age, same test). The larger the anti-seepage pressure ratio, the better the self-healing performance of the self-healing concrete; the larger the crack width of the non-water-seepage specimen, the better the self-healing performance of the self-healing concrete.

[0062] In this example, the cross-shaped plug is made of ordinary metal sheets, and the cross intersection coincides with the second bottom point of the truncated cone. After repeated experiments, it was found that the data of the impermeability pressure and the impermeability pressure ratio of the cracked concrete specimen were highly discrete. The main reason is that the ordinary metal plug is not easy to be pulled out of the specimen and is prone to rust, resulting in irregular concave and convex marks on both sides of the crack.

[0063] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A method for testing the self-healing performance of self-repairing concrete cracks, characterized in that: include: The cracked concrete self-healing specimen and the reference concrete self-healing specimen are subjected to an anti-seepage pressure test under the same conditions to obtain the anti-seepage pressure of the cracked concrete self-healing specimen and the anti-seepage pressure of the reference concrete self-healing specimen, and the self-healing performance of the self-repairing concrete cracks is evaluated by the anti-seepage pressure ratio of the cracked concrete self-healing specimen to the reference concrete self-healing specimen; the anti-seepage pressure test conditions include: the water pressure applied in the anti-seepage pressure test is in the range of 0.1-2.0 MPa, the initial water pressure of the test is 0.1 MPa, and then the water pressure is increased by 0.1 MPa every 7-9 hours; The cross section of the crack is cross-shaped, and the crack is obtained by a cross-shaped plug. The thickness of the cross-shaped plug is 0.3±0.05mm, 0.4±0.05mm, 0.5±0.05mm, 0.6±0.05mm, 0.8±0.05mm, 1.0±0.05mm. The crack width of the self-healing concrete specimen with cracks corresponds to the thickness of the cross-shaped plug. The long side of the cross-shaped plug is 70~90mm, the wide side is 50~70mm, and the height is 145~155mm; the long side of the cross-shaped crack is 70~90mm, the short side is 50~70mm, and the crack depth is 95~105mm; the cross-shaped plug is made of stainless steel 304, and the surface is sprayed with a polyfluoro coating with a thickness of 20~30µm; The number of the cracked concrete self-healing specimens and the reference concrete self-healing specimens is 1 to 4, and during the anti-seepage pressure test, each group of specimens is 6±1, and the average water pressure when 3 to 4 specimens in each group do not seep water is taken as the anti-seepage pressure; The self-healing performance of cracks of different widths of the self-repairing concrete is evaluated according to the anti-seepage pressure ratio and the crack width of the self-healing concrete specimen with cracks without water seepage; the larger the anti-seepage pressure ratio, the better the self-healing performance of the self-repairing concrete cracks; the larger the crack width, the better the self-healing performance of the self-repairing concrete cracks.

2. The method for testing the self-healing performance of self-repairing concrete cracks according to claim 1, characterized in that: The long side of the cross-shaped plug is 80±1mm, the wide side is 60±1mm, and the height is 100±5mm; the long side of the cross-shaped crack is 80±1mm, the short side is 60±1mm, and the crack depth is 100±5mm.

3. The method for testing the self-healing performance of self-repairing concrete cracks according to claim 2, characterized in that: The cracked concrete self-healing specimen and the reference concrete self-healing specimen are both truncated cones.

4. The method for testing the self-healing performance of self-repairing concrete cracks according to claim 3 is characterized in that: The first bottom surface diameter of the truncated cone is 175±5 mm, the second bottom surface diameter is 185±5 mm, and the height is 150±5 mm.

5. The method for testing the self-healing performance of self-repairing concrete cracks according to claim 4, characterized in that: The cracks of the cracked concrete self-healing test piece are formed on the second bottom surface of the truncated cone body.

6. The method for testing the self-healing performance of self-repairing concrete cracks according to claim 1, characterized in that: The preparation of the cracked concrete self-healing specimen comprises: inserting a cross-shaped plug into the specimen before the initial setting of the concrete, and pulling out the plug after the final setting of the concrete.

7. The method for testing the self-healing performance of self-repairing concrete cracks according to claim 6, characterized in that: When the cracked concrete self-healing specimen is formed, two layers of material are loaded, and the surface is smoothed with a spatula by manual tamping. Before the initial setting of the concrete, a cross-shaped plug is inserted into the specimen, and the intersection of the cross coincides with the second bottom surface point of the truncated cone. After the final setting of the concrete, the cross-shaped plug is pulled out.

8. The method for testing the self-healing performance of self-repairing concrete cracks according to any one of claims 1 to 7, characterized in that: During the anti-seepage pressure test, when water is found to be seeping out from the periphery of the cracked concrete self-healing specimen or the reference concrete self-healing specimen, the reagent seal is performed again.

Citation Information

Cited By

  • Permeation reaction calculation method of inorganic gel in porous medium

    CN120452634A