A continuous fiber reinforced thermoplastic prepreg yarn surface treatment method and use method thereof

By treating the surface of continuous fiber-reinforced thermoplastic prepreg filaments, coating the resin matrix and removing the solvent, the problems of low material interface performance and insufficient bonding are solved, and the interface shear of the automatic filament laying and winding in-situ curing processes is improved. Shear strength improves the accuracy and application effect of the molding process.

CN114701091BActive Publication Date: 2024-10-25江苏亨博复合材料有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210248474.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-14
Publication Date
2024-10-25
Estimated Expiration
2042-03-14

Smart Images

  • Figure CN114701091B_ABST
    Figure CN114701091B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for treating the surface of continuous fiber reinforced thermoplastic prepreg and its use method, belonging to the technical field of surface treatment of prepreg. The present invention proposes a method for treating the surface of continuous fiber reinforced thermoplastic prepreg and its use method, wherein the upper nozzle and the lower nozzle face the upper and lower surfaces of the prepreg, and the pump body is used to draw the solution to the spray box, and the solution is sprayed on the upper and lower surfaces of the prepreg in two ways. The heating ring is driven to rotate by a reduction motor; the power-on ring is in contact with the conductive ring sheet, the position of the power-on ring is fixed, and the conductive ring sheet rotates synchronously with the heating ring, and the power-on ring and the conductive ring sheet are energized in the contact state, so that the inner ring and the heating ring can always provide electric energy to the heating sheet during the rotation process, so that the heating sheet can generate heat while rotating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of prepreg filament surface, and in particular to a continuous fiber reinforced thermoplastic prepreg surface treatment method and a use method thereof. Background Art

[0002] A continuous carbon fiber reinforced thermoplastic prepreg, especially a continuous carbon fiber reinforced high-performance thermoplastic prepreg, is used in some domestic special equipment as well as aerospace, nuclear power and other industries. The molding processes involved mainly include rapid molding, automatic wire placement in-situ curing, winding in-situ curing, etc. Among them, the automatic wire placement in-situ curing and winding in-situ curing processes have the advantages of fast efficiency, no need for secondary curing, and the ability to form large parts. It has always been a high-tech molding process vigorously developed by aerospace and special equipment.

[0003] A continuous fiber reinforced thermoplastic prepreg can be manufactured by co-extrusion, slurry method, powder method and the like. The continuous fiber reinforced thermoplastic prepreg filaments suitable for automatic filament placement in-situ curing and winding in-situ curing processes need to have good wettability. At present, some materials provided by domestic and foreign companies have basically solved the wettability problem, and some companies have successfully made corresponding products using this material. However, these materials were found to have low interface performance, high requirements for precision control of molding process parameters, and defects such as unbonded and insufficient bonding at the material interface during the manufacturing process using automatic filament placement in-situ curing and winding in-situ curing processes, which greatly affect the application of the materials. Summary of the invention

[0004] The object of the present invention is to provide a continuous fiber reinforced thermoplastic prepreg surface treatment method and a use method thereof, so as to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for surface treatment of continuous fiber reinforced thermoplastic prepreg yarn, comprising the following steps:

[0006] S1: The prepreg filaments are conveyed through the surface coating device and the post-processing device through the unwinding device and the winding device;

[0007] S2: wherein the resin coated on the surface of the prepreg by the surface coating device is consistent with or has similar properties to the resin matrix of the prepreg filaments;

[0008] S3: The post-processing device is used to remove the solvent of the solution and emulsion coating applied in S2, so that the solute adheres to the surface of the prepreg yarn, thereby achieving the requirement of increasing the resin-rich content of the prepreg surface.

[0009] Further, with respect to S1, the prepreg filaments are composed of a resin matrix of thermoplastic prepreg filaments and prepreg reinforcing fibers;

[0010] The unwinding device and the winding device are controlled by tension, wherein the tension control range is 5-100N / cm, and the resin matrix of the thermoplastic prepreg filament includes but is not limited to PAEK, PPS, PEI, PI, PP, PC, and PA;

[0011] Prepreg reinforcing fibers include but are not limited to carbon fibers, glass fibers, aramid fibers, basalt fibers, PBO fibers, etc.; the prepreg fiber surface density is 10-300 g / ㎡; and the prepreg resin volume content is 30-60%.

[0012] Further, with respect to S2, the coating material form includes but is not limited to solution form and emulsion form; the coating method of the solution and emulsion form coating includes but is not limited to spraying and dipping;

[0013] The solvent of the coating in the form of solution and emulsion can be water or organic solvent, and the coating amount coated on the surface of the prepreg is controlled, and the amount of the coating is 1-10% of the mass of the prepreg yarn.

[0014] Furthermore, in S3, the post-processing device 4 has heating and ventilation functions to accelerate the volatilization of the solvent, and the heating temperature is greater than 100°C; if the solvent is an organic matter, a solvent recovery device 5 needs to be added.

[0015] Furthermore, the unwinding device comprises an unwinding wheel, a front pressing wheel and a front support frame, wherein the unwinding wheel is mounted on the front support frame, and the front pressing wheel is mounted on the front support frame through a position adjustment device, wherein the unwinding wheel is sleeved with prepreg filaments, the front pressing wheel is pressed against the prepreg filaments, and the position adjustment device is used to adjust the front pressing wheel so that it is always pressed against the prepreg filaments when the unwinding wheel rotates;

[0016] The position adjustment device includes a wheel frame, a cylinder and a cylinder rod, wherein the cylinder is fixed on the front support frame, one end of the cylinder rod is connected to the piston rod in the cylinder, and the other end of the cylinder rod is connected to the wheel frame, wherein both ends of the front pressure wheel are inserted into the bearings of the wheel frame.

[0017] Furthermore, the winding device includes a winding wheel, a rear support frame and a two-stage reduction motor. The two-stage reduction motor is installed on the rear support frame. The shaft of the two-stage reduction motor is connected to one end of the winding wheel. The other end of the winding wheel is inserted into the bearing of the rear support frame. The winding wheel is driven to rotate by the two-stage reduction motor, and the winding wheel winds the prepreg filament.

[0018] Further, the surface coating device includes a front baffle plate, a rear baffle plate, a front support wheel, a rear support wheel, a spray box and a double-sided coating assembly, the front support wheel and the rear support wheel are inserted side by side on the bearing between the front baffle plate and the rear baffle plate, and the spray box is connected to the double-sided coating assembly;

[0019] The double-sided coating assembly includes an upper nozzle, a lower nozzle, a spray pipe and a nozzle. The spray box is connected to the spray pipe through a pump body. The spray pipe is divided into two paths and connected to the upper nozzle and the lower nozzle respectively. The upper nozzle and the lower nozzle face the upper and lower surfaces of the prepreg filaments.

[0020] Furthermore, the post-processing device includes a heating ring, an air guide ring, an energizing ring, a limiting ring, a heating plate, a reduction motor and a transmission wheel. The limiting ring is sleeved on the outside of the heating ring, and the heating ring rotates inside the limiting ring. The transmission wheel connected to the reduction motor is in contact with the heating ring, and the heating ring is driven to rotate by the reduction motor.

[0021] The heating ring is provided with a concentric inner ring inside, and the annular channel formed between the inner ring and the heating ring is divided into a plurality of independent spaces by a partition, wherein the heating plates are placed one by one in the space between the inner ring and the heating ring, and the cables connected to the heating plates are connected to the conductive ring plates on the sealing inner ring and the heating ring port, and the energized ring is in contact with the conductive ring plates;

[0022] The air guide ring seals the inner ring and the other port of the heating ring. The hole on the air guide ring is connected to the hole in the independent space. The ring sheet for introducing gas is sleeved on the air guide ring, and the gas enters the space where the heating sheet is located.

[0023] The inner ring is provided with ventilation holes corresponding to and communicating with the space where the heating plate is located, and the ventilation holes face the prepreg filaments.

[0024] Furthermore, the solvent recovery device includes a receiving dish, a negative pressure pipe and a gas collecting hood. The receiving dish is placed below the prepreg filaments. The negative pressure pipe is connected to the gas collecting hood. The gas collecting hood spans across both sides of the heating ring and is used to absorb organic solvents.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. A method for surface treatment of continuous fiber reinforced thermoplastic prepreg and a method for using the same are provided in the present invention. Both ends of the front pressure wheel are inserted into the bearings of the wheel frame. During the rotation of the unwinding wheel, the amount of prepreg filaments gradually decreases, and the cylinder drives the front pressure wheel to move toward the unwinding wheel, so that the front pressure wheel can always exert a certain extrusion force on the prepreg filaments, thereby preventing the prepreg filaments from detaching quickly.

[0027] 2. The present invention proposes a method for surface treatment of continuous fiber reinforced thermoplastic prepreg and its use method. The upper nozzle and the lower nozzle are directed to the upper and lower surfaces of the prepreg filaments. The solution is drawn to the spray box by a pump body and sprayed on the upper and lower surfaces of the prepreg filaments in two ways. The heating ring is driven to rotate by a reduction motor; the power-on ring is in contact with the conductive ring sheet, the position of the power-on ring is fixed, and the conductive ring sheet rotates synchronously with the heating ring. When the power-on ring and the conductive ring sheet are energized in the contact state, the inner ring and the heating ring can always provide electrical energy to the heating sheet during the rotation process, so that it can generate heat while rotating. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is the overall structure diagram of the present invention;

[0029] Figure 2 It is a side view of the unwinding device of the present invention;

[0030] Figure 3 It is a structural diagram of the winding device of the present invention;

[0031] Figure 4 It is a structural diagram of the surface coating device of the present invention;

[0032] Figure 5 A top view of the surface coating device of the present invention;

[0033] Figure 6 It is a three-dimensional diagram of the post-processing device of the present invention;

[0034] Figure 7 is a cross-sectional view of a post-processing device of the present invention;

[0035] Figure 8 It is a side view of the post-processing device of the present invention;

[0036] Fig. 9 It is a structural diagram of the solvent recovery device of the present invention.

[0037] In the figure: 1. unwinding device; 11. unwinding wheel; 12. front pressure wheel; 13. front support frame; 14. position adjustment device; 141. wheel frame; 142. cylinder; 143. cylinder rod; 2. winding device; 21. winding wheel; 22. rear support frame; 23. two-stage reduction motor; 3. surface coating device; 31. front baffle plate; 32. rear baffle plate; 33. front support wheel; 34. rear support wheel; 35. spray box; 36. double-sided coating assembly; 361. upper nozzle; 362. lower nozzle; 363. spray pipe; 4. post-processing device; 41. heating ring; 411. inner ring; 42. air guide ring; 43. power ring; 44. limit ring; 45. heating plate; 46. reduction motor; 47. transmission wheel; 5. solvent recovery device; 51. collecting dish; 52. negative pressure pipe; 53. gas collecting hood. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Embodiment 1:

[0040] See also Figure 1-8 A method for surface treatment of continuous fiber reinforced thermoplastic prepreg yarns comprises the following steps:

[0041] Step 1: The prepreg yarn is continuously conveyed through the surface coating device 3 and the post-processing device 4 by the unwinding device 1 and the winding device 2, wherein the prepreg yarn is composed of a resin matrix of the thermoplastic prepreg yarn and prepreg reinforcing fibers;

[0042] The unwinding device 1 and the rewinding device 2 are controlled by tension, wherein the tension control range is 5-100N / cm, and the resin matrix of the thermoplastic prepreg filament includes but is not limited to PAEK, PPS, PEI, PI, PP, PC, and PA;

[0043] Prepreg reinforcing fibers include but are not limited to carbon fibers, glass fibers, aramid fibers, basalt fibers, PBO fibers, etc.; the prepreg fiber surface density is 10-300 g / ㎡; and the prepreg resin volume content is 30-60%.

[0044] Step 2: wherein the resin coated on the surface of the prepreg by the surface coating device 3 is consistent with or has similar properties to the resin matrix of the prepreg wire, and the coating material form includes but is not limited to solution form and emulsion form; the coating method of the solution and emulsion form coating includes but is not limited to spraying and dipping;

[0045] The coating solution and emulsion coating solvent can be water or organic solvent, and the coating amount on the prepreg surface is controlled, and the coating amount is 1-10% of the prepreg yarn mass;

[0046] Step three: the post-processing device 4 is used to remove the solvent of the solution and emulsion coating applied in S2, so that the solute adheres to the surface of the prepreg yarn, thereby achieving the requirement of increasing the resin-rich content of the prepreg surface. The post-processing device 4 has heating and ventilation functions to accelerate the volatilization of the solvent, and the heating temperature is greater than 100°C; if the solvent is an organic matter, a solvent recovery device 5 needs to be added.

[0047] The unwinding device 1 comprises an unwinding wheel 11, a front pressing wheel 12 and a front support frame 13, wherein the unwinding wheel 11 is mounted on the front support frame 13, and the front pressing wheel 12 is mounted on the front support frame 13 via a position adjusting device 14, wherein the unwinding wheel 11 is sleeved with prepreg filaments, the front pressing wheel 12 is pressed against the prepreg filaments, and the position adjusting device 14 is used to adjust the front pressing wheel 12 to always press on the prepreg filaments when the unwinding wheel 11 is rotating;

[0048] The position adjustment device 14 includes a wheel frame 141, a cylinder 142 and a cylinder rod 143. The cylinder 142 is fixed on the front support frame 13. One end of the cylinder rod 143 is connected to the piston rod in the cylinder 142, and the other end of the cylinder rod 143 is connected to the wheel frame 141. The two ends of the front pressure wheel 12 are inserted into the bearings of the wheel frame 141. When the unwinding wheel 11 rotates, the amount of prepreg filaments gradually decreases, and the cylinder 142 drives the front pressure wheel 12 to move toward the unwinding wheel 11, so that the front pressure wheel 12 can always have a certain extrusion force on the prepreg filaments, thereby preventing the prepreg filaments from detaching quickly.

[0049] The winding device 2 includes a winding wheel 21, a rear support frame 22 and a two-stage reduction motor 23. The two-stage reduction motor 23 is installed on the rear support frame 22. The shaft of the two-stage reduction motor 23 is connected to one end of the winding wheel 21. The other end of the winding wheel 21 is inserted into the bearing of the rear support frame 22. The winding wheel 21 is driven to rotate by the two-stage reduction motor 23. The winding wheel 21 winds the prepreg wire. The two-stage reduction motor 23 controls the winding rate.

[0050] The surface coating device 3 includes a front baffle plate 31, a rear baffle plate 32, a front support wheel 33, a rear support wheel 34, a spray box 35 and a double-sided coating assembly 36. The front support wheel 33 and the rear support wheel 34 are inserted side by side on the bearing between the front baffle plate 31 and the rear baffle plate 32, and the spray box 35 is connected to the double-sided coating assembly 36.

[0051] The double-sided coating assembly 36 includes an upper nozzle 361, a lower nozzle 362, and a spray pipe 363. The spray box 35 is connected to the spray pipe 363 through a pump body. The spray pipe 363 is connected to the upper nozzle 361 and the lower nozzle 362 in two ways, wherein the upper nozzle 361 and the lower nozzle 362 are directed toward the upper and lower surfaces of the prepreg filaments. The pump body is used to draw the solution into the spray box 35 and spray it on the upper and lower surfaces of the prepreg filaments in two ways.

[0052] The post-processing device 4 includes a heating ring 41, an air guide ring 42, an electric ring 43, a limit ring 44, a heating plate 45, a reduction motor 46 and a transmission wheel 47. The limit ring 44 is sleeved on the outside of the heating ring 41, and the heating ring 41 rotates inside the limit ring 44. The transmission wheel 47 connected to the reduction motor 46 is in contact with the heating ring 41, and the heating ring 41 is driven to rotate through the reduction motor 46.

[0053] A concentric inner ring 411 is provided inside the heating ring 41, and an annular channel formed between the inner ring 411 and the heating ring 41 is divided into a plurality of independent spaces by a partition, wherein the heating plates 45 are placed one by one in the space between the inner ring 411 and the heating ring 41, and the cables connected to the heating plates 45 are connected to the conductive ring plates on the ports of the sealed inner ring 411 and the heating ring 41, and the power-on ring 43 is in contact and connected with the conductive ring plates, the position of the power-on ring 43 is fixed, and the conductive ring plates rotate synchronously with the heating ring 41, and the power-on ring 43 and the conductive ring plates are energized in the contact state, so that the inner ring 411 and the heating ring 41 can always provide electrical energy to the heating plates 45 during the rotation process, so that they can generate heat while rotating;

[0054] The air guide ring 42 seals the other port of the inner ring 411 and the heating ring 41. The hole opened on the air guide ring 42 is connected to the hole of the independent space. The ring sheet for introducing gas is sleeved on the air guide ring 42. The gas enters the space where the heating plate 45 is located. The air guide ring 42 also rotates synchronously with the inner ring 411 and the heating ring 41. The ring sheet does not rotate. There is a certain gap between the ring sheet and the air guide ring 42. The pipe for introducing gas transports the gas to the gap between the ring sheet and the air guide ring 42. The inner ring 411 is provided with ventilation holes corresponding to the space where the heating plate 45 is located, and the ventilation holes face the prepreg filaments. By introducing gas, the gas flows evenly into the space where the heating plate 45 is located, and the gas is discharged after being heated to heat the prepreg filaments.

[0055] The rotating heating method avoids heating or ventilation on the upper and lower sides, which may cause the dripping liquid to heat the lower side.

[0056] The solvent recovery device 5 comprises a collecting dish 51, a negative pressure pipe 52 and a gas collecting hood 53. The collecting dish 51 is placed below the prepreg filaments. The negative pressure pipe 52 is connected to the gas collecting hood 53. The gas collecting hood 53 spans across both sides of the heating ring 41 and is used to absorb organic solvents.

[0057] It solves the defect problem of materials used in automatic wire placement in-situ curing and winding in-situ curing molding processes on the market, greatly reduces the bonding defects of the materials during the automatic wire placement in-situ curing and winding in-situ curing processes, and improves the interface shear strength by more than 20%.

[0058] Embodiment 2:

[0059] See also Fig. 9 The surface coating device 3 is different from the first embodiment in that a container for storing the solution is provided, and the prepreg surface wire passes through the solution in the container and is coated by immersion.

[0060] In summary, in the surface treatment method of continuous fiber reinforced thermoplastic prepreg yarn of the present invention, the two ends of the front pressure wheel 12 are inserted into the bearings of the wheel frame 141. During the rotation of the unwinding wheel 11, the amount of prepreg yarn slowly decreases, and the cylinder 142 drives the front pressure wheel 12 to move toward the unwinding wheel 11, and always maintains that the front pressure wheel 12 can have a certain squeezing force on the prepreg yarn, thereby preventing the prepreg yarn from detaching quickly. The upper nozzle 361 and the lower nozzle 362 are facing the upper and lower surfaces of the prepreg yarn, and the pump body is used to draw the solution to the spray box 35, and spray it on the upper and lower surfaces of the prepreg yarn in two ways. The heating ring 41 is driven to rotate by the reduction motor 46; the power-on ring 43 is in contact and connected with the conductive ring sheet, the position of the power-on ring 43 is fixed, and the conductive ring sheet rotates synchronously with the heating ring 41. When the power-on ring 43 and the conductive ring sheet are energized in the contact state, the inner ring 411 and the heating ring 41 can always provide electric energy to the heating sheet 45 during the rotation process, so that it can generate heat while rotating.

[0061] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for surface treatment of continuous fiber reinforced thermoplastic prepreg yarn, characterized in that: The following steps are involved: S1: The prepreg filaments are conveyed continuously through the surface coating device (3) and the post-processing device (4) by means of the unwinding device (1) and the winding device (2); S2: wherein the resin coated on the surface of the prepreg by the surface coating device (3) is consistent with the resin matrix of the prepreg filaments; S3: a post-processing device (4) is used to remove the solvent of the solution or emulsion coating applied in S2, so that the solute adheres to the surface of the prepreg yarn, thereby achieving the requirement of increasing the resin-rich content of the prepreg surface; The post-processing device (4) comprises a heating ring (41), an air guide ring (42), an energizing ring (43), a limiting ring (44), a heating plate (45), a reduction motor (46) and a transmission wheel (47); the limiting ring (44) is sleeved on the outside of the heating ring (41); the heating ring (41) rotates inside the limiting ring (44); the transmission wheel (47) connected to the reduction motor (46) is in contact with the heating ring (41); the heating ring (41) is driven to rotate by the reduction motor (46); a concentric inner ring (411) is provided inside the heating ring (41); an annular channel formed between the inner ring (411) and the heating ring (41) is divided into a plurality of independent spaces by a partition, wherein the heating plate (41) The sealing ring (411) and the heating ring (41) are placed in a one-to-one correspondence in the space between the inner ring (411) and the heating ring (41), and the cable connected to the heating plate (45) is connected to the conductive ring plate on the port of the sealed inner ring (411) and the heating ring (41), and the power ring (43) is in contact with the conductive ring plate; the air guide ring (42) is arranged at the other port of the sealed inner ring (411) and the heating ring (41), the hole opened on the air guide ring (42) is connected to the hole of the independent space, and the ring plate for introducing gas is sleeved on the air guide ring (42), and the gas enters the space where the heating plate (45) is located; the inner ring (411) is provided with ventilation holes corresponding to the space where the heating plate (45) is located, and the ventilation holes face the prepreg filaments.

2. A method for surface treatment of continuous fiber reinforced thermoplastic prepreg yarn according to claim 1, characterized in that: In S1, the prepreg filaments are composed of a resin matrix of thermoplastic prepreg filaments and prepreg reinforcing fibers; The unwinding device (1) and the rewinding device (2) are controlled by tension, wherein the tension control range is 5-100 N / cm, and the resin matrix of the thermoplastic prepreg filaments comprises PAEK, PPS, PEI, PI, PP, PC, and PA; Prepreg reinforcing fibers include carbon fiber, glass fiber, aramid fiber, basalt fiber and PBO fiber; the fiber surface density of prepreg is 10-300g / ㎡; the volume content of prepreg resin is 30-60%.

3. A method for surface treatment of continuous fiber reinforced thermoplastic prepreg yarn according to claim 1, characterized in that: In S2, the coating material forms include solution form and emulsion form; the coating methods of solution and emulsion form coatings include spraying and dipping; The solvents of the coating in the form of solution and emulsion are water and organic solvents, and the coating amount coated on the surface of the prepreg is controlled, and the amount of the coating is 1-10% of the mass of the prepreg yarn.

4. A method for surface treatment of continuous fiber reinforced thermoplastic prepreg yarn according to claim 1, characterized in that: In S3, the post-treatment device (4) has heating and ventilation functions to accelerate the volatilization of the solvent, and the heating temperature is greater than 100°C; if the solvent is an organic matter, a solvent recovery device (5) needs to be added.

5. The method for surface treatment of continuous fiber reinforced thermoplastic prepreg yarn according to claim 1, characterized in that: The unwinding device (1) comprises an unwinding wheel (11), a front pressing wheel (12) and a front support frame (13), wherein the unwinding wheel (11) is mounted on the front support frame (13), and the front pressing wheel (12) is mounted on the front support frame (13) via a position adjustment device (14), wherein a prepreg filament is sleeved on the unwinding wheel (11), and the front pressing wheel (12) is pressed against the prepreg filament, and the position adjustment device (14) is used to adjust the front pressing wheel (12) so that it is always pressed against the prepreg filament when the unwinding wheel (11) is rotating; The position adjustment device (14) comprises a wheel frame (141), a cylinder (142) and a cylinder rod (143); the cylinder (142) is fixed on the front support frame (13); one end of the cylinder rod (143) is connected to a piston rod in the cylinder (142); and the other end of the cylinder rod (143) is connected to the wheel frame (141); wherein both ends of the front pressure wheel (12) are inserted into bearings of the wheel frame (141).

6. A method for surface treatment of continuous fiber reinforced thermoplastic prepreg yarn according to claim 1, characterized in that: The winding device (2) comprises a winding wheel (21), a rear support frame (22) and a two-stage reduction motor (23); the two-stage reduction motor (23) is mounted on the rear support frame (22); the shaft of the two-stage reduction motor (23) is connected to one end of the winding wheel (21); the other end of the winding wheel (21) is inserted into a bearing of the rear support frame (22); the two-stage reduction motor (23) drives the winding wheel (21) to rotate, and the winding wheel (21) winds the prepreg filament.

7. A method for surface treatment of continuous fiber reinforced thermoplastic prepreg yarn according to claim 1, characterized in that: The surface coating device (3) comprises a front baffle plate (31), a rear baffle plate (32), a front support wheel (33), a rear support wheel (34), a spray box (35) and a double-sided coating assembly (36); the front support wheel (33) and the rear support wheel (34) are inserted side by side on a bearing between the front baffle plate (31) and the rear baffle plate (32); and the spray box (35) is connected to the double-sided coating assembly (36); The double-sided coating assembly (36) comprises an upper nozzle (361), a lower nozzle (362) and a spray pipe (363); the spray box (35) is connected to the spray pipe (363) via a pump body; the spray pipe (363) is divided into two paths and respectively connected to the upper nozzle (361) and the lower nozzle (362); wherein the upper nozzle (361) and the lower nozzle (362) face the upper and lower surfaces of the prepreg filaments.

8. A method for surface treatment of continuous fiber reinforced thermoplastic prepreg yarn according to claim 4, characterized in that: The solvent recovery device (5) comprises a material collecting dish (51), a negative pressure pipe (52) and a gas collecting hood (53); the material collecting dish (51) is placed below the prepreg filaments; the negative pressure pipe (52) is connected to the gas collecting hood (53); the gas collecting hood (53) spans across both sides of the heating ring (41) and is used to absorb organic solvents.

Citation Information

Patent Citations

  • Method for producing semi-curing piece and device thereof

    CN101462361A

  • Preparation method of continuous fiber enhanced thermoplastic resin prepreg and apparatus used therein

    CN105082566A

  • Cloth unwinding device for textile

    CN108820969A

  • Drying device for yarn processing

    CN211575790U

  • Heat treatment of coatings on continuous webs

    GB1412614A