Light gasoline olefin reduction-modification catalyst and preparation method thereof, light gasoline olefin reduction-modification method

The preparation of multi-stage structure Beta molecular sieve catalysts containing magnesium, nickel and gallium by liquid phase hydrothermal synthesis, solving the problems of small pores and high metal modification costs in traditional Beta molecular sieve, achieving efficient catalyst preparation and light gasoline reduction olefins- Improved reaction performance.

CN114713279BActive Publication Date: 2024-11-26PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110015518.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-06
Publication Date
2024-11-26
Estimated Expiration
2041-01-06

AI Technical Summary

Technical Problem

The small pore size of traditional Beta molecular sieve leads to diffusion limitations, and the metal modification method is costly and has a long cycle, making it difficult to achieve industrial application.

Method used

The liquid phase hydrothermal synthesis method is used to prepare Beta molecular sieve with a multi-stage structure containing magnesium, nickel and gallium with low silicon-aluminum ratio. Through hydrothermal loading, the synchronous precipitation of the metal salt precursor and the silicon-aluminum gel are controlled to form uniform dispersion. The catalyst is optimized by using two-stage temperature crystallization method and multi-stage calcination procedure.

Benefits of technology

The efficient diffusion performance and reaction activity of the catalyst are achieved, the preparation cost and cycle are reduced, and it is suitable for industrial production, and it shows excellent selective conversion ability in light gasoline reduction-olefin modification reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114713279B_ABST
    Figure CN114713279B_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a catalyst for reducing olefins in light gasoline. The preparation method adopts a hydrothermal synthesis method and comprises at least the following steps: first, mixing a silicon-containing source solution with an aluminum-containing source solution to form a mixed solution, wherein the silicon-containing source solution comprises a silicon source, a template agent, a nickel source and water; the aluminum-containing source solution comprises a silicon source, an aluminum source, a template agent, an alkali metal, a magnesium source, a gallium source and water; in the mixed solution, based on corresponding oxides, the molar ratio of each component is 1: 0.5-0.9: 0.02-0.1: 0.1-0.5: 0-0.03: 0-0.1: 0.005-0.015: 12-20; then, the mixed solution is subjected to hydrothermal crystallization, post-treatment and calcination to obtain a multi-level structure Beta molecular sieve catalyst containing in-situ doped gallium and nickel or / and magnesium. The present invention also relates to a catalyst for reducing olefins in light gasoline and a method for reducing olefins in light gasoline.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of olefin reduction and modification of light gasoline, and specifically relates to a catalyst for olefin reduction and modification of light gasoline and a preparation method thereof, and a method for olefin reduction and modification of light gasoline. Background Art

[0002] Beta zeolite is a molecular sieve with a cross-twelve-membered ring channel structure. It has high hydrothermal stability and lipophilicity and hydrophobicity. It is a good catalyst in itself and is often used as a solid acid catalyst in hydrocarbon polymerization, alkyl transfer, alkylation of aromatics, hydrocarbon cracking and other catalytic reactions. At the same time, because of its high specific surface area and excellent ion exchange performance, it is also an excellent carrier of catalytically active metal ions or metal compounds. The silicon-aluminum ratio of Beta zeolite is adjustable in a wide range, and its hydrothermal and thermal stability are high. Compared with other zeolite materials, Beta zeolite has very important application prospects in the field of petrochemicals. However, the small pore size of traditional Beta molecular sieves has caused diffusion limitations that seriously affect its catalytic application. At the same time, Beta is used in olefin aromatization reactions and often requires one or more metal modifications. The modification method involves the length of the operation cycle and the cost, which in turn affects its industrial application.

[0003] The problem of small pores and diffusion limitation in traditional Beta molecular sieves is currently basically solved by preparing multi-level Beta molecular sieves. The current preparation methods of multi-level Beta molecular sieves mainly include post-treatment method, hard template method and soft template method.

[0004] Post-treatment methods include dealumination and desiliconization. The dealumination method usually uses high-temperature hydrothermal treatment and acid treatment to remove aluminum atoms from the zeolite framework to generate mesopores. Similarly, the desiliconization method mainly uses alkali treatment to remove silicon atoms in the framework to obtain mesopores. The hard template method often uses carbon materials as templates, which can produce a variety of mesoporous structures. In the preparation process of the soft template method, it was found that the matching of charge density between surfactants and inorganic substances at the interface is the key to the successful assembly of mesoporous materials. The post-treatment methods of desiliconization and dealumination have different post-treatment effects when treating zeolites with different silicon-aluminum ratios; the hard template method can obtain highly ordered multi-level structure zeolites, but the route is costly and has a long cycle; the product mesopores obtained by the soft template method are highly controllable, but it requires expensive structure-directing agents and the steps are relatively cumbersome, making industrialization difficult.

[0005] In addition, for the introduction of metals, the current introduction methods are mainly divided into hydrothermal loading, impregnation, ion exchange and mechanical mixing. The hydrothermal method is to directly add a metal salt solution during the hydrothermal synthesis process, load it on the catalyst during the subsequent crystallization process, and transfer most of it to the surface of the molecular sieve channel after calcination. This preparation method can make the metal oxide uniformly loaded, and the operation is very simple, and the loaded metal is not easy to lose. The impregnation method is that the molecular sieve is immersed in a metal inorganic salt solution, and the metal ions adsorbed on the molecular sieve channel obtain active components such as metal oxides after calcination. This method is more troublesome to operate and takes a long time to prepare. The ion exchange method is to put the molecular sieve into a metal salt solution under certain temperature and pH conditions to exchange and replace metal ions with skeleton aluminum atoms. This method is also more troublesome and cannot control the amount of metal loaded. The mechanical mixing method is to physically mix and stir the metal salt and the molecular sieve. Although this method is simple, its metal ions are difficult to enter the pore surface to achieve a synergistic effect with the acidic sites on the pore surface. Summary of the invention

[0006] In view of the above problems of the prior art, the purpose of the present invention is to provide a method for preparing a light gasoline olefin reduction-modification catalyst, which adopts a liquid phase hydrothermal synthesis method to synthesize a Beta molecular sieve with a multi-level structure containing magnesium, nickel, gallium and a low silicon-to-aluminum ratio. The preparation method adopts a hydrothermal loading method and has many advantages such as being simple, green, having a short operation cycle, low cost and being more conducive to industrialization.

[0007] To this end, the present invention provides a method for preparing a light gasoline olefin reduction-upgrading catalyst, characterized in that a hydrothermal synthesis method is adopted, and the preparation method at least comprises the following steps:

[0008] First, a silicon source solution and an aluminum source solution are mixed to form a mixed solution, wherein the silicon source solution is composed of: a silicon source (in the form of SiO 2 ), template, nickel source (in NiO) and water; the composition of the aluminum source solution is: silicon source (in SiO 2 ), aluminum source (in Al 2 O 3 ), template, alkali metal (Na 2 O), magnesium source (in MgO), gallium source (in Ga 2 O 3 and water;

[0009] In the mixed solution, the molar ratio of each component, calculated on the basis of the corresponding oxide, is:

[0010] Silicon source: template: aluminum source: alkali metal: nickel source: magnesium source: gallium source: water is 1: 0.5-0.9: 0.02-0.1: 0.1-0.5: 0-0.03: 0-0.1: 0.005-0.015: 12-20;

[0011] Then, the mixed solution is subjected to hydrothermal crystallization, post-treatment and calcination to obtain a multi-level structure Beta molecular sieve catalyst containing in-situ doped gallium and nickel and / or magnesium.

[0012] The present invention relates to the preparation method of the catalyst. First, by mixing different metal salt precursors and silicon or aluminum sources in a specific ratio, a suitable pH value is constructed, and the hydrolysis and condensation reactions of the metal salt precursors and the silicon or aluminum sources are controlled to ensure that the precipitation process of the metal ions and the silicon or aluminum source during the hydrothermal synthesis process can be synchronized with the crystallization of the silica-alumina gel, thereby avoiding the generation of large particles of metal hydroxides or oxides that cannot enter the pores of the zeolite, and ensuring that the size of the metal salt hydrolysis and condensation products is small enough to enter the pores of the zeolite and be evenly dispersed. Secondly, by using a specific ratio of silica-alumina gel, the Beta zeolite can generate a multi-level pore structure of nanocrystal accumulation, and the intercrystalline mesopores generated by the accumulation of nanocrystals can be used to increase the size and number of the generation space of the metal hydroxide or oxide during the synthesis process, and on the other hand, improve the problem of pore blockage between the metal and the zeolite pores, solve the problem of excess reactants and products during the reaction process, and improve the performance of the catalyst.

[0013] In the preparation method described in the present invention, the template agent is introduced in the following manner: the template agent is introduced into the silicon-containing source solution and the aluminum-containing source solution respectively. The present invention also successfully and more reasonably prepares the magnesium, nickel, gallium low-silicon multi-level structure Beta molecular sieve by designing the processing and adding sequence of the raw materials. In the processing of the silicon source and the nickel source, since nickel is a non-bipolar metal, only a certain amount of water can be added without adding alkali metal. In this way, the silicon source and the nickel source solution can be kept in a neutral condition of about pH 7, so that the metal nickel ions can be dissolved to the greatest extent and evenly dispersed in the SiO 2 In the treatment of aluminum source, magnesium source and gallium source, since aluminum is a dual metal and magnesium is an alkaline earth metal, and gallium source has a high solubility in alkaline solution, a small amount of water and a certain amount of alkali metal can be added. This can keep the aluminum source, magnesium source and gallium source solutions at a higher alkalinity, so that the aluminum source, magnesium source and gallium source can be fully dissolved and evenly mixed in the state of ions.

[0014] The preparation method of the light gasoline olefin reduction-modification catalyst of the present invention is preferably that the hydrothermal crystallization is a two-stage hydrothermal crystallization, comprising the following steps: (1) heating the mixed solution to 100-120°C and performing pre-crystallization for 12-48 hours; (2) heating the mixed solution after pre-crystallization to 160-180°C and performing re-crystallization for 12-24 hours.

[0015] The present invention combines the control of the crystallization process, further proposes a crystallization theory that uses low temperature to facilitate nucleation, and recommends a two-stage crystallization method. First, under low temperature conditions, the growth of crystals is restricted, the generation of crystal nuclei is promoted, and the metal salt precursor and the silica-alumina gel are controlled to generate crystal nuclei with smaller particle sizes at low temperatures. When the number of crystal nuclei is generated sufficiently large, the temperature is rapidly increased, and the crystals are rapidly grown into small particles in a short period of time at high temperature, so that the growth of the silica-alumina gel on the crystal nuclei is achieved, and the metal oxide can be coated inside the zeolite pores, ensuring that the transition metal is more evenly dispersed on the zeolite molecular sieve. Due to the high surface activation energy of small particles, they will spontaneously agglomerate to form large particles of multi-level structure molecular sieves. The two-stage temperature crystallization method can successfully prepare multi-level structure Beta molecular sieves, while also saving energy and time.

[0016] In the preparation method described in the present invention, it is preferred that an aging treatment is performed before and / or after the silicon-containing source solution and the aluminum-containing source solution are mixed; wherein, before mixing, the aging treatment conditions of the silicon-containing source solution are: stirring and aging for 2-10 hours at a temperature of 50-90°C, preferably 60-80°C; before mixing, the aging treatment conditions of the aluminum-containing source solution are: stirring and aging for 5-10 hours at a temperature of 30-90°C, preferably 40-60°C, until completely dissolved; after mixing, the aging treatment conditions of the mixed solution are: aging for 2-5 hours at a temperature of 30-90°C, preferably 50-70°C.

[0017] The present invention finds that due to the addition of metal elements such as magnesium, nickel and gallium, these metal ions will affect the crystallization and growth process of silicon and aluminum gel in the zeolite synthesis process in the hydrothermal system, making the crystallization of zeolite more difficult. Therefore, the present invention preferably performs an aging treatment at a specific temperature for a period of time before and / or after mixing the silicon-containing source solution with the aluminum-containing source solution, and by combining the physical properties of different metal ions, reasonably adjusting the addition order and addition conditions so that two metal ions with different physical properties can be successfully loaded on the Beta molecular sieve with a low silicon-aluminum ratio, avoiding the technical problem of difficulty in zeolite synthesis caused by the introduction of metal ions.

[0018] The preparation method described in the present invention is preferably that the post-treatment includes the following steps: separating the hydrothermal crystallization product by suction filtration, then washing with ammonium chloride solution until the pH of the product eluent is 7-8, and then drying at 60-100°C for 8-12 hours; the roasting refers to roasting in a programmed temperature manner, the roasting temperature is 150-600°C, preferably using a muffle furnace, first rising from room temperature to 150-220°C for roasting for 2-5 hours, then rising to 250-320°C for roasting for 4-7 hours, and finally rising to 500-600°C for roasting for 4-7 hours; preferably repeating the washing, drying and roasting twice or more, more preferably three times or more.

[0019] According to the preparation method of the present invention, the calcination is preferably carried out in a programmed temperature manner. Under low temperature conditions of 150-220° C., calcination for 2-5 hours can achieve the removal of moisture on the surface of the molecular sieve catalyst; under medium temperature conditions of rising to 250-320° C., calcination for 4-7 hours is conducive to the decomposition of the ammonium salt of the organic template; under high temperature conditions of 500-600° C., calcination for 4-7 hours can achieve the removal of free carbon, which helps to achieve smooth pores of the molecular sieve catalyst.

[0020] The preparation method of the present invention is preferably that, in the silicon-containing solution, the molar ratio of each component is silicon source: template: nickel source: water, calculated as the corresponding oxide, 1:0.4-0.6:0-0.03:10-15; in the aluminum-containing solution, the molar ratio of each component is silicon source: aluminum source: template: alkali metal: magnesium source: gallium source: H 2 O is 1: 0.02-0.1: 0.1-0.3: 0.1-0.5: 0-0.1: 0.005-0.015: 2-5.

[0021] The silicon source, aluminum source, magnesium source, nickel source, and gallium source in the present invention are not particularly limited, and any commonly used source in the technical field can be used. In the preparation method described in the present invention, it is preferred that the silicon source is tetraethyl orthosilicate, macroporous silica gel, or white carbon black; the aluminum source is aluminum isopropoxide, pseudoboehmite, or sodium metaaluminate; the magnesium source is magnesium nitrate or magnesium sulfate; the nickel source is nickel nitrate or nickel chloride; the gallium source is gallium nitrate or gallium chloride; and the template agent is tetraethylammonium hydroxide or tetrapropylammonium hydroxide.

[0022] The preparation method of the present invention is preferably:

[0023] The preparation of the silicon source-containing solution comprises the following steps: adding a silicon source, or adding a silicon source and a nickel source to a template solution, and then performing pretreatment to obtain a silicon source-containing solution;

[0024] The preparation of the aluminum source solution comprises the following steps: adding an aluminum source, a gallium source, or an aluminum source, a gallium source and a magnesium source to an alkaline aqueous solution containing a template, and then performing pretreatment to obtain an aluminum source solution;

[0025] The mixing of the silicon-containing source solution and the aluminum-containing source solution comprises the following steps: slowly dropping the aluminum-containing source solution into the silicon-containing source solution and mixing.

[0026] To this end, the present invention also provides a light gasoline olefin reduction-modification catalyst, in which, based on the corresponding oxides, the molar ratio of each component is 0.01-0.1:0-0.1:0-0.03:0.001-0.02:1 of aluminum source:magnesium source:nickel source:gallium source:silicon source.

[0027] The catalyst for catalytic olefin reduction and upgrading of light gasoline of the present invention is preferably characterized in that the ratio of silicon to aluminum is SiO 2 / Al 2 O 3 = 10-50; nickel oxide content 0-5.0wt%, magnesium oxide content 0-5.0wt%, gallium oxide content 1.0-5.0wt%; the mesopore volume of the catalyst is 0.2-0.5cm 3 / g, specific surface area is 200~280m 2 / g, and the pore size distribution is 1nm~7nm.

[0028] To this end, the present invention also provides a method for reducing olefins in light gasoline and upgrading the quality of the light gasoline, comprising the following steps:

[0029] Using catalytic cracking light gasoline and C4 liquefied gas mixed feed, olefin reduction-modification reaction is carried out in a fixed bed reactor under the action of the above catalyst. The conditions of the olefin reduction-modification reaction are: reaction temperature 360°C to 420°C, reaction pressure 0.1 to 2.0 MPa, carrier gas flow rate 1 to 5 L / h, liquid space velocity 0.5 to 2.5 h -1 ; The carrier gas is nitrogen containing hydrogen, and the hydrogen content is 1-10v%;

[0030] Wherein, the distillation range of the catalytic cracking light gasoline is less than 70°C, and the C 4 The olefin content in the liquefied gas is ≮40% by volume, and the mass ratio of the catalytic cracking light gasoline to the C4 liquefied gas is 1:0-0.5.

[0031] As can be seen from the above, in the preparation method of the catalyst of the present invention, firstly, by using the specific mixing and aging treatment of different metal salt precursors and silicon sources or aluminum sources, a suitable pH value is constructed, the rate of hydrolysis and condensation reaction of the metal salt precursor and the silicon source or aluminum source is controlled, and the precipitation process of the metal ions and the silicon source or aluminum source during the hydrothermal synthesis process can be synchronized with the crystallization of the silica-alumina gel, avoiding the generation of large particles of metal hydroxides or oxides that cannot enter the pores of the zeolite, and ensuring that the size of the metal salt hydrolysis and condensation products is small enough to enter the pores of the zeolite and be evenly dispersed. Secondly, by using the specific ratio of silica-alumina gel, Beta zeolite can generate a multi-level pore structure of nanocrystal accumulation, and the intercrystalline mesopores generated by the accumulation of nanocrystals can be used to increase the size and number of the generation space of metal hydroxides or oxides during the synthesis process, and on the other hand, improve the problem of metal presence and pore blocking inside the zeolite pores, solve the problem of excess reactants and products during the reaction process, and improve the performance of the catalyst.

[0032] The present invention also provides a more specific and preferred method for preparing a multi-level pore structure low-silicon Beta molecular sieve catalyst containing gallium and nickel and / or magnesium by a hydrothermal method without a mesoporous template agent. The preparation method comprises the following steps:

[0033] Step 1: Preparation of silicon-containing source solution and aluminum-containing source solution

[0034] A silicon source or a silicon source and a nickel source are added to a template solution, and the solution is pretreated to obtain a silicon source solution;

[0035] Adding an aluminum source, or an aluminum source and a gallium source, or / and a magnesium source into an alkaline aqueous solution containing a small amount of a template agent, and pretreating the solution to obtain an aluminum source solution;

[0036] Step 2: Mixing, aging and hydrothermal crystallization of silicon-containing and aluminum-containing source solutions

[0037] The aluminum source solution is slowly added dropwise to the silicon source solution, and after aging treatment, the solution is transferred into a hydrothermal crystallization reactor for crystallization treatment;

[0038] Step 3: Treatment of crystallized emulsion and calcination of catalyst

[0039] The obtained crystallized emulsion is filtered, washed, exchanged and calcined to finally obtain a multi-level structure Beta molecular sieve catalyst containing gallium and nickel and / or magnesium.

[0040] In summary, the preparation method provided by the present invention is a preparation method for a Beta molecular sieve catalyst with a multi-level pore structure and a low silicon-to-aluminum ratio containing gallium and nickel or / and magnesium by hydrothermal synthesis without a mesoporous template. In this preparation method, the hydrothermal loading method is simple, green, has a short operation cycle, and is low in cost, which is more conducive to industrialization. However, it is very difficult to synthesize a Beta molecular sieve with a low silicon-to-aluminum ratio and high crystallinity by a liquid phase hydrothermal synthesis method. If one or more metal salts are added in situ, the gel concentration is bound to be further increased, making the synthesis more difficult. Therefore, the hydrothermal synthesis of a low-silicon Beta molecular sieve containing magnesium, nickel, and gallium with a multi-level structure is of great significance, and the synthesis is very challenging, and there has been no relevant literature report before.

[0041] The catalyst prepared by the preparation method provided by the present invention has a lower silicon-aluminum ratio (SiO / Al 2 O 3 =10-50), it also has a high metal content and a multi-level pore structure, and the mesopore volume can reach 0.2-0.5cm 3 / g, specific surface area 200~280m 2 / g, pore size distribution 1-7nm. The whole catalyst preparation process is simple to operate and convenient for industrial production. The multi-level pore structure is conducive to the diffusion of macromolecular reactants or products and the accessibility of catalytic active centers. Applied to catalytic light gasoline reforming, the product olefin reduction is not less than 20v%, and the research octane number loss is less than 3 units, showing a good ability to selectively convert olefins into high-octane products.

[0042] In the present invention, gallium and nickel or / and magnesium are added by in-situ doping. First, through specific mixing and aging treatment, a suitable pH value is constructed to control the rate of hydrolysis and condensation reaction of metal salt precursor and silicon source or aluminum source, and ensure that the precipitation process and the formation of silica-alumina gel in the metal ion and silicon source or aluminum source system are synchronized; secondly, through a two-stage hydrothermal crystallization method, crystal growth is restricted, crystal nucleation is promoted, and metal salt precursor and silica-alumina gel are regulated to generate crystal nuclei with smaller particle size at low temperature. When the number of crystal nuclei is generated enough, the temperature is rapidly increased, and the crystals are rapidly grown into small particles in a short time at high temperature, so as to realize the growth of silica-alumina gel on the crystal nuclei and construct the multi-level pore structure of molecular sieve catalyst. Secondly, through a multi-stage program heating method, dehydration, ammonium salt removal, and free carbon removal are gradually realized, and finally a Beta molecular sieve catalyst with a multi-level pore structure and a low silicon-aluminum ratio containing gallium and nickel or / and magnesium is obtained.

[0043] The present invention has the following advantages:

[0044] 1. The prepared Beta molecular sieve catalyst has a more mesoporous structure, excellent diffusion performance and reaction activity. No mesoporous template or organic additive is needed in the synthesis process, which saves costs and reduces environmental pollution.

[0045] 2. Compared with the prior art, the multi-level Beta molecular sieve catalyst containing gallium and nickel and / or magnesium prepared by the hydrothermal method of the present invention has a lower silicon-aluminum ratio SiO 2 / Al 2 O 3 =10-50, high metal loading rate and excellent modification effect.

[0046] 3. The preparation method is simple to operate, and the prepared multi-level structure Beta molecular sieve containing gallium and nickel and / or magnesium has high crystallinity, good experimental repeatability, and low industrial separation cost.

[0047] 4. The multi-level Beta molecular sieve catalyst containing in-situ doped gallium and nickel and / or magnesium prepared by the hydrothermal synthesis system of the present invention can be used to catalyze the olefin reduction-upgrading reaction of light gasoline. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 The XRD diagram of the molecular sieve catalyst obtained in Example 7 of the present invention is shown. DETAILED DESCRIPTION

[0049] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.

[0050] Example 1: Preparation of Nickel and Magnesium-Containing Beta Molecular Sieve Catalyst without Aging Treatment

[0051] (1) Preparation of silicon source, nickel source solution and aluminum source, magnesium source solution:

[0052] 4.12 g of coarse pore silica gel and 0.18 g of nickel nitrate hexahydrate were weighed at 30° C., added to 17.3 g of 25% tetraethylammonium hydroxide (TEAOH) solution, and stirred for about 30 minutes to obtain a silicon source solution containing a silicon source and a nickel source;

[0053] Weigh 2.33 g of 25% TEAOH and 1.33 g of water at 30°C, mix well, add 0.23 g of sodium aluminate to the TEAOH aqueous solution, stir for 5 min, add 0.82 g of magnesium nitrate hexahydrate, add 0.12 g of sodium hydroxide, continue stirring for about 40 min until completely dissolved, and obtain an aluminum source solution containing aluminum source and magnesium source;

[0054] (2) Solution mixing and hydrothermal crystallization

[0055] The silicon source and nickel source solutions were slowly added dropwise to the aluminum source and magnesium source solutions. The raw material solution was transferred to a reaction kettle and placed in an oven at 110° C. for pre-crystallization for 36 hours, and then heated to 170° C. for crystallization for 24 hours.

[0056] (3) Treatment of crystallized emulsion and calcination of catalyst

[0057] The crystallized product was conventionally filtered and washed with 1 mol / L ammonium chloride solution until the pH of the product eluent was 7-8 (ammonia exchange, washing), then dried in an oven at 60°C for 12 hours, and then calcined in a muffle furnace at a rate of 1.7°C / min from room temperature to 200°C for 4 hours, then to 300°C for 6 hours, and finally to 550°C for 6 hours. The ammonia exchange, washing, drying and calcination were repeated three times to finally obtain a Beta molecular sieve catalyst containing nickel and magnesium.

[0058] Example 2: Preparation of one-step crystallization nickel and magnesium containing Beta molecular sieve catalyst

[0059] (1) Preparation of silicon source, nickel source solution and aluminum source, magnesium source solution:

[0060] Weigh 4.12 g of coarse-pore silica gel and 0.18 g of nickel nitrate hexahydrate at 30°C, add them to 17.3 g of 25% tetraethylammonium hydroxide (TEAOH) solution, and continue stirring for about 30 minutes to obtain a silicon source solution containing a silicon source and a nickel source, and then age at 70°C for 4 hours to obtain a uniform solution.

[0061] Weigh 2.33 g of 25% TEAOH and 1.33 g of water at 30°C, mix them evenly, add 0.23 g of sodium aluminate to the TEAOH aqueous solution, stir for 5 minutes, add 0.82 g of magnesium nitrate hexahydrate, add 0.12 g of sodium hydroxide, continue stirring for about 40 minutes until completely dissolved, and obtain an aluminum source solution containing an aluminum source and a magnesium source, and then age at 50°C for 5 hours to obtain a uniform solution;

[0062] (2) Solution mixing, aging and hydrothermal crystallization

[0063] The solution containing silicon source and nickel source was slowly added dropwise to the aluminum source and magnesium source solution, and aged at 50°C for 5 hours to obtain a hydrothermal synthesis system. The above raw material preparation solution was transferred to a reaction kettle and placed in a 170°C oven for crystallization for 24 hours.

[0064] (3) Treatment of crystallized emulsion and calcination of catalyst

[0065] The crystallized product was conventionally filtered, washed with 1 mol / L ammonium chloride solution until the pH of the product eluent was 7-8, and then dried in an oven at 60°C for 12 hours, and then calcined in a muffle furnace at a rate of 1.7°C / min from room temperature to 200°C for 4 hours, then to 300°C for 6 hours, and finally to 550°C for 6 hours. The ammonia exchange, washing, drying and calcination were repeated three times to finally obtain a Beta molecular sieve catalyst containing nickel and magnesium.

[0066] Example 3: Preparation of multi-level structure Beta molecular sieve catalyst containing nickel and magnesium

[0067] (1) Preparation of silicon source, nickel source solution and aluminum source, magnesium source solution:

[0068] 4.12 g of coarse-pore silica gel and 0.18 g of nickel nitrate hexahydrate were weighed at 30°C, added to 17.3 g of 25% tetraethylammonium hydroxide (TEAOH) solution, and stirred for about 30 minutes to obtain a silicon source solution, which was then aged at 70°C for 4 hours to obtain a uniform solution.

[0069] Weigh 2.33 g of 25% TEAOH and 1.33 g of water at 30°C, mix them evenly, add 0.23 g of sodium aluminate to the TEAOH aqueous solution, stir for 5 minutes, add 0.82 g of magnesium nitrate hexahydrate, add 0.12 g of sodium hydroxide, continue stirring for about 40 minutes until completely dissolved, and obtain an aluminum source solution containing an aluminum source and a magnesium source, and then age at 50°C for 5 hours to obtain a uniform solution;

[0070] (2) Solution mixing and hydrothermal crystallization

[0071] The silicon-containing nickel source solution was slowly added dropwise to the aluminum-containing and magnesium-containing source solutions, and aged at 50°C for 5 hours to obtain a hydrothermal synthesis system. The above raw material solution was transferred to a reaction kettle and placed in an oven at 110°C for pre-crystallization for 36 hours, and then heated to 170°C for crystallization for 24 hours.

[0072] (3) Treatment of crystallized emulsion and calcination of catalyst

[0073] The crystallized product was conventionally filtered, washed with 1 mol / L ammonium chloride solution until the pH of the product eluent was 7-8, and then dried in an oven at 60°C for 12 hours, and then calcined in a muffle furnace at a rate of 1.7°C / min from room temperature to 200°C for 4 hours, then to 300°C for 6 hours, and finally to 550°C for 6 hours. The ammonia exchange, washing, drying and calcination were repeated three times to finally obtain a multi-level structure Beta molecular sieve catalyst containing nickel and magnesium.

[0074] Example 4: Preparation of Beta zeolite molecular sieve catalyst containing magnesium and gallium

[0075] (1) Preparation of silicon source solution and aluminum source, magnesium source, and gallium source solution:

[0076] 4.12 g of coarse pore silica gel was weighed and added to 17.3 g of 25% tetraethylammonium hydroxide (TEAOH) solution at 30° C., and stirred for about 30 minutes to obtain a silicon source solution, which was then aged at 70° C. for 4 hours to obtain a uniform solution.

[0077] 2.33 g of 25% TEAOH and 1.33 g of water were weighed at 30° C., mixed evenly, 0.23 g of sodium aluminate was added to the TEAOH aqueous solution, stirred for 5 min, 0.82 g of magnesium nitrate hexahydrate was added, 0.23 g of gallium nitrate and 0.12 g of sodium hydroxide were added, and stirring was continued for about 40 min until completely dissolved to obtain an aluminum source solution containing an aluminum source, a magnesium source and a gallium source, and then aged at 50° C. for 5 hours to obtain a uniform solution;

[0078] (2) Solution mixing, aging and hydrothermal crystallization

[0079] Finally, the silicon source solution was slowly added dropwise to the aluminum source, magnesium source and gallium source solutions, and aged at 50°C for 5 hours to obtain a hydrothermal synthesis system. The above raw material preparation solution was transferred to a reaction kettle and placed in an oven at 110°C for pre-crystallization for 36 hours, and then heated to 170°C for crystallization for 24 hours.

[0080] (3) Treatment of crystallized emulsion and calcination of catalyst

[0081] The crystallized product was conventionally filtered, washed with 1 mol / L ammonium chloride solution until the pH of the product eluent was 7-8, and then dried in an oven at 60°C for 12 hours, and then calcined in a muffle furnace at a rate of 1.7°C / min from room temperature to 200°C for 4 hours, then to 300°C for 6 hours, and finally to 550°C for 6 hours. The ammonia exchange, washing, drying and calcination were repeated three times to finally obtain a magnesium-gallium multi-level structure Beta molecular sieve catalyst.

[0082] Example 5: Preparation of Nickel- and Gallium-Containing Multi-Level Structure Beta Zeolite Molecular Sieve Catalyst

[0083] (1) Preparation of silicon source, nickel source solution and aluminum source, gallium source solution:

[0084] At 30°C, 4.12g of white carbon black and 0.17g of nickel nitrate hexahydrate were weighed separately, added to 17.3g of 25% tetraethylammonium hydroxide (TEAOH) solution, and stirred for about 30 minutes to obtain a solution containing a silicon source and a nickel source, and then aged at 70°C for 4 hours to obtain a uniform solution.

[0085] 2.33 g of 25% TEAOH and 1.33 g of water were weighed and mixed at 30°C, 0.56 g of aluminum isopropoxide was added to the TEAOH aqueous solution, 0.23 g of gallium nitrate and 0.12 g of sodium hydroxide were added after stirring for 5 minutes, and stirring was continued for about 40 minutes until completely dissolved to obtain an aluminum source solution containing an aluminum source and a gallium source, and then aged at 50°C for 5 hours to obtain a uniform solution;

[0086] (2) Solution mixing, aging and hydrothermal crystallization

[0087] Finally, the silicon source and nickel source solutions were slowly added dropwise to the aluminum source and gallium source solutions, and aged at 50°C for 5 hours to obtain a hydrothermal synthesis system. The above raw material preparation solution was transferred to a reaction kettle and placed in an oven at 110°C for pre-crystallization for 36 hours, and then heated to 170°C for crystallization for 24 hours.

[0088] (3) Treatment of crystallized emulsion and calcination of catalyst

[0089] The crystallized product was conventionally filtered, washed with 1 mol / L ammonium chloride solution until the pH of the product eluent was 7-8, and then dried in an oven at 60°C for 12 hours, and then calcined in a muffle furnace at a rate of 1.7°C / min from room temperature to 250°C for 4 hours, then to 300°C for 6 hours, and finally to 550°C for 6 hours. The washing, drying and calcination were repeated three times to finally obtain a nickel- and gallium-containing multi-level structure Beta molecular sieve catalyst.

[0090] Example 6: Preparation of low silicon multi-level Beta zeolite molecular sieve catalyst containing magnesium, nickel and gallium

[0091] (1) Preparation of silicon source, nickel source solution and aluminum source, magnesium source, and gallium source solution:

[0092] At 30°C, 4.12 g of coarse-pore silica gel and 0.18 g of nickel nitrate hexahydrate were weighed separately, added to 17.3 g of 25% tetraethylammonium hydroxide (TEAOH) solution, and stirred for about 30 minutes to obtain a solution containing a silicon source and a nickel source, and then aged at 70°C for 4 hours to obtain a uniform solution.

[0093] 2.33 g of 25% TEAOH and 1.33 g of water were weighed and mixed at 30° C., 0.52 g of pseudo-boehmite was added to the TEAOH aqueous solution, and after stirring for 5 minutes, 0.86 g of magnesium nitrate hexahydrate, 0.24 g of gallium nitrate and 0.12 g of sodium hydroxide were added, and stirring was continued for about 40 minutes until they were completely dissolved to obtain an aluminum source solution containing an aluminum source, a magnesium source and a gallium source, and then aged at 50° C. for 5 hours to obtain a uniform solution;

[0094] (2) Solution mixing, aging and hydrothermal crystallization

[0095] Finally, the silicon source and nickel source solutions were slowly added dropwise to the aluminum source, magnesium source and gallium source solutions, and aged at 50°C for 5 hours to obtain a hydrothermal synthesis system. The above raw material preparation solution was transferred to a reaction kettle and placed in an oven at 110°C for pre-crystallization for 36 hours, and then heated to 170°C for crystallization for 24 hours.

[0096] (3) Treatment of crystallized emulsion and calcination of catalyst

[0097] The crystallized product was conventionally filtered, washed with 1 mol / L ammonium chloride solution until the pH of the product eluent was 7-8, and then dried in an oven at 60°C for 12 hours, and then calcined in a muffle furnace at a rate of 1.7°C / min from room temperature to 250°C for 4 hours, then to 300°C for 6 hours, and finally to 550°C for 6 hours. The washing, drying and calcination were repeated three times to finally obtain a low-silicon multi-level structure Beta molecular sieve catalyst containing magnesium, nickel and gallium.

[0098] Example 7: Preparation of multi-level Beta molecular sieve catalyst containing magnesium, nickel and gallium with ultra-low silicon-aluminum ratio

[0099] (1) Preparation of silicon source, nickel source solution and aluminum source, magnesium source, and gallium source solution:

[0100] 14.3 g of ethyl orthosilicate and 0.2 g of nickel nitrate hexahydrate were weighed separately at 30° C., added to 17.3 g of 25% tetraethylammonium hydroxide (TEAOH) solution, and stirred for about 30 minutes to obtain a solution containing a silicon source and a nickel source, and then aged at 70° C. for 4 hours to obtain a uniform solution.

[0101] 2.33 g of 25% TEAOH and 1.33 g of water were weighed at 30°C, mixed evenly, 1.13 g of sodium aluminate was added to the TEAOH aqueous solution, stirred for 5 minutes, 0.99 g of magnesium nitrate hexahydrate was added, 0.28 g of gallium nitrate and 0.12 g of sodium hydroxide were added, and stirring was continued for about 40 minutes until completely dissolved to obtain an aluminum source solution containing an aluminum source, a magnesium source and a gallium source, and then aged at 50°C for 5 hours to obtain a uniform solution;

[0102] (2) Solution mixing, aging and hydrothermal crystallization

[0103] Finally, the silicon source and nickel source solutions were slowly added dropwise to the aluminum source, magnesium source and gallium source solutions, and aged at 50°C for 5 hours to obtain a hydrothermal synthesis system. The above raw material preparation solution was transferred to a reaction kettle and placed in an oven at 110°C for pre-crystallization for 36 hours, and then heated to 170°C for crystallization for 24 hours.

[0104] (3) Treatment of crystallized emulsion and calcination of catalyst

[0105] The crystallized product was conventionally filtered, washed with 1 mol / L ammonium chloride solution until the pH of the product eluent was 7-8, and then dried in an oven at 60°C for 12 hours, and then calcined in a muffle furnace at a rate of 1.7°C / min from room temperature to 250°C for 4 hours, then to 300°C for 6 hours, and finally to 550°C for 6 hours. The washing, drying and calcination were repeated three times to finally obtain an ultra-low silicon multi-level structure Beta molecular sieve catalyst containing magnesium, nickel and gallium.

[0106] XRD test of samples (see Figure 1 ).from Figure 1 It can be seen that the prepared Beta molecular sieve catalyst with a multi-level pore structure containing magnesium, nickel and gallium has typical characteristic diffraction peaks of Beta molecular sieve, indicating that the prepared catalyst can still maintain the characteristic structure of Beta molecular sieve under the introduction of metal elements and a lower silicon-aluminum ratio.

[0107] Comparative Example 1: Preparation of non-in-situ loaded magnesium, nickel, gallium multi-level structure Beta zeolite molecular sieve catalyst

[0108] (1) Preparation of silicon source and aluminum source solutions:

[0109] 4.12 g of coarse-porous silica gel was weighed at 30° C. and added to 17.3 g of 25% tetraethylammonium hydroxide (TEAOH) solution. The mixture was stirred for about 30 min to obtain a silicon source solution. The solution was then aged at 70° C. for 4 hours to obtain a uniform solution.

[0110] 2.33 g of 25% TEAOH and 1.33 g of water were weighed and mixed at 30°C, 0.52 g of pseudo-boehmite was added to the TEAOH aqueous solution, and 0.12 g of sodium hydroxide was added, and the mixture was stirred for about 40 minutes until it was completely dissolved to obtain an aluminum source solution, and then aged at 50°C for 5 hours to obtain a uniform solution;

[0111] (2) Solution mixing, aging and hydrothermal crystallization

[0112] Finally, the silicon source solution was slowly added dropwise to the aluminum source solution and aged at 50°C for 2 hours to obtain a hydrothermal synthesis system. The above raw material solution was transferred to a reaction kettle and placed in an oven at 110°C for pre-crystallization for 36 hours, and then heated to 170°C for crystallization for 24 hours.

[0113] (3) Treatment of crystallized emulsion and calcination of catalyst

[0114] The crystallized product was conventionally filtered, washed with 1 mol / L ammonium chloride solution until the pH of the product eluent was 7-8, and then dried in an oven at 60°C for 12 hours, and then calcined in a muffle furnace at a rate of 1.7°C / min from room temperature to 250°C for 4 hours, then to 300°C for 6 hours, and finally to 550°C for 6 hours. The washing and calcination were repeated three times to finally obtain a low-silicon multi-level structure Beta molecular sieve.

[0115] (4) Preparation of Beta molecular sieve catalyst loaded with magnesium, nickel and gallium: 4.30g of the Beta molecular sieve synthesized by the above method was used as the carrier, and the metal impregnation solution was prepared according to the water absorption rate of the molecular sieve carrier. A certain amount of deionized water was weighed, 0.25g of gallium nitrate was added, and stirred for 30 minutes until dissolved, 0.88g of magnesium nitrate was added, and stirred for 10 minutes until dissolved, 0.18g of nickel nitrate hexahydrate was added, and stirred for 10 minutes until dissolved, and finally the volume was fixed with deionized water. The carrier was impregnated by the equal volume impregnation method, and after standing for 12 hours, the carrier was dried at 120°C for 4 hours and calcined at 550°C for 4 hours to prepare a multi-stage Beta molecular sieve catalyst loaded with magnesium, nickel and gallium.

[0116] Experimental Example 1:

[0117] The catalysts prepared in Examples 1-7 of the present invention were subjected to BET tests, and the results are shown in Table 1. The specific surface area and pore volume were obtained by nitrogen adsorption and desorption, and the data were given by a detection device (nitrogen adsorption and desorption analyzer).

[0118] Table 1: Specific surface area and pore volume of samples

[0119]

[0120] The results in Table 1 show that the multi-level pore structure Beta molecular sieve catalyst containing gallium and nickel or / and magnesium prepared by the hydrothermal synthesis method in Examples 1-7 has a large surface area and pore volume. In particular, it can be seen from the comparison between Example 7 and Comparative Example 1 that the multi-level pore structure Beta molecular sieve catalyst containing gallium and nickel or / and magnesium prepared by the present invention has a large surface area and pore volume compared with the conventional preparation method of Comparative Example 1.

[0121] Experimental Example 2: Study on the performance of catalytic light gasoline olefin reduction-modification reaction

[0122] The multi-level pore structure Beta molecular sieve catalyst containing gallium and nickel or / and magnesium prepared according to the embodiment of the present invention is used to catalyze the light gasoline-liquefied gas olefin reduction-reforming reaction. The evaluation reaction device is a 5ml small fixed bed microreactor, and the evaluation is filled with 2ml 20-40 purpose multi-level structure Beta molecular sieve catalyst of Examples 1 to 4. Catalytic light gasoline and C4 liquefied gas are used as reaction raw materials, 1% hydrogen nitrogen is used as carrier gas, and the reaction pressure is 0.5Mpa, the temperature is 400℃, and the mixed feed mass ratio of C4 liquefied gas / catalytic light gasoline is 1:0.5. The product composition is analyzed by gas chromatograph to evaluate the reaction performance of the catalyst. Tables 2 and 3 are the evaluation results of the catalytic performance of the series of catalysts.

[0123] Table 2: Catalytic performance results of nickel-containing and magnesium-containing Beta molecular sieve series catalysts prepared by different preparation methods

[0124]

[0125] Table 3: Catalytic performance results of multi-level Beta molecular sieve series catalysts containing gallium and nickel and / or magnesium

[0126]

[0127] The results show that the multi-level Beta molecular sieve series catalysts containing gallium and nickel and / or magnesium provided by the present invention catalyze the olefin reduction-upgrading reaction of light gasoline. The evaluation results show that the olefin reduction of the product is ≮20v%, the research octane number loss is ≯3, and the minimum octane number.

[0128] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.

Claims

1. Application of a catalyst in olefin reduction-upgrading reaction of light gasoline, characterized in that: Using catalytic cracking light gasoline and C4 liquefied gas as mixed feed, olefin reduction and upgrading reaction is carried out in a fixed bed reactor under the action of catalyst; Wherein, the distillation range of the catalytic cracking light gasoline is less than 70°C; The preparation method of the catalyst adopts a hydrothermal synthesis method, and the preparation method at least comprises the following steps: First, a mixture containing a silicon source and a solution containing an aluminum source are mixed to form a mixed solution, wherein the mixture containing the silicon source comprises a silicon source, a template, a nickel source and water; and the solution containing the aluminum source comprises an aluminum source, a template, an alkali metal, a magnesium source, a gallium source and water; In the mixed solution, the molar ratio of each component, calculated on the basis of the corresponding oxide, is: Silicon source: template: aluminum source: alkali metal: nickel source: magnesium source: gallium source: water is 1: 0.5-0.9: 0.02-0.1: 0.1-0.5: 0-0.03: 0-0.1: 0.005-0.015: 12-20; the content of nickel and magnesium is not 0; Then, the mixed solution is subjected to hydrothermal crystallization, post-treatment, and calcination to obtain a multi-level structure Beta molecular sieve catalyst containing in-situ doped gallium, nickel, and magnesium; Performing an aging treatment before and / or after mixing the silicon source-containing mixture with the aluminum source-containing solution; The hydrothermal crystallization is a two-stage hydrothermal crystallization.

2. The use according to claim 1, characterized in that: The two-stage hydrothermal crystallization comprises the following steps: (1) heating the mixed solution to 100-120° C. and performing pre-crystallization for 12-48 hours; (2) heating the mixed solution after pre-crystallization to 160-180° C. and performing re-crystallization for 12-24 hours.

3. The use according to claim 1, characterized in that: Before the silicon source-containing mixture is mixed with the aluminum source-containing solution, the aging treatment conditions of the silicon source-containing mixture are: stirring and aging for 2-10 hours at a temperature of 50-90°C; before mixing, the aging treatment conditions of the aluminum source-containing solution are: stirring and aging for 5-10 hours at a temperature of 30-90°C until complete dissolution; after mixing, the aging treatment conditions of the mixed solution are: aging for 2-5 hours at a temperature of 30-90°C.

4. The use according to claim 3, characterized in that: The temperature of the aging treatment of the mixture containing the silicon source is 60-80°C.

5. The use according to claim 3, characterized in that: The temperature of the aging treatment of the aluminum source solution is 40-60°C.

6. The use according to claim 3, characterized in that: The temperature of the aging treatment of the mixed solution is 50-70°C.

7. The use according to claim 1, characterized in that: The post-treatment comprises the following steps: separating the hydrothermal crystallization product by suction filtration, washing with ammonium chloride solution until the pH value of the product eluent is 7-8, and then drying at 60-100°C for 8-12 hours; the roasting refers to roasting in a programmed temperature rising manner, the roasting temperature is 150-600°C, firstly rising from room temperature to 150-220°C for roasting for 2-5 hours, then rising to 250-320°C for roasting for 4-7 hours, and finally rising to 500-600°C for roasting for 4-7 hours.

8. The use according to claim 7, characterized in that: The washing, drying and calcining were repeated two more times.

9. The use according to claim 8, characterized in that: The washing, drying and calcining were repeated three more times.

10. The use according to claim 1 or 7, characterized in that: The calcination is carried out in a muffle furnace.

11. The use according to claim 1, characterized in that: In the silicon source-containing mixture, the molar ratio of each component, calculated on the basis of the corresponding oxides, is silicon source: template: nickel source: water, which is 1:0.4-0.6:0-0.03:10-15; in the aluminum source-containing solution, the molar ratio of each component, calculated on the basis of the corresponding oxides, is aluminum source: template: alkali metal: magnesium source: gallium source: H2O, which is 0.02-0.1:0.1-0.3:0.1-0.5:0-0.1:0.005-0.015:2-5.

12. The use according to claim 1, characterized in that: The silicon source is tetraethyl orthosilicate, macroporous silica gel or white carbon black; the aluminum source is aluminum isopropoxide, pseudoboehmite or sodium aluminate; the magnesium source is magnesium nitrate or magnesium sulfate; the nickel source is nickel nitrate or nickel chloride; the gallium source is gallium nitrate or gallium chloride; and the template agent is tetraethylammonium hydroxide or tetrapropylammonium hydroxide.

13. The use according to claim 1, characterized in that: The preparation of the mixture containing silicon source comprises the following steps: Adding a silicon source and a nickel source into a template solution, and then pre-treating the solution to obtain a mixture containing a silicon source; The preparation of the aluminum source solution comprises the following steps: adding an aluminum source, a gallium source and a magnesium source to an alkaline aqueous solution containing a template, and then performing pretreatment to obtain an aluminum source solution; The mixing of the silicon source-containing mixture and the aluminum source-containing solution comprises the following steps: slowly dropping the aluminum source-containing solution into the silicon source-containing mixture for mixing.

14. The use according to claim 1, characterized in that: The catalyst has a silicon-aluminum ratio of 10-50 (SiO2 / Al2O3); a nickel oxide content of 0-5.0 wt%, a magnesium oxide content of 0-5.0 wt%, and a gallium oxide content of 1.0-5.0 wt%; and a mesopore volume of 0.2-0.5 cm 3 / g, specific surface area is 200~280m 2 / g, and the pore size distribution is 1nm~7nm.

15. The use according to claim 1, characterized in that: The conditions of the olefin reduction-modification reaction are: reaction temperature 360°C-420°C, reaction pressure 0.1-2.0Mpa, carrier gas flow rate 1-5L / h, liquid space velocity 0.5-2.5h -1 ; The carrier gas is nitrogen containing hydrogen, and the hydrogen content is 1-10v%.

16. The use according to claim 1, characterized in that: The olefin content in the C4 liquefied gas is ≮40v%, and the mass ratio of the catalytic cracking light gasoline to the C4 liquefied gas is 1:0-0.5.