Silicon-based negative electrode material and preparation method thereof, silicon-based negative electrode and lithium ion battery

By using the combination technology of prelithiated mesoporous silicon material with carbon cladding and organic polymer cladding on the silicon-based anode material, the problem of irreversible consumption and volume expansion of silicon-based anode material during lithium embedding is solved. Improves the cycle stability and safety of the battery.

CN119008899APending Publication Date: 2024-11-22XIAOGAN CORNEX NEW ENERGY INNOVATION TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411109438.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing silicon-based negative electrode materials produce irreversible lithium oxide and lithium silicate during the first lithium embedding process, resulting in irreversible consumption of lithium ions. Due to volume expansion problems, the material has poor stability during charging and discharging and poor circulation performance.

Method used

Prelithiated mesoporous silicon material plus carbon cladding and organic polymer cladding from the inside to the outside can improve the conductivity and inhibit volume expansion; organic polymer cladding is made of acrylate single The copolymer formed by the bulk and silicone resin precursor is made with lithium supplement additives to enhance the tear resistance and structural stability of the material.

Benefits of technology

It effectively inhibits the volume expansion of silicon material, improves electrochemical performance, enhances lithium ion conduction capabilities, and improves the cycle stability and safety of lithium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008899A_ABST
    Figure CN119008899A_ABST
Patent Text Reader

Abstract

The invention provides a silicon-based negative electrode material and a preparation method thereof, a silicon-based negative electrode and a lithium ion battery, and relates to the technical field of batteries. The silicon-based negative electrode material comprises a pre-lithiated meso-porous silicon material, and a carbon coating layer and an organic polymer coating layer which are sequentially arranged on the surface of the pre-lithiated meso-porous silicon material from inside to outside, wherein the pre-lithiated meso-porous silicon material can reserve a certain space for expansion of silicon material particles, and meanwhile, an additional lithium intercalation path is generated; a carbon coating layer on the surface of the pre-lithiated meso-porous silicon material can improve the conductivity of the silicon-based negative electrode material and can inhibit the expansion of silicon material particles to a certain extent; the organic polymer coating layer prepared from specific raw materials can well inhibit the occurrence of interface side reactions, and meanwhile, the organic polymer coating layer and the carbon coating layer act together to further improve the structural stability of the electrode active material, reduce the expansion of the silicon-based negative electrode material in the charging and discharging process, and improve the cycling stability and safety of the battery. The invention also provides a preparation method of the silicon-based negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a silicon-based negative electrode material and a preparation method thereof, a silicon-based negative electrode and a lithium-ion battery. Background Art

[0002] During the first lithium insertion process, silicon-based negative electrode materials will generate irreversible lithium oxide and lithium silicate, resulting in irreversible consumption of lithium ions. Pre-lithiation is the process of silicon oxide reacting with lithium in advance to generate lithium silicate, which can avoid irreversible consumption during the first lithium insertion. However, the silicon material particles after pre-lithiation will still have a certain degree of volume expansion problem.

[0003] In order to improve the expansion problem of silicon material particles, they can be coated. At present, the selection of silicon coating materials is mainly based on inorganic materials, such as porous carbon, carbon nanotubes, phosphorus aluminum compounds, etc. Although the use of inorganic materials for silicon coating in the prior art has achieved a certain effect of inhibiting volume expansion, the effect of limiting expansion is limited. Research on the use of organic matter as a coating layer is relatively rare, and because the chain segments of polymer materials are relatively long, silicon particles are easily agglomerated during coating. Therefore, how to effectively inhibit the volume expansion of silicon materials and ensure their good electrochemical properties is a technical problem that needs to be solved urgently.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a silicon-based negative electrode material and a preparation method thereof, a silicon-based negative electrode and a lithium-ion battery, so as to improve the above-mentioned technical problems existing in the prior art.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The first object of the present invention is to provide a silicon-based negative electrode material, comprising a pre-lithiation mesoporous silicon material and a carbon coating layer and an organic polymer coating layer sequentially arranged on the surface of the pre-lithiation mesoporous silicon material from the inside to the outside;

[0008] The organic polymer coating layer is mainly made of a copolymer formed by an acrylic ester monomer and an organic silicon resin precursor and a lithium supplement additive.

[0009] Further, on the basis of the above technical solution of the present invention, the particle size of the pre-lithiation mesoporous silicon material is 1-5 μm, and the pore size is 5-30 nm;

[0010] And / or, the thickness of the carbon coating layer is 1-5 nm;

[0011] And / or, the mass fraction of the carbon coating layer in the silicon-based negative electrode material is 0.5-3wt%.

[0012] Further, based on the above technical solution of the present invention, the acrylic acid ester monomer includes at least one of methyl methacrylate, butyl acrylate, isobutyl acrylate or epoxy acrylate;

[0013] and / or, the organosilicon resin precursor comprises at least one of polymethyl silicone resin, polyethyl silicone resin or polyaryl silicone resin;

[0014] And / or, the lithium supplement additive includes at least one of lithium powder, lithium foil, lithium sheet, lithium block, lithium hydride, lithium hydroxide or lithium carbonate;

[0015] And / or, the thickness of the organic polymer coating layer is 3-10 nm;

[0016] And / or, the mass fraction of the organic polymer coating layer in the silicon-based negative electrode material is 0.5-5wt%.

[0017] The second object of the present invention is to provide a method for preparing a silicon-based negative electrode material, comprising the following steps:

[0018] (a) carbon-coating the pre-lithiated mesoporous silicon material to form a carbon coating layer to obtain a carbon-coated mesoporous silicon material;

[0019] (b) coating the carbon-coated mesoporous silicon material with an organic polymer to form an organic polymer coating layer on the surface of the carbon coating layer to obtain a silicon-based negative electrode material.

[0020] Further, based on the above technical solution of the present invention, in step (a), the method for preparing the pre-lithiated mesoporous silicon material comprises the following steps:

[0021] After the silicon material is pore-formed by a pore-forming agent, a mesoporous silicon material is obtained;

[0022] The mesoporous silicon material is subjected to a pre-lithiation treatment to obtain a pre-lithiation mesoporous silicon material.

[0023] Further, on the basis of the above technical solution of the present invention, the silicon material includes at least one of silicon, silicon oxide, modified silicon oxide, silicon-carbon composite material or silicon alloy material;

[0024] and / or, the pore-forming agent comprises at least one of silicon oxide, calcium oxide, magnesium oxide or molybdenum oxide;

[0025] And / or, the pre-physical and chemical treatment includes solid-phase pre-lithiation and liquid-phase pre-lithiation; preferably, the sintering temperature of the solid-phase pre-lithiation is 500-1000°C, and the sintering time is 15-24h; preferably, the pre-lithiation reagent of the solid-phase pre-lithiation includes at least one of lithium hydride, lithium nitride or lithium borohydride; preferably, the sintering temperature of the liquid-phase pre-lithiation is 600-1000°C, and the sintering time is 20-30h; preferably, the pre-lithiation reagent of the liquid-phase pre-lithiation includes an aromatic radical anion complex of lithium.

[0026] Further, based on the above technical solution of the present invention, in step (a), carbon coating is performed by chemical vapor deposition;

[0027] and / or, the temperature for carbon coating by chemical vapor deposition is 600-900° C., and the carbon coating time is 2-8 hours;

[0028] And / or, the carbon source used for carbon coating by chemical vapor deposition includes at least one of acetylene, graphene, cracked carbon, carbon nanotubes, carbon nanofibers, graphite or amorphous carbon.

[0029] Further, on the basis of the above technical solution of the present invention, in step (b), a copolymer formed by an acrylic ester monomer and a silicone resin precursor, a lithium supplement additive and a carbon-coated mesoporous silicon material are mixed, and heated and cured under vacuum conditions to perform organic polymer coating;

[0030] Preferably, the heating temperature is 500-1000° C., and the heating time is 1-4 hours.

[0031] The third object of the present invention is to provide a silicon-based negative electrode, comprising the above-mentioned silicon-based negative electrode material or the silicon-based negative electrode material prepared by the above-mentioned preparation method.

[0032] A fourth object of the present invention is to provide a lithium-ion battery comprising the above-mentioned silicon-based negative electrode material or silicon-based negative electrode.

[0033] Compared with the prior art, the technical solution of the present invention has at least the following technical effects:

[0034] (1) The present invention provides a silicon-based negative electrode material, comprising a pre-lithiated mesoporous silicon material and a carbon coating layer and an organic polymer coating layer sequentially arranged on the surface of the pre-lithiated mesoporous silicon material from the inside to the outside, wherein the organic polymer coating layer is mainly made of a copolymer formed by an acrylate monomer and an organic silicone resin precursor and a lithium supplement additive; wherein the pre-lithiated mesoporous silicon material can reserve a certain space for the expansion of silicon material particles and generate additional lithium insertion paths; and the carbon coating layer on the surface of the pre-lithiated mesoporous silicon material can improve the conductivity of the silicon-based negative electrode material and can also inhibit the expansion of silicon material particles to a certain extent; the organic polymer coating layer made of specific raw materials can well inhibit the occurrence of interfacial side reactions, and at the same time, cooperate with the carbon coating layer to further improve the structural stability of the electrode active material, reduce the expansion of the silicon-based negative electrode material during the charging and discharging process, and improve the cycle stability and safety of the battery, and the copolymer in the organic polymer coating layer has a certain synergistic effect with the lithium-containing additive, so that the electrode of the present invention has excellent ionic conductivity, thereby improving the lithium ion conductivity at the interface.

[0035] (2) The present invention provides a method for preparing the above-mentioned silicon-based negative electrode material. The raw materials used in the preparation method are widely available, low in cost, and simple in process, and are relatively easy to industrialize.

[0036] (3) The present invention also provides a lithium-ion battery, comprising the above silicon-based negative electrode material or a silicon-based negative electrode made from the above silicon-based negative electrode material. In view of the advantages of the silicon-based negative electrode material or the above silicon-based negative electrode of the present invention, the lithium-ion battery comprising the same has good cycle stability and safety. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. Among them:

[0038] Figure 1 A schematic structural diagram of a silicon-based negative electrode material according to an embodiment of the present invention.

[0039] Icons: 1-pre-lithiation mesoporous silicon material; 2-pores in pre-lithiation mesoporous silicon material; 3-carbon coating layer; 4-organic polymer coating layer. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0041] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in the present invention.

[0042] According to a first aspect of the present invention, a silicon-based negative electrode material is provided, comprising a pre-lithiated mesoporous silicon material 1 and a carbon coating layer 3 and an organic polymer coating layer 4 sequentially arranged on the surface of the pre-lithiated mesoporous silicon material 1 from the inside to the outside, as shown in the structural schematic diagram Figure 1 As shown;

[0043] The organic polymer coating layer 4 is mainly made of a copolymer formed by an acrylic ester monomer and an organic silicon resin precursor and a lithium supplement additive.

[0044] Specifically, the pre-lithiation mesoporous silicon material refers to a mesoporous silicon material that has been pre-lithiation treated. The mesoporous silicon material used in the present invention mainly reserves a certain space for the expansion of silicon material particles through the mesopores on the silicon material, and at the same time generates additional lithium insertion paths. The mesopores on the silicon material become the pores 2 in the pre-lithiation mesoporous silicon material. The mesoporous silicon material is pre-lithiation, and the generated lithium silicate and the like will be formed on at least part of the surface of the mesoporous silicon grains.

[0045] The carbon coating layer on the surface of the pre-lithiation mesoporous silicon material can improve the conductivity of the silicon-based negative electrode material on the one hand, and can also inhibit the expansion of the silicon material particles to a certain extent on the other hand. However, the inventors have found through a lot of practice that when the pre-lithiation mesoporous silicon material particles expand to a large extent, it may cause the surface carbon coating layer to rupture, and cause the residual lithium and lithium silicate formed by pre-lithiation to dissolve from the rupture of the carbon coating layer, making the material more alkaline in the aqueous slurry, and the active substances at the rupture of the carbon layer will react with water under alkaline conditions to produce hydrogen, resulting in poor slurry stability.

[0046] Therefore, the present invention further provides an organic polymer coating layer on the surface of the carbon coating layer of the pre-lithiation mesoporous silicon material to repair the rupture of the surface carbon coating layer, inhibit the dissolution of lithium silicate, and avoid contact between active substances and water. At the same time, there are cross-linking sites in the organic coating layer that can cross-link amorphous polymer blocks, which also include dynamic forces such as hydrogen bonds and coordination bonds, thereby significantly improving the tear resistance of the polymer material, and also significantly improving the strength, ductility and toughness of the polymer material, and having a self-repairing function, thereby being able to well inhibit the occurrence of interfacial side reactions and electrode expansion, and can improve the structural stability of the electrode active material, reduce the expansion of the silicon-based negative electrode material during the charge and discharge process, and improve the cycle stability and safety of the battery. At the same time, the copolymer in the organic polymer coating layer of the present invention can also form a synergistic effect with the lithium supplement additive, so that the electrode of the present invention has excellent ionic conductivity, thereby improving the lithium ion conductivity at the interface.

[0047] As an optional embodiment of the present invention, the particle size of the pre-lithiated mesoporous silicon material is 1-5 μm, and the pore size is 5-30 nm. Typical but non-limiting particle sizes are 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3.0 μm, 3.5 μm, 4 μm, 4.5 μm or 5.0 μm, and the numerical range between any two points, and typical but non-limiting pore sizes are 5 nm, 10 nm, 15 nm, 20 nm, 25 nm or 30 nm, and the numerical range between any two points.

[0048] By limiting the particle size of pre-lithiation mesoporous silicon materials, the material can be controlled to have a more appropriate particle size and specific surface area. If the particle size is too small and the specific surface area is too large, it is easier to agglomerate and the processing performance is poor. If the particle size is too large, the compaction density is reduced, which affects the energy density of the material system. Further limiting the pore size of pre-lithiation mesoporous silicon materials is mainly to form a suitable lithium insertion path and reserve a suitable space for silicon expansion.

[0049] As an optional embodiment of the present invention, the thickness of the carbon coating layer is 1-6 nm, and a typical but non-limiting thickness of the carbon coating layer is 1 nm, 2 nm, 3 nm, 4 nm, 5 nm or 6 nm.

[0050] As an optional embodiment of the present invention, the mass fraction of the carbon coating layer in the silicon-based negative electrode material is 0.5-3wt%, and the typical but non-limiting mass fraction is 0.5wt%, 0.8wt%, 1.0wt%, 1.2wt%, 1.5wt%, 1.8wt%, 2.0wt%, 2.2wt%, 2.5wt%, 2.8wt% or 3.0wt%, etc.

[0051] By further limiting the thickness and mass fraction of the carbon coating layer, the appropriate carbon content can be controlled. Too high or too low a carbon content is not conducive to the performance of the material.

[0052] As an optional embodiment of the present invention, the acrylate monomer includes at least one of methyl methacrylate, butyl acrylate, isobutyl acrylate or epoxy acrylate.

[0053] As an optional embodiment of the present invention, the organosilicon resin precursor includes at least one of polymethyl silicone resin, polyethyl silicone resin or polyaryl silicone resin.

[0054] As an optional embodiment of the present invention, the lithium supplement additive includes at least one of metallic lithium powder (or lithium foil, lithium sheet, lithium block), lithium hydride, lithium hydroxide or lithium carbonate.

[0055] As an optional embodiment of the present invention, the thickness of the organic polymer coating layer is 3-10 nm. A typical but non-limiting thickness of the organic polymer coating layer is 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm or 10 nm.

[0056] As an optional embodiment of the present invention, the mass fraction of the organic polymer coating layer in the silicon-based negative electrode material is 0.5-5wt%, and the typical but non-limiting mass fraction is 0.5wt%, 1.0wt%, 1.5wt%, 2.0wt%, 2.5wt%, 3.0wt%, 3.5wt%, 4.0wt%, 4.5wt% or 5.0wt%, etc. and the numerical range between any two points.

[0057] By further limiting the thickness and mass fraction of the organic polymer coating layer, the surface of the pre-lithiation mesoporous silicon material has an appropriate content of organic polymer. If the polymer content is too low, it cannot play a role in inhibiting expansion. If the polymer content is too high, it will affect the content of active substances and the energy density of the material system.

[0058] According to a second aspect of the present invention, there is also provided a method for preparing the above silicon-based negative electrode material, comprising the following steps:

[0059] (a) carbon-coating the pre-lithiated mesoporous silicon material to form a carbon coating layer to obtain a carbon-coated mesoporous silicon material;

[0060] (b) coating the carbon-coated mesoporous silicon material with an organic polymer to form an organic polymer coating layer on the surface of the carbon coating layer to obtain a silicon-based negative electrode material.

[0061] The preparation method of the present invention can avoid irreversible consumption during the first lithium insertion by pre-lithiation of a silicon material with a mesoporous structure (mesoporous silicon material), thereby improving the first coulombic efficiency of the material, and then carbon-coating the pre-lithiation mesoporous silicon material. The larger pre-lithiation mesoporous silicon material grains have higher thermodynamic stability, and at the same time, smaller silicon grains will be preferentially allowed to grow, and the growth of larger silicon grains will be inhibited, thereby obtaining a carbon-coated mesoporous silicon material with uniform particle size, and then organic polymer coating can effectively reduce the occurrence of side reactions, and coating on the surface of the carbon-coated mesoporous silicon material can effectively alleviate the electrode active material from being destroyed, collapsed or aggregated due to corrosion, so as to improve the structural stability of the electrode active material. At the same time, the organic polymer coating layer has excellent segment mobility, and has certain rigidity and elasticity, so that it will not break even when subjected to large stress during the cycle, thereby effectively inhibiting the expansion problem of the silicon-based negative electrode during the cycle, so as to further improve the safety performance and cycle stability of the battery.

[0062] The source of the pre-lithiated mesoporous silicon material is not limited. As an optional embodiment of the present invention, in step (a), the preparation method of the pre-lithiated mesoporous silicon material comprises the following steps:

[0063] After the silicon material is pore-formed by a pore-forming agent, a mesoporous silicon material is obtained;

[0064] The mesoporous silicon material is subjected to a pre-lithiation treatment to obtain a pre-lithiation mesoporous silicon material.

[0065] The silicon material may be a silicon source commonly used in the art. As an optional embodiment of the present invention, the silicon material includes at least one of silicon, silicon oxide, modified silicon oxide, silicon-carbon composite material or silicon alloy material.

[0066] As an optional embodiment of the present invention, the pore-forming agent includes at least one of silicon oxide, calcium oxide, magnesium oxide or molybdenum oxide. The present invention can utilize the pore-forming effect of the pore-forming agent during high temperature treatment to prepare a silicon material with a certain mesoporous structure.

[0067] As an optional embodiment of the present invention, the mass ratio of the pore former to the silicon material is (0.01-0.05):1, and a typical but non-limiting mass ratio is 0.01:1, 0.02:1, 0.03:1, 0.04:1 or 0.05:1, etc.

[0068] As an optional embodiment of the present invention, the pre-lithiation treatment includes solid-phase pre-lithiation and liquid-phase pre-lithiation.

[0069] When solid phase pre-lithiation is used, as a preferred embodiment of the present invention, the pre-lithiation reagent of the solid phase pre-lithiation includes at least one of lithium hydride, lithium nitride or lithium borohydride.

[0070] As a preferred embodiment of the present invention, the mass ratio of the pre-lithiation agent used in solid phase pre-lithiation to the mesoporous silicon material is (0.03-0.08):1, and a typical but non-limiting mass ratio is 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1 or 0.08:1, etc.

[0071] As a preferred embodiment of the present invention, the sintering temperature of solid phase pre-lithiation is 500-1000°C, and the sintering time is 15-24h. Typical but non-limiting sintering temperatures are 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or 1000°C, and typical but non-limiting sintering times are 15h, 16h, 18h, 20h, 22h or 24h, etc.

[0072] When liquid phase pre-lithiation is used, as a preferred embodiment of the present invention, the pre-lithiation reagent of the liquid phase pre-lithiation includes an aromatic radical anion complex of lithium. The aromatic radical anion complex of lithium is a complex system composed of lithium and aromatic radical anions, wherein the solvent composition of the complex is an ether solvent, the solute composition is a polycyclic aromatic compound, the reaction is carried out at 120° C. for 12 hours, the slurry is distilled for 5 hours, and finally sintered.

[0073] As a preferred embodiment of the present invention, the mass ratio of the pre-lithiation agent used in liquid phase pre-lithiation to the mesoporous silicon material is (0.1-0.15):1, and a typical but non-limiting mass ratio is 0.1:1, 0.11:1, 0.12:1, 0.13:1, 0.14:1 or 0.15:1, etc.

[0074] As a preferred embodiment of the present invention, the sintering temperature of liquid phase pre-lithiation is 600-1000°C, and the sintering time is 20-30h; typical but non-limiting sintering temperatures are 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or 1000°C, and typical but non-limiting sintering times are 20h, 22h, 24h, 25h, 26h, 28h or 30h, etc.

[0075] The coating method and process conditions of carbon coating will affect the coating effect of the carbon coating layer. As an optional embodiment of the present invention, in step (a), chemical vapor deposition method is used for carbon coating.

[0076] As an optional embodiment of the present invention, the temperature of carbon coating by chemical vapor deposition is 600-900°C, and the carbon coating time is 2-8h. Typical but non-limiting carbon coating temperatures are 600°C, 650°C, 680°C, 700°C, 720°C, 750°C, 780°C, 800°C, 820°C, 850°C, 880°C or 900°C, and typical but non-limiting carbon coating times are 2h, 3h, 4h, 5h, 6h, 7h or 8h, etc.

[0077] As an optional embodiment of the present invention, the carbon source used for carbon coating by chemical vapor deposition includes at least one of acetylene, graphene, cracked carbon, carbon nanotubes, carbon nanofibers, graphite or amorphous carbon.

[0078] By limiting the specific method of carbon coating and the process parameters, the carbon coating layer can be evenly coated on the surface of the pre-lithiated mesoporous silicon material.

[0079] As an optional embodiment of the present invention, in step (b), a copolymer formed by an acrylic ester monomer and a silicone resin precursor, a lithium supplement additive and a carbon-coated mesoporous silicon material are mixed and heated and cured under vacuum conditions to perform organic polymer coating.

[0080] As an optional embodiment of the present invention, the lithium supplement additive includes at least one of lithium powder, lithium foil, lithium sheet, lithium block, lithium hydride, lithium hydroxide or lithium carbonate.

[0081] As an optional embodiment of the present invention, the mass ratio of the copolymer formed by the acrylic ester monomer and the silicone resin precursor, the lithium supplement additive and the carbon-coated mesoporous silicon material is (0.005-0.03): (0.002-0.02):1. Typical but non-limiting mass ratios are 0.005:0.002:1, 0.01:0.002:1, 0.02:0.002:1, 0.03:0.002:1, 0.005:0.005:1, 0.01:0.005:1, 0.02:0.005:1, 0.03:0.005:1, 0.005:0.01:1, 0.01:0.01:1, 0.02:0.01:1, 0.03:0.01:1, 0.005:0.02:1, 0.01:0.01:1, 0.02:0.01:1, 0.03:0.01:1 or 0.03:0.02:1, etc.

[0082] As an optional embodiment of the present invention, the heating temperature is 500-1000°C, and the heating time is 1-4h. Typical but non-limiting heating temperatures are 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or 1000°C, and the heating time is 1h, 2h, 3h or 4h, etc.

[0083] According to a third aspect of the present invention, there is also provided a silicon-based negative electrode, comprising the above-mentioned silicon-based negative electrode material or the silicon-based negative electrode material prepared by the above-mentioned preparation method.

[0084] A fourth aspect of the present invention further provides a lithium-ion battery comprising the above-mentioned silicon-based negative electrode material or the above-mentioned silicon-based negative electrode.

[0085] In view of the advantages of the silicon-based negative electrode material of the present invention or the above silicon-based negative electrode, the lithium-ion battery containing the same has good cycle stability and safety.

[0086] The present invention is further described in detail below in conjunction with specific embodiments and comparative examples. Among them, the raw materials used in the embodiments and comparative examples are described as follows: methyl methacrylate, chemical formula CH2=C(CH3)COOCH3, purchased from Nanjing Chemical Reagent Co., Ltd., AR grade, content 99%, molecular weight 100.12; butyl acrylate, chemical formula CH2CHCOO(CH2)3CH3, purchased from Nanjing Chemical Reagent Co., Ltd., CP grade, molecular weight 128.17; isobutyl acrylate, purchased from Suzhou Hechuang Chemical Co., Ltd., purity 99%, glass transition temperature -24°C; polymethyl silicone resin and polyethyl silicone resin were purchased from Shandong Dongyue Organic Silicone Materials Co., Ltd.

[0087] Example 1

[0088] This embodiment provides a silicon-based negative electrode material, including a pre-lithiated mesoporous silicon material and a carbon coating layer and an organic polymer coating layer sequentially arranged on the surface of the pre-lithiated mesoporous silicon material from the inside to the outside;

[0089] Among them, the thickness of the carbon coating layer is about 6nm, and the mass fraction of the carbon coating layer accounts for 2% of the entire silicon-based negative electrode material; the organic polymer coating layer is mainly made of a copolymer formed by an acrylate monomer and a silicone resin precursor and a lithium supplement additive. The thickness of the organic polymer coating layer is 5nm, and the mass fraction of the organic polymer coating layer accounts for 2% of the entire silicon-based negative electrode material.

[0090] The method for preparing the silicon-based negative electrode material of this embodiment comprises the following steps:

[0091] (a) Preparation of pre-lithiated mesoporous silicon materials

[0092] a1. Silicon and silicon dioxide (mass ratio of silicon to silicon dioxide is 1:0.9) are mixed and sintered at high temperature in a vacuum furnace (sintering temperature is 1300°C, sintering time at sintering temperature is 2h) to generate silicon dioxide (SiOx, x is close to 1 but not strictly equal to 1);

[0093] a2. The silicon oxide obtained in step a1 is pulverized and classified by air flow to a D50 particle size of about 2.5 μm, and then mesoporous silicon oxide is prepared by the pore-forming effect of a silicon oxide pore-forming agent during high temperature (900° C.) treatment. The particle size of the mesoporous silicon oxide is about 2.5 μm and the pore size is 20 nm.

[0094] a3, subjecting the mesoporous silicon oxide obtained in step a2 to solid phase pre-lithiation treatment, sintering at 700° C. for 18 h in a CVD furnace containing a pre-lithiation agent, lithium hydride (the concentration of the pre-lithiation agent solution is 1.2 mol / L, and the mass ratio of lithium hydride to mesoporous silicon oxide is 0.06:1), to obtain pre-lithiation mesoporous silicon oxide;

[0095] (b) the pre-lithiated mesoporous silicon oxide is subjected to CVD carbon coating treatment at 800° C. for 8 h to form a carbon coating layer to obtain carbon-coated mesoporous silicon oxide (silicon grain size is between 4 and 6 μm);

[0096] The carbon source gas of the CVD method is acetylene, the coating temperature is 800°C, the coating time is 8h, the thickness of the formed carbon coating layer is 6nm, and the mass fraction of the carbon coating layer in the entire silicon-based negative electrode material is 2%;

[0097] (c) placing the carbon-coated mesoporous silica prepared in step (b) in a copolymer of an acrylate monomer (methyl methacrylate) and a silicone resin precursor (polymethyl silicone resin), and a powder of a lithium supplement additive (lithium powder) (the mass ratio of the carbon-coated mesoporous silica, the copolymer and the lithium supplement additive is 1:0.03:0.02), and heating and curing at 600°C under vacuum conditions for 2 hours to form an organic polymer coating layer on the surface of the carbon coating layer to obtain a silicon-based negative electrode material.

[0098] Example 2

[0099] This embodiment provides a silicon-based negative electrode material, including a pre-lithiated mesoporous silicon material and a carbon coating layer and an organic polymer coating layer sequentially arranged on the surface of the pre-lithiated mesoporous silicon material from the inside to the outside;

[0100] Among them, the thickness of the carbon coating layer is about 5nm, and the mass fraction of the carbon coating layer accounts for 2.5% of the entire silicon-based negative electrode material. The organic polymer coating layer is mainly made of a copolymer formed by an acrylate monomer and a silicone resin precursor and a lithium supplement additive. The thickness of the organic polymer coating layer is 6nm, and the mass fraction of the organic polymer coating layer accounts for 2.8% of the entire silicon-based negative electrode material.

[0101] The method for preparing the silicon-based negative electrode material of this embodiment comprises the following steps:

[0102] (a) Preparation of pre-lithiated mesoporous silicon materials

[0103] a1. Silicon and silicon dioxide (mass ratio of silicon to silicon dioxide is 1:0.85) are mixed and sintered at high temperature in a vacuum furnace (sintering temperature is 1450°C, sintering time at sintering temperature is 2.5h) to generate silicon dioxide (SiOx, x is close to 1 but not strictly equal to 1);

[0104] a2. The silicon oxide obtained in step a1 is pulverized and classified by air flow to a particle size of about 3.0 μm, and then mesoporous silicon oxide is prepared by the pore-forming effect of a silicon oxide pore-forming agent during high temperature (900° C.) treatment. The particle size of the mesoporous silicon oxide is about 3.0 μm and the pore size is 25 nm.

[0105] a3, subjecting the mesoporous silicon oxide obtained in step a2 to solid phase pre-lithiation treatment, sintering at 650° C. for 20 h in a CVD furnace containing pre-lithiation agents lithium hydride and lithium nitride (the concentration of the pre-lithiation agent solution is 1 mol / L, and the mass ratio of lithium hydride, lithium nitride and mesoporous silicon oxide is 0.025:0.025:1), to obtain pre-lithiation silicon oxide (silicon grain size is between 4-6 μm);

[0106] (b) The pre-lithiated silicon dioxide is subjected to CVD carbon coating treatment at 850° C. for 3 h to form a carbon coating layer to obtain carbon-coated mesoporous silicon dioxide (with a grain size of 4-6 μm);

[0107] The carbon source gas of the CVD method is methane, the thickness of the formed carbon coating layer is 5nm, and the mass fraction of the carbon coating layer in the entire silicon-based negative electrode material is 2.5%;

[0108] (c) placing the carbon-coated mesoporous silica prepared in step (b) in a copolymer formed by butyl acrylate and polyethyl silicone resin and a powder of a lithium supplement additive (the mass ratio of the carbon-coated mesoporous silica, the copolymer and the lithium supplement additive is 1:0.02:0.015), and solid-phase sintering them in a rail kiln at 60-200°C under vacuum conditions to obtain a silicon-based negative electrode material.

[0109] Example 3

[0110] This embodiment provides a silicon-based negative electrode material. Except that the thickness of the carbon coating layer is about 2 nm and the mass fraction of the carbon coating layer in the whole silicon-based negative electrode material is 0.75%, the types and amounts of other raw materials are the same as those in Embodiment 1.

[0111] The method for preparing the silicon-based negative electrode material in this embodiment is the same as that in Embodiment 1 except that the parameters of the CVD carbon coating treatment in step (b) are adjusted accordingly.

[0112] The specific steps of step (b) are: the pre-lithiated silicon dioxide is subjected to CVD carbon coating treatment at 850° C. for 4 hours to form a carbon coating layer to obtain carbon-coated mesoporous silicon dioxide (with a grain size of 6-8 μm);

[0113] The carbon source gas of the CVD method is methane, the thickness of the formed carbon coating layer is 2 nm, and the mass fraction of the carbon coating layer in the entire silicon-based negative electrode material is 0.75 wt%.

[0114] Example 4

[0115] This embodiment provides a silicon-based negative electrode material. Except that the thickness of the organic polymer coating layer is about 1.5 nm, the types and amounts of other raw materials are the same as those in Embodiment 1.

[0116] The preparation method of the silicon-based negative electrode material in this embodiment is the same as that in Example 1, except that the mass ratio of carbon-coated mesoporous silicon oxide, copolymer and lithium supplement additive in step (c) is adjusted from 1:0.03:0.02 to 1:0.012:0.01. The remaining steps and process parameters are the same as those in Example 1.

[0117] Example 5

[0118] This embodiment provides a silicon-based negative electrode material. Except that the type of acrylic ester monomer in the organic polymer coating layer is replaced by isobutyl acrylate from methyl methacrylate, the types and amounts of other raw materials are the same as those in Example 1.

[0119] The method for preparing the silicon-based negative electrode material in this embodiment is the same as that in Embodiment 1 except that the type of acrylic ester monomer in step (c) is replaced by isobutyl acrylate from methyl methacrylate. The remaining steps and process parameters are the same as those in Embodiment 1.

[0120] Comparative Example 1

[0121] This comparative example provides a silicon-based negative electrode material, including a pre-lithiation silicon material and a carbon coating layer and an organic polymer coating layer sequentially arranged on the surface of the pre-lithiation silicon material from the inside to the outside;

[0122] Among them, the thickness of the carbon coating layer is about 6nm, and the mass fraction of the carbon coating layer accounts for 2% of the entire silicon-based negative electrode material. The organic polymer coating layer is mainly made of a copolymer formed by an acrylate monomer (methyl methacrylate) and a silicone resin precursor (polymethyl silicone resin) and a lithium supplement additive. The thickness of the organic polymer coating layer is 5nm, and the mass fraction of the organic polymer coating layer accounts for 2% of the entire silicon-based negative electrode material.

[0123] The preparation method of the silicon-based negative electrode material of this comparative example comprises the following steps:

[0124] a1. Silicon and silicon dioxide (mass ratio of silicon to silicon dioxide is 1:0.9) are mixed and sintered at high temperature in a vacuum furnace (sintering temperature is 1300°C, sintering time at sintering temperature is 2h) to generate silicon dioxide (SiOx, x is close to 1 but not strictly equal to 1);

[0125] a2. The silicon oxide obtained in step a1 is pulverized and classified to a particle size of about 2.5 μm by air flow, and then subjected to solid phase pre-lithiation treatment, and sintered at 700° C. for 18 h in a CVD furnace containing a pre-lithiation agent, lithium hydride (the concentration of the pre-lithiation agent solution is 1.2 mol / L, and the mass ratio of lithium hydride to silicon oxide is 0.06:1), to obtain pre-lithiation silicon oxide;

[0126] (b) the pre-lithiated silicon oxide is subjected to a CVD carbon coating treatment at 800° C. for 8 h to form a carbon coating layer to obtain a carbon-coated silicon oxide;

[0127] The carbon source gas of the CVD method is acetylene, the coating temperature is 800°C, the coating time is 8h, the thickness of the formed carbon coating layer is 6nm, and the mass fraction of the carbon coating layer in the entire silicon-based negative electrode material is 2%;

[0128] (c) The carbon-coated silicon oxide prepared in step (b) is placed in a copolymer of an acrylate monomer (methyl methacrylate) and a silicone resin precursor (polymethyl silicone resin), and a powder of a lithium supplement additive (lithium powder) (the mass ratio of the carbon-coated mesoporous silicon oxide, the copolymer and the lithium supplement additive is 1:0.03:0.02), and heated and cured at 600°C under vacuum conditions for 2 hours to form an organic polymer coating layer on the surface of the carbon coating layer to obtain a silicon-based negative electrode material.

[0129] Comparative Example 2

[0130] This comparative example provides a silicon-based negative electrode material. Except that no organic polymer coating layer is provided on the surface of the pre-lithiation mesoporous silicon material, the other raw material types and structures are the same as those in Example 1.

[0131] The preparation method of the silicon-based negative electrode material in this comparative example is the same as that in Example 1 except that step (c) is not provided. The remaining steps and process parameters are the same as those in Example 1.

[0132] Comparative Example 3

[0133] This comparative example provides a silicon-based negative electrode material, except that the organic polymer coating layer in Example 1 is made of bisphenol A solid epoxy resin (purchased from Shanghai Yuanbang Group, brand YPE-011, white or light yellow flaky solid, epoxy equivalent 450-500, epoxy value 0.200-0.222, softening point 60-70°C) and a lithium supplement additive, the remaining raw materials, amounts and structures are the same as those in Example 1.

[0134] The preparation method of the silicon-based negative electrode material in this comparative example is the same as that in Example 1, except that the copolymer of the acrylate monomer and the silicone resin precursor in step (c) is replaced by an epoxy resin copolymer. The remaining steps and process parameters are the same as those in Example 1.

[0135] Comparative Example 4

[0136] This comparative example provides a silicon-based negative electrode material. Except that no lithium supplement additive is added to the organic polymer coating layer in Example 1, the remaining raw materials, dosage and structure are the same as those in Example 1.

[0137] The preparation method of the silicon-based negative electrode material in this comparative example is the same as that in Example 1, except that no lithium supplement additive is added in step (c). The remaining steps and process parameters are the same as those in Example 1.

[0138] In order to further verify the technical effects of the above embodiments and comparative examples, the following experimental examples are specially designed.

[0139] Experimental Example 1

[0140] The silicon-based negative electrode materials provided in each embodiment and comparative example are made into lithium-ion batteries, and the specific preparation method is as follows:

[0141] The silicon-based negative electrode material prepared in each embodiment and comparative example was mixed with the conductive agent SP (carbon black) and the binder PAA (polyacrylic acid) in a mass ratio of 8:1:1, and stirred for 2 hours to obtain a slurry with suitable viscosity. The slurry was coated on a copper foil with a thickness of 9 μm, and then dried under vacuum at 75°C to obtain a negative electrode sheet. A sheet punching machine was used to obtain a disc with a diameter of 10 mm, and the weight of the active material was weighed and calculated. The surface density of the obtained negative electrode sheet is 50 mg / 10 cm 2 , thickness 142μm.

[0142] A metallic lithium sheet was used as the counter electrode, a polypropylene microporous membrane was used as the separator, and 1 mol / L LiPF6 (the solvent was a mixture of ethylene carbonate and dimethyl carbonate in a volume ratio of 0.8:1, to which vinylidene fluoride carbonate (accounting for 4.5% by mass of the electrolyte) and vinylene carbonate (accounting for 1.8% by mass of the electrolyte) were added) was used as the electrolyte, and a button battery with a theoretical capacity of 5 mAh was assembled in a glove box.

[0143] The button cell was placed at room temperature and subjected to charge and discharge tests and cycle tests on a blue power test system. The specific test methods are as follows:

[0144] (1) First Coulomb efficiency:

[0145] In the power-off test at 25°C, 0.1C, 0.05C, and 0.01C were continuously discharged to 0.005V respectively, and then charged to 2V at 0.1C after being left alone. The first coulomb efficiency = first charge capacity / first discharge capacity;

[0146] (2) Charge and discharge cycle life test:

[0147] 1) Place at 25℃±2℃ for 120min;

[0148] 2) Charge to 3.4V at 1C CC (constant current), then charge to 0.05C at CV (constant voltage);

[0149] 3) Leave for 5 minutes.

[0150] 4) Discharge at 0.2C DC (constant current) to 2.0V, recorded as C0;

[0151] 5) Place at 25℃±2℃ for 120min;

[0152] 6) Leave for 5 minutes.

[0153] 7) Charge to 3.4V with 1C0 CC (constant current), then charge to 0.05C0 with CV (constant voltage);

[0154] 8) Leave for 5 minutes;

[0155] 9) Discharge at 1C0 DC (constant current) to 2.0V;

[0156] 10) Leave for 5 minutes;

[0157] 11) Repeat steps 7-10 500 times;

[0158] The 500th cycle charging capacity / the 1st cycle charging capacity is the 500-cycle cycle capacity retention rate, and the 500th cycle negative electrode sheet thickness / the negative electrode sheet thickness before the test is the 500-cycle battery negative electrode sheet expansion rate (%). The specific results are shown in Table 1.

[0159] Table 1

[0160]

[0161] It can be seen from the data in Table 1 that Examples 1 to 5 only vary the processes within the design range, and there are no significant differences in the first coulomb efficiency, the 500-cycle capacity retention rate, and the 500-cycle battery negative electrode sheet expansion rate.

[0162] Comparative Examples 1-4 are all comparative experiments of Example 1. Compared with Example 1, Comparative Example 1 does not use mesoporous silicon material, Comparative Example 2 does not set an organic polymer coating layer, and Comparative Example 3 does not use the organic polymer defined in the present invention in the organic polymer coating layer, but uses other copolymers. Combined with the data in the above table, it can be seen that the first coulomb efficiency, 500-cycle cycle capacity retention rate, and 500-cycle battery negative electrode plate expansion rate of Comparative Examples 1-3 have all deteriorated to a certain extent. Compared with Example 1, Comparative Example 4 does not add lithium supplement additives, and its first coulomb efficiency deteriorates more seriously, and the 500-cycle cycle capacity retention rate and 500-cycle battery negative electrode plate expansion rate deteriorate less than Comparative Examples 1-3, indicating that the organic polymer coating still plays a role in improving circulation and inhibiting expansion.

[0163] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A silicon-based negative electrode material, characterized in that: It comprises a pre-lithiated mesoporous silicon material and a carbon coating layer and an organic polymer coating layer sequentially arranged on the surface of the pre-lithiated mesoporous silicon material from the inside to the outside; The organic polymer coating layer is mainly made of a copolymer formed by an acrylic ester monomer and an organic silicon resin precursor and a lithium supplement additive.

2. The silicon-based negative electrode material according to claim 1, characterized in that: The particle size of the pre-lithiation mesoporous silicon material is 1-5 μm, and the pore size is 5-30 nm; And / or, the thickness of the carbon coating layer is 1-6 nm; And / or, the mass fraction of the carbon coating layer in the silicon-based negative electrode material is 0.5-3wt%.

3. The silicon-based negative electrode material according to claim 1, characterized in that: The acrylic acid ester monomer includes at least one of methyl methacrylate, butyl acrylate, isobutyl acrylate or epoxy acrylate; and / or, the organosilicon resin precursor comprises at least one of polymethyl silicone resin, polyethyl silicone resin or polyaryl silicone resin; And / or, the lithium supplement additive includes at least one of metallic lithium powder, lithium hydride, lithium hydroxide or lithium carbonate; And / or, the thickness of the organic polymer coating layer is 3-10 nm; And / or, the mass fraction of the organic polymer coating layer in the silicon-based negative electrode material is 0.5-5wt%.

4. The method for preparing the silicon-based negative electrode material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (a) carbon-coating the pre-lithiated mesoporous silicon material to form a carbon coating layer to obtain a carbon-coated mesoporous silicon material; (b) coating the carbon-coated mesoporous silicon material with an organic polymer to form an organic polymer coating layer on the surface of the carbon coating layer to obtain a silicon-based negative electrode material.

5. The method for preparing a silicon-based negative electrode material according to claim 4, characterized in that: In step (a), the method for preparing the pre-lithiated mesoporous silicon material comprises the following steps: After the silicon material is pore-formed by a pore-forming agent, a mesoporous silicon material is obtained; The mesoporous silicon material is subjected to a pre-lithiation treatment to obtain a pre-lithiation mesoporous silicon material.

6. The method for preparing a silicon-based negative electrode material according to claim 5, characterized in that: The silicon material includes at least one of silicon, silicon oxide, modified silicon oxide, silicon-carbon composite material or silicon alloy material; and / or, the pore-forming agent comprises at least one of silicon oxide, calcium oxide, magnesium oxide or molybdenum oxide; And / or, the pre-physical and chemical treatment includes solid-phase pre-lithiation and liquid-phase pre-lithiation; preferably, the sintering temperature of the solid-phase pre-lithiation is 500-1000°C, and the sintering time is 15-24h; preferably, the pre-lithiation reagent of the solid-phase pre-lithiation includes at least one of lithium hydride, lithium nitride or lithium borohydride; preferably, the sintering temperature of the liquid-phase pre-lithiation is 600-1000°C, and the sintering time is 20-30h; preferably, the pre-lithiation reagent of the liquid-phase pre-lithiation includes an aromatic radical anion complex of lithium.

7. The method for preparing a silicon-based negative electrode material according to claim 4, characterized in that: In step (a), carbon coating is performed by chemical vapor deposition; and / or, the temperature for carbon coating by chemical vapor deposition is 600-900° C., and the carbon coating time is 2-8 hours; And / or, the carbon source used for carbon coating by chemical vapor deposition includes at least one of acetylene, graphene, cracked carbon, carbon nanotubes, carbon nanofibers, graphite or amorphous carbon.

8. The method for preparing a silicon-based negative electrode material according to any one of claims 4 to 7, characterized in that: In step (b), a copolymer formed by an acrylic ester monomer and an organic silicon resin precursor, a lithium supplement additive and a carbon-coated mesoporous silicon material are mixed, and heated and cured under vacuum conditions to perform organic polymer coating; Preferably, in step (b), the heating temperature is 500-1000° C., and the heating time is 1-4 h.

9. A silicon-based negative electrode, characterized in that: The invention relates to a silicon-based negative electrode material comprising the silicon-based negative electrode material according to any one of claims 1 to 3 or the silicon-based negative electrode material prepared by the preparation method according to any one of claims 4 to 8.

10. A lithium ion battery, characterized in that: Contains the silicon-based negative electrode material according to any one of claims 1 to 3 or the silicon-based negative electrode according to claim 9.

Citation Information

Patent Citations

  • Negative electrode material with multiple coating structures as well as preparation method and application of negative electrode material

    CN110993949A

  • Organic coating layer, electrode active material containing same and lithium ion battery

    CN113707883A

  • Negative electrode material, preparation method, negative electrode slurry, negative electrode pole piece and battery

    CN117878290A

  • Pre-lithiated silica composite material, preparation method, negative pole piece and lithium ion battery

    CN118335927A

  • Method for manufacturing negative electrode active material for nonaqueous secondary batteries, active material for nonaqueous secondary batteries manufactured thereby, negative electrode for nonaqueous secondary batteries, and nonaqueous secondary battery

    JP2015035315A

Cited By

  • Silicon-based self-supporting electrode material and preparation method and application thereof

    CN121905825A