Graphite materials, secondary batteries and electronic devices

By using graphite materials with suitable crystallinity and alignment in secondary batteries, the problem of high expansion rate of secondary batteries is solved, the battery energy density and cycling performance are improved, and the battery life is extended.

CN114709415BActive Publication Date: 2024-11-22NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210375159.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-04
Publication Date
2024-11-22
Estimated Expiration
2040-12-04

AI Technical Summary

Technical Problem

The expansion rate of existing secondary batteries is high during charging and discharging, which affects the thickness and energy density of the battery and is difficult to meet the needs of high endurance.

Method used

Using graphite materials with crystallinity in the range of 2.5 to 7.0, combined with specific arrangement and tap density, graphite secondary particles with excellent processing properties were prepared by powder X-ray diffraction and graphitization treatment, and used for the negative electrode. The energy density and cyclic expansion rate of the battery are controlled.

Benefits of technology

The energy density and expansion rate of the secondary battery are improved, ensuring the thinning of the battery and the optimization of the cycle performance, and extending the battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003590079700000081
    Figure BDA0003590079700000081
  • Figure BDA0003590079700000091
    Figure BDA0003590079700000091
  • Figure BDA0003590079700000101
    Figure BDA0003590079700000101
Patent Text Reader

Abstract

The present application provides a graphite material, a secondary battery and an electronic device. The crystallinity K of the graphite material is 2.5 to 7.0; wherein K=A 002 / A 111 , and K is the ratio of the peak area of ​​the graphite material (002) to the peak area of ​​silicon (111) obtained by testing the graphite material with 25wt% silicon powder standard sample by X-ray diffraction method, and the arrangement degree I of the graphite material is 2.0 to 4.0; the tap density of the graphite material is TD g / cm 3 , TD≥0.86, and the following relationship is satisfied: 3×TD≤K≤6×TD+1.0. The secondary battery of the present application includes a negative electrode plate; wherein the negative electrode plate includes the graphite material described in the present application, and the negative electrode plate has a stable structure and few side reactions. When the negative electrode plate is used in a secondary battery, the battery thickness growth rate is small, and the capacity retention rate and cycle performance are high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of secondary batteries, and specifically relates to a graphite material and a secondary battery and an electronic device using the graphite material. Background Art

[0002] In recent years, the emergence of large-screen smartphones has changed people's lifestyles. Now people rely on mobile phones not only for communication, but also for shopping, games, socializing, and entertainment. This requires that the thickness of mobile phone batteries should not expand too much during production and use. Reducing the expansion of the negative electrode sheet can reduce the thickness of the battery, which is one of the important methods to increase the volume energy density of the battery.

[0003] The continuous development of mobile Internet has put forward higher requirements on secondary batteries as power sources and further demands on the battery life of mobile phones. It is particularly urgent to develop secondary batteries with higher volume energy density. Summary of the invention

[0004] In order to overcome the above defects, the present application provides a graphite material having a higher energy density and a lower expansion rate.

[0005] One aspect of the present application provides a graphite material, wherein the crystallinity K of the graphite material is 2.5 to 7.0; wherein K=A 002 / A 111 , and K is the ratio of the peak area of ​​the graphite material (002) plane to the peak area of ​​the silicon (111) plane obtained by testing the graphite material added with 25wt% silicon powder standard sample by powder X-ray diffraction method;

[0006] The degree of arrangement I of the graphite material is 2.0 to 4.0;

[0007] The tap density of graphite material is TD g / cm 3 , TD≥0.86, and satisfies the following relationship with K: 3×TD≤K≤6×TD+1.0.

[0008] In the above scheme, in order to take into account the processability of graphite materials, the energy density, cycle expansion and deformation of secondary batteries, the applicant found that: when the crystallinity of graphite materials is within the range of 2.5 to 7.0, the arrangement degree I of graphite materials is limited to 2.0 to 4.0, and the crystallinity K of graphite materials satisfies the formula: 3×TD≤K≤6×TD+1.0, it can ensure that the secondary battery has a higher energy density and can also reduce the expansion rate of the secondary battery as much as possible, so that the energy density and cycle expansion of the secondary battery are controlled within a suitable range. Moreover, graphite materials have excellent processability.

[0009] Among them, when the value of the crystallinity K of the graphite material is large, the energy density of the secondary battery is high, and the expansion rate of the secondary battery (also known as the battery thickness growth rate) will increase. On the contrary, when the value of the crystallinity K of the graphite material is small, the energy density exerted in the secondary battery is low, the expansion rate of the secondary battery is low, and the deformation of the secondary battery is small. When the crystallinity is in the range of 2.5 to 7.0, it can not only ensure that the secondary battery has a high energy density, but also minimize the expansion rate of the secondary battery.

[0010] Among them, I=I C / I Si To determine the degree of alignment, graphite powder (with 25 wt% silicon powder standard sample added, such as Shanghai Guoyao Metal Silicon Powder 200 mesh) is tested by powder X-ray diffraction (XRD) to obtain the peak intensity of the graphite material (002) surface and the peak intensity of the silicon (111) surface. The intensity ratio I (002 ) / I (111) That is, I. The value of the arrangement degree I of the graphite material can reflect the overall orientation degree of the graphite material particles. When the value of I is large, the overall orientation degree of the graphite material particles is relatively high, the particles are arranged regularly, it is difficult to insert lithium into the secondary battery (i.e., the secondary battery discharge process), and the secondary battery has a large cycle expansion; when the value of I is small, the overall orientation degree of the graphite material particles is low, the particles are arranged in a disorderly manner, it is easier to insert lithium into the secondary battery (i.e., the secondary battery discharge process), and the secondary battery has a small cycle expansion; therefore, the value of I is limited to 2.0 to 4.0, within which the secondary battery has a higher energy density and a reduced secondary battery expansion rate.

[0011] Graphite materials contain graphite secondary particles formed by the agglomeration of multiple graphite primary particles. The content of secondary particles affects the tap density of graphite materials, and the tap density of graphite materials affects the processability of graphite materials. Moreover, the content of secondary particles affects the overall particle distribution of negative electrode active materials, and then affects the crystallinity K of negative electrode active materials. In order to take into account the processability of graphite materials, the energy density, cycle expansion and deformation of secondary batteries, when the crystallinity K of graphite materials satisfies the formula: 3×TD≤K≤6×TD+1.0, better processing performance can be obtained, and the energy density and cycle expansion of secondary batteries can be within a suitable range.

[0012] In some embodiments of the present application, the sphericity of the graphite material is 0.81 to 0.93. The sphericity test is performed using a QICPIC image graphic analyzer.

[0013] The sphericity of graphite material can represent the overall shape of graphite material particles. When the sphericity of graphite material is in the range of 0.81 to 0.93, the electrolyte can form a uniform and stable protective film on the surface of graphite material particles to reduce the consumption of lithium ions, increase the initial efficiency, and improve the cycle performance of secondary batteries. There are fewer byproducts on the surface of graphite material particles and the expansion rate is reduced. In some embodiments of the present application, in the Raman spectrum, when a 532nm laser is used, the graphite material is at 1300cm -1 Up to 1400cm -1 The peak intensity ID in the range is at 1580 cm -1 Up to 1620cm -1 The ratio of the peak intensity IG in the range of ID / IG is 0.06 to 0.16. In some embodiments of the present application, in the Raman spectrum, when a 532 nm laser is used, the peak intensity IG at 1300 cm -1 Up to 1400cm -1 The peak intensity ID in the range is at 1580 cm -1 Up to 1620cm -1 The ratio ID / IG of the peak intensity IG in the range is 0.06, 0.07, 0.09, 0.10, 0.12, 0.14, 0.15, 0.16 or in the range of any two of the above values. ID / IG affects the thickness of the protective film formed when the secondary battery is first charged, the consumption of lithium ions, and the speed of lithium ion insertion and extraction, thereby affecting the initial efficiency of the secondary battery and the expansion rate of the secondary battery.

[0014] In some embodiments of the present application, the graphitization degree Gr of the graphite material is 93.5% to 96.0%. In some embodiments of the present application, the graphitization degree Gr of the graphite material is 93.5%, 94.0%, 94.4%, 94.7%, 95.0%, 95.2%, 95.4%, 95.6%, 95.8%, 96.0% or within the range of any two of the above values. The graphitization degree affects the overall order of the graphite material and the interlayer spacing of the graphite material, thereby affecting the capacity, energy density and battery thickness growth rate of the graphite material during the secondary battery cycle. Taking the above into consideration, better performance can be obtained when the graphitization degree of the graphite material is 93.5% to 96.0%.

[0015] In some embodiments of the present application, the particle size Dv50 of the graphite material is 10 μm to 20 μm. In some embodiments of the present application, the particle size Dv50 of the graphite material is 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm or within the range of any two of the above values. The Dv50 of the particles can reflect the overall particle distribution of the graphite material, and the proportion of secondary particles will also affect Dv50. The Dv50 of the graphite particles will affect the speed of lithium ion insertion and extraction during the cycle, the energy density of the secondary battery, and the expansion rate of the secondary battery. Therefore, the Dv50 of the graphite material can obtain better performance within a suitable range.

[0016] In some embodiments of the present application, the specific surface area (abbreviated as BET) of the graphite material is 1.0 m 2 / g to 2.0m 2 In some embodiments of the present application, the specific surface area BET is 1.0 m 2 / g, 1.2m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.7m 2 / g, 1.9m 2 / g, 2.0m 2 / g or in the range of any two of the above values. The specific surface area affects the initial efficiency of the secondary battery, the amount of by-products during the cycle, the cycle performance and the kinetic performance. In summary, all indicators must be considered comprehensively to achieve better comprehensive performance of graphite materials, that is, high energy density, good cycle and small expansion rate.

[0017] The present application also provides a secondary battery, which includes a positive electrode plate, an electrolyte, a separator and a negative electrode plate, wherein the negative electrode plate includes a negative electrode collector and a negative electrode film layer arranged on at least one surface of the negative electrode collector, the negative electrode film layer includes a negative electrode active material, and the negative electrode active material includes the graphite material as described above.

[0018] In some embodiments of the secondary battery described in the present application, the compaction density of the negative electrode sheet is 1.45 g / cm 3 Up to 1.80g / cm 3 The compacted density can be specifically 1.45 g / cm 3 , 1.55g / cm 3 , 1.65g / cm 3 , 1.75g / cm 3 , 1.8g / cm 3 Or within the range of any two of the above values.

[0019] In some embodiments of the secondary battery described in the present application, the porosity of the negative electrode sheet is 20% to 30%, and the porosity of the negative electrode sheet can specifically be 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30% or within the range of any two of the above values.

[0020] The porosity test adopts the gas replacement method, and the percentage of the sample pore volume to the total volume is P = (V-V0) / V×100%; wherein V0 represents the true volume and V represents the apparent volume.

[0021] The higher the porosity of the negative electrode sheet, the more electrolyte the negative electrode sheet can store, which is beneficial to the circulation of the secondary battery. However, from another perspective, if too much electrolyte is stored in the pores of the negative electrode sheet, the corresponding by-products will also increase, which is not conducive to circulation. The lower the porosity, the more difficult it is for the electrolyte in the secondary battery to infiltrate the negative electrode sheet. During the battery cycle, the conduction of lithium ions is hindered, affecting the battery's cycle performance and kinetic performance. Therefore, the porosity should be selected within a suitable range. In the secondary battery of the present application, the porosity of the negative electrode membrane is 20% to 30%.

[0022] In some embodiments of the secondary battery of the present application, the OI value of the negative electrode plate is 8 to 18; wherein the OI value is the ratio of the peak area of ​​the surface (004) to the peak area of ​​the surface (110) obtained by testing the negative electrode plate by X-ray diffraction (XRD).

[0023] The OI value can indicate the orientation degree of the particles of the graphite material in the negative electrode sheet at the electrode sheet level, and the OI value affects the cycle performance and the cycle expansion rate. In order to take into account the cycle expansion rate and the cycle performance, in the present application, the OI value of the negative electrode sheet is 8 to 18, and the OI value of the negative electrode sheet can be 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18 or within the range of any two of the above values.

[0024] In some embodiments of the secondary battery of the present application, the bonding strength between the negative electrode film layer and the negative electrode current collector is 6 N / m to 15 N / m, and the bonding strength between the negative electrode film layer and the negative electrode current collector can specifically be 6 N / m, 7 N / m, 8 N / m, 9 N / m, 10 N / m, 11 N / m, 12 N / m, 13 N / m, 14 N / m, 15 N / m or within the range of any two of the above values.

[0025] The bonding force between the negative electrode film layer and the negative electrode current collector is too small. Under the stress of lithium ion insertion and extraction during the cycle, the negative electrode film layer is easily detached from the negative electrode current collector (referred to as film stripping), which affects the battery kinetics and cycle performance, and further affects the cycle expansion. The bonding force between the negative electrode film layer and the negative electrode current collector is too high, requiring the addition of more binder to reduce the battery energy density.

[0026] In some embodiments of the secondary battery of the present application, the negative electrode plate further comprises one or more of carbon fiber, mesophase carbon microspheres, silicon-based materials, tin-based materials, and lithium titanate. In addition to graphite, the negative electrode plate may also include other negative electrode active materials. The mass content of these negative electrode active materials in the negative electrode plate is preferably 5% to 10%. The present application also provides an electronic device, including the secondary battery as described above.

[0027] The present application also provides a method for preparing a graphite material, the method comprising:

[0028] (1) crushing a precursor of a graphite material into primary particles having a Dv50 of 7 μm to 13 μm;

[0029] (3) mixing the primary particles with asphalt in a weight ratio of 90:10 to 80:20 and calcining in an atmosphere of protective gas to form secondary particles;

[0030] (3) The primary particles in step (1) and the secondary particles in step (2) are mixed in a weight ratio of 90:10 to 10:90 and then graphitized to obtain the graphite material.

[0031] In some embodiments of the preparation method of the present application, in the step (1), the precursor comprises needle coke.

[0032] In some embodiments of the preparation method of the present application, in the step (2), the protective gas includes: at least one of nitrogen or argon.

[0033] In some embodiments of the preparation method of the present application, in the step (2), the calcination temperature is 500°C to 700°C.

[0034] In some embodiments of the preparation method of the present application, in the step (3), the graphitization temperature is 2500°C to 3500°C.

[0035] In some embodiments of the preparation method of the present application, in the step (3), the primary particles and the secondary particles are mixed in a weight ratio of 60:40 to 10:90.

[0036] Beneficial effects of this application

[0037] Compared with existing graphite materials, the graphite material of the present application can reduce the expansion during the cycle of the secondary battery. At the same time, the deformation of the secondary battery using the negative electrode plate of the present application is not obvious. The thickness of the secondary battery matches the reduction in the expansion of the negative electrode plate, thereby improving the energy density of the secondary battery. In addition, the negative electrode plate expands less during the cycle process, the negative electrode plate can better maintain a relatively stable structure, and has relatively fewer side reactions, which is conducive to improving the cycle performance of the secondary battery. DETAILED DESCRIPTION

[0038] The present application is further described below by examples and comparative examples, which are only used to illustrate the present application and are not limited to the following examples. Any modification or equivalent replacement of the technical solution of the present application without departing from the scope of the technical solution of the present application shall be included in the protection scope of the present application.

[0039] In this application, K (K = A C / A Si ) is the crystallinity of the graphite material. The crystallinity can indicate the degree of crystallinity of the graphite material. The larger the value, the higher the crystallinity of the graphite material. Specifically, for graphite materials, the K value is affected by the orientation degree of graphite and the size of the particles. In order to achieve the purpose of reducing the thickness growth of the battery while controlling deformation, the crystallinity K of the negative active material of the present application needs to satisfy 2.5≤K≤7.0.

[0040] In this application, I (I = I C / I Si ) is defined as the graphite material arrangement degree, which can explain the orientation degree of the graphite material, which is closely related to the expansion degree of the graphite material. In order to achieve the purpose of reducing the thickness growth of the battery while controlling the deformation of the battery, the graphite material arrangement degree I of the present application needs to satisfy 2.0≤I≤4.0. At this time, the thickness growth rate of the negative electrode sheet and the deformation of the battery can be well taken into account.

[0041] The tap density of the graphite material in this application is TD g / cm 3 , TD≥0.86g / cm 3 The testing instrument is FZS4-4B tap density tester, and the specific method reference standard is GB / T 5162-2006 "Determination of tap density of metal powders".

[0042] The OI value of the negative electrode sheet made of graphite material in the present application is 8≤OI≤18. The testing instrument is PANalytical / X'pert PRO, wherein the XRD reference standard is JIS K 0131-1996 "General rules of X-ray diffractometric analysis".

[0043] The interplanar spacing of the (002) plane of the graphite material of the present application is tested by powder X-ray diffraction (XRD) on graphite crystals, and the testing instrument is PANalytical / X'pert PRO, wherein the XRD reference standard is JIS K 0131-1996 "General rules of X-ray diffractometric analysis X-ray diffractometric analysis general rules".

[0044] The particle size of the graphite material in this application is measured by a laser particle size analyzer, and the test instrument is MasterSizer 2000. Reference standard GB / T19077-2016 / ISO 13320:2009 particle size distribution laser diffraction method. Dv50 means that 50% of the total volume of particles have a diameter greater than this value, and another 50% of the total volume of particles have a diameter less than this value, which is often used to indicate the median particle size of the powder.

[0045] The graphitization degree test instrument of the present application is PANalytical / X'pert PRO, wherein the XRD reference standard is JISK 0131-1996 "General rules of X-ray diffractometric analysis". During the test, silicon powder accounts for 25% of the total mass of silicon powder and graphite.

[0046] Example 1

[0047] Preparation of lithium-ion batteries

[0048] 1. Preparation of graphite materials

[0049] (1) The needle coke raw material is pulverized by a mechanical mill to obtain primary particles with a Dv50 of 9 μm.

[0050] (2) Mix the crushed primary particles with asphalt in a mixer at a ratio of 85:15 for 1 hour until the mixture is uniform. Put the mixed materials into a granulation equipment (drum furnace), and heat them to 600°C under the protection of N2 atmosphere to granulate into secondary particles.

[0051] (3) The primary particles and secondary particles prepared above are mixed in a mixing device at a weight ratio of 40:60. After being evenly mixed, they are placed in a graphitization furnace for graphitization treatment at 3000° C., and after cooling, they are demagnetized and sieved to obtain graphite materials.

[0052] The density of the negative electrode is 1.70g / cm 3 , the OI value is 15.

[0053] Examples 2 to 34 and Comparative Examples 1 to 3 can be prepared by controlling the ratio of primary particles to secondary particles, the calcination temperature, the composition of the precursor and the particle size of the precursor in the above preparation process, as long as the parameters of the present examples and comparative examples can be achieved.

[0054] 2. Preparation of negative electrode sheet

[0055] The graphite material, styrene-butadiene rubber and sodium carboxymethyl cellulose prepared as above were mixed in a weight ratio of 96:2:2, deionized water was added for further mixing, and stirred evenly to obtain a negative electrode slurry. The negative electrode slurry was coated on a copper foil with a thickness of 12 μm, dried, cold pressed, cut into pieces, and welded to the pole ears to obtain a negative electrode sheet.

[0056] 3. Diaphragm

[0057] A polyethylene diaphragm with a thickness of 10 μm is used, and an inorganic particle layer with a thickness of 2 μm is provided on one side of the diaphragm, and the inorganic particle layer includes Al2O3.

[0058] 4. Electrolyte

[0059] In a dry argon environment, ethylene carbonate (EC), propylene carbonate (PC) and diethyl carbonate (DEC) (according to a weight ratio of 1:1:1) are mixed, and lithium hexafluorophosphate (LiPF6) is added and mixed evenly to obtain an electrolyte, wherein the mass content of LiPF6 is 12.5%. Based on the weight of the electrolyte, 3% of fluoroethylene carbonate (FEC) is added to the electrolyte.

[0060] 5. Preparation of positive electrode

[0061] The positive electrode active material lithium cobalt oxide, the conductive agent SP, and the binder polyvinylidene fluoride are mixed in a weight ratio of 97:1.4:1.6, N-methylpyrrolidone (NMP) is added, and the system is stirred under the action of a vacuum mixer until it becomes a uniform slurry to obtain a positive electrode slurry, wherein the solid content of the positive electrode slurry is 72wt%; the positive electrode slurry is coated on the surface of the positive electrode collector, dried, cold pressed, and then cut into pieces and welded to the pole ears to obtain a positive electrode sheet.

[0062] 6. Preparation of lithium-ion batteries

[0063] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then they are wound to obtain a battery cell; the battery cell is placed in an outer packaging foil aluminum-plastic film, and the prepared electrolyte is injected into the dried battery cell. After vacuum packaging, standing, formation, shaping, capacity testing and other processes, a lithium-ion battery is obtained.

[0064] Test Method

[0065] 1. First efficiency test

[0066] After the lithium-ion battery is prepared, it is first charged at a constant current of 0.5C to 4.45V, and then charged at a constant voltage of 4.45V to 0.05C to obtain the first charging capacity (C0); then after standing for 5 minutes, it is discharged at a current of 0.5C to 3V to obtain the first discharge capacity (D0), and the first charge and discharge efficiency (i.e., the first efficiency) = D0 / C0×100%.

[0067] 2. Negative electrode sheet thickness growth rate (%)

[0068] Take the prepared negative electrode sheet, take five points on the polymer film of the same length before winding, test the negative electrode thickness corresponding to the five points, take the average value, record it as L0, assemble it into a lithium-ion battery, and place it in a 25°C constant temperature box for 30 minutes to allow the lithium-ion battery to reach a constant temperature; charge it to 4.45V at a constant current of 0.5C, and charge it at a constant voltage until the current is 0.05C; then discharge it to 3.0V at 0.5C, and after 200 cycles of this step, charge it to 4.45V at a constant current of 0.5C, and charge it at a constant voltage until the current is 0.05C; disassemble the battery, take out the negative electrode sheet, and after the surface of the negative electrode is dry, use the polymer film to determine the position of the negative electrode sheet in the previous step, and test the thickness of the negative electrode sheet at the 5 points again, take the average value, and record it as L 200 ,

[0069] 200 cycles negative electrode thickness growth rate (%) = (L 200 -L0) / L0×100%.

[0070] 3. Battery thickness growth rate

[0071] After the lithium-ion battery is left at rest for 5 minutes at 25°C, it is charged to 4.45V at a constant current of 0.5C, and then charged to 0.05C at a constant voltage of 4.45V, and left to rest for 5 minutes. The lithium-ion battery is determined at three locations, and the thickness of the points at the three locations is determined, and the average value is recorded as MMC0. The lithium-ion battery is then discharged to 3.0V at a constant current of 0.5C, and left to rest for 5 minutes. Repeat the above charge and discharge cycle 200 times, and test the thickness of the lithium-ion battery at three locations each time, and take the average value MMC 200 .

[0072] The battery thickness growth rate is calculated by the following formula:

[0073] 200 cycles battery thickness growth rate (%) = (MMC 200 -MMC0) / MMC0×100%.

[0074] 4. Cycle times at 45℃

[0075] Place the lithium-ion battery in a 45°C constant temperature box and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature; charge it to 4.45V at a constant current of 0.5C, and charge it at a constant voltage until the current is 0.05C; then discharge it to 3.0V at 0.5C to obtain the first charge capacity (C0); this step is cycled until the capacity is 80% of the first charge capacity, and the number of cycles is recorded.

[0076] The graphite material parameters in each embodiment and comparative example are shown in Table 1.

[0077] Table 1

[0078]

[0079]

[0080]

[0081] The electrochemical performance test results of Examples 1 to 34 and Comparative Examples 1 to 3 are shown in Table 2.

[0082] Table 2

[0083]

[0084]

[0085]

[0086] It can be seen from Table 1 and Table 2 that the lithium-ion batteries using the graphite materials of Examples 1 to 34 of the present application all have a smaller thickness growth rate, and the number of cycles at 45°C is significantly higher than that of Comparative Examples 1 to 3, and the battery life is significantly longer than that of the batteries in Comparative Examples 1 to 3.

[0087] In Examples 1 to 34, the crystallinity K and arrangement I of the graphite material in the negative electrode sheet satisfy 2.5≤K≤7.0 and 2.0≤I≤4.0. The expansion of the negative electrode sheet is reduced during the battery cycle, and the risk of warping and deformation of the battery is suppressed, ensuring that the reduction in the thickness of the negative electrode sheet matches the thinning of the battery thickness, achieving the goal of improving the battery energy density.

[0088] Example 35 to Example 39

[0089] The preparation process of the lithium-ion battery is the same as that of Example 12, except that the negative electrode plate parameters in Example 12 are replaced with the negative electrode plate parameters of Examples 35 to 39. The relevant parameters of the negative electrode plate are shown in Table 3.

[0090] Table 3 Performance parameters of lithium-ion batteries using different negative electrode plate parameters

[0091]

[0092] As shown in Table 3, the battery using the negative electrode sheet made of the graphite material of the present application can reduce the thickness growth rate of the negative electrode sheet and improve the energy density of the battery. The battery using the graphite material of the present application achieves a balance between the thickness growth rate and the battery life and cycle performance.

[0093] It can be seen from the data in Table 3 that the negative electrode plate of the present application has a stable structure, few side reactions, and a battery using the negative electrode plate has a small thickness growth rate and high cycle performance.

Claims

1. A secondary battery, It is characterized in that The invention comprises a positive electrode sheet, an electrolyte, a separator and a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, wherein the negative electrode film layer comprises a negative electrode active material, wherein the negative electrode active material comprises a graphite material, The crystallinity K of the graphite material is 2.5 to 7.0; Wherein, K=A002 / A111, and K is the ratio of the peak area of ​​the graphite material (002) plane to the peak area of ​​the silicon (111) plane obtained by testing the graphite material added with 25wt% silicon powder by X-ray diffraction method; The arrangement degree I of the graphite material is 2.0 to 4.0; The tap density of the graphite material is TD g / cm 3 , TD≥0.86, and satisfy the following relationship: 3×TD≤K≤6×TD+1.0; the compaction density of the negative electrode sheet is 1.45g / cm 3 Up to 1.80g / cm 3 .

2. The secondary battery according to claim 1, It is characterized in that The graphite material satisfies at least one of the conditions (1)-(5): (1) The sphericity of the graphite material is 0.81 to 0.93; (2) In the Raman spectrum test, the graphite material is at 1300 cm -1 Up to 1400cm -1 Peak intensity range I D and at 1580cm -1 Up to 1620cm -1 Peak intensity range I G The ratio is 0.06 to 0.16; (3) The graphitization degree Gr of the graphite material is 93.5% to 96.0%; (4) The particle size Dv50 of the graphite material particles is 10 μm to 20 μm; (5) The specific surface area of ​​the graphite material is 1.0 m 2 / g to 2.0m 2 / g.

3. The secondary battery according to claim 1, It is characterized in that The porosity of the negative electrode sheet is 20% to 30%.

4. The secondary battery according to claim 3, It is characterized in that The OI value of the negative electrode plate is 8 to 18; wherein the OI value is the ratio of the peak area of ​​the surface (004) to the peak area of ​​the surface (110) obtained by testing the negative electrode plate using an X-ray diffraction method.

5. The secondary battery according to claim 3, It is characterized in that The bonding strength between the negative electrode film layer and the negative electrode current collector is 6 N / m to 15 N / m.

6. An electronic device, It is characterized in that A secondary battery comprising the secondary battery according to any one of claims 1 to 5.