A method and device for quickly detecting welding defects in metal spot welding joints
Through the DC resistance bridge detection method, resistance changes are used to determine welding defects, which solves the existing problems of slow and high cost in welding defect detection, achieving fast and economical welding defect detection, and is suitable for various metal materials.
Patent Information
- Application Number
- CN202210329612.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-30
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-03-30
AI Technical Summary
Existing welding defect detection methods have the problems of slow detection speed, high cost, requiring professional equipment, and are not suitable for welding defect detection of lightweight materials such as aluminum alloys and hot-formed steel.
The DC resistance bridge detection method is used to determine the welding defects by measuring the resistance change of the spot welding joint. The variable resistor and galvanometer are used to realize fast and economical welding defect detection. It is suitable for the spot welding process development and welding quality of metal materials. evaluate.
It realizes fast and low-cost welding defect detection without requiring professional equipment. It is suitable for various metal materials, has fast detection speed and short result determination cycle.
Smart Images

Figure CN114705726B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resistance spot welding process control, and in particular to a method and a device for quickly detecting welding defects in metal spot welding joints. Background Art
[0002] Resistance spot welding is a welding process that uses the Joule heat generated under the action of electrode pressure to melt the surfaces of the contacting metal workpieces, thereby producing a permanent metallurgical bond. Resistance spot welding is widely used in the modern automobile manufacturing industry. There are up to thousands of resistance spot welded joints on an ordinary car. With the development trend of low carbonization of automobiles, the proportion of lightweight materials used in automobiles will gradually increase, such as aluminum alloys, hot-formed high-strength steel, etc. Aluminum alloys have the characteristics of high thermal conductivity, large thermal expansion coefficient, easy oxidation, and large difference in hydrogen solubility in solid / liquid, which makes it easy for defects such as shrinkage cavities and cracks to appear in aluminum alloy weld cores. Hot-formed steel has a high carbon equivalent and often has a layer of aluminum-silicon coating on the surface, which makes its resistance spot welding process parameter window narrow. If the process parameters are not properly controlled, some defects such as shrinkage cavities and incomplete penetration will often appear inside the weld joint, thereby reducing the effective bearing area of the weld joint and affecting the service life and fatigue durability of the welded parts. How to quickly, effectively and economically detect defects in metal resistance spot welded joints has become one of the issues that automotive engineers are increasingly concerned about.
[0003] At present, the non-destructive testing methods for welding defects mainly include: visual inspection, liquid penetrant inspection, X-ray inspection, magnetic particle inspection, ultrasonic inspection and eddy current inspection. Visual inspection and liquid penetrant inspection are only applicable to the inspection of welding surface defects, and the visual inspection method also requires the inspectors to have rich experience. X-ray inspection has high reliability, but X-rays have strong radiation and are extremely harmful to the human body. The inspection cost is high and the inspection cycle is relatively long. Magnetic particle inspection is only applicable to the detection of welding defects of ferromagnetic materials.
[0004] Prior art CN106198721A discloses a non-destructive testing method for thin plate stainless steel resistance spot welding joints, including the following steps: 1) First, check the surface condition of the weld to be inspected to make the surface of the weld flat and free of defects; 2) According to the width range of the weld, select a far-field eddy current detection probe with a matching form and size; 3) According to the thickness of the workpiece, select a matching eddy current excitation frequency; 4) According to the defect-free weld joint, calibrate the instrument; 5) Use the calibrated equipment to detect the resistance spot welding joint to be inspected; 6) According to whether the detection signal changes or not, determine the quality of the resistance spot welding joint. The above eddy current detection is only suitable for the detection of surface defects, but requires professional eddy current flaw detection equipment.
[0005] Prior art CN112756768A discloses a welding quality evaluation method and system based on ultrasonic image feature fusion, including the following steps: 1) First, ultrasonic detection is performed on the backfill stir friction spot welding joint, and the B-scan image and C-scan image of the welding area are collected; 2) The obtained B-scan image and C-scan image are analyzed and processed to extract the effective information in the image and the defect characteristics inside the weld to form a three-dimensional information representation of the welding quality; 3) Different weight coefficients are assigned to the feature quantities in the three-dimensional information representation using information entropy, and then fused into a comprehensive indicator as the evaluation result. The above ultrasonic detection requires that the surface to be detected has a certain degree of smoothness, and requires a coupling medium, and the detection speed is slow. Summary of the invention
[0006] In order to make up for the shortcomings of existing welding defect detection methods, the present invention proposes a method for quickly detecting welding defects in metal spot welding joints based on the conductive principle of metal materials. The method can be used for the development and optimization of metal material spot welding processes and the rapid evaluation of the welding quality of metal spot welding joints.
[0007] In order to solve the above technical problems, the present invention is implemented by the following technical solutions:
[0008] On the one hand, the present invention provides a method for quickly detecting welding defects in metal spot welding joints, wherein the detection device comprises a DC resistance bridge, the DC resistance bridge comprises a power supply, a switch and four bridge arms, the first bridge arm and the second bridge arm are connected in series to form a first series bridge arm group, the third bridge arm and the fourth bridge arm are connected in series to form a second series bridge arm group, the first series bridge arm group and the second series bridge arm group are connected in parallel, a galvanometer is connected between the series connection point of the first bridge arm series group and the series connection point of the second bridge arm series group, the first bridge arm, the second bridge arm and the third bridge arm are sequentially provided with a first resistor R1, a second resistor R2 and a third resistor R3, at least one of the first resistor R1, the second resistor R2 and the third resistor R3 is a variable resistor, and the fourth bridge arm has two connection terminals for connecting a test piece with an external resistor Rs; the detection method comprises:
[0009] S1. Obtain the size of the welding joint at the point to be tested and clean its surface;
[0010] S2, calibrate the variable resistor so that when the relationship between the resistors satisfies R1 / R2=R3 / Rs, the current detection count value is zero;
[0011] S3. Connect the welding head of the test point to a calibrated DC resistance bridge to form a closed circuit, and then record the reading of the galvanometer; if the reading of the galvanometer is zero, it can be determined that there is no welding defect in the area; if the reading of the galvanometer is not zero, it can be determined that there is a welding defect in the area.
[0012] Preferably, in step S1, the step of cleaning the surface of the spot welding joint to be tested is: firstly, cleaning the oil stains on the surface of the spot welding joint, and then removing the oxide layer on the surface of the spot welding joint after drying.
[0013] Preferably, in step S1, the step of obtaining the size of the spot welding joint is: measuring the size of the spot welding joint along mutually perpendicular directions on the surface of the spot welding joint, measuring at least 3 times, and then taking the average value.
[0014] Further preferably, the diameter of the electrode can be determined to be 1 / 3 to 1 / 4 of the measured size of the spot welding joint.
[0015] Preferably, in step S2, the calibration step is: a spot welding joint having the same welding process as the spot welding joint to be tested and known to have no welding defects is placed between two electrodes and clamped, and then the two electrodes are respectively connected to two connecting terminals and a DC resistance bridge to form a closed circuit, and the galvanometer reading is returned to zero by adjusting the variable resistor, and the spot welding joint is removed after the calibration is completed.
[0016] Preferably, in step S3, the step of connecting the spot welding joint to be tested is: placing the spot welding joint to be tested between two electrodes and clamping them, and then connecting the two electrodes to two connection terminals and a DC resistance bridge to form a closed circuit.
[0017] Preferably, the defect type of the spot welding joint can be further determined based on step S3, including: moving the electrode in any direction, recording a reading every time it moves a certain distance, if the electrode movement distance does not exceed the first threshold value, the galvanometer reading returns to zero, then it can be determined that the defect type is a single hole-type defect; if the electrode movement distance exceeds the second threshold value, the galvanometer reading is still not zero, then it can be determined that the defect type is a crack-type defect.
[0018] In another aspect, the present invention provides a device for quickly detecting welding defects in metal spot welding joints, the device comprising:
[0019] A DC resistance bridge, the DC resistance bridge comprises a power supply, a switch and four bridge arms, the first bridge arm and the second bridge arm are connected in series to form a first series bridge arm group, the third bridge arm and the fourth bridge arm are connected in series to form a second series bridge arm group, the first series bridge arm group and the second series bridge arm group are connected in parallel, a galvanometer is connected between the series connection point of the first bridge arm series group and the series connection point of the second bridge arm series group, the first bridge arm, the second bridge arm and the third bridge arm are provided with a first resistor R1, a second resistor R2 and a third resistor R3 in sequence, at least one of the first resistor R1, the second resistor R2 and the third resistor R3 is a variable resistor, and the fourth bridge arm has two connection terminals;
[0020] Two electrodes, the two electrodes are respectively connected to the two connection terminals and form a closed circuit with the DC resistance bridge, and a clamping space for clamping a metal spot welding joint is reserved between the two electrodes; and
[0021] The clamping assembly is fixedly connected to the two electrodes and is used to adjust the clamping distance between the two electrodes.
[0022] Preferably, the clamping assembly comprises:
[0023] Two electrode bases, the two electrode bases are used to fix two electrodes respectively;
[0024] A first connecting member, one end of which is fixedly connected to one of the electrodes;
[0025] a second connecting member, one end of which is fixedly connected to the other electrode, and the other end of which is in contact with the other end of the first connecting member and can move relatively thereto; and
[0026] The locking structure is used to lock the relative displacement distance between the first connecting member and the second connecting member.
[0027] It is further preferred that the first connecting member and the second connecting member both adopt L-shaped metal tubes, the diameter of the first connecting member is smaller than the diameter of the second connecting member, and the end of the first connecting member can be inserted into the second connecting member and can slide relatively; the locking structure includes a bolt and a threaded hole opened on the side wall of the end of the second connecting member, and the bolt can pass through the threaded hole and press the outer wall of the first connecting member inward to lock the first connecting member and the second connecting member.
[0028] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0029] 1) This application utilizes the conductive properties of metal materials to determine whether welding defects occur in the joint by measuring the resistance change of the weld joint at the test point. The detection method is simple and easy to operate, and does not require the operator to have rich experience.
[0030] 2) The method of the present application has low detection cost and does not require expensive professional detection equipment.
[0031] 3) The method of the present application has a fast detection speed and a short result determination cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is the schematic diagram of resistance spot welding defect detection;
[0033] Figure 2 It is a schematic diagram of the structure of a device for quickly detecting welding defects in metal spot welding joints according to the present invention;
[0034] Figure 3It is a side view of the connection portion between the first connecting member and the second connecting member of the present invention (bolts omitted).
[0035] Figure numerals: 1. DC resistance bridge; 2. Metal wire; 3. Pure copper wire; 4. Spot welding joint; 5. Metal plates connected by spot welding; 6. Clamping assembly; 61. Electrode base; 62. First connecting piece; 63. Second connecting piece; 64. Locking structure; 641. Bolt; 642. Threaded hole; 7. Electrode; 8. Connecting terminal. DETAILED DESCRIPTION
[0036] In order to enable those skilled in the art to better understand the technical solution of the present invention, the preferred implementation scheme of the present invention is described below in conjunction with specific embodiments. However, it should be understood that the drawings are only for illustrative purposes and cannot be understood as limiting the present invention. In order to better illustrate the present embodiment, some parts of the drawings may be omitted, enlarged or reduced, and do not represent the size of the actual product. For those skilled in the art, it is understandable that some well-known structures and their descriptions in the drawings may be omitted. The positional relationship described in the drawings is only for illustrative purposes and cannot be understood as limiting the present invention.
[0037] like Figure 1 As shown, the detection principle based on the present invention is as follows:
[0038] The resistance of a metal conductor is not only related to its own resistivity, but also to its geometric shape, inversely proportional to its cross-sectional area, and proportional to its length. When there are welding defects such as holes and microcracks in the spot welding joint, the effective cross-sectional area of the spot welding joint will be reduced, and the resistance value of the spot welding joint will be increased. The present invention is based on the principle of measuring resistance by a Wheatstone bridge to measure the resistance change of the spot welding joint, and then judge whether there are defects in the spot welding joint.
[0039] In a closed circuit, when the resistance Rs of the conductor to be measured and the variable resistor R2 (the resistor R2 is selected as the variable resistor for illustration only, and other resistors may be used) satisfy the relationship R1 / R2=R3 / Rs, the potential difference across the galvanometer is zero, so no current passes through the galvanometer, and its reading is zero; when the resistance Rs of the test piece to be measured and the variable resistor R2 do not satisfy the relationship R1 / R2=R3 / Rs, there will be a potential difference across the galvanometer, which will generate current, causing the pointer of the ammeter to deflect to the left or right, and its reading is not zero. The galvanometer can use a sensitive ammeter to improve the measurement accuracy, and can measure very small current changes in a closed circuit.
[0040] During the calibration and detection process of the present invention, there is no need to determine the specific resistance values used by the first resistor R1, the second resistor R2 and the third resistor R3 and the ratio of R1 / R2. It is only necessary to adjust the variable resistor so that the relationship between the resistors satisfies Rs / R3=R1 / R2, so that the current detection count value is zero, thereby completing the calibration of the spot welding joint known to have no defects.
[0041] like Figure 2 and 3 As shown, the present invention provides a device for quickly detecting welding defects in metal spot welding joints, the device comprising:
[0042] A DC resistance bridge 1, the DC resistance bridge 1 comprises a power supply, a switch and four bridge arms, the first bridge arm and the second bridge arm are connected in series to form a first series bridge arm group, the third bridge arm and the fourth bridge arm are connected in series to form a second series bridge arm group, the first series bridge arm group and the second series bridge arm group are connected in parallel, a galvanometer is connected between the series connection point of the first bridge arm series group and the series connection point of the second bridge arm series group, the first bridge arm, the second bridge arm and the third bridge arm are provided with a first resistor R1, a second resistor R2 and a third resistor R3 in sequence, at least one of the first resistor R1, the second resistor R2 and the third resistor R3 is a variable resistor, and two connection terminals 8 for an external test piece with a resistance Rs are formed on the fourth bridge arm;
[0043] Two electrodes 7, the two electrodes 7 are respectively connected to the two connection terminals and form a closed circuit with the DC resistance bridge 1, and a clamping space for clamping the metal spot welding joint 4 is reserved between the two electrodes 7; and
[0044] The clamping assembly 6 is fixedly connected to the two electrodes 7 and is used to adjust the size of the clamping space between the two electrodes 7 .
[0045] Wherein, the clamping assembly 6 comprises:
[0046] Two electrode bases 61, the two electrode bases 61 are used to fix the two electrodes 7 respectively;
[0047] A first connecting member 62, one end of which is fixedly connected to one of the electrodes 7;
[0048] A second connecting member 63, one end of which is fixedly connected to another electrode 7, and the other end of which is in contact with the other end of the first connecting member 62 and can move relatively thereto; and
[0049] The locking structure 64 is used to lock the relative displacement distance between the first connecting member 62 and the second connecting member 63 .
[0050] In a specific implementation process, both the first connecting member 62 and the second connecting member 63 are L-shaped metal tubes, the diameter of the first connecting member 62 is smaller than the diameter of the second connecting member 63, and the end of the first connecting member 62 can be inserted into the second connecting member 63 and can slide relatively. The locking structure 64 includes a bolt 641 and a threaded hole 642 opened on the side wall of the end of the second connecting member 63, the bolt 641 can pass through the threaded hole 642 and press the outer wall of the first connecting member 62 inwardly to lock the first connecting member 62 and the second connecting member 63, and the bolt 641 and the threaded hole 642 are adapted.
[0051] In the specific implementation process, the electrode base 61 is made of insulating material, preferably phenolic resin, which mainly plays the role of fixing and supporting the electrode 7. Phenolic resin has high strength, good insulation, heat resistance and corrosion resistance.
[0052] The electrode base 61 is embedded with a pure copper wire 3, one end of which is connected to the electrode 7, and the other end is connected to the DC resistance bridge 1 through the metal wire 2. The pure copper wire 3 runs through the electrode base 61, and mainly serves to connect the electrode 7 and the metal wire 2. This design is mainly considered to be convenient for actual detection operations, and two wires (metal wire 2 and pure copper wire 3) are used. In this way, the electrode 7 connected with the pure copper wire 3 can be fixed to the welding point joint first, and then the metal wire 2 is used to connect the DC resistance bridge 1 after it is fixed.
[0053] In the specific implementation process, the electrode 7 is a cylindrical chromium zirconium copper electrode 7, the clamping surface of which is gold-plated to enhance its conductivity, and the height is 10-15 mm. The chromium zirconium copper electrode 7 has good conductivity, high hardness and strength, and is relatively cheap.
[0054] Based on the above structure, the present invention provides a method for quickly detecting welding defects in metal spot welding joints, the method comprising the following steps:
[0055] S1, obtain the size of the welding head 4 to be tested and clean its surface;
[0056] Specifically, the surface pretreatment of the spot welding joint: use industrial alcohol to clean the oil stains on the upper and lower surfaces of the spot welding joint 4, then use a hair dryer to dry the surface, and then use 2000# or more fine sandpaper to gently grind the upper and lower surfaces of the welding point to remove the oxide layer on the upper and lower surfaces of the spot welding joint 4; the presence of oil stains and oxide layers on the surface of the welding point will increase the interface contact resistance, thereby affecting the measurement accuracy, so they must be removed before measurement;
[0057] Measure the size of the spot welding joint: Use a vernier caliper to measure the size of the spot welding joint 4 along mutually perpendicular directions on the horizontal plane (referring to any two mutually perpendicular directions on the horizontal plane), measure at least 3 times, and then take the average value (the average value is the average value calculated from the test data in all directions);
[0058] Determine the size of the electrode: During the resistance spot welding process, the electrode pressure will cause the spot welding surface to dent under high temperature. When the diameter of the cylindrical electrode 7 is larger than the spot welding size, the end of the cylindrical electrode 7 cannot directly contact the upper and lower surfaces of the electric welding head during defect detection, and the detection work cannot be carried out effectively; when the diameter of the cylindrical electrode 7 is too small, the contact resistance between the electrode 7 and the surface of the weld will increase, affecting the accuracy of the detection results. In this test method, the diameter of the cylindrical electrode 7 is taken as 1 / 3 to 1 / 4 of the measured size of the weld (i.e., the average value obtained above).
[0059] S2, calibrate the variable resistor so that when the relationship between the resistors satisfies R1 / R2=R3 / Rs, the current detection count value is zero;
[0060] The calibration steps are as follows: place a spot weld joint with the same size as the spot weld joint to be tested and known to have no defects between the two electrodes 7 and clamp it, then connect the two electrodes to two connection terminals and a DC resistance bridge to form a closed circuit, adjust the variable resistor to return the galvanometer reading to zero, and remove the spot weld joint after calibration.
[0061] S3, connect the welding head 4 of the test point to the calibrated DC resistance bridge 1 to form a closed circuit, and then record the reading of the galvanometer; if the reading of the galvanometer is zero, it can be determined that there is no welding defect in the area; if the reading of the galvanometer is not zero, it can be determined that there is a welding defect in the area.
[0062] Specifically, the spot welding head 4 to be tested is first clamped by two electrodes, and then the two electrodes are respectively connected to two connecting terminals to form a closed circuit with the calibrated DC resistance bridge 1.
[0063] Furthermore, the defect type of the spot welding joint can be determined based on step S5, including:
[0064] Move the electrode 7 in any direction (the length direction or the width direction of the metal plate 5), and record a reading every time it moves a certain distance (each time it moves 1 / 4 of the diameter of the electrode 7). If the distance moved by the electrode 7 does not exceed the first threshold value (the first threshold value is the upper limit of the conventional hole size range), the galvanometer reading will return to zero, and it can be determined that the defect type is a separate hole defect; if the distance moved by the electrode 7 exceeds the second threshold value (the second threshold value is the lower limit of the conventional crack size range), the galvanometer reading is still not zero, and it can be determined that the defect type is a crack defect. The second threshold value is not less than the first threshold value. In order to make the result judgment more accurate, the distance that the electrode 7 moves each time can be further reduced.
[0065] The metal resistance spot welding defect detection method of the present invention is, firstly, different from other traditional welding defect detection methods, in that it is based on the influence of welding defects on the resistance of spot welding joints; secondly, a set of resistance spot welding defect detection equipment is built; and then, a Wheatstone bridge is used to directly measure the current change in the circuit, which has high accuracy and sensitivity.
[0066] The above is only a preferred embodiment of the present invention, but the present invention is not limited to the above specific embodiments. Those skilled in the art may make some modifications, supplements or use similar methods instead without departing from the principle of the present invention, which should also be regarded as the protection scope of the present invention.
Claims
1. A method for quickly detecting welding defects in metal spot welding joints, characterized in that: The detection device comprises a DC resistance bridge (1), the DC resistance bridge (1) comprises a power supply, a switch and four bridge arms, the first bridge arm and the second bridge arm are connected in series to form a first series bridge arm group, the third bridge arm and the fourth bridge arm are connected in series to form a second series bridge arm group, the first series bridge arm group and the second series bridge arm group are connected in parallel, and a galvanometer is connected between the first bridge arm series group and the second bridge arm series group; the first bridge arm, the second bridge arm and the third bridge arm are provided with a first resistor R1, a second resistor R2 and a third resistor R3 in sequence, at least one of which is a variable resistor; the fourth bridge arm has two connection terminals (8) for connecting an external test piece with a resistance Rs; the detection method comprises: S1. Obtain the size of the spot weld joint (4) to be tested and clean its surface; S2, calibrate the variable resistor so that when the relationship between the resistors satisfies R1 / R2=R3 / Rs, the current sense count value is zero; S3, connecting the welding joint (4) to be tested to the calibrated DC resistance bridge (1) to form a closed circuit, and then recording the reading of the galvanometer; if the reading of the galvanometer is zero, it can be determined that there is no welding defect; if the reading of the galvanometer is not zero, it can be determined that there is a welding defect; In step S2, the calibration step is: placing a spot weld joint that has the same welding process as the spot weld joint to be tested and is known to have no defects between two electrodes (7) and clamping them, then connecting the two electrodes to two connection terminals (8) and a DC resistance bridge to form a closed circuit, adjusting the variable resistor so that the galvanometer reading returns to zero, and removing the spot weld joint after the calibration is completed; In step S3, the connection steps of the spot welding joint to be tested are: placing the spot welding joint to be tested between two electrodes (7) and clamping them, and then connecting the two electrodes to two connection terminals (8) and a DC resistance bridge to form a closed circuit; Based on step S3, the defect type of the spot welding joint (4) can be further determined, including: The electrode (7) is moved in any direction, and a reading is recorded every time it moves a certain distance. If the distance moved by the electrode (7) does not exceed a first threshold value, the reading of the galvanometer returns to zero, and it can be determined that the defect type is a single hole defect; if the distance moved by the electrode (7) exceeds a second threshold value, and the reading of the galvanometer is still not zero, it can be determined that the defect type is a crack defect.
2. The method for rapidly detecting welding defects in metal spot welding joints according to claim 1, characterized in that: In step S1, the surface cleaning steps of the spot welding joint to be tested are as follows: first, the oil stains on the surface of the spot welding joint (4) are cleaned, and then the oxide layer on the surface of the spot welding joint (4) is removed after drying.
3. The method for rapidly detecting welding defects in metal spot welding joints according to claim 1, characterized in that: In step S1, the step of obtaining the size of the spot welding joint is as follows: measuring the size of the spot welding joint (4) along mutually perpendicular directions on the surface of the spot welding joint, measuring at least 3 times, and then taking an average value.
4. The method for rapidly detecting welding defects in metal spot welding joints according to claim 3, characterized in that: The diameter of the electrode (7) can be determined to be 1 / 3 to 1 / 4 of the measured size of the spot welding joint (4).
5. A device for quickly detecting welding defects in metal spot welding joints, characterized in that: The device is adapted to the method for rapidly detecting welding defects in metal spot welding joints according to claim 1, and the device comprises: A direct current resistance bridge (1), the direct current resistance bridge (1) comprising a power supply, a switch and four bridge arms, the first bridge arm and the second bridge arm are connected in series to form a first series bridge arm group, the third bridge arm and the fourth bridge arm are connected in series to form a second series bridge arm group, the first series bridge arm group and the second series bridge arm group are connected in parallel, a galvanometer is connected between the series connection point of the first bridge arm series group and the series connection point of the second bridge arm series group, the first bridge arm, the second bridge arm and the third bridge arm are provided with a first resistor R1, a second resistor R2 and a third resistor R3 in sequence, at least one of the first resistor R1, the second resistor R2 and the third resistor R3 is a variable resistor, and the fourth bridge arm has two connection terminals (8); Two electrodes (7), the two electrodes (7) are respectively connected to two connection terminals (8) and form a closed circuit with the DC resistance bridge (1), and a clamping space for clamping the metal spot welding joint (4) is left between the two electrodes (7); and A clamping assembly (6) is fixedly connected to the two electrodes (7) and is used to adjust a clamping distance between the two electrodes (7).
6. The device for rapidly detecting welding defects in metal spot welding joints according to claim 5, characterized in that: The clamping assembly (6) comprises: Two electrode bases (61), the two electrode bases (61) are used to fix two electrodes (7) respectively; A first connecting member (62), one end of the first connecting member (62) being fixedly connected to one of the electrodes (7); A second connecting member (63), one end of the second connecting member (63) being fixedly connected to another electrode (7), and the other end of the second connecting member (63) being in contact with the other end of the first connecting member (62) and being relatively movable; and A locking structure, the locking structure is used to lock the relative displacement distance between the first connecting member (62) and the second connecting member (63).
7. The device for rapidly detecting welding defects in metal spot welding joints according to claim 6, characterized in that: The first connecting piece (62) and the second connecting piece (63) are both L-shaped metal tubes. The diameter of the first connecting piece (62) is smaller than the diameter of the second connecting piece (63). The end of the first connecting piece (62) can be inserted into the second connecting piece (63) and can slide relatively. The locking structure comprises a bolt (641) and a threaded hole (642) formed on the side wall of the end of the second connecting piece (63). The bolt (641) can pass through the threaded hole (642) and press the outer wall of the first connecting piece (62) inwardly, thereby locking the first connecting piece (62) and the second connecting piece (63).