Polyimide film, copper sheet laminate and circuit substrate

By introducing specific acid anhydrides and diamine compounds into polyimide films to form non-thermoplastic and thermoplastic polyimide layers, the problems of insufficient dielectric loss and dimensional stability in high-frequency signal transmission are solved, and polyimide films with low dielectric tangent and low hygroscopicity are realized, thereby improving the reliability and yield of circuit boards.

CN114716707BActive Publication Date: 2024-10-11NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202210504040.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2016-12-28
Filing Date
2017-09-11
Publication Date
2024-10-11
Estimated Expiration
2037-09-11

AI Technical Summary

Technical Problem

Existing polyimide films suffer from problems such as high dielectric loss, signal delay, and insufficient dimensional stability in high-frequency signal transmission, especially performing poorly in high-frequency and bending applications.

Method used

By introducing specific acid anhydrides and diamine compounds into the polyimide film, non-thermoplastic and thermoplastic polyimide layers are formed, controlling the dielectric constant and dielectric tangent, improving dimensional stability and low moisture absorption, and combining with copper foil to form a copper sheet laminate.

Benefits of technology

The polyimide film with low dielectric tangent and low moisture absorption improves the reliability and yield of circuit boards and is suitable for high-frequency signal transmission and bending applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003636631740000031
    Figure BDA0003636631740000031
  • Figure BDA0003636631740000032
    Figure BDA0003636631740000032
  • Figure BDA0003636631740000041
    Figure BDA0003636631740000041
Patent Text Reader

Abstract

A kind of polyimide film with non-thermoplastic polyimide layer, copper sheet laminate and circuit substrate, the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer is preferably relative to 100 molar parts of tetracarboxylic acid residues and contains 80 molar parts or more of BPDA residues derived from 3,3',4,4'-biphenyltetracarboxylic acid dianhydride (BPDA) and TAHQ residues derived from 1,4-phenylene bis (trimellitic acid monoester) dianhydride (TAHQ) and PMDA residues derived from pyromellitic acid dianhydride (PMDA) and NTCDA residues derived from 2,3,6,7-naphthalenetetracarboxylic acid dianhydride (NTCDA) At least one, and preferably dielectric tangent (Df) is 0.004 or less. By forming a non-thermoplastic polyimide layer with specific anhydride as raw material, it is possible to achieve the coexistence of ensuring the physical properties of the matrix resin layer and low moisture absorption rate, and low dielectric tangent can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention is a divisional application of the invention patent application with application number 201780059180.2 filed on September 11, 2017 and invention name “Polyimide film, copper sheet laminate and circuit substrate”.

[0002] CROSS-REFERENCE TO RELATED APPLICATIONS

[0003] This application claims priority based on Japanese Patent Application No. 2016-191786 filed on September 29, 2016, Japanese Patent Application No. 2016-191787 filed on September 29, 2016, Japanese Patent Application No. 2016-256927 filed on December 28, 2016, and Japanese Patent Application No. 2016-256928 filed on December 28, 2016, and all the contents of these applications are cited in this application. Technical Field

[0004] The invention relates to a polyimide film, a copper sheet laminate and a circuit substrate. Background Art

[0005] In recent years, with the progress of miniaturization, lightness and space saving of electronic devices, the demand for thin, light, flexible and durable flexible printed wiring boards (Flexible Printed Circuits, FPC) has increased. FPC can be installed three-dimensionally and at a high density even in a limited space, so its use is gradually expanding in the wiring of movable parts of electronic devices such as hard disk drives (HDD), digital video disks (DVD), and smart phones, or in parts such as cables and connectors.

[0006] In addition to the high density, the high performance of the equipment is promoted, so it is also necessary to deal with the high frequency of the transmission signal. When transmitting a high-frequency signal, if the transmission loss of the signal transmission path is large, undesirable conditions such as the loss of the electrical signal or the delay time of the signal will be prolonged. Therefore, it is important to reduce the transmission loss of the FPC. In order to cope with the high frequency, a liquid crystal polymer characterized by a low dielectric constant and a low dielectric tangent is used as an FPC of the dielectric layer. However, although the liquid crystal polymer has excellent dielectric properties, there is room for improvement in heat resistance or adhesion to metal foil.

[0007] In order to improve heat resistance or adhesion, a metal sheet laminate (patent document 1) using polyimide as an insulating layer has been proposed. According to patent document 1, it is known that the dielectric constant is usually reduced by using aliphatic monomers as monomers of polymer materials. The heat resistance of the polyimide obtained by using aliphatic (chain) tetracarboxylic dianhydride is significantly low, so it cannot be used for processing such as welding and has practical problems. However, if alicyclic tetracarboxylic dianhydride is used, a polyimide with improved heat resistance can be obtained compared with chain tetracarboxylic dianhydride. However, regarding the polyimide film formed by the polyimide, although the dielectric constant at 10GHz is less than 3.2, the dielectric tangent exceeds 0.01, and the dielectric properties are not sufficient. In addition, regarding the polyimide using the aliphatic monomer, there are the following problems: the linear expansion coefficient is large, the dimensional change rate of the polyimide film is large, or the flame retardancy decreases.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2004-358961 Summary of the invention

[0011] Problems to be solved by the invention

[0012] An object of the present invention is to provide a polyimide film which has high dimensional stability and low hygroscopicity and can reduce transmission loss by making the dielectric tangent of the insulating layer small, and which can be preferably used for a high-frequency circuit substrate.

[0013] Technical means of solving problems

[0014] The inventors of the present invention have conducted diligent research and have found that in a circuit substrate, regarding the non-thermoplastic polyimide layer that mainly performs the function of controlling the dimensional change rate, and further regarding the thermoplastic polyimide layer that optionally performs the function of bonding with the copper foil, by selecting monomers as raw materials for polyimide, it is possible to ensure the necessary dimensional stability as a circuit substrate, and to achieve low moisture absorption and low dielectric tangent by controlling the order (crystallinity) of the polyimide, thereby completing the present invention.

[0015] That is, the polyimide film according to the first aspect of the present invention is a polyimide film having a thermoplastic polyimide layer containing a thermoplastic polyimide on at least one surface of a non-thermoplastic polyimide layer containing a non-thermoplastic polyimide.

[0016] Furthermore, the polyimide film according to the first aspect of the present invention satisfies the following conditions (ai) to (a-iv).

[0017] (ai) the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer comprises a tetracarboxylic acid residue and a diamine residue, and

[0018] With respect to 100 parts by mole of the tetracarboxylic acid residue,

[0019] a total of at least one of a tetracarboxylic acid residue derived from 3,3',4,4'-biphenyl tetracarboxylic dianhydride (BPDA) (BPDA residue) and a tetracarboxylic acid residue derived from 1,4-phenylene bis(trimellitic acid monoester) dianhydride (TAHQ) (TAHQ residue), and at least one of a tetracarboxylic acid residue derived from pyromellitic dianhydride (PMDA) (PMDA residue) and a tetracarboxylic acid residue derived from 2,3,6,7-naphthalenetetracarboxylic dianhydride (NTCDA residue) (NTCDA residue) in an amount of 80 parts by mole or more,

[0020] The molar ratio of at least one of the BPDA residue and the TAHQ residue to at least one of the PMDA residue and the NTCDA residue {(BPDA residue+TAHQ residue) / (PMDA residue+NTCDA residue)} is in the range of 0.6 to 1.3.

[0021] (a-ii) The thermoplastic polyimide constituting the thermoplastic polyimide layer comprises a tetracarboxylic acid residue and a diamine residue, and the amount of the diamine residue is 100 parts by mole.

[0022] The diamine residue derived from at least one diamine compound selected from the diamine compounds represented by the following general formula (B1) to (B7) is 70 mol parts or more, and the diamine residue derived from the diamine compound represented by the following general formula (A1) is in the range of 1 mol part to 30 mol parts.

[0023] (a-iii) The thermal expansion coefficient is within the range of 10 ppm / K to 30 ppm / K.

[0024] (a-iv) The dielectric tangent (Dissipation factor, Df) at 10 GHz is less than 0.004.

[0025] [Chemistry 1]

[0026]

[0027] [In formula (B1) to formula (B7), R 1 independently represents a monovalent hydrocarbon group or alkoxy group having 1 to 6 carbon atoms, and the linking group A independently represents a group selected from -O-, -S-, -CO-, -SO-, -SO 2 -、-COO-、-CH 2 -、-C(CH 3 ) 2 -, -NH- or -CONH- in the divalent group, n 1 Each independently represents an integer from 0 to 4. In addition, the formula (B3) excluding the repeating formula (B2), and the formula (B5) excluding the repeating formula (B4)]

[0028] [Chemistry 2]

[0029]

[0030] In formula (A1), the linking group X represents a single bond or -COO-, Y independently represents hydrogen, a monovalent hydrocarbon group having 1 to 3 carbon atoms, or an alkoxy group, n represents an integer of 0 to 2, and p and q independently represent an integer of 0 to 4.

[0031] In the polyimide film according to the first aspect of the present invention, the diamine residue derived from the diamine compound represented by the general formula (A1) may account for 80 mol parts or more per 100 mol parts of the diamine residue in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer.

[0032] The polyimide film of the first aspect of the present invention may also be: the diamine residue derived from at least one diamine compound selected from the diamine compounds represented by the general formula (B1) to the general formula (B7) is in the range of 70 mol parts to 99 mol parts, relative to 100 mol parts of the diamine residue in the thermoplastic polyimide constituting the thermoplastic polyimide layer.

[0033] The polyimide film according to the second aspect of the present invention is a polyimide film having a thermoplastic polyimide layer containing a thermoplastic polyimide on at least one surface of a non-thermoplastic polyimide layer containing a non-thermoplastic polyimide.

[0034] Furthermore, the polyimide film according to the second aspect of the present invention satisfies the following conditions (bi) to (b-iv).

[0035] (bi) The thermal expansion coefficient is within the range of 10 ppm / K to 30 ppm / K.

[0036] (b-ii) the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer comprises a tetracarboxylic acid residue and a diamine residue, and

[0037] With respect to 100 parts by mole of the tetracarboxylic acid residue,

[0038] The tetracarboxylic acid residue derived from at least one tetracarboxylic acid dianhydride selected from 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) and 1,4-phenylenebis(trimellitic acid monoester) dianhydride (TAHQ) is within a range of 30 mol parts to 60 mol parts,

[0039] The tetracarboxylic acid residue derived from pyromellitic dianhydride (PMDA) is in the range of 40 parts by mole or more and 70 parts by mole or less.

[0040] (b-iii) relative to 100 parts by mole of the diamine residue in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer,

[0041] The diamine residue derived from the diamine compound represented by the following general formula (A1) is 80 parts by mole or more.

[0042] (b-iv) The thermoplastic polyimide constituting the thermoplastic polyimide layer comprises a tetracarboxylic acid residue and a diamine residue, and the amount of the diamine residue is 100 parts by mole.

[0043] The diamine residue derived from at least one diamine compound selected from the diamine compounds represented by the following general formula (B1) to (B7) is within a range of 70 parts by mole or more and 99 parts by mole or less,

[0044] The diamine residue derived from the diamine compound represented by the following general formula (A1) is in the range of 1 part by mole or more and 30 parts by mole or less.

[0045] [Chemistry 3]

[0046]

[0047] [In formula (A1), the linking group X represents a single bond or -COO-, Y independently represents hydrogen, a monovalent hydrocarbon group having 1 to 3 carbon atoms, or an alkoxy group, n represents an integer of 0 to 2, and p and q independently represent an integer of 0 to 4]

[0048] [Chemistry 4]

[0049]

[0050] [In formula (B1) to formula (B7), R 1 independently represents a monovalent hydrocarbon group or alkoxy group having 1 to 6 carbon atoms, and the linking group A independently represents a group selected from -O-, -S-, -CO-, -SO-, -SO 2 -、-COO-、-CH 2 -、-C(CH 3 ) 2 -, -NH- or -CONH- in the divalent group, n1 Each independently represents an integer from 0 to 4. In addition, the formula (B3) excluding the repeating formula (B2), and the formula (B5) excluding the repeating formula (B4)]

[0051] In the polyimide film according to the first aspect or the second aspect of the present invention, the imide group concentration of the non-thermoplastic polyimide and the thermoplastic polyimide may be 33% by weight or less.

[0052] The polyimide film according to the third aspect of the present invention is a polyimide film having at least one non-thermoplastic polyimide layer, and the polyimide film satisfies the following conditions (ci) to (c-iii).

[0053] (ci) the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer comprises a tetracarboxylic acid residue and a diamine residue, and

[0054] The present invention relates to a tetracarboxylic acid residue of at least one of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride (BPDA) and 1,4-phenylenebis(trimellitic acid monoester) dianhydride (TAHQ) in an amount of 30 to 60 mol parts, and a tetracarboxylic acid residue of at least one of pyromellitic acid dianhydride (PMDA) and 2,3,6,7-naphthalenetetracarboxylic acid dianhydride (NTCDA) in an amount of 40 to 70 mol parts, based on 100 mol parts of the tetracarboxylic acid residue.

[0055] The present invention contains 70 mol parts or more of diamine residues derived from a diamine compound represented by the following general formula (A1) based on 100 mol parts of the diamine residues, and contains 2 mol parts to 15 mol parts of diamine residues derived from diamine compounds represented by the following general formulas (C1) to (C4).

[0056] (c-ii) The glass transition temperature is 300°C or higher.

[0057] (c-iii) The dielectric tangent (Df) at 10 GHz is 0.004 or less.

[0058] [Chemistry 5]

[0059]

[0060] [In formula (A1), the linking group X represents a single bond or -COO-, Y independently represents hydrogen, a monovalent hydrocarbon group having 1 to 3 carbon atoms, or an alkoxy group, n represents an integer of 1 or 2, and p and q independently represent an integer of 0 to 4]

[0061] [Chemistry 6]

[0062]

[0063] [In formula (C1) to formula (C4), R 2 independently represents a monovalent hydrocarbon group, an alkoxy group or an alkylthio group having 1 to 6 carbon atoms, and the linking group A' independently represents a group selected from -O-, -SO 2 -、-CH 2 -or-C(CH 3 ) 2 - is a divalent group, and the linking group X1 independently represents -CH 2 -、-O-CH 2 -O-, -OC 2 H 4 -O-, -OC 3 H 6 -O-, -OC 4 H 8 -O-, -OC 5 H 10 -O-, -O-CH 2 -C(CH 3 ) 2 -CH 2 -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 -or-SO 2 -, n 3 independently represents an integer from 1 to 4, n 4 independently represent an integer of 0 to 4, but in formula (C3), the linking group A' does not contain -CH 2 -、-C(CH 3 ) 2 -、-C(CF 3 ) 2 -or-SO 2 -In the case of n 4 Any one of is 1 or more]

[0064] The copper sheet laminate according to the first, second or third aspect of the present invention comprises an insulating layer and copper foil on at least one surface of the insulating layer, wherein the insulating layer of the copper sheet laminate comprises the polyimide film according to any one of the aspects.

[0065] The circuit board according to the first aspect, the second aspect, or the third aspect of the present invention is one in which the copper foil of the copper sheet laminate is processed into wiring.

[0066] Effects of the Invention

[0067] The polyimide films according to the first to third aspects of the present invention can achieve both the physical properties of the matrix resin layer and low moisture absorption, and can also achieve low dielectric tangent by forming a non-thermoplastic polyimide layer using a specific acid anhydride as a raw material.

[0068] In addition, the polyimide film of the first aspect or the second aspect of the present invention can achieve low moisture absorption and low dielectric tangent by forming a thermoplastic polyimide layer using a thermoplastic polyimide into which a specific diamine compound is introduced. In addition, the multilayer film combining two resin layers has low hygroscopicity and dielectric tangent, and also has excellent dimensional stability after thermal compression bonding of copper foil.

[0069] Therefore, by using the polyimide film of the present invention and the copper sheet laminate using the same as FPC materials, the reliability and yield of the circuit board can be improved, and it can also be applied to circuit boards that transmit high-frequency signals of 10 GHz or more. DETAILED DESCRIPTION

[0070] Next, embodiments of the present invention will be described.

[0071] [Polyimide film]

[0072] The polyimide film according to the first embodiment of the present invention has a thermoplastic polyimide layer containing a thermoplastic polyimide on at least one side of a non-thermoplastic polyimide layer containing a non-thermoplastic polyimide, and satisfies the above-mentioned conditions (ai) to (a-iv).

[0073] The polyimide film according to the second embodiment of the present invention includes a thermoplastic polyimide layer including a thermoplastic polyimide on at least one side of a non-thermoplastic polyimide layer including a non-thermoplastic polyimide, and satisfies the above conditions (bi) to (b-iv).

[0074] Furthermore, in the first embodiment or the second embodiment, the thermoplastic polyimide layer is provided on one side or both sides of the non-thermoplastic polyimide layer. For example, in the case where the polyimide film of the first embodiment or the second embodiment and copper foil are laminated to form a copper sheet laminate, the copper foil may be laminated on the surface of the thermoplastic polyimide layer. In the case where the thermoplastic polyimide layer is provided on both sides of the non-thermoplastic polyimide layer, it is sufficient that the thermoplastic polyimide layer on one side satisfies the above-mentioned condition (a-ii) or condition (b-iv), but it is preferred that the thermoplastic polyimide layers on both sides satisfy the above-mentioned condition (a-ii) or condition (b-iv).

[0075] The polyimide film according to the third embodiment of the present invention has at least one non-thermoplastic polyimide layer containing a non-thermoplastic polyimide and satisfies the above-mentioned conditions (ci) to (c-iii).

[0076] Hereinafter, regarding the first to third embodiments, common aspects will be collectively described, and different aspects will be described individually.

[0077] The so-called "non-thermoplastic polyimide" is generally a polyimide that does not show softening and adhesiveness even when heated, but in the present invention, it means a polyimide having a storage elastic coefficient of 1.0×10 9 Pa, the storage elastic coefficient at 280°C is 3.0×10 8 Pa or more polyimide.

[0078] The so-called "thermoplastic polyimide" is generally a polyimide whose glass transition temperature (glass transition temperature, Tg) can be clearly confirmed, but in the present invention, it means a polyimide whose storage elastic modulus at 30°C measured by DMA is 1.0×10 9 Pa or more, and the storage elastic coefficient at 280°C is less than 3.0×10 8 Polyimide of Pa.

[0079] In the polyimide film of the first embodiment, the second embodiment or the third embodiment, the resin component of the non-thermoplastic polyimide layer preferably includes a non-thermoplastic polyimide, and in the first embodiment or the second embodiment, the resin component of the thermoplastic polyimide layer preferably includes a thermoplastic polyimide. In addition, the non-thermoplastic polyimide layer constitutes a polyimide layer of low thermal expansion, and the thermoplastic polyimide layer constitutes a polyimide layer of high thermal expansion. Here, the polyimide layer of low thermal expansion refers to a polyimide layer having a thermal expansion coefficient (Coefficient of Thermal Expansion, CTE) preferably in the range of 1ppm / K or more and 25ppm / K or less, more preferably in the range of 3ppm / K or more and 25ppm / K or less. In addition, the polyimide layer of high thermal expansion refers to a polyimide layer having a CTE preferably in the range of 35ppm / K or more, more preferably in the range of 35ppm / K or more and 80ppm / K or less, and further preferably in the range of 35ppm / K or more and 70ppm / K or less. The polyimide layer can be made into a polyimide layer having a desired CTE by appropriately changing the combination of raw materials used, thickness, and drying and curing conditions.

[0080] Generally, polyimide can be produced by reacting tetracarboxylic dianhydride and diamine compound in a solvent and heating and ring-closing after generating polyamic acid. For example, tetracarboxylic dianhydride and diamine compound are dissolved in an organic solvent in approximately equal moles, and stirred for 30 minutes to 24 hours at a temperature in the range of 0°C to 100°C to perform a polymerization reaction, thereby obtaining a polyamic acid as a polyimide precursor. During the reaction, the reaction components are dissolved in a manner such that the generated precursor becomes within the range of 5% by weight to 30% by weight, more preferably within the range of 10% by weight to 20% by weight in an organic solvent. As the organic solvent used in the polymerization reaction, for example, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), 2-butanone, dimethylsulfoxide (DMSO), hexamethylphosphoramide, N-methylcaprolactam, dimethyl sulfate, cyclohexanone, dioxane, tetrahydrofuran, diglyme, triglyme, cresol, etc. It is also possible to use two or more of these solvents in combination, and further, aromatic hydrocarbons such as xylene and toluene can also be used in combination. In addition, there is no particular limitation on the amount of the organic solvent used, but it is preferably used in an amount adjusted to a concentration of about 5% by weight to 30% by weight of the polyamic acid solution obtained by the polymerization reaction.

[0081] The synthesized polyamic acid is usually advantageously used as a reaction solvent solution, but can be concentrated, diluted or replaced with other organic solvents as needed. In addition, polyamic acid is generally excellent in solvent solubility, so it can be used advantageously. The viscosity of the polyamic acid solution is preferably in the range of 500cps to 100,000cps. If it deviates from the range, the film is prone to undesirable conditions such as thickness deviation and streaks during the coating operation performed using a coating machine or the like. There is no particular limitation on the method for imidizing the polyamic acid, for example, it is preferably adopted to heat the solvent under the temperature conditions in the range of 80°C to 400°C for 1 hour to 24 hours.

[0082] The polyimide is obtained by imidizing the polyamic acid and is produced by reacting a specific acid anhydride with a diamine compound. Therefore, by describing the acid anhydride and the diamine compound, specific examples of the non-thermoplastic polyimide of the first embodiment, the second embodiment or the third embodiment and the thermoplastic polyimide of the first embodiment or the second embodiment can be understood.

[0083] <Non-thermoplastic polyimide>

[0084] In the polyimide film of the first embodiment, the second embodiment or the third embodiment, the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer is a non-thermoplastic polyimide containing a tetracarboxylic acid residue and a diamine residue. Furthermore, in the present invention, the so-called tetracarboxylic acid residue represents a tetravalent group derived from a tetracarboxylic dianhydride, and the so-called diamine residue represents a divalent group derived from a diamine compound. The polyimide film of the first embodiment, the second embodiment or the third embodiment preferably contains an aromatic tetracarboxylic acid residue derived from an aromatic tetracarboxylic dianhydride and an aromatic diamine residue derived from an aromatic diamine.

[0085] (Tetracarboxylic acid residue)

[0086] In the first embodiment, the second embodiment or the third embodiment, the tetracarboxylic acid residues contained in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer include tetracarboxylic acid residues derived from at least one of 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) and 1,4-phenylenebis(trimellitic acid monoester) dianhydride (TAHQ) and tetracarboxylic acid residues derived from at least one of pyromellitic acid dianhydride (PMDA) and 2,3,6,7-naphthalenetetracarboxylic dianhydride (NTCDA).

[0087] The tetracarboxylic acid residue derived from BPDA (hereinafter, also referred to as "BPDA residue") and the tetracarboxylic acid residue derived from TAHQ (hereinafter, also referred to as "TAHQ residue") easily form an ordered structure of the polymer, and can reduce the dielectric tangent or hygroscopicity by inhibiting the movement of molecules. However, on the other hand, the BPDA residue can impart self-supporting properties to the gel film of polyamic acid, which is a polyimide precursor, but tends to increase the CTE after imidization, reduce the glass transition temperature, and reduce the heat resistance.

[0088] From the above viewpoint, the polyimide film of the first embodiment, the second embodiment or the third embodiment is controlled in such a way that the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer contains BPDA residues and TAHQ residues in a total amount preferably in a range of 30 mol parts or more and 60 mol parts or less, more preferably in a range of 40 mol parts or more and 50 mol parts or less, relative to 100 mol parts of tetracarboxylic acid residues. If the total amount of BPDA residues and TAHQ residues is less than 30 mol parts, the formation of the ordered structure of the polymer becomes insufficient, the hygroscopicity resistance decreases, or the reduction of the dielectric tangent becomes insufficient. If it exceeds 60 mol parts, in addition to the increase in CTE or the increase in the amount of change in the in-plane retardation (RO), there is a risk of a decrease in heat resistance.

[0089] In addition, tetracarboxylic acid residues derived from pyromellitic acid dianhydride (hereinafter also referred to as "PMDA residues") and tetracarboxylic acid residues derived from 2,3,6,7-naphthalenetetracarboxylic acid dianhydride (hereinafter also referred to as "NTCDA residues") have rigidity, and are residues that improve in-plane orientation, suppress CTE to a low level, and assume the role of controlling RO or controlling the glass transition temperature. On the other hand, PMDA residues have a small molecular weight, so if the amount becomes too much, the imide group concentration of the polymer becomes high, the polar groups increase, the hygroscopicity becomes larger, and the dielectric tangent increases due to the influence of moisture inside the molecular chain. In addition, NTCDA residues tend to make the film brittle and increase the elastic coefficient due to the highly rigid naphthalene skeleton.

[0090] Therefore, in the first embodiment, the second embodiment or the third embodiment, the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer contains PMDA residues and NTCDA residues in a total amount of preferably 40 mol parts or more and 70 mol parts or less, more preferably 50 mol parts or more and 60 mol parts or less, and further preferably 50 mol parts to 55 mol parts relative to 100 mol parts of tetracarboxylic acid residues. If the total amount of PMDA residues and NTCDA residues is less than 40 mol parts, there is a risk of an increase in CTE or a decrease in heat resistance, and if it exceeds 70 mol parts, there is a risk of an increase in the imide group concentration of the polymer, an increase in polar groups and a loss of low hygroscopicity, an increase in dielectric tangent, or a risk of a film becoming brittle and a decrease in the self-supporting property of the film.

[0091] In the first embodiment, as specified in the condition (ai), the total amount of at least one of BPDA residues and TAHQ residues and at least one of PMDA residues and NTCDA residues is 80 mol parts or more, preferably 90 mol parts or more, relative to 100 mol parts of tetracarboxylic acid residues.

[0092] In addition, in the first embodiment, as specified in the condition (ai), the molar ratio of at least one of the BPDA residue and the TAHQ residue to at least one of the PMDA residue and the NTCDA residue {(BPDA residue + TAHQ residue) / (PMDA residue + NTCDA residue)} is set to a range of greater than 0.6 and less than 1.3, preferably within a range of greater than 0.7 and less than 1.3, and more preferably within a range of greater than 0.8 and less than 1.2, so as to control the formation of the CTE and the ordered structure of the polymer.

[0093] In the first embodiment, the second embodiment or the third embodiment, PMDA and NTCDA have a rigid skeleton, so compared with other general anhydride components, the in-plane orientation of the molecules in the polyimide can be controlled, and the thermal expansion coefficient (CTE) can be suppressed and the glass transition temperature (Tg) can be improved. In addition, compared with PMDA, BPDA and TAHQ have a large molecular weight, so the imide group concentration decreases due to the increase in the loading ratio, which has an effect on the decrease in dielectric tangent or the decrease in moisture absorption. On the other hand, if the loading ratio of BPDA and TAHQ increases, the in-plane orientation of the molecules in the polyimide decreases, resulting in an increase in CTE. Furthermore, the formation of an ordered structure in the molecule is promoted, and the haze value increases. From the above point of view, the total loading amount of PMDA and NTCDA can be in the range of 40 to 70 mol parts, preferably in the range of 50 to 60 mol parts, and more preferably in the range of 50 to 55 mol parts relative to 100 mol parts of all anhydride components of the raw materials. If the total amount of PMDA and NTCDA charged is less than 40 parts by mole relative to 100 parts by mole of all the acid anhydride components of the raw materials, the in-plane orientation of the molecules decreases, and it becomes difficult to lower the CTE. In addition, the heat resistance or dimensional stability of the film during heating due to the decrease in Tg decreases. On the other hand, if the total amount of PMDA and NTCDA charged exceeds 70 parts by mole, there is a tendency that the moisture absorption rate deteriorates due to the increase in the imide group concentration, or the elastic modulus increases.

[0094] In addition, BPDA and TAHQ have an effect on lowering the dielectric tangent and moisture absorption rate caused by suppressing molecular motion or reducing the imide group concentration, but increase the CTE of the polyimide film after imidization. From this point of view, the total amount of BPDA and TAHQ charged can be within the range of 30 to 60 mol parts, preferably within the range of 40 to 50 mol parts, and more preferably within the range of 40 to 45 mol parts relative to 100 mol parts of all acid anhydride components of the raw materials.

[0095] Examples of the tetracarboxylic acid residue other than the BPDA residue, TAHQ residue, PMDA residue and NTCDA residue contained in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer include 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride, 2,3',3,4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-benzophenone tetracarboxylic dianhydride, 2,3,3',4'-benzophenone tetracarboxylic dianhydride or 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,3',3,4'-diphenyl ether tetracarboxylic dianhydride, bis(2,3-dicarboxyphenyl) ether dianhydride, 3 ,3",4,4"-terphenyltetracarboxylic dianhydride, 2,3,3",4"-terphenyltetracarboxylic dianhydride or 2,2",3,3"-terphenyltetracarboxylic dianhydride, 2,2-bis(2,3-dicarboxyphenyl)-propane dianhydride or 2,2-bis(3,4-dicarboxyphenyl)-propane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride or bis(3,4-dicarboxyphenyl)methane dianhydride, bis(2,3-dicarboxyphenyl)sulfone dianhydride or bis(3,4-dicarboxyphenyl)sulfone dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride or 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,2,7,8-phenanthrene-tetracarboxylic dianhydride carboxylic acid dianhydride, 1,2,6,7-phenanthrene-tetracarboxylic dianhydride or 1,2,9,10-phenanthrene-tetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)tetrafluoropropane dianhydride, 2,3,5,6-cyclohexane dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, 2,6-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride or 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-(or 1,4,5,8-) A tetracarboxylic acid residue derived from an aromatic tetracarboxylic acid dianhydride such as tetrachloronaphthalene-1,4,5,8-(or 2,3,6,7-)tetracarboxylic dianhydride, 2,3,8,9-perylene-tetracarboxylic dianhydride, 3,4,9,10-perylene-tetracarboxylic dianhydride, 4,5,10,11-perylene-tetracarboxylic dianhydride or 5,6,11,12-perylene-tetracarboxylic dianhydride, cyclopentane-1,2,3,4-tetracarboxylic dianhydride, pyrazine-2,3,5,6-tetracarboxylic dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic dianhydride, thiophene-2,3,4,5-tetracarboxylic dianhydride, 4,4'-bis(2,3-dicarboxyphenoxy)diphenylmethane dianhydride, and ethylene glycol bis-trimellitic anhydride.

[0096] (Diamine residue)

[0097] In the first embodiment, the second embodiment, or the third embodiment, the diamine residue contained in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer is preferably a diamine residue derived from a diamine compound represented by the general formula (A1).

[0098] [Chemistry 7]

[0099]

[0100] In formula (A1), the linking group X represents a single bond or -COO-, Y independently represents hydrogen, a monovalent hydrocarbon group having 1 to 3 carbon atoms, or an alkoxy group, n represents an integer of 0 to 2, and p and q independently represent integers of 0 to 4. Here, the term "independently" means that the multiple linking groups X, the multiple substituents Y, and the integers p and q in the formula (A1) may be the same or different. Furthermore, in the formula (A1), the hydrogen atoms in the two terminal amino groups may be substituted, for example, they may be -NR 3 R 4 (Here, R 3 , R 4 (a) independently represents an arbitrary substituent such as an alkyl group.

[0101] The diamine compound represented by the general formula (A1) (hereinafter, sometimes expressed as "diamine (A1)") is an aromatic diamine having two benzene rings. Diamine (A1) has a rigid structure, so it has the effect of imparting an ordered structure to the polymer as a whole. Therefore, a polyimide with low air permeability and low hygroscopicity can be obtained, and the moisture inside the molecular chain can be reduced, so the dielectric tangent can be reduced. Here, as the linking group X, a single bond is preferred.

[0102] Examples of the diamine (A1) include 1,4-diaminobenzene (p-phenylenediamine (p-PDA)), 2,2'-dimethyl-4,4'-diaminobiphenyl (m-TB), 2,2'-n-propyl-4,4'-diaminobiphenyl (m-NPB), and 4-aminophenyl-4'-aminobenzoate (APAB).

[0103] The non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer of the first embodiment or the second embodiment may contain preferably 80 mol parts or more, more preferably 85 mol parts or more of diamine residues derived from diamine (A1) relative to 100 mol parts of diamine residues. When the diamine (A1) is used in an amount within the above range, it is easy to form an ordered structure for the entire polymer by utilizing the rigid structure derived from the monomer, and it is easy to obtain a non-thermoplastic polyimide with low air permeability, low hygroscopicity and low dielectric tangent.

[0104] In the first embodiment or the second embodiment, when the diamine residue derived from the diamine (A1) is in the range of 80 mol parts to 85 mol parts with respect to 100 mol parts of the diamine residues in the non-thermoplastic polyimide, 1,4-diaminobenzene is preferably used as the diamine (A1) from the viewpoint of having a more rigid structure with excellent in-plane orientation.

[0105] In the first embodiment or the second embodiment, examples of other diamine residues contained in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer include 2,2-bis-[4-(3-aminophenoxy)phenyl]propane, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)]biphenyl, bis[1-(3-aminophenoxy)]biphenyl, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)]benzophenone, 9,9-bis[4-(3-aminophenoxy)phenyl]ether, ... phenoxy)phenyl]fluorene, 2,2-bis-[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis-[4-(3-aminophenoxy)phenyl]hexafluoropropane, 3,3'-dimethyl-4,4'-diaminobiphenyl, 4,4'-methylenebis-o-toluidine, 4,4'-methylenebis-2,6-dimethylaniline, 4,4'-methylenebis-2,6-diethylaniline, 3,3'-diaminodiphenylethane, 3,3'-diaminobiphenyl, 3,3'-dimethoxybenzidine, 3,3"-diamino-p-terphenyl, 4,4'-[1,4-phenylenebis bis(p-aminocyclohexyl)methane, bis(p-β-amino-tert-butylphenyl)ether, bis(p-β-methyl-δ-aminopentyl)benzene, p-bis(2-methyl-4-aminopentyl)benzene, p-bis(1,1-dimethyl-5-aminopentyl)benzene, 1,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,4-bis(β-amino-tert-butyl)toluene, 2,4-diaminotoluene, m-xylene-2,5-diamine, p-xylene-2,5-diamine, m-xylene-2,5-diamine Diamine residues derived from aromatic diamine compounds such as toluenediamine, p-xylylenediamine, 2,6-diaminopyridine, 2,5-diaminopyridine, 2,5-diamino-1,3,4-oxadiazole, piperazine, 2'-methoxy-4,4'-diaminobenzanilide, 4,4'-diaminobenzanilide, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, and 6-amino-2-(4-aminophenoxy)benzoxazole; and diamine residues derived from aliphatic diamine compounds such as dimer acid-type diamines in which both terminal carboxylic acid groups of a dimer acid are substituted with primary aminomethyl or amino groups.

[0106] In addition, in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer of the third embodiment, the diamine (A1) may be 70 mol parts or more, for example, in the range of 70 mol parts to 90 mol parts, preferably in the range of 80 mol parts to 90 mol parts, relative to 100 mol parts of all diamine components of the raw material as specified in the condition (ci). On the other hand, if the amount of the diamine (A1) charged exceeds 90 mol parts, the elongation of the film may decrease.

[0107] In addition, the non-thermoplastic polyimide used in the third embodiment is preferably a diamine component using at least one aromatic diamine selected from the group consisting of aromatic diamines represented by general formula (C1) to general formula (C4) as a raw material. Diamines (C1) to diamines (C4) have bulky substituents or curved parts, so they can impart flexibility to the polyimide. In addition, diamines (C1) to diamines (C4) can improve air permeability, so they have the effect of suppressing foaming when manufacturing multilayer films and metal sheet laminates. From the above viewpoint, it is preferred to use one or more aromatic diamines selected from diamines (C1) to diamines (C4) in a range of 2 to 15 mol parts relative to 100 mol parts of all diamine components of the raw materials. If the amount of diamines (C1) to diamines (C4) charged is less than 2 mol parts, foaming may sometimes occur when manufacturing multilayer films and metal sheet laminates. On the other hand, when the amount of the diamine (C1) to the diamine (C4) charged exceeds 15 parts by mole, the molecular orientation decreases and it becomes difficult to lower the CTE.

[0108] [Chemistry 8]

[0109]

[0110] In the formulas (C1) to (C4), R 2 independently represents a monovalent hydrocarbon group, an alkoxy group or an alkylthio group having 1 to 6 carbon atoms, and the linking group A' independently represents a group selected from -O-, -SO 2 -、-CH 2 -or-C(CH 3 ) 2 - is preferably a divalent group selected from -O-, -CH 2 -or-C(CH 3 ) 2 - is a divalent group, and the linking group X1 independently represents -CH 2 -、-O-CH 2 -O-, -OC 2 H 4 -O-, -OC 3 H 6 -O-, -OC 4 H 8 -O-, -OC 5 H 10 -O-, -O-CH 2 -C(CH 3 ) 2 -CH 2 -O-, -C(CH 3 ) 2 -、-C(CF 3 ) 2 -or-SO2 -, n 3 independently represents an integer from 1 to 4, n 4 independently represent an integer of 0 to 4, but in formula (C3), the linking group A' does not contain -CH 2 -、-C(CH 3 ) 2 -、-C(CF 3 ) 2 -or-SO 2 -In the case of n 4 Here, the term "independently" means that a plurality of linking groups A', a plurality of linking groups X1, a plurality of substituents R in one or more of the formulas (C1) to (C4) are 2 or multiple n 3 、n 4 Furthermore, in the formulas (C1) to (C4), the hydrogen atoms in the two amino groups at the terminals may be substituted, for example, -NR 3 R 4 (Here, R 3 , R 4 (a) independently represents an arbitrary substituent such as an alkyl group.

[0111] Examples of the aromatic diamine represented by the general formula (C1) include 2,6-diamino-3,5-diethyltoluene and 2,4-diamino-3,5-diethyltoluene.

[0112] Examples of the aromatic diamine represented by the general formula (C2) include 2,4-diamino-3,3′-diethyl-5,5′-dimethyldiphenylmethane and bis(4-amino-3-ethyl-5-methylphenyl)methane.

[0113] Examples of the aromatic diamine represented by the general formula (C3) include 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene, and 1,4-bis(4-aminophenoxy)-2,5-di-tert-butylbenzene.

[0114] Examples of the aromatic diamine represented by the general formula (C4) include 2,2-bis[4-(4-aminophenoxy)phenyl]propane and the like.

[0115] As described above, the non-thermoplastic polyimide constituting the polyimide film of the third embodiment can be controlled in such a manner that it contains residues derived from diamine (A1) in an amount of more than 70 mol parts, preferably in a range of 70 mol parts to 90 mol parts, relative to 100 mol parts of the diamine residues, and residues derived from diamines (C1) to (C4) in an amount of 2 mol parts to 15 mol parts.

[0116] In the third embodiment, other diamines that can be used as a raw material for the polyimide include, for example, 2,2-bis-[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis[4-(2-trifluoro-4-aminophenoxy)phenyl]hexafluoropropane, 1,4-bis(4-aminophenoxy)2,3,6-trimethyl-benzene, 1,4-bis(4-aminophenoxymethyl)propane, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)methane, 1,4-bis(4-aminophenoxy)ethane, 1,4-bis(4-aminophenoxy)ethane, and 1,4-bis(4-aminophenoxy)-2,3,6-trimethylbenzene. 1,4-bis(4-aminophenoxy)propane, 1,4-bis(4-aminophenoxy)butane, 1,4-bis(4-aminophenoxy)pentane, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)]biphenyl, bis[1-(3-aminophenoxy)]biphenyl, bis[4-(3-aminophenoxy)phenyl]methane, 1,4-bis(4-aminophenoxy)2-phenyl-benzene, 1,4-bis(2-trifluoromethyl-4-aminophenoxy)benzene, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)]benzophenone, 9,9-bis[4-(3-aminophenoxy)phenyl]fluorene, 2,2-bis-[4-(3-aminophenoxy)] phenyl]hexafluoropropane, 3,3'-dimethyl-4,4'-diaminobiphenyl, 4,4'-methylenebis-o-toluidine, 4,4'-methylenebis-2,6-dimethylaniline, 4,4'-methylene-2,6-diethylaniline, 3,3'-diaminodiphenylethane, 2-trifluoromethyl-4,4'-diaminodiphenyl ether, 2,2'-bis-trifluoromethyl-4,4'-diaminodiphenyl ether, 3,3'-diaminobiphenyl, 3,3'-dimethoxybenzidine, 3,3"-diamino-p-terphenyl, 4,4'-[1,4-phenylenebis(1-methylethylidene)]dianiline, 4,4'-[1,3-phenylenebis(1-methylethylidene)]dianiline, bis(p-aminocyclohexane Aromatic diamine compounds such as bis(p-β-amino-tert-butylphenyl) ether, bis(p-β-methyl-δ-aminopentyl) benzene, p-bis(2-methyl-4-aminopentyl) benzene, p-bis(1,1-dimethyl-5-aminopentyl) benzene, 1,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,4-bis(β-amino-tert-butyl) toluene, 2,4-diaminotoluene, m-xylene-2,5-diamine, p-xylene-2,5-diamine, m-xylene diamine, p-xylene diamine, 2,6-diaminopyridine, 2,5-diaminopyridine, 2,5-diamino-1,3,4-oxadiazole, piperazine, 2'-methoxy-4,4'-diaminobenzene anilide, and 4,4'-diaminobenzene anilide.

[0117] In the third embodiment, by using BPDA, TAHQ, PMDA and NTCDA as acid anhydride components that become raw materials of polyimide and diamine (A1) and diamine (C1) to diamine (C4) as diamine components in the above-mentioned molar ratios, the amount of residues derived from these raw material compounds can be controlled, so that the dielectric tangent and moisture absorption rate can be reduced, and foaming can be suppressed when manufacturing multilayer films and metal sheet laminates.

[0118] The polyimide film of the third embodiment has low dielectric constant and low dielectric tangent and low hygroscopicity, so it is preferably used as a matrix resin in an insulating resin layer of a copper sheet laminate that is a raw material of FPC. In addition, since aromatic tetracarboxylic anhydride and aromatic diamine are used as monomers that are raw materials of polyimide, the problem of dimensional change caused by heating is not likely to occur, and it has flame retardancy without the need to prepare a flame retardant. Therefore, by using the polyimide film of the third embodiment and the copper sheet laminate using the same, the reliability and yield of circuit substrates such as FPC can be improved.

[0119] In the non-thermoplastic polyimide of the first embodiment, the second embodiment or the third embodiment, by selecting the types of the tetracarboxylic acid residue and the diamine residue, or by using two or more tetracarboxylic acid residues or diamine residues, the respective molar ratios can be controlled to control the thermal expansion coefficient, storage elastic coefficient, tensile elastic coefficient, etc. In addition, in the non-thermoplastic polyimide, when there are a plurality of polyimide structural units, they may exist in the form of blocks or randomly, but from the viewpoint of suppressing the deviation of the in-plane retardation (RO), it is preferably randomly present.

[0120] In the first or second embodiment, the tetracarboxylic acid residue and the diamine residue contained in the non-thermoplastic polyimide are both aromatic groups, which is preferred because the dimensional accuracy of the polyimide film in a high temperature environment can be improved and the variation in in-plane retardation (RO) can be reduced.

[0121] In the first embodiment or the second embodiment, the imide group concentration of the non-thermoplastic polyimide is preferably 33 wt % or less. Here, the “imide group concentration” refers to the imide group (—(CO) 2 -N-) divided by the molecular weight of the entire structure of the polyimide. If the imide group concentration exceeds 33% by weight, the molecular weight of the resin itself decreases, and the low hygroscopicity also deteriorates due to the increase in polar groups. In the first embodiment or the second embodiment, the orientation of the molecules in the non-thermoplastic polyimide is controlled by selecting a combination of the acid anhydride and the diamine compound, thereby suppressing the increase in CTE associated with the decrease in the imide group concentration and ensuring low hygroscopicity.

[0122] In the first embodiment, the second embodiment or the third embodiment, the weight average molecular weight of the non-thermoplastic polyimide is preferably in the range of 10,000 to 400,000, and more preferably in the range of 50,000 to 350,000. If the weight average molecular weight is less than 10,000, the strength of the film decreases and tends to become brittle. On the other hand, if the weight average molecular weight exceeds 400,000, the viscosity increases excessively and the film thickness is uneven, streaks, and other undesirable conditions tend to occur during the coating operation.

[0123] <Thermoplastic polyimide>

[0124] In the polyimide film of the first embodiment or the second embodiment, the thermoplastic polyimide constituting the thermoplastic polyimide layer contains a tetracarboxylic acid residue and a diamine residue, and preferably contains an aromatic tetracarboxylic acid residue derived from an aromatic tetracarboxylic dianhydride and an aromatic diamine residue derived from an aromatic diamine.

[0125] (Tetracarboxylic acid residue)

[0126] As the tetracarboxylic acid residue used in the thermoplastic polyimide constituting the thermoplastic polyimide layer, the same ones as exemplified as the tetracarboxylic acid residue in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer can be used.

[0127] (Diamine residue)

[0128] As the diamine residue contained in the thermoplastic polyimide constituting the thermoplastic polyimide layer, a diamine residue derived from a diamine compound represented by General Formula (B1) to General Formula (B7) is preferred.

[0129] [Chemistry 9]

[0130]

[0131] In formula (B1) to formula (B7), R 1 independently represents a monovalent hydrocarbon group or alkoxy group having 1 to 6 carbon atoms, and the linking group A independently represents a group selected from -O-, -S-, -CO-, -SO-, -SO 2 -、-COO-、-CH 2 -、-C(CH 3 ) 2 -, -NH- or -CONH- in the divalent group, n 1 Independence represents an integer of 0 to 4. In formula (B3), the repeating of formula (B2) is excluded, and the repeating of formula (B4) is excluded from formula (B5). Here, the term "independently" means that a plurality of linking groups A, a plurality of R in one or more of the formulas (B1) to (B7) are 1 or multiple n 1Furthermore, in the formulas (B1) to (B7), the hydrogen atoms in the two amino groups at the terminals may be substituted, for example, -NR 3 R 4 (Here, R 3 , R 4 (a) independently represents an arbitrary substituent such as an alkyl group.

[0132] The diamine represented by formula (B1) (hereinafter, sometimes expressed as "diamine (B1)") is an aromatic diamine having two benzene rings. It is believed that the diamine (B1) is directly bonded to the amino group on at least one benzene ring and is in the meta position with the divalent linking group A, and the degree of freedom of the polyimide molecular chain is increased and has high flexibility, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using diamine (B1), the thermoplasticity of the polyimide is improved. Here, as the linking group A, -O-, -CH 2 -、-C(CH 3 ) 2 -, -CO-, -SO 2 -, -S-.

[0133] Examples of the diamine (B1) include 3,3'-diaminodiphenylmethane, 3,3'-diaminodiphenylpropane, 3,3'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylpropane, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminobenzophenone, and (3,3'-bisamino)diphenylamine.

[0134] The diamine represented by formula (B2) (hereinafter, sometimes described as "diamine (B2)") is an aromatic diamine having three benzene rings. It is believed that the diamine (B2) is in the meta position with the divalent linking group A through the amino group directly bonded to at least one benzene ring, and the degree of freedom of the polyimide molecular chain is increased and has high flexibility, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using diamine (B2), the thermoplasticity of the polyimide is improved. Here, as the linking group A, -O- is preferred.

[0135] As a diamine (B2), 1, 4- bis (3-aminophenoxy) benzene, 3- [4- (4-aminophenoxy) phenoxy] aniline, 3- [3- (4-aminophenoxy) phenoxy] aniline etc. are mentioned, for example.

[0136] The diamine represented by formula (B3) (hereinafter, sometimes described as "diamine (B3)") is an aromatic diamine having three benzene rings. It is believed that the diamine (B3) is in the meta position with two divalent linking groups A directly bonded to one benzene ring, and the degree of freedom of the polyimide molecular chain is increased and has high flexibility, which contributes to the improvement of the flexibility of the polyimide molecular chain. Therefore, by using diamine (B3), the thermoplasticity of the polyimide is improved. Here, as the linking group A, -O- is preferred.

[0137] Examples of the diamine (B3) include 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,3-bis(3-aminophenoxy)benzene (APB), 4,4'-[2-methyl-(1,3-phenylene)bisoxy]dianiline, 4,4'-[4-methyl-(1,3-phenylene)bisoxy]dianiline, and 4,4'-[5-methyl-(1,3-phenylene)bisoxy]dianiline.

[0138] The diamine represented by formula (B4) (hereinafter, sometimes expressed as "diamine (B4)") is an aromatic diamine having four benzene rings. It is believed that the diamine (B4) has high flexibility due to the amino group directly bonded to at least one benzene ring and the divalent linking group A being in the meta position, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using diamine (B4), the thermoplasticity of the polyimide is improved. Here, as the linking group A, -O-, -CH 2 -、-C(CH 3 ) 2 -、-SO 2 -, -CO-, -CONH-.

[0139] Examples of the diamine (B4) include bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]propane, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)]benzophenone, and bis[4,4′-(3-aminophenoxy)]benzanilide.

[0140] The diamine represented by formula (B5) (hereinafter, sometimes described as "diamine (B5)") is an aromatic diamine having four benzene rings. It is believed that the diamine (B5) is in the meta position with two divalent linking groups A directly bonded to at least one benzene ring, and the degree of freedom of the polyimide molecular chain is increased and has high flexibility, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using diamine (B5), the thermoplasticity of the polyimide is improved. Here, as the linking group A, -O- is preferred.

[0141] Examples of the diamine (B5) include 4-[3-[4-(4-aminophenoxy)phenoxy]phenoxy]aniline and 4,4′-[oxybis(3,1-phenyleneoxy)]dianiline.

[0142] The diamine represented by formula (B6) (hereinafter, sometimes referred to as "diamine (B6)") is an aromatic diamine having four benzene rings. It is believed that the diamine (B6) has high flexibility due to having at least two ether bonds, which contributes to the improvement of the flexibility of the polyimide molecular chain. Therefore, by using diamine (B6), the thermoplasticity of the polyimide is improved. Here, as the linking group A, -C(CH 3 ) 2 -、-O-、-SO 2 -, -CO-.

[0143] Examples of the diamine (B6) include 2,2-Bis[4-(4-aminophenoxy)phenyl]propane (BAPP), bis[4-(4-aminophenoxy)phenyl]ether (BAPE), bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), and bis[4-(4-aminophenoxy)phenyl]ketone (BAPK).

[0144] The diamine represented by formula (B7) (hereinafter, sometimes expressed as "diamine (B7)") is an aromatic diamine having four benzene rings. The diamine (B7) has a divalent linking group A with high flexibility on both sides of the diphenyl skeleton, and is therefore believed to contribute to the improvement of the flexibility of the polyimide molecular chain. Therefore, by using diamine (B7), the thermoplasticity of the polyimide is improved. Here, as the linking group A, -O- is preferred.

[0145] As a diamine (B7), bis[4-(3-aminophenoxy)]biphenyl, bis[4-(4-aminophenoxy)]biphenyl, etc. are mentioned, for example.

[0146] In the first embodiment or the second embodiment, the thermoplastic polyimide constituting the thermoplastic polyimide layer contains a diamine residue derived from at least one diamine compound selected from diamine (B1) to diamine (B7) in an amount of 70 mol parts or more, preferably in a range of 70 mol parts or more and 99 mol parts or less, and more preferably in a range of 80 mol parts or more and 95 mol parts or less, relative to 100 mol parts of diamine residues. Since diamine (B1) to diamine (B7) have a molecular structure having flexibility, by using at least one diamine compound selected from these compounds in an amount within the above range, the flexibility of the polyimide molecular chain can be improved and thermoplasticity can be imparted. If the total amount of diamine (B1) to diamine (B7) is less than 70 mol parts relative to 100 mol parts of all diamine components, the flexibility of the polyimide resin is insufficient and sufficient thermoplasticity cannot be obtained.

[0147] In addition, as the diamine residue contained in the thermoplastic polyimide constituting the thermoplastic polyimide layer, it is also preferably a diamine residue derived from a diamine compound represented by the general formula (A1). Regarding the diamine compound [diamine (A1)] represented by the formula (A1), as described in the description of the non-thermoplastic polyimide. Diamine (A1) has a rigid structure and has the effect of imparting an ordered structure to the polymer as a whole, so that the dielectric tangent or hygroscopicity can be reduced by inhibiting the movement of molecules. Furthermore, by being used as a raw material for thermoplastic polyimide, a polyimide with low air permeability and excellent long-term heat resistance and adhesion can be obtained.

[0148] In the first embodiment or the second embodiment, the thermoplastic polyimide constituting the thermoplastic polyimide layer may contain a diamine residue derived from the diamine (A1) in an amount preferably in the range of 1 mol or more and 30 mol or less, more preferably in the range of 5 mol or more and 20 mol or less. By using the diamine (A1) in an amount in the above range, the polymer as a whole forms an ordered structure by utilizing the rigid structure derived from the monomer, and thus a thermoplastic polyimide having low air permeability and hygroscopicity and excellent long-term heat-resistant adhesion can be obtained.

[0149] The thermoplastic polyimide constituting the thermoplastic polyimide layer may contain a diamine residue derived from a diamine compound other than the diamine (A1) and the diamines (B1) to (B7) within a range that does not impair the effects of the invention.

[0150] In the thermoplastic polyimide, by selecting the types of the tetracarboxylic acid residue and the diamine residue, or by using two or more tetracarboxylic acid residues or diamine residues, their respective molar ratios can be controlled to control the thermal expansion coefficient, tensile elastic coefficient, glass transition temperature, etc. In addition, in the thermoplastic polyimide, when there are a plurality of polyimide structural units, they may exist in the form of blocks or randomly, but preferably randomly.

[0151] In the first or second embodiment, by making both the tetracarboxylic acid residue and the diamine residue contained in the thermoplastic polyimide an aromatic group, the dimensional accuracy of the polyimide film in a high temperature environment can be improved and the change in in-plane retardation (RO) can be suppressed.

[0152] The imide group concentration of the thermoplastic polyimide is preferably 33 wt % or less. Here, "imide group concentration" refers to the imide group (-(CO) 2 -N-) divided by the molecular weight of the entire structure of the polyimide. If the imide group concentration exceeds 33% by weight, the molecular weight of the resin itself decreases, and the low hygroscopicity also deteriorates due to the increase in polar groups. In the first embodiment or the second embodiment, the orientation of the molecules in the thermoplastic polyimide is controlled by selecting the combination of the diamine compounds, thereby suppressing the increase in CTE associated with the decrease in the imide group concentration and ensuring low hygroscopicity.

[0153] The weight average molecular weight of the thermoplastic polyimide is preferably in the range of 10,000 to 400,000, and more preferably in the range of 50,000 to 350,000. If the weight average molecular weight is less than 10,000, the strength of the film decreases and the film tends to become brittle. On the other hand, if the weight average molecular weight exceeds 400,000, the viscosity increases excessively and the film thickness is uneven, streaks, and other undesirable conditions tend to occur during the coating operation.

[0154] In the polyimide film of the first or second embodiment, the thermoplastic polyimide constituting the thermoplastic polyimide layer can improve adhesion with copper foil. The thermoplastic polyimide has a glass transition temperature in the range of 200°C to 350°C, preferably 200°C to 320°C.

[0155] The thermoplastic polyimide constituting the thermoplastic polyimide layer, for example, becomes an adhesive layer in the insulating resin of the circuit substrate, so in order to suppress the diffusion of copper, a completely imidized structure is most preferably used. Among them, a part of the polyimide can also become an amic acid. The imidization rate is measured by using a Fourier transform infrared spectrophotometer (commercial product: FT / IR620 manufactured by JASCO Corporation) and using the attenuated total reflection (Attenuated Total Reflectance, ATR) method to measure the infrared absorption spectrum of the polyimide film, thereby measuring the infrared absorption spectrum of the polyimide film at 1015 cm -1 Based on the benzene ring absorber near 1780cm -1 The absorbance of the C=O expansion and contraction of the imide group was calculated.

[0156] <Polyimide film form>

[0157] The polyimide film of the first embodiment, the second embodiment or the third embodiment is not particularly limited as long as it satisfies the above conditions, and may be a film (sheet) containing an insulating resin, or a film of an insulating resin in a state of being laminated on a substrate such as a resin sheet such as a copper foil, a glass plate, a polyimide film, a polyamide film, a polyester film, etc.

[0158] <Thickness>

[0159] The thickness of the polyimide film of the first embodiment, the second embodiment or the third embodiment can be set to a thickness within a specified range according to the purpose of use. The thickness of the polyimide film is preferably, for example, in the range of 8 μm to 50 μm, more preferably in the range of 11 μm to 26 μm. If the thickness of the polyimide film is less than the lower limit, problems such as the inability to ensure electrical insulation or difficulty in operation in the manufacturing step due to a decrease in handling properties may sometimes occur. On the other hand, if the thickness of the polyimide film exceeds the upper limit, for example, it is necessary to control the manufacturing conditions for controlling the in-plane delay (RO) with high precision, resulting in undesirable conditions such as decreased productivity.

[0160] In addition, in the polyimide film of the first embodiment or the second embodiment, the thickness ratio of the non-thermoplastic polyimide layer to the thermoplastic polyimide layer (non-thermoplastic polyimide layer / thermoplastic polyimide layer) may be in the range of 1.5 to 6.0. If the value of the ratio is less than 1.5, the non-thermoplastic polyimide layer becomes thinner relative to the entire polyimide film, so the deviation of the in-plane retardation (RO) tends to become larger, and if it exceeds 6.0, the thermoplastic polyimide layer becomes thinner, so the adhesion reliability between the polyimide film and the copper foil tends to decrease. The control of the in-plane retardation (RO) is related to the resin composition and thickness of each polyimide layer constituting the polyimide film. Regarding the thermoplastic polyimide layer, which is a resin that imparts adhesion, i.e., high thermal expansion or softening properties, the greater its thickness, the more significant the impact on the RO value of the polyimide film. Therefore, the ratio of the thickness of the non-thermoplastic polyimide layer is increased, and the ratio of the thickness of the thermoplastic polyimide layer is reduced, and the deviation between the RO value of the polyimide film and the RO value is reduced.

[0161] <Film width>

[0162] In the second embodiment, from the viewpoint of more significantly showing the improvement effect of the dimensional accuracy of the polyimide film, the polyimide film is preferably a film width of 490 mm or more and 1100 mm or less, and the length of the long strip is 20 m or more. In the case of continuously manufacturing the polyimide film of the second embodiment, the wider the film in the width direction (hereinafter, also referred to as the TD direction), the more significant the effect of the invention becomes. Furthermore, in the case of continuously manufacturing the polyimide film of the second embodiment, the long side direction of the long strip of polyimide film is referred to as the MD direction.

[0163] <In-plane retardation (RO)>

[0164] Regarding the polyimide film of the second embodiment, the value of the in-plane retardation (RO) is within the range of 5 nm to 50 nm, preferably within the range of 5 nm to 20 nm, and more preferably within the range of 5 nm to 15 nm. In addition, the deviation (ΔRO) of RO in the TD direction is 10 nm or less, preferably 5 nm or less, and more preferably 3 nm or less. Since it is controlled within the above range, the dimensional accuracy is high even for a film with a thickness of 25 μm or more.

[0165] The polyimide film of the second embodiment was subjected to a temperature of 320° C. and a pressure of 340 MPa / m 2, the change in in-plane retardation (RO) before and after the pressurization with a holding time of 15 minutes is 20 nm or less, preferably 10 nm or less, and more preferably 5 nm or less. Even if the polyimide film of the second embodiment is at a temperature exceeding the glass transition temperature of the polyimide constituting the thermoplastic polyimide layer, the change in RO is controlled to be below the upper limit value. For example, before and after the step of laminating the polyimide film of the second embodiment to the copper foil by thermal lamination, RO is not easy to change, so it becomes a polyimide film with excellent dimensional stability.

[0166] <Coefficient of thermal expansion>

[0167] When the polyimide film of the first embodiment or the second embodiment is used as an insulating layer of a circuit board, for example, in order to prevent the occurrence of warping or the decrease in dimensional stability, as specified in the above condition (a-iii) or condition (bi), it is important that the coefficient of thermal expansion (CTE) of the entire film is within the range of 10 ppm / K or more and 30 ppm / K or less, preferably within the range of 10 ppm / K or more and 25 ppm / K or less, and more preferably within the range of 10 ppm / K to 20 ppm / K. If the CTE is less than 10 ppm / K or exceeds 30 ppm / K, warping may occur or the dimensional stability may decrease. In addition, the coefficient of thermal expansion (CTE) of the polyimide film of the third embodiment is also the same as that of the first embodiment or the second embodiment.

[0168] <Dielectric tangent>

[0169] The polyimide film of the first embodiment, the second embodiment or the third embodiment is, for example, as specified in the conditions (a-iv) or (c-iii), for example, when used as an insulating layer of a circuit substrate, in order to ensure impedance matching, as an insulating layer as a whole, the dielectric tangent (Tanδ) at 10GHz when measured by a split dielectric resonator (split postdielectric resonator (SPDR)) can be less than 0.004, more preferably within the range of more than 0.001 and less than 0.004, and further preferably within the range of more than 0.002 and less than 0.003. In order to improve the dielectric properties of the circuit substrate, it is particularly important to control the dielectric tangent of the insulating layer, and by setting the dielectric tangent within the range, the effect of reducing the transmission loss is increased. Therefore, when the polyimide film is used, for example, as an insulating layer of a high-frequency circuit substrate, the transmission loss can be reduced efficiently. If the dielectric tangent of the insulating layer at 10 GHz exceeds 0.004, when used in a circuit substrate such as an FPC, it is easy to cause disadvantages such as loss of electrical signals in the transmission path of high-frequency signals. There is no particular restriction on the lower limit of the dielectric tangent of the insulating layer at 10 GHz, but it is considered to control the physical properties when polyimide is used as an insulating layer of a circuit substrate.

[0170] <Dielectric constant>

[0171] When the polyimide film of the first embodiment, the second embodiment or the third embodiment is used as an insulating layer of a circuit substrate, for example, in order to ensure impedance matching, the dielectric constant of the insulating layer as a whole at 10 GHz is preferably 4.0 or less. If the dielectric constant of the insulating layer at 10 GHz exceeds 4.0, when used in a circuit substrate such as an FPC, the dielectric loss of the insulating layer will be deteriorated, and the loss of electric signals will be easily generated in the transmission path of high-frequency signals.

[0172] <Moisture absorption rate>

[0173] Regarding the polyimide film of the first embodiment or the second embodiment, in order to reduce the influence of humidity when used in a circuit substrate such as an FPC, it is preferably that the moisture absorption rate at 23°C and 50%RH is 0.7 wt% or less. If the moisture absorption rate of the polyimide film exceeds 0.7 wt%, it is easily affected by humidity when used in a circuit substrate such as an FPC, and it is easy to cause undesirable conditions such as changes in the transmission speed of high-frequency signals. That is, if the moisture absorption rate of the polyimide film exceeds the above range, it is easy to absorb water with high dielectric constant and dielectric tangent, thereby causing an increase in dielectric constant and dielectric tangent, and it is easy to cause undesirable conditions such as loss of electrical signals on the transmission path of high-frequency signals.

[0174] In addition, considering the influence on the dimensional stability or dielectric properties of the polyimide film, the polyimide film of the third embodiment preferably has a moisture absorption of 0.65 wt % or less when humidified for 24 hours at 23°C and 50% RH. If the moisture absorption exceeds 0.65 wt %, the dimensional stability or dielectric properties of the polyimide film may sometimes be deteriorated. Regarding the situation where the moisture absorption is less than 0.65 wt %, it is believed that the concentration of polar groups in the polyimide is low and it is easy to form an ordered structure of a polymer chain, so it is preferred for improving dimensional stability or dielectric properties. Among them, if the moisture absorption becomes lower, there is a tendency for the haze (HAZE) value to increase with the formation of an ordered structure of a polymer chain, so it is preferred to also consider the haze value described later.

[0175] <Tensile elasticity coefficient>

[0176] In addition, the tensile elastic coefficient of the polyimide film of the second embodiment is preferably in the range of 3.0 GPa to 10.0 GPa, and can be in the range of 4.5 GPa to 8.0 GPa. If the tensile elastic coefficient of the polyimide film is less than 3.0 GPa, sometimes due to the decrease in the strength of the polyimide itself, problems in processing such as film rupture occur when the copper sheet laminate is processed into a circuit substrate. On the contrary, if the tensile elastic coefficient of the polyimide film exceeds 10.0 GPa, the rigidity relative to the bending of the copper sheet laminate increases, resulting in an increase in the bending stress applied to the copper wiring when the copper sheet laminate is bent, and a decrease in bending resistance. By setting the tensile elastic coefficient of the polyimide film within the above range, the strength and flexibility of the polyimide film are ensured.

[0177] <Glass transition temperature>

[0178] The polyimide film of the third embodiment has a glass transition temperature of 300°C or more as specified in the condition (c-ii). If the glass transition temperature is less than 300°C, when manufacturing a copper-clad plate (CCL) or FPC using the polyimide film of the third embodiment, problems such as expansion of the film or peeling off from the wiring are likely to occur. On the other hand, by setting the glass transition temperature to 300°C or more, the solder heat resistance or dimensional stability of the polyimide film is improved.

[0179] <Haze value>

[0180] In addition, the polyimide film of the third embodiment is preferably processed into a polyimide film with a thickness of 25 μm as follows, and the haze (HAZE) value based on Japanese Industrial Standards (JIS) K 7136 is in the range of 62% to 75%, and the polyimide film is obtained by etching away the copper foil of a laminate formed by applying a solution of polyamic acid, which is a precursor of polyimide, on a copper foil with a ten-point average roughness (Rz) of 0.6 μm and imidizing it. If the haze value exceeds 75%, the visibility of the polyimide film through the third embodiment becomes low. Therefore, in the photolithography step of the copper sheet laminate (CCL) obtained using the polyimide film, or in the process of installing the FPC (flexible printed circuit board) using the CCL, the visibility of the alignment mark provided on the CCL is reduced, and it becomes difficult to align the position of the alignment mark, thereby reducing the practicality. On the other hand, if the haze value is lower than 62%, visibility becomes high, and the formation of the ordered structure of the polyimide polymer chain is not promoted, so there is a risk of impairing the hygroscopic properties or dielectric properties. In the third embodiment, in order to achieve low dielectric tangent and low moisture absorption rate brought about by the formation of the ordered structure and maintain visibility, the preferred value of the haze value is set to be within the range of 62% to 75%.

[0181] <Film elongation>

[0182] The polyimide film of the third embodiment preferably has a film elongation of 30% or more. When the polyimide film of the third embodiment is used as an insulating layer of an FPC, for example, it needs to be folded and stored in a small space in a frame of a mobile device or the like. In the above-mentioned usage, if the film elongation is low, it will cause the wiring to be disconnected. Therefore, with respect to the polyimide film of the third embodiment, the preferred film elongation is set to 30% or more.

[0183] <Packing>

[0184] The polyimide film of the first embodiment, the second embodiment or the third embodiment may contain an inorganic filler in the non-thermoplastic polyimide layer or the thermoplastic polyimide layer as needed. Specifically, for example, silicon dioxide, aluminum oxide, magnesium oxide, beryllium oxide, boron nitride, aluminum nitride, silicon nitride, aluminum fluoride, calcium fluoride, etc. These may be used alone or in combination of two or more.

[0185] [Manufacturing method]

[0186] As the aspect of the method for producing the polyimide film of the first embodiment, the second embodiment or the third embodiment, for example, there are [1] a method for producing the polyimide film by coating a polyamic acid solution on a supporting substrate and drying it, and then performing imidization; [2] a method for producing the polyimide film by coating a polyamic acid solution on a supporting substrate and drying it, peeling off a gel film of polyamic acid from the supporting substrate, and performing imidization. In addition, the polyimide film of the first embodiment or the second embodiment is a polyimide film comprising a plurality of polyimide layers, and therefore, as the aspect of its production method, for example, there are [3] a method of repeatedly coating a polyamic acid solution on a supporting substrate and drying it, and then performing imidization (hereinafter, a casting method); [4] a method of coating and drying the polyamic acid in a state of being stacked into multiple layers by multilayer extrusion, and then performing imidization (hereinafter, a multilayer extrusion method), etc. About the situation that the polyimide film of the 3rd embodiment is used as a layer in the multilayer polyimide film comprising multilayer polyimide layer, it is also the same.As the method that polyimide solution (or polyamic acid solution) is coated on substrate, there is no particular restriction, for example, coating machines such as notch wheel, mould, scraper, die lip can be utilized to be coated.When forming multilayer polyimide layer, it is preferably repeated that polyimide solution (or polyamic acid solution) is coated on substrate and dried operation.

[0187] The method [1] may include, for example, the following steps 1a to 1c:

[0188] (1a) a step of coating a polyamic acid solution on a supporting substrate and drying the solution;

[0189] (1b) forming a polyimide layer by heat-treating and imidizing polyamic acid on a supporting substrate;

[0190] (1c) A step of obtaining a polyimide film by separating the supporting substrate from the polyimide layer.

[0191] The method [2] may include, for example, the following steps 2a to 2c:

[0192] (2a) coating a polyamic acid solution on a supporting substrate and drying the solution;

[0193] (2b) a step of separating the supporting substrate from the gel film of polyamic acid;

[0194] (2c) A step of obtaining a polyimide film by heat-treating and imidizing the gel film of polyamic acid.

[0195] The method [3] may be carried out in the same manner as the method [1] or the method [2], except that step 1a or step 2a is repeated a plurality of times in the method [1] or the method [2] to form a laminated structure of polyamic acid on a supporting substrate.

[0196] The method [4] may be carried out in the same manner as the method [1] or the method [2], except that in step 1a of the method [1] or step 2a of the method [2], the laminated structure of polyamic acid is simultaneously coated by multilayer extrusion and dried.

[0197] The polyimide film manufactured in the first embodiment, the second embodiment or the third embodiment is preferably imidized with polyamic acid on a supporting substrate. Since the resin layer of polyamic acid is imidized while being fixed on a supporting substrate, the expansion and contraction change of the polyimide layer during the imidization process can be suppressed, and the thickness or dimensional accuracy of the polyimide film can be maintained. In addition, when the polyimide film of the third embodiment is used as one layer of a multilayer polyimide film including a multilayer polyimide layer, a heat treatment for imidization is performed in stages at a temperature in the range of, for example, 120°C to 360°C, and the heat treatment time is controlled to be more than 5 minutes, preferably in the range of 10 minutes to 20 minutes, thereby effectively suppressing foaming and preventing undesirable conditions such as expansion of the polyimide layer.

[0198] Regarding the polyimide film in which imidization of polyamic acid is completed on a supporting substrate, the polyimide film is stretched by the tension applied to the polyimide film when separating the polyimide film from the supporting substrate, or the stress on the polyimide film generated when peeling using a knife, etc., and the in-plane retardation (RO) of the polyimide film is easily deviated. In particular, regarding the polyimide film of the second embodiment, any of the polyimides constituting the non-thermoplastic polyimide layer and the thermoplastic polyimide layer are easy to form an ordered structure, so the RO can be controlled by dispersing the stress required for peeling in each layer of the polyimide film.

[0199] In addition, the in-plane retardation (RO) can be controlled by separating the gel film of polyamic acid on the supporting substrate and imidizing the gel film of polyamic acid simultaneously or continuously with uniaxial stretching or biaxial stretching. In this case, in order to control the RO with higher accuracy, it is preferable to appropriately adjust the conditions such as the heating rate during the stretching operation and imidization, the completion temperature of imidization, and the load.

[0200] [Copper sheet laminate]

[0201] The copper sheet laminate of the first embodiment, the second embodiment or the third embodiment has an insulating layer, and has a copper foil on at least one surface of the insulating layer, and a part or all of the insulating layer can be formed using the polyimide film of the first embodiment, the second embodiment or the third embodiment. In addition, in order to improve the adhesion between the insulating layer and the copper foil, the layer in the insulating layer that is in contact with the copper foil is preferably a thermoplastic polyimide layer. Therefore, with respect to the polyimide film of the third embodiment, it is preferably used as a copper sheet laminate in a state of being laminated with a thermoplastic polyimide layer. The copper foil is provided on one or both surfaces of the insulating layer. That is, the copper sheet laminate of the first embodiment, the second embodiment or the third embodiment may be a single-sided copper sheet laminate (single-sided CCL) or a double-sided copper sheet laminate (double-sided CCL). In the case of a single-sided CCL, the copper foil laminated on a single surface of the insulating layer is set as the "first copper foil layer" of the present invention. In the case of a double-sided CCL, the copper foil laminated on one side of the insulating layer is set as the "first copper foil layer" of the present invention, and the copper foil laminated on the surface opposite to the surface laminated with the first copper foil in the insulating layer is set as the "second copper foil layer" of the present invention. The copper sheet laminate of the first embodiment, the second embodiment, or the third embodiment is used as an FPC by etching the copper foil and performing wiring circuit processing to form copper wiring.

[0202] The copper sheet laminate can be produced, for example, by preparing a resin film composed of the polyimide film of the first, second or third embodiment, sputtering a metal thereon to form a seed layer, and then forming a copper foil layer by, for example, copper plating.

[0203] Alternatively, a copper sheet laminate may be produced by preparing a resin film composed of the polyimide film of the first embodiment, the second embodiment, or the third embodiment, and laminating copper foil thereon by a method such as thermocompression bonding.

[0204] Furthermore, a copper sheet laminate can also be produced by casting a coating liquid containing a polyamic acid as a precursor of a polyimide onto a copper foil, drying it to form a coating film, and then heat-treating it for imidization to form a polyimide layer.

[0205] <1st copper foil layer>

[0206] In the copper sheet laminate of the first embodiment, the second embodiment or the third embodiment, the copper foil used in the first copper foil layer (hereinafter sometimes referred to as "first copper foil") is not particularly limited, and may be, for example, a rolled copper foil or an electrolytic copper foil. As the first copper foil, a commercially available copper foil may be used.

[0207] In the first embodiment, the second embodiment or the third embodiment, the thickness of the first copper foil is preferably 18 μm or less, more preferably in the range of 6 μm to 13 μm, and further preferably in the range of 6 μm to 12 μm. By setting the thickness of the first copper foil to 18 μm or less, preferably 13 μm or less, and further preferably 12 μm or less, the bendability of the copper sheet laminate (or FPC) can be improved. In addition, from the viewpoint of production stability and handling properties, the lower limit of the thickness of the first copper foil is preferably set to 6 μm.

[0208] In addition, in the first embodiment, the second embodiment or the third embodiment, the tensile elastic coefficient of the first copper foil is preferably within the range of 10 GPa to 35 GPa, and more preferably within the range of 15 GPa to 25 GPa. In the case of using a rolled copper foil as the first copper foil, if annealing is performed by heat treatment, the flexibility tends to become higher. Therefore, if the tensile elastic coefficient of the copper foil is less than the lower limit, in the step of forming an insulating layer on the long first copper foil, the rigidity of the first copper foil itself decreases due to heating. On the other hand, if the tensile elastic coefficient exceeds the upper limit, a large bending stress is applied by copper wiring when the FPC is bent, and the bending resistance decreases. Furthermore, there is a tendency for the rolled copper foil to change its tensile elastic coefficient by the heat treatment conditions when the insulating layer is formed on the copper foil, or the annealing treatment of the copper foil after the insulating layer is formed. Therefore, in the first embodiment, the second embodiment or the third embodiment, in the finally obtained copper sheet laminate, as long as the tensile elastic coefficient of the first copper foil is within the range.

[0209] <Second copper foil layer>

[0210] In the first embodiment, the second embodiment or the third embodiment, the second copper foil layer is laminated on the surface of the insulating layer opposite to the first copper foil layer. The copper foil (second copper foil) used in the second copper foil layer is not particularly limited, and may be, for example, a rolled copper foil or an electrolytic copper foil. In addition, a commercially available copper foil may be used as the second copper foil. Furthermore, the same copper foil as the first copper foil may be used as the second copper foil.

[0211] [Circuit board]

[0212] The copper sheet laminate of the first embodiment, the second embodiment or the third embodiment is mainly useful as a circuit substrate material of an FPC, etc. That is, the copper foil of the copper sheet laminate of the first embodiment, the second embodiment or the third embodiment can be processed into a pattern to form a wiring layer by a conventional method, thereby manufacturing an FPC as one embodiment of the present invention.

[0213] Example

[0214] The following examples are shown to more specifically describe the features of the present invention. However, the scope of the present invention is not limited to the examples. Furthermore, in the following examples, various measurements and evaluations are performed using the following methods unless otherwise specified.

[0215] [Viscosity measurement]

[0216] The viscosity at 25° C. was measured using an E-type viscometer (Brookfield, trade name: DV-II+Pro). The rotation speed was set so that the torque was 10% to 90%, and the value when the viscosity stabilized was read 2 minutes after the start of the measurement.

[0217] [Measurement of glass transition temperature (Tg)]

[0218] The glass transition temperature was measured using a dynamic viscoelasticity measuring device (DMA: manufactured by UBM, trade name: E4000F) at a temperature increase rate of 4°C / min and a frequency of 11 Hz from 30°C to 400°C for a polyimide film of 5 mm×20 mm, and the temperature at which the change in elastic modulus (tan δ) was the maximum was defined as the glass transition temperature. The storage elastic modulus at 30°C measured using DMA was 1.0×10 9 Pa or more and the storage elastic coefficient at 280°C is less than 3.0×10 8 Pa is set as "thermoplastic", and the storage elastic coefficient at 30°C is 1.0×10 9 Pa and the storage elastic coefficient at 280°C is 3.0×10 8 Those with a value of Pa or above are considered as "non-thermoplastic".

[0219] [Determination of coefficient of thermal expansion (CTE)]

[0220] Using a thermomechanical analyzer (manufactured by Bruker, trade name: 4000SA), a load of 5.0 g was applied to a polyimide film of size 3 mm × 20 mm, and the temperature was raised from 30°C to 265°C at a certain heating rate. The film was then kept at the temperature for 10 minutes and then cooled at a rate of 5°C / min to determine the average thermal expansion coefficient (thermal expansion coefficient) from 250°C to 100°C.

[0221] [Determination of moisture absorption rate]

[0222] Two polyimide film test pieces (4 cm wide x 25 cm long) were prepared and dried at 80°C for 1 hour. Immediately after drying, they were placed in a constant temperature and humidity room at 23°C / 50%RH and left to stand for more than 24 hours. The weight change before and after was calculated using the following formula.

[0223] Moisture absorption rate (weight %) = [(weight after moisture absorption - weight after drying) / weight after drying] × 100

[0224] [Determination of dielectric constant and dielectric tangent]

[0225] The dielectric constant and dielectric tangent of the resin sheet at a frequency of 10 GHz were measured using a vector network analyzer (manufactured by Agilent, trade name E8363C) and a separated dielectric resonator (SPDR resonator). The material used in the measurement was left for 24 hours under the conditions of temperature: 24°C to 26°C and humidity: 45% to 55%.

[0226] [Calculation of Imide Group Concentration]

[0227] The imide group (-(CO) 2 The value obtained by dividing the molecular weight of the polyimide (-N-) by the molecular weight of the entire polyimide structure was defined as the imide group concentration.

[0228] [Measurement of surface roughness of copper foil]

[0229] Regarding the surface roughness of the copper foil, an atomic force microscope (AFM) (manufactured by Bruker AXS, trade name: Dimension Icon SPM) and a probe (manufactured by Bruker AXS, trade name: TESPA (NCHV), with a tip curvature radius of 10 nm and a spring constant of 42 N / m) were used to measure the surface roughness of the copper foil in an area of ​​80 μm×80 μm using a tapping mode to determine the ten-point average roughness (Rz).

[0230] [Determination of peel strength]

[0231] The copper foils on both sides of the thermocompression bonding side and the cast side of the double-sided copper sheet laminate (copper foil / resin layer / copper foil) were processed into a circuit with a width of 0.8 mm (wiring was processed in such a way that the copper foils on both sides were in the same position), and then cut into a width of 8 cm × a length of 4 cm to prepare a measurement sample. The peel strength of the cast side and the thermocompression bonding side of the measurement sample was measured using a Tensilon Tester (manufactured by Toyo Seiki Seisaku-sho, trade name: Strograph VE-1D), and the copper foil surface of the thermocompression bonding side or the cast side of the measurement sample was fixed to an aluminum plate with a double-sided tape, and the other copper foil was peeled off at a speed of 50 mm / min in a 90° direction, and the central value strength when peeled off 10 mm from the resin layer was obtained. At this time, the peel strength was 1.0 kN / m or more as ◎ (excellent), 0.7 kN / m or more and less than 1.0 kN / m as ○ (good), 0.4 kN / m or more and less than 0.7 kN / m as △ (acceptable), and less than 0.4 kN / m as × (unacceptable).

[0232] [Measurement of in-plane retardation (RO)]

[0233] In-plane retardation (RO) is the retardation in the in-plane direction of the polyimide film obtained using a birefringence meter (manufactured by Photonic-Lattice, trade name: Wide Range Birefringence Evaluation System WPA-100) The measurement wavelength is 543 nm.

[0234] [Determination of haze value]

[0235] The haze value was measured using a haze measuring device (turbidimeter: manufactured by Nippon Denshoku Industries, trade name: NDH5000) by the measuring method described in JIS K 7136 on a polyimide film having a size of 5 cm×5 cm.

[0236] [Determination of film elongation]

[0237] A polyimide film cut into a size of 12.7 mm in width and 127 mm in length was subjected to a tensile test at 50 mm / min using a tension tester (Tensilon manufactured by Orientec) to determine the film elongation at 25°C.

[0238] The abbreviations used in Examples and Reference Examples represent the following compounds.

[0239] BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride

[0240] PMDA: Pyromellitic Dianhydride

[0241] NTCDA: 2,3,6,7-Naphthalenetetracarboxylic dianhydride

[0242] TAHQ: 1,4-phenylene bis(trimellitic acid monoester) dianhydride

[0243] TMEG: Ethylene glycol bis(trimellitic anhydride)

[0244] m-TB: 2,2'-dimethyl-4,4'-diaminobiphenyl

[0245] TPE-R: 1,3-bis(4-aminophenoxy)benzene

[0246] TPE-Q: 1,4-bis(4-aminophenoxy)benzene

[0247] APB: 1,3-bis(3-aminophenoxy)benzene

[0248] 3,3'-DAPM: 3,3'-diamino-diphenylmethane

[0249] DTBAB: 1,4-bis(4-aminophenoxy)-2,5-di-tert-butylbenzene

[0250] BAPP: 2,2-bis[4-(4-aminophenoxy)phenyl]propane

[0251] APAB: 4-aminophenyl-4'-aminobenzoate

[0252] Bisaniline-M: 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene

[0253] Dianiline-P: 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene (manufactured by Mitsui Fine Chemicals Co., Ltd., trade name: Dianiline-P)

[0254] AABOZ: 6-amino-2-(4-aminophenoxy)benzoxazole

[0255] DTAm: A mixture of 2,6-diamino-3,5-diethyltoluene and 2,4-diamino-3,5-diethyltoluene (manufactured by Ihara Chemical Industry Co., Ltd., trade name: Hardcure 10, amine value: 629 KOHmg / g)

[0256] BAPM: bis(4-amino-3-ethyl-5-methylphenyl)methane (manufactured by Ihara Chemical Industry, trade name: Curehard MED)

[0257] DMAc: N,N-dimethylacetamide

[0258] (Synthesis Example A-1)

[0259] Under nitrogen flow, 1.335 g of m-TB (0.0063 mol) and 10.414 g of TPE-R (0.0356 mol) and DMAc in an amount of 12 wt% solid content concentration after polymerization were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 0.932 g of PMDA (0.0043 mol) and 11.319 g of BPDA (0.0385 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-1. The solution viscosity of polyamic acid solution A-1 was 1,420 cps.

[0260] Next, after the polyamic acid solution A-1 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-1 (thermoplastic, Tg: 256°C, moisture absorption rate: 0.36 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-1 was 26.4 wt %.

[0261] (Synthesis Example A-2)

[0262] Under nitrogen flow, 0.451 g of m-TB (0.0021 mole) and 11.794 g of TPE-R (0.0403 mole) and DMAc in an amount of 12% by weight of solid content after polymerization were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 2.834 g of PMDA (0.0130 mole) and 8.921 g of BPDA (0.0303 mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-2. The solution viscosity of polyamic acid solution A-2 was 1,510 cps.

[0263] Next, after the polyamic acid solution A-2 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-2 (thermoplastic, Tg: 242°C, moisture absorption rate: 0.35 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-2 was 26.5 wt %.

[0264] (Synthesis Example A-3)

[0265] Under nitrogen flow, 0.908 g of m-TB (0.0043 mole) and 11.253 g of TPE-R (0.0385 mole) and DMAc in an amount of 12% by weight of solid content after polymerization were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 2.855 g of PMDA (0.0131 mole) and 8.985 g of BPDA (0.0305 mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-3. The solution viscosity of polyamic acid solution A-3 was 1,550 cps.

[0266] Next, after the polyamic acid solution A-3 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-3 (thermoplastic, Tg: 240°C, moisture absorption rate: 0.31 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-3 was 26.9 wt %.

[0267] (Synthesis Example A-4)

[0268] Under nitrogen flow, 1.372 g of m-TB (0.0065 mol) and 10.704 g of TPE-R (0.0366 mol) and DMAc in an amount of 12 wt% solid content concentration after polymerization were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 2.875 g of PMDA (0.0132 mol) and 9.049 g of BPDA (0.0308 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-4. The solution viscosity of polyamic acid solution A-4 was 1,580 cps.

[0269] Next, after the polyamic acid solution A-4 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-4 (thermoplastic, Tg: 240°C, moisture absorption rate: 0.29 wt%). In addition, the imide group concentration of the polyimide constituting the polyimide film A-4 was 27.1 wt%.

[0270] (Synthesis Example A-5)

[0271] Under nitrogen flow, 1.842 g of m-TB (0.0087 mol) and 10.147 g of TPE-R (0.0347 mol) and DMAc in an amount of 12 wt% solid content concentration after polymerization were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 2.896 g of PMDA (0.0133 mol) and 9.115 g of BPDA (0.0310 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-5. The solution viscosity of polyamic acid solution A-5 was 1,610 cps.

[0272] Next, after the polyamic acid solution A-5 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-5 (thermoplastic, Tg: 244°C, moisture absorption rate: 0.27 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-5 was 27.4 wt %.

[0273] (Synthesis Example A-6)

[0274] Under nitrogen flow, 2.804 g of m-TB (0.0132 mol) and 9.009 g of TPE-R (0.0308 mol) and DMAc in an amount of 12 wt% solid content concentration after polymerization were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 2.938 g of PMDA (0.0135 mol) and 9.249 g of BPDA (0.0314 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-6. The solution viscosity of polyamic acid solution A-6 was 1,720 cps.

[0275] Next, after the polyamic acid solution A-6 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-6 (thermoplastic, Tg: 248°C, moisture absorption rate: 0.27 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-6 was 27.8 wt %.

[0276] (Synthesis Example A-7)

[0277] Under nitrogen flow, 1.469 g of APAB (0.0064 mol) and 10.658 g of TPE-R (0.0365 mol) and DMAc in an amount such that the solid content concentration after polymerization becomes 12% by weight were added to a 300 ml split flask, stirred and dissolved at room temperature. Next, after adding 2.863 g of PMDA (0.0131 mol) and 9.011 g of BPDA (0.0306 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-7. The solution viscosity of polyamic acid solution A-7 is 1,280 cps.

[0278] Next, after the polyamic acid solution A-7 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-7 (thermoplastic, Tg: 239°C, moisture absorption rate: 0.31 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-7 was 27.0 wt %.

[0279] (Synthesis Example A-8)

[0280] Under nitrogen flow, 1.372 g of m-TB (0.0065 mol) and 10.704 g of APB (0.0366 mol) and DMAc in an amount such that the solid content concentration after polymerization becomes 12 wt% were added to a 300 ml separable flask, and stirred and dissolved at room temperature. Next, after adding 2.875 g of PMDA (0.0132 mol) and 9.049 g of BPDA (0.0308 mol), stirring was continued for 3 hours at room temperature to carry out polymerization reaction, and polyamic acid solution A-8 was obtained. The solution viscosity of polyamic acid solution A-8 was 1,190 cps.

[0281] Next, after the polyamic acid solution A-8 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-8 (thermoplasticity, Tg: 235°C, moisture absorption rate: 0.31 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-8 was 27.1 wt %.

[0282] (Synthesis Example A-9)

[0283] Under nitrogen flow, 1.162 g of m-TB (0.0055 mol) and 12.735 g of BAPP (0.0310 mol) and DMAc in an amount such that the solid content concentration after polymerization becomes 12% by weight were added to a 300 ml separable flask, and stirred and dissolved at room temperature. Next, after adding 2.436 g of PMDA (0.0112 mol) and 7.667 g of BPDA (0.0261 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-9. The solution viscosity of polyamic acid solution A-9 was 1,780 cps.

[0284] Next, after the polyamic acid solution A-9 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-9 (thermoplasticity, Tg: 278°C, moisture absorption rate: 0.34 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-9 was 22.6 wt %.

[0285] (Synthesis Example A-10)

[0286] Under nitrogen flow, 1.411 g of m-TB (0.0066 mol) and 11.011 g of TPE-R (0.0377 mol) and DMAc in an amount of 12 wt% solid content concentration after polymerization were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 4.929 g of PMDA (0.0226 mol) and 6.649 g of BPDA (0.0226 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-10. The solution viscosity of polyamic acid solution A-10 was 2,330 cps.

[0287] Next, after the polyamic acid solution A-10 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-10 (thermoplasticity, Tg: 276°C, moisture absorption rate: 0.41 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-10 was 28.0 wt %.

[0288] (Synthesis Example A-11)

[0289] Under nitrogen flow, 12.327 parts by weight of TPE-R (0.0422 mol) and DMAc in an amount such that the solid content concentration after polymerization becomes 12% by weight were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 2.815 g of PMDA (0.0129 mol) and 8.858 g of BPDA (0.0301 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-11. The solution viscosity of polyamic acid solution A-11 was 1,530 cps.

[0290] Next, after the polyamic acid solution A-11 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-11 (thermoplasticity, Tg: 244°C, moisture absorption rate: 0.39 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-11 was 26.5 wt %.

[0291] (Synthesis Example A-12)

[0292] Under nitrogen flow, 12.128 g of m-TB (0.0571 mol) and 1.856 g of TPE-R (0.0063 mol) and DMAc in an amount of 15 wt% solid content concentration after polymerization were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 6.819 g of PMDA (0.0313 mol) and 9.198 g of BPDA (0.0313 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-12. The solution viscosity of polyamic acid solution A-12 was 29,100 cps.

[0293] Next, after the polyamic acid solution A-12 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-12 (non-thermoplastic, Tg: 322°C, moisture absorption rate: 0.57 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-12 was 31.8 wt %.

[0294] (Synthesis Example A-13)

[0295] Under nitrogen flow, 13.707 g of m-TB (0.0646 mole) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 6.936 g of PMDA (0.0318 mole) and 9.356 g of BPDA (0.0318 mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-13. The solution viscosity of polyamic acid solution A-13 was 29,900 cps.

[0296] Next, after the polyamic acid solution A-13 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-13 (non-thermoplastic, Tg: 332°C, moisture absorption rate: 0.63 wt%). In addition, the imide group concentration of the polyimide constituting the polyimide film A-13 was 32.4 wt%.

[0297] (Synthesis Example A-14)

[0298] Under nitrogen flow, 12.061 g of m-TB (0.0568 mol), 0.923 g of TPE-Q (0.0032 mol), 1.0874 g of dianiline-M (0.0032 mol), and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a 300 ml separable flask, and stirred and dissolved at room temperature. Next, after adding 6.781 g of PMDA (0.0311 mol) and 9.147 g of BPDA (0.0311 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-14. The solution viscosity of polyamic acid solution A-14 was 29,800 cps.

[0299] Next, after the polyamic acid solution A-14 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-14 (non-thermoplastic, Tg: 322°C, moisture absorption rate: 0.61 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-14 was 31.6 wt %.

[0300] (Synthesis Example A-15)

[0301] Under nitrogen flow, 11.978 g of m-TB (0.0564 mol), 0.916 g of TPE-Q (0.0031 mol), 1.287 g of BAPP (0.0031 mol), and DMAc in an amount such that the solid content concentration after polymerization becomes 15 wt % were added to a 300 ml separable flask, and stirred and dissolved at room temperature. Next, after adding 6.735 g of PMDA (0.0309 mol) and 9.084 g of BPDA (0.0309 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-15. The solution viscosity of polyamic acid solution A-15 was 29,200 cps.

[0302] Next, after the polyamic acid solution A-15 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete the imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-15 (non-thermoplastic, Tg: 324°C, moisture absorption rate: 0.58 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-15 was 31.4 wt %.

[0303] (Synthesis Example A-16)

[0304] Under nitrogen flow, 12.128 g of m-TB (0.0571 mole) and 1.856 g of TPE-Q (0.0063 mole) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 6.819 g of PMDA (0.0313 mole) and 9.198 g of BPDA (0.0313 mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-16. The solution viscosity of polyamic acid solution A-16 was 32,800 cps.

[0305] Next, after the polyamic acid solution A-16 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-16 (non-thermoplastic, Tg: 330°C, moisture absorption rate: 0.59 wt%). In addition, the imide group concentration of the polyimide constituting the polyimide film A-16 was 31.8 wt%.

[0306] (Synthesis Example A-17)

[0307] Under nitrogen flow, 12.323 g of m-TB (0.0580 mol) and 1.886 g of TPE-R (0.0064 mol) and DMAc in an amount of 15 wt% solid content concentration after polymerization were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 8.314 g of PMDA (0.0381 mol) and 7.477 g of BPDA (0.0254 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-17. The solution viscosity of polyamic acid solution A-17 was 31,500 cps.

[0308] Next, after the polyamic acid solution A-17 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-17 (non-thermoplastic, Tg: 342°C, moisture absorption rate: 0.56 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-17 was 32.3 wt %.

[0309] (Synthesis Example A-18)

[0310] Under nitrogen flow, 13.434 g of m-TB (0.0633 mol) and DMAc in an amount of 15 wt% solid content concentration after polymerization were added to a 300 ml split flask, stirred and dissolved at room temperature. Next, after adding 6.118 g of PMDA (0.0281 mol), 9.170 g of BPDA (0.0312 mol) and 1.279 g of TMEG (0.0031 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-18. The solution viscosity of polyamic acid solution A-18 was 14,100 cps.

[0311] Next, after the polyamic acid solution A-18 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-18 (non-thermoplastic, Tg: 314°C, moisture absorption rate: 0.59 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-18 was 31.7 wt %.

[0312] (Synthesis Example A-19)

[0313] Under nitrogen flow, 12.003 g of m-TB (0.0565 mol) and 1.836 g of TPE-R (0.0063 mol) and DMAc in an amount such that the solid content concentration after polymerization becomes 15 wt % were added to a 300 ml separable flask, and stirred and dissolved at room temperature. Next, after adding 5.399 g of PMDA (0.0248 mol), 9.103 g of BPDA (0.0309 mol) and 1.659 g of NTCDA (0.0062 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-19. The solution viscosity of polyamic acid solution A-19 was 31,200 cps.

[0314] Next, after the polyamic acid solution A-19 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-19 (non-thermoplastic, Tg: 311°C, moisture absorption rate: 0.58 wt%). In addition, the imide group concentration of the polyimide constituting the polyimide film A-19 was 31.4 wt%.

[0315] (Synthesis Example A-20)

[0316] Under nitrogen flow, 8.778g of m-TB (0.0414 mol), 1.860g of TPE-R (0.0064 mol) and 3.582g of AABOZ (0.0159 mol) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to a 300ml separable flask, stirred and dissolved at room temperature. Next, after adding 8.309g of PMDA (0.0381 mol) and 7.472g of BPDA (0.0254 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-20. The solution viscosity of polyamic acid solution A-20 was 42,300cps.

[0317] Next, after the polyamic acid solution A-20 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-20 (non-thermoplastic, Tg: 312°C, moisture absorption rate: 0.61 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-20 was 32.1 wt %.

[0318] (Synthesis Example A-21)

[0319] Under nitrogen flow, 5.365 g of m-TB (0.0253 mol), 1.847 g of TPE-R (0.0063 mol), 7.116 g of AABOZ (0.0316 mol), and DMAc in an amount of 15 wt % solid content concentration after polymerization were added to a 300 ml split flask, stirred and dissolved at room temperature. Next, after adding 8.252 g of PMDA (0.0378 mol) and 7.421 g of BPDA (0.0252 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-21. The solution viscosity of polyamic acid solution A-21 was 22,700 cps.

[0320] Next, after the polyamic acid solution A-21 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-21 (non-thermoplastic, Tg: 320°C, moisture absorption rate: 0.65 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-21 was 31.9 wt %.

[0321] (Synthesis Example A-22)

[0322] Under nitrogen flow, 8.110 g of m-TB (0.0382 mol), 1.861 g of TPE-R (0.0064 mol), 4.360 g of APAB (0.0191 mol), and DMAc in an amount such that the solid content concentration after polymerization becomes 15 wt % were added to a 300 ml split flask, and stirred and dissolved at room temperature. Next, after adding 8.250 g of PMDA (0.0378 mol) and 7.419 g of BPDA (0.0252 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-22. The solution viscosity of polyamic acid solution A-22 is 24,500 cps.

[0323] Next, after the polyamic acid solution A-22 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-22 (non-thermoplastic, Tg: 322°C, moisture absorption rate: 0.57 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-22 was 32.0 wt %.

[0324] (Synthesis Example A-23)

[0325] Under nitrogen flow, 11.755 g of m-TB (0.0554 mole) and 1.799 g of TPE-R (0.0062 mole) and DMAc in an amount of 15% by weight of solid content after polymerization were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 3.966 g of PMDA (0.0182 mole) and 12.481 g of BPDA (0.0424 mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-23. The solution viscosity of polyamic acid solution A-23 was 26,800 cps.

[0326] Next, after the polyamic acid solution A-23 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-23 (non-thermoplastic, Tg: 291°C, moisture absorption rate: 0.59 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-23 was 30.7 wt %.

[0327] (Synthesis Example A-24)

[0328] Under nitrogen flow, 14.405 g of m-TB (0.0679 mol) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to a 300 ml separable flask, stirred and dissolved at room temperature. Next, after adding 11.663 g of PMDA (0.0535 mol) and 3.933 g of BPDA (0.0134 mol), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution A-24. The solution viscosity of polyamic acid solution A-24 was 33,600 cps.

[0329] Next, after the polyamic acid solution A-24 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-24 (non-thermoplastic, Tg: 400°C or above, moisture absorption rate: 0.78 wt%). In addition, the imide group concentration of the polyimide constituting the polyimide film A-24 was 34.2 wt%.

[0330] (Synthesis Example A-25)

[0331] Under nitrogen flow, 12.201 g of m-TB (0.0575 mol) and 1.042 g of dianiline-M (0.0030 mol) and DMAc in an amount such that the solid content concentration after polymerization becomes 15 wt % were added to a 300 ml separable flask, and stirred and dissolved at room temperature. Next, after adding 7.991 g of NTCDA (0.0298 mol) and 8.766 g of BPDA (0.0298 mol), stirring was continued for 3 hours at room temperature to carry out polymerization reaction, thereby obtaining polyamic acid solution A-25. The solution viscosity of polyamic acid solution A-25 is 30,100 cps.

[0332] Next, after the polyamic acid solution A-25 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-25 (non-thermoplastic, Tg: above 400°C, moisture absorption rate: 0.57 wt%). In addition, the imide group concentration of the polyimide constituting the polyimide film A-25 was 30.2 wt%.

[0333] (Synthesis Example A-26)

[0334] Under nitrogen flow, 11.204 g of m-TB (0.0528 mol) and 0.670 g of BAPP (0.0016 mol) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a 300 ml separable flask, and stirred and dissolved at room temperature. Next, after adding 5.845 g of PMDA (0.0268 mol) and 12.281 g of TAHQ (0.0268 mol), stirring was continued for 3 hours at room temperature to carry out polymerization reaction, and polyamic acid solution A-26 was obtained. The solution viscosity of polyamic acid solution A-26 was 26,600 cps.

[0335] Next, after the polyamic acid solution A-26 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film A-26 (non-thermoplastic, Tg: 304°C, moisture absorption rate: 0.49 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film A-26 was 26.9 wt %.

[0336] [Example A-1]

[0337] After the polyamic acid solution A-1 is evenly applied to a single surface of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 0.6 μm) in a manner that the thickness after curing becomes about 2 μm to 3 μm, the mixture is heated and dried at 120°C and the solvent is removed. Secondly, the polyamic acid solution A-15 is evenly applied thereon in a manner that the thickness after curing becomes about 21 μm, and the mixture is heated and dried at 120°C and the solvent is removed. Furthermore, after the polyamic acid solution A-1 is evenly applied thereon in a manner that the thickness after curing becomes about 2 μm to 3 μm, the mixture is heated and dried at 120°C and the solvent is removed. In this way, after three polyamic acid layers are formed, a staged heat treatment is performed from 120°C to 360°C within 30 minutes to complete imidization. The copper foil of the obtained metal sheet laminate was etched away using an aqueous solution of ferric chloride to prepare a multilayer polyimide film A-1 (CTE: 22 ppm / K, moisture absorption: 0.54 wt%, dielectric constant: 3.58, dielectric tangent: 0.0031).

[0338] [Example A-2 to Example A-21, Reference Example A-1 to Reference Example A-2]

[0339] Except for using the polyamic acid solutions shown in Tables 1 to 4, multilayer polyimide films A-2 to A-23 of Examples A-2 to A-21 and Reference Examples A-1 to A-2 were obtained in the same manner as in Example A-1. The CTE, moisture absorption rate, dielectric constant, and dielectric tangent of the obtained multilayer polyimide films A-2 to A-23 were determined. The measurement results are shown in Tables 1 to 4.

[0340] [Table 1]

[0341]

[0342] [Table 2]

[0343]

[0344] [Table 3]

[0345]

[0346] [Table 4]

[0347]

[0348] [Example A-22 to Example A-23]

[0349] Multilayer polyimide films A-24 and A-25 of Examples A-22 and A-23 were obtained in the same manner as in Example A-1 except that the polyamic acid solution shown in Table 5 was used. The CTE, moisture absorption rate, dielectric constant, and dielectric tangent of the obtained multilayer polyimide films A-24 and A-25 were determined. The measurement results are shown in Table 5.

[0350] [Table 5]

[0351]

[0352] (Synthesis Example B-1)

[0353] Under nitrogen flow, 66.727 parts by weight of m-TB (0.314 molar parts) and 520.681 parts by weight of TPE-R (1.781 molar parts) and DMAc in an amount of 12% by weight of solid content after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 46.620 parts by weight of PMDA (0.214 molar parts) and 565.972 parts by weight of BPDA (1.924 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-1. The solution viscosity of polyamic acid solution B-1 was 1,420 cps.

[0354] Next, after the polyamic acid solution B-1 is uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing becomes about 25 μm, it is dried by heating at 120°C and the solvent is removed. Furthermore, a stepwise heat treatment is performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil is etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-1 (thermoplastic, Tg: 256°C, moisture absorption rate: 0.36 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-1 is 26.4 wt %.

[0355] (Synthesis Example B-2)

[0356] Under nitrogen flow, 22.538 parts by weight of m-TB (0.106 molar parts) and 589.682 parts by weight of TPE-R (2.017 molar parts) and DMAc in an amount of 12% by weight of solid content after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 141.722 parts by weight of PMDA (0.650 molar parts) and 446.058 parts by weight of BPDA (1.516 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-2. The solution viscosity of polyamic acid solution B-2 was 1,510 cps.

[0357] Next, after the polyamic acid solution B-2 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-2 (thermoplastic, Tg: 242°C, moisture absorption rate: 0.35 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-2 was 26.5 wt %.

[0358] (Synthesis Example B-3)

[0359] Under nitrogen flow, 45.398 parts by weight of m-TB (0.214 molar parts) and 562.630 parts by weight of TPE-R (1.925 molar parts) and DMAc in an amount of 12% by weight of solid content after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 142.733 parts by weight of PMDA (0.654 molar parts) and 449.239 parts by weight of BPDA (1.527 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-3. The solution viscosity of polyamic acid solution B-3 was 1,550 cps.

[0360] Next, after the polyamic acid solution B-3 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-3 (thermoplastic, Tg: 240°C, moisture absorption rate: 0.31 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-3 was 26.9 wt %.

[0361] (Synthesis Example B-4)

[0362] Under nitrogen flow, 68.586 parts by weight of m-TB (0.323 molar parts) and 535.190 parts by weight of TPE-R (1.831 molar parts) and DMAc in an amount of 12% by weight of solid content concentration after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 143.758 parts by weight of PMDA (0.659 molar parts) and 452.466 parts by weight of BPDA (1.538 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to obtain polyamic acid solution B-4. The solution viscosity of polyamic acid solution B-4 was 1,580 cps.

[0363] Next, after the polyamic acid solution B-4 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-4 (thermoplastic, Tg: 240°C, moisture absorption rate: 0.29 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-4 was 27.1 wt %.

[0364] (Synthesis Example B-5)

[0365] Under nitrogen flow, 92.110 parts by weight of m-TB (0.434 molar parts) and 507.352 parts by weight of TPE-R (1.736 molar parts) and DMAc in an amount of 12% by weight of solid content concentration after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 144.798 parts by weight of PMDA (0.664 molar parts) and 455.740 parts by weight of BPDA (1.549 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to obtain polyamic acid solution B-5. The solution viscosity of polyamic acid solution B-5 was 1,610 cps.

[0366] Next, after the polyamic acid solution B-5 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-5 (thermoplasticity, Tg: 244°C, moisture absorption rate: 0.27 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-5 was 27.4 wt %.

[0367] (Synthesis Example B-6)

[0368] Under nitrogen flow, 140.193 parts by weight of m-TB (0.660 molar parts) and 450.451 parts by weight of TPE-R (1.541 molar parts) and DMAc in an amount of 12% by weight of solid content after polymerization were added to a reaction tank, stirred and dissolved at room temperature. Next, after adding 146.924 parts by weight of PMDA (0.674 molar parts) and 462.431 parts by weight of BPDA (1.572 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-6. The solution viscosity of polyamic acid solution B-6 was 1,720 cps.

[0369] Next, after the polyamic acid solution B-6 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-6 (thermoplasticity, Tg: 248°C, moisture absorption rate: 0.27 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-6 was 27.8 wt %.

[0370] (Synthesis Example B-7)

[0371] Under nitrogen flow, 73.427 parts by weight of APAB (0.322 parts by mole) and 532.900 parts by weight of TPE-R (1.823 parts by mole) and DMAc in an amount such that the solid content concentration after polymerization becomes 12% by weight were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 143.143 parts by weight of PMDA (0.656 parts by mole) and 450.530 parts by weight of BPDA (1.531 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-7. The solution viscosity of polyamic acid solution B-7 is 1,280 cps.

[0372] Next, after the polyamic acid solution B-7 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-7 (thermoplasticity, Tg: 239°C, moisture absorption rate: 0.31 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-7 was 27.0 wt %.

[0373] (Synthesis Example B-8)

[0374] Under nitrogen flow, 68.586 parts by weight of m-TB (0.323 molar parts) and 535.190 parts by weight of APB (1.831 molar parts) and DMAc in an amount such that the solid content concentration after polymerization becomes 12% by weight were added to the reaction tank, and stirred and dissolved at room temperature. Next, after adding 143.758 parts by weight of PMDA (0.659 molar parts) and 452.466 parts by weight of BPDA (1.538 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-8. The solution viscosity of polyamic acid solution B-8 was 1,190 cps.

[0375] Next, after the polyamic acid solution B-8 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-8 (thermoplasticity, Tg: 235°C, moisture absorption rate: 0.31 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-8 was 27.1 wt %.

[0376] (Synthesis Example B-9)

[0377] Under nitrogen flow, 58.109 parts by weight of m-TB (0.274 molar parts) and 636.745 parts by weight of BAPP (1.551 molar parts) and DMAc in an amount such that the solid content concentration after polymerization becomes 12% by weight were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 121.798 parts by weight of PMDA (0.558 molar parts) and 383.348 parts by weight of BPDA (1.303 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-9. The solution viscosity of polyamic acid solution B-9 was 1,780 cps.

[0378] Next, after the polyamic acid solution B-9 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-9 (thermoplasticity, Tg: 278°C, moisture absorption rate: 0.34 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-9 was 22.6 wt %.

[0379] (Synthesis Example B-10)

[0380] Under nitrogen flow, 70.552 parts by weight of m-TB (0.332 molar parts) and 550.530 parts by weight of TPE-R (1.883 molar parts) and DMAc in an amount such that the solid content concentration after polymerization becomes 12% by weight were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 246.465 parts by weight of PMDA (1.130 molar parts) and 332.454 parts by weight of BPDA (1.130 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-10. The solution viscosity of polyamic acid solution B-10 was 2,330 cps.

[0381] Next, after the polyamic acid solution B-10 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-10 (thermoplasticity, Tg: 276°C, moisture absorption rate: 0.41 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-10 was 28.0 wt %.

[0382] (Synthesis Example B-11)

[0383] Under nitrogen flow, 616.353 parts by weight of TPE-R (2.108 parts by mole) and DMAc in an amount such that the solid content concentration after polymerization becomes 12% by weight were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 140.726 parts by weight of PMDA (0.645 parts by mole) and 442.921 parts by weight of BPDA (1.505 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-11. The solution viscosity of polyamic acid solution B-11 was 1,530 cps.

[0384] Next, after the polyamic acid solution B-11 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-11 (thermoplasticity, Tg: 244°C, moisture absorption rate: 0.39 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-11 was 26.5 wt %.

[0385] (Synthesis Example B-12)

[0386] Under nitrogen flow, 240.725 parts by weight of m-TB (1.134 molar parts) and 331.485 parts by weight of TPE-R (1.134 molar parts) and DMAc in an amount such that the solid content concentration after polymerization becomes 12% by weight were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 151.369 parts by weight of PMDA (0.694 molar parts) and 476.421 parts by weight of BPDA (1.619 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-12. The solution viscosity of polyamic acid solution B-12 was 3,240 cps.

[0387] Next, after the polyamic acid solution B-12 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-12 (thermoplasticity, Tg: 260°C, moisture absorption rate: 0.28 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-12 was 28.7 wt %.

[0388] (Synthesis Example B-13)

[0389] Under nitrogen flow, 596.920 parts by weight of m-TB (2.812 parts by mole) and 91.331 parts by weight of TPE-R (0.312 parts by mole) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 268.495 parts by weight of PMDA (1.231 parts by mole) and 543.255 parts by weight of BPDA (1.846 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-13. The solution viscosity of polyamic acid solution B-13 was 27,310 cps.

[0390] Next, after the polyamic acid solution B-13 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete the imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-13 (non-thermoplastic, Tg: 305°C, moisture absorption rate: 0.52 wt%). In addition, the imide group concentration of the polyimide constituting the polyimide film B-13 was 31.2 wt%.

[0391] (Synthesis Example B-14)

[0392] Under nitrogen flow, 606.387 parts by weight of m-TB (2.856 molar parts) and 92.779 parts by weight of TPE-R (0.317 molar parts) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 340.941 parts by weight of PMDA (1.563 molar parts) and 459.892 parts by weight of BPDA (1.563 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to obtain polyamic acid solution B-14. The solution viscosity of polyamic acid solution B-14 was 29,100 cps.

[0393] Next, after the polyamic acid solution B-14 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-14 (non-thermoplastic, Tg: 322°C, moisture absorption rate: 0.57 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-14 was 31.8 wt %.

[0394] (Synthesis Example B-15)

[0395] Under nitrogen flow, 685.370 parts by weight of m-TB (3.228 parts by mole) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to a reaction tank, stirred and dissolved at room temperature. Next, after adding 346.815 parts by weight of PMDA (1.590 parts by mole) and 467.815 parts by weight of BPDA (1.590 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-15. The solution viscosity of polyamic acid solution B-15 was 29,900 cps.

[0396] Next, after the polyamic acid solution B-15 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-15 (non-thermoplastic, Tg: 332°C, moisture absorption rate: 0.63 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-15 was 32.4 wt %.

[0397] (Synthesis Example B-16)

[0398] Under nitrogen flow, 603.059 parts by weight of m-TB (2.841 molar parts), 46.135 parts by weight of TPE-Q (0.158 molar parts), 54.368 parts by weight of dianiline-M (0.158 molar parts), and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to the reaction tank, and stirred and dissolved at room temperature. Next, after adding 339.070 parts by weight of PMDA (1.555 molar parts) and 457.368 parts by weight of BPDA (1.555 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to obtain polyamic acid solution B-16. The solution viscosity of polyamic acid solution B-16 is 29,800 cps.

[0399] Next, after the polyamic acid solution B-16 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-16 (non-thermoplastic, Tg: 322°C, moisture absorption rate: 0.61 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-16 was 31.6 wt %.

[0400] (Synthesis Example B-17)

[0401] Under nitrogen flow, 598.899 parts by weight of m-TB (2.821 parts by mole), 45.817 parts by weight of TPE-Q (0.157 parts by mole), 64.339 parts by weight of BAPP (0.157 parts by mole), and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to the reaction tank, and stirred and dissolved at room temperature. Next, after adding 336.731 parts by weight of PMDA (1.544 parts by mole) and 454.214 parts by weight of BPDA (1.544 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-17. The solution viscosity of polyamic acid solution B-17 was 29,200 cps.

[0402] Next, after the polyamic acid solution B-17 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-17 (non-thermoplastic, Tg: 324°C, moisture absorption rate: 0.58 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-17 was 31.4 wt %.

[0403] (Synthesis Example B-18)

[0404] Under nitrogen flow, 606.387 parts by weight of m-TB (2.856 molar parts) and 92.779 parts by weight of TPE-Q (0.317 molar parts) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 340.941 parts by weight of PMDA (1.563 molar parts) and 459.892 parts by weight of BPDA (1.563 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to obtain polyamic acid solution B-18. The solution viscosity of polyamic acid solution B-18 was 32,800 cps.

[0405] Next, after the polyamic acid solution B-18 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-18 (non-thermoplastic, Tg: 330°C, moisture absorption rate: 0.59 wt%). In addition, the imide group concentration of the polyimide constituting the polyimide film B-18 was 31.8 wt%.

[0406] (Synthesis Example B-19)

[0407] Under nitrogen flow, 616.159 parts by weight of m-TB (2.902 molar parts) and 94.275 parts by weight of TPE-R (0.322 molar parts) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 415.723 parts by weight of PMDA (1.906 molar parts) and 373.843 parts by weight of BPDA (1.271 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to obtain polyamic acid solution B-19. The solution viscosity of polyamic acid solution B-19 was 31,500 cps.

[0408] Next, after the polyamic acid solution B-19 is uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing becomes about 25 μm, it is dried by heating at 120°C and the solvent is removed. Furthermore, a stepwise heat treatment is performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil is etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-19 (non-thermoplastic, Tg: 342°C, moisture absorption rate: 0.56 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-19 is 32.3 wt %.

[0409] (Synthesis Example B-20)

[0410] Under nitrogen flow, 626.252 parts by weight of m-TB (2.950 parts by mole) and 95.819 parts by weight of TPE-R (0.328 parts by mole) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 492.954 parts by weight of PMDA (2.260 parts by mole) and 284.975 parts by weight of BPDA (0.969 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-20. The solution viscosity of polyamic acid solution B-20 was 34,100 cps.

[0411] Next, after the polyamic acid solution B-20 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-20 (non-thermoplastic, Tg: 364°C, moisture absorption rate: 0.68 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-20 was 32.9 wt %.

[0412] (Synthesis Example B-21)

[0413] Under nitrogen flow, 517.831 parts by weight of m-TB (2.439 parts by mole) and 79.230 parts by weight of TPE-R (0.271 parts by mole) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 291.151 parts by weight of PMDA (1.335 parts by mole) and 611.788 parts by weight of TAHQ (1.335 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-21. The solution viscosity of polyamic acid solution B-21 was 33,200 cps.

[0414] Next, after the polyamic acid solution B-21 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-21 (non-thermoplastic, Tg: 296°C, moisture absorption rate: 0.54 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-21 was 26.8 wt %.

[0415] (Synthesis Example B-22)

[0416] Under nitrogen flow, 587.744 parts by weight of m-TB (2.769 parts by mole) and 89.927 parts by weight of TPE-R (0.308 parts by mole) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 198.275 parts by weight of PMDA (0.909 parts by mole) and 624.054 parts by weight of BPDA (2.121 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-22. The solution viscosity of polyamic acid solution B-22 was 26,800 cps.

[0417] Next, after the polyamic acid solution B-22 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-22 (non-thermoplastic, Tg: 291°C, moisture absorption rate: 0.59 wt %). In addition, the imide group concentration of the polyimide constituting the polyimide film B-22 was 30.7 wt %.

[0418] (Synthesis Example B-23)

[0419] Under nitrogen flow, 456.183 parts by weight of m-TB (2.149 parts by mole) and 269.219 parts by weight of TPE-R (0.921 parts by mole) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 329.772 parts by weight of PMDA (1.512 parts by mole) and 444.826 parts by weight of BPDA (1.512 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-23. The solution viscosity of polyamic acid solution B-23 was 26,400 cps.

[0420] Next, after the polyamic acid solution B-23 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing became about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-23 (non-thermoplastic, Tg: 285°C, moisture absorption rate: 0.53 wt%). In addition, the imide group concentration of the polyimide constituting the polyimide film B-23 was 30.7 wt%.

[0421] (Synthesis Example B-24)

[0422] Under nitrogen flow, 720.230 parts by weight of m-TB (3.393 parts by mole) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to a reaction tank, stirred and dissolved at room temperature. Next, after adding 583.127 parts by weight of PMDA (2.673 parts by mole) and 196.644 parts by weight of BPDA (0.668 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to obtain polyamic acid solution B-24. The solution viscosity of polyamic acid solution B-24 was 33,600 cps.

[0423] Next, after the polyamic acid solution B-24 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 2.1 μm) in such a manner that the thickness after curing was about 25 μm, it was dried by heating at 120°C and the solvent was removed. Furthermore, a stepwise heat treatment was performed from 120°C to 360°C within 30 minutes to complete imidization. For the obtained metal sheet laminate, the copper foil was etched away using an aqueous solution of ferric chloride to prepare a polyimide film B-24 (non-thermoplastic, Tg: 400°C or above, moisture absorption rate: 0.78% by weight). In addition, the imide group concentration of the polyimide constituting the polyimide film B-24 was 34.2% by weight.

[0424] [Example B-1]

[0425] Using a multi-manifold 3-layer co-extrusion multilayer die, a three-layer structure in the order of polyamic acid solution B-2 / polyamic acid solution B-18 / polyamic acid solution B-2 is continuously extruded and coated on a stainless steel support substrate in an endless belt shape, and heated and dried for 3 minutes at 130°C and the solvent is removed. Thereafter, a staged heat treatment is performed from 130°C to 360°C to complete imidization, and a polyimide film B-1' having a thickness of 2.0 μm / 21 μm / 2.0 μm is prepared for the preparation of a thermoplastic polyimide layer / non-thermoplastic polyimide layer / thermoplastic polyimide layer. The polyimide film B-1' on the support substrate is peeled off by a knife edge method, and a long strip polyimide film B-1 having a length of 1100 mm in the width direction is prepared.

[0426] The evaluation results of the long polyimide film B-1 are as follows.

[0427] CTE: 19ppm / K

[0428] In-plane retardation (RO): 9nm

[0429] Deviation (ΔRO) of in-plane retardation (RO) in the width direction (TD direction): 2nm

[0430] At a temperature of 320°C and a pressure of 340 MPa / m 2 , Change in in-plane retardation (RO) before and after pressurization for 15 minutes: 13nm

[0431] Moisture absorption rate: 0.56% by weight

[0432] Dielectric constant (10GHz): 3.56, dielectric tangent (10GHz): 0.0032

[0433] [Example B-2 to Example B-18, Reference Example B-1 to Reference Example B-5]

[0434] Except for using the polyamic acid solutions shown in Tables 6 to 9, the long strip polyimide films B-2 to B-23 of Examples B-2 to B-18 and Reference Examples B-1 to B-5 were obtained in the same manner as in Example B-1. The CTE, in-plane retardation (RO), deviation (ΔRO) of in-plane retardation (RO) in the width direction (TD direction) of the obtained long strip polyimide films B-2 to B-23 were determined. 2 , the change in in-plane retardation (RO) before and after pressurization during a holding period of 15 minutes, and the moisture absorption rate. The measurement results are shown in Tables 6 to 9.

[0435] [Table 6]

[0436]

[0437] [Table 7]

[0438]

[0439] [Table 8]

[0440]

[0441] [Table 9]

[0442]

[0443] [Example B-19]

[0444] The polyamic acid solution B-2 was uniformly applied to the surface of a long copper foil (rolled copper foil, manufactured by JX Metal Co., Ltd., trade name: GHY5-93F-HA-V2 foil, thickness: 12 μm, tensile elastic modulus after heat treatment: 18 GPa) in a manner that the thickness after hardening becomes 2.0 μm, and heated and dried at 120°C for 1 minute to remove the solvent. After the polyamic acid solution B-18 was uniformly applied thereon in a manner that the thickness after hardening becomes 21 μm, it was heated and dried at 120°C for 3 minutes to remove the solvent. Furthermore, after the polyamic acid solution B-2 was uniformly applied thereon in a manner that the thickness after hardening becomes 2.0 μm, it was heated and dried at 120°C for 1 minute to remove the solvent. Thereafter, a staged heat treatment was performed from 130°C to 360°C to complete imidization, and a single-sided copper sheet laminate B-1 was prepared. A copper foil was stacked on the polyimide layer side of the single-sided copper sheet laminate B-1 and heated at a temperature of 320° C. and a pressure of 340 MPa / m 2 The double-sided copper sheet laminate B-1 was prepared by thermal pressing for 15 minutes under the conditions of .

[0445] Casting side peel strength: ◎, Pressed side peel strength: ○

[0446] [Example B-20 to Example B-36, Reference Example B-6 to Reference Example B-10]

[0447] Except for using the polyamic acid solutions shown in Tables 10 to 13, the double-sided copper sheet laminates B-2 to B-23 of Examples B-20 to B-36 and Reference Examples B-6 to B-10 were obtained in the same manner as in Example B-19. The peel strength on the cast surface side and the peel strength on the pressure-bonded surface side of the obtained double-sided copper sheet laminates B-2 to B-23 were determined. The measurement results are shown in Tables 10 to 13.

[0448] [Table 10]

[0449]

[0450] [Table 11]

[0451]

[0452] [Table 12]

[0453]

[0454] [Table 13]

[0455]

[0456] (Synthesis Example C-1)

[0457] Under nitrogen flow, 606.387 parts by weight of m-TB (2.856 molar parts) and 92.779 parts by weight of TPE-R (0.317 molar parts) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 340.941 parts by weight of PMDA (1.563 molar parts) and 459.892 parts by weight of BPDA (1.563 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to prepare polyamic acid solution C-1. The solution viscosity of polyamic acid solution C-1 was 29,100 cps.

[0458] (Synthesis Example C-2)

[0459] Under nitrogen flow, 606.387 parts by weight of m-TB (2.856 molar parts) and 92.779 parts by weight of TPE-Q (0.317 molar parts) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 340.941 parts by weight of PMDA (1.563 molar parts) and 459.892 parts by weight of BPDA (1.563 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to prepare polyamic acid solution C-2. The solution viscosity of polyamic acid solution C-2 was 32,800 cps.

[0460] (Synthesis Example C-3)

[0461] Under nitrogen flow, 616.159 parts by weight of m-TB (2.902 parts by mole) and 94.275 parts by weight of TPE-R (0.322 parts by mole) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to a reaction tank, stirred and dissolved at room temperature. Next, after adding 415.723 parts by weight of PMDA (1.906 parts by mole) and 373.843 parts by weight of BPDA (1.271 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to prepare polyamic acid solution C-3. The solution viscosity of polyamic acid solution C-3 was 31,500 cps.

[0462] (Synthesis Example C-4)

[0463] Under nitrogen flow, 637.503 parts by weight of m-TB (3.003 molar parts) and 64.882 parts by weight of BAPP (0.158 molar parts) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 339.571 parts by weight of PMDA (1.557 molar parts) and 458.044 parts by weight of BPDA (1.557 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to prepare polyamic acid solution C-4. The solution viscosity of polyamic acid solution C-4 was 24,100 cps.

[0464] (Synthesis Example C-5)

[0465] Under nitrogen flow, 591.594 parts by weight of m-TB (2.787 molar parts) and 127.109 parts by weight of BAPP (0.310 molar parts) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 332.624 parts by weight of PMDA (1.525 molar parts) and 448.673 parts by weight of BPDA (1.525 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to prepare polyamic acid solution C-5. The solution viscosity of polyamic acid solution C-5 was 23,200 cps.

[0466] (Synthesis Example C-6)

[0467] Under nitrogen flow, 641.968 parts by weight of m-TB (3.024 molar parts) and 54.830 parts by weight of dianiline-M (0.159 molar parts) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to a reaction tank, stirred and dissolved at room temperature. Next, after adding 341.950 parts by weight of PMDA (1.568 molar parts) and 461.252 parts by weight of BPDA (1.568 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to prepare polyamic acid solution C-6. The solution viscosity of polyamic acid solution C-6 was 26,500 cps.

[0468] (Synthesis Example C-7)

[0469] Under nitrogen flow, 538.432 parts by weight of m-TB (2.536 parts by mole) and 185.359 parts by weight of TPE-R (0.634 parts by mole) and DMAc in an amount of 15% by weight of solid content after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 408.690 parts by weight of PMDA (1.874 parts by mole) and 367.519 parts by weight of BPDA (1.249 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to prepare polyamic acid solution C-7. The solution viscosity of polyamic acid solution C-7 was 31,100 cps.

[0470] (Synthesis Example C-8)

[0471] Under nitrogen flow, 674.489 parts by weight of m-TB (3.177 parts by mole) and DMAc in an amount of 15% by weight of solid content concentration after polymerization were added to a reaction tank, stirred and dissolved at room temperature. Next, after adding 273.047 parts by weight of PMDA (1.252 parts by mole) and 552.465 parts by weight of BPDA (1.878 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to prepare polyamic acid solution C-8. The solution viscosity of polyamic acid solution C-8 was 26,400 cps.

[0472] (Synthesis Example C-9)

[0473] Under nitrogen flow, 463.290 parts by weight of m-TB (2.182 molar parts) and 273.414 parts by weight of TPE-R (0.935 molar parts) and DMAc in an amount of 15% by weight of solid content after polymerization were added to a reaction tank, stirred and dissolved at room temperature. Next, after adding 401.891 parts by weight of PMDA (1.843 molar parts) and 361.405 parts by weight of BPDA (1.228 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to prepare polyamic acid solution C-9. The solution viscosity of polyamic acid solution C-9 was 29,000 cps.

[0474] (Synthesis Example C-10)

[0475] Under nitrogen flow, 589.033 parts by weight of m-TB (2.775 parts by mole) and 111.762 parts by weight of APAB (0.490 parts by mole) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, stirred and dissolved at room temperature. Next, after adding 420.798 parts by weight of PMDA (1.929 parts by mole) and 378.407 parts by weight of BPDA (1.286 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to prepare polyamic acid solution C-10. The solution viscosity of polyamic acid solution C-10 was 22,700 cps.

[0476] (Synthesis Example C-11)

[0477] Under nitrogen flow, 500.546 parts by weight of m-TB (2.358 parts by mole) and 229.756 parts by weight of TPE-R (0.786 parts by mole) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 405.262 parts by weight of PMDA (1.858 parts by mole) and 364.436 parts by weight of BPDA (1.239 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to prepare polyamic acid solution C-11. The solution viscosity of polyamic acid solution C-11 was 29,600 cps.

[0478] (Synthesis Example C-12)

[0479] Under nitrogen flow, 779.571 parts by weight of BAPP (1.899 parts by mole) and DMAc in an amount such that the solid content concentration after polymerization becomes 12% by weight were added to the reaction tank, stirred and dissolved at room temperature. Next, 420.430 parts by weight of PMDA (1.928 parts by mole) were added, and the mixture was stirred for 3 hours at room temperature to carry out polymerization reaction, thereby preparing polyamic acid solution C-12. The solution viscosity of polyamic acid solution C-12 was 2,210 cps.

[0480] (Synthesis Example C-13)

[0481] Under nitrogen flow, 616.159 parts by weight of m-TB (2.902 parts by mole) and 94.275 parts by weight of APB (0.322 parts by mole) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred and dissolved at room temperature. Next, after adding 415.723 parts by weight of PMDA (1.906 parts by mole) and 373.843 parts by weight of BPDA (1.271 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to prepare polyamic acid solution C-13. The solution viscosity of polyamic acid solution C-13 was 12,700 cps.

[0482] (Synthesis Example C-14)

[0483] Under nitrogen flow, 628.877 parts by weight of m-TB (2.962 parts by mole) and 65.261 parts by weight of 3,3'-DAPM (0.329 parts by mole) and DMAc in an amount of 15% by weight of solid content after polymerization were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 424.303 parts by weight of PMDA (1.945 parts by mole) and 381.559 parts by weight of BPDA (1.297 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to prepare polyamic acid solution C-14. The solution viscosity of polyamic acid solution C-14 was 31,400 cps.

[0484] (Synthesis Example C-15)

[0485] Under nitrogen flow, 613.786 parts by weight of m-TB (2.891 molar parts), 28.652 parts by weight of DTAm (0.161 molar parts), 46.956 parts by weight of TPE-Q (0.161 molar parts), and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred and dissolved at room temperature. Next, after adding 345.102 parts by weight of PMDA (1.582 molar parts) and 465.504 parts by weight of BPDA (1.582 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to prepare polyamic acid solution C-15. The solution viscosity of polyamic acid solution C-15 was 24,400 cps.

[0486] (Synthesis Example C-16)

[0487] Under nitrogen flow, 607.034 parts by weight of m-TB (2.859 molar parts), 44.840 parts by weight of BAPM (0.159 molar parts), and 46.439 parts by weight of TPE-Q (0.159 molar parts) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred and dissolved at room temperature. Next, after adding 341.305 parts by weight of PMDA (1.565 molar parts) and 460.383 parts by weight of BPDA (1.565 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to prepare polyamic acid solution C-16. The solution viscosity of polyamic acid solution C-16 was 27,100 cps.

[0488] (Synthesis Example C-17)

[0489] Under nitrogen flow, 603.059 parts by weight of m-TB (2.841 molar parts), 54.368 parts by weight of dianiline-P (0.158 molar parts), 46.135 parts by weight of TPE-Q (0.158 molar parts), and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred and dissolved at room temperature. Next, after adding 339.070 parts by weight of PMDA (1.555 molar parts) and 457.368 parts by weight of BPDA (1.555 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to prepare polyamic acid solution C-17. The solution viscosity of polyamic acid solution C-17 was 29,200 cps.

[0490] (Synthesis Example C-18)

[0491] Under nitrogen flow, 599.272 parts by weight of m-TB (2.823 molar parts), 63.445 parts by weight of DTBAB (0.157 molar parts), 45.845 parts by weight of TPE-Q (0.157 molar parts), and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred and dissolved at room temperature. Next, after adding 336.941 parts by weight of PMDA (1.545 molar parts) and 454.497 parts by weight of BPDA (1.545 molar parts), stirring was continued for 3 hours at room temperature and polymerization reaction was carried out to prepare polyamic acid solution C-18. The solution viscosity of polyamic acid solution C-18 was 28,800 cps.

[0492] (Synthesis Example C-19)

[0493] Under nitrogen flow, 610.050 parts by weight of m-TB (2.874 parts by mole) and 52.104 parts by weight of dianiline-M (0.151 parts by mole) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred and dissolved at room temperature. Next, after adding 399.526 parts by weight of NTCDA (1.490 parts by mole) and 438.320 parts by weight of BPDA (1.490 parts by mole), stirring was continued for 3 hours at room temperature to carry out polymerization reaction, thereby preparing polyamic acid solution C-19. The solution viscosity of polyamic acid solution C-19 was 29,200 cps.

[0494] (Synthesis Example C-20)

[0495] Under nitrogen flow, 560.190 parts by weight of m-TB (2.639 parts by mole) and 33.503 parts by weight of BAPP (0.082 parts by mole) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to the reaction tank, stirred and dissolved at room temperature. Next, after adding 292.237 parts by weight of PMDA (1.340 parts by mole) and 614.071 parts by weight of TAHQ (1.340 parts by mole), stirring was continued for 3 hours at room temperature and polymerization reaction was performed to prepare polyamic acid solution C-20. The solution viscosity of polyamic acid solution C-20 was 26,100 cps.

[0496] [Example C-1]

[0497] After the polyamic acid solution C-1 is uniformly applied to a single surface of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 0.6 μm) in a manner that the thickness after curing becomes about 25 μm, it is heated and dried at 120°C to remove the solvent. Furthermore, a stepwise heat treatment is performed from 120°C to 360°C within 30 minutes to complete the imidization. The copper foil is etched away using an aqueous solution of ferric chloride to prepare a polyimide film C-1 (CTE: 18.1 ppm / K, Tg: 322°C, moisture absorption: 0.57 wt%, haze: 74.5%, film elongation: 48%, dielectric constant: 3.42, dielectric tangent: 0.0028).

[0498] [Example C-2 to Example C-9 and Reference Example C-1 to Reference Example C-2]

[0499] Polyimide films C-2 to C-11 were prepared in the same manner as Example C-1 except that the polyamic acid solutions shown in Tables 14 and 15 were used. CTE, Tg, moisture absorption, haze, film elongation, dielectric constant, and dielectric tangent were determined for polyimide films C-2 to C-11. These measurement results are shown in Tables 14 and 15.

[0500] [Table 14]

[0501]

[0502] [Table 15]

[0503]

[0504] [Example C-10]

[0505] Except for using polyamic acid solution C-11 and performing a step-by-step heat treatment from 120°C to 360°C for 5 hours, polyimide film C-12 (CTE: 10.2 ppm / K, Tg: 307°C, moisture absorption: 0.61 wt%, haze: 74.2%, film elongation: 41%) was prepared in the same manner as Example C-1.

[0506] [Example C-11]

[0507] After the polyamic acid solution C-15 was uniformly applied to one side of an electrolytic copper foil having a thickness of 12 μm (surface roughness Rz: 0.6 μm) in such a manner that the thickness after curing was about 2 μm to 3 μm, the foil was dried by heating at 120°C to remove the solvent. Next, the polyamic acid solution C-1 was uniformly applied thereon in such a manner that the thickness after curing was about 21 μm, the foil was dried by heating at 120°C to remove the solvent. Furthermore, the polyamic acid solution C-15 was uniformly applied thereon in such a manner that the thickness after curing was about 2 μm to 3 μm, the foil was dried by heating at 120°C to remove the solvent. Thus, after forming three polyamic acid layers, a stepwise heat treatment was performed from 120°C to 360°C for 30 minutes to complete imidization, thereby preparing a metal sheet laminate C-11. No adverse conditions such as expansion of the polyimide layer in the metal sheet laminate C-11 were confirmed.

[0508] [Example C-12 to Example C-17]

[0509] Metal sheet laminates C-12 to C-17 were prepared in the same manner as Example C-11 except that polyamic acid solutions C-2 to C-7 were used instead of polyamic acid solution C-1. In any of the metal sheet laminates C-12 to C-17, no defect such as expansion of the polyimide layer was observed.

[0510] (Reference Example C-3)

[0511] A metal sheet laminate was prepared in the same manner as in Example C-11 except that a stepwise heat treatment was performed from 120° C. to 360° C. for 15 minutes. However, expansion was observed in the polyimide layer.

[0512] [Example C-18 to Example C-20]

[0513] Metal sheet laminates C-18 to C-20 were prepared in the same manner as in Example C-11, except that polyamic acid solutions C-4 to C-6 were used instead of polyamic acid solution C-1 in Example C-11 and heat treatment was performed stepwise from 120° C. to 360° C. for 15 minutes. In any of the metal sheet laminates C-18 to C-20, no defect such as expansion of the polyimide layer was observed.

[0514] (Reference Example C-4 to Reference Example C-6)

[0515] Metal sheet laminates were prepared in the same manner as in Example C-11 except that polyamic acid solution C-2, polyamic acid solution C-3, and polyamic acid solution C-7 were used instead of polyamic acid solution C-1 in Example C-11 and heat treatment was performed stepwise from 120°C to 360°C for 15 minutes. However, expansion was confirmed in the polyimide layer in any of the metal sheet laminates.

[0516] [Example C-21 to Example C-26]

[0517] Polyimide films C-13 to C-18 were prepared in the same manner as in Example C-1 except that the polyamic acid solutions shown in Table 16 were used. CTE, Tg, dielectric constant, and dielectric tangent were determined for polyimide films C-13 to C-18. These measurement results are shown in Table 16.

[0518] [Table 16]

[0519]

[0520] [Example C-27 to Example C-30]

[0521] Metal sheet laminates C-27 to C-30 were prepared in the same manner as in Example C-11 except that polyamic acid solutions C-15 to C-18 were used instead of polyamic acid solution C-1 in Example C-11 and heat treatment was performed stepwise from 120° C. to 360° C. for 15 minutes. In any of the metal sheet laminates C-27 to C-30, no defect such as expansion of the polyimide layer was observed.

[0522] (Reference Example C-7 to Reference Example C-8)

[0523] Metal sheet laminates were prepared in the same manner as in Example C-11 except that polyamic acid solution C-13 and polyamic acid solution C-14 were used instead of polyamic acid solution C-1 in Example C-11 and heat treatment was performed stepwise from 120°C to 360°C for 15 minutes. However, expansion was confirmed in the polyimide layer in all the metal sheet laminates.

[0524] [Example C-31 to Example C-32]

[0525] Polyimide films C-19 and C-20 were prepared in the same manner as in Example C-1 except that the polyamic acid solutions shown in Table 17 were used. CTE, Tg, dielectric constant, and dielectric tangent were determined for the polyimide films C-19 and C-20. These measurement results are shown in Table 17.

[0526] [Table 17]

[0527]

[0528] As mentioned above, although the embodiment of the present invention was described in detail for the purpose of illustration, the present invention is not limited to the above-described embodiment, and various modifications can be made.

Claims

1. A polyimide film, comprising a thermoplastic polyimide layer comprising a thermoplastic polyimide on at least one side of a non-thermoplastic polyimide layer comprising a non-thermoplastic polyimide, wherein the polyimide film is characterized in that the following conditions ai to a-iv are satisfied: Condition ai: The residue of the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer consists of an aromatic tetracarboxylic acid residue and an aromatic diamine residue, and With respect to 100 parts by mole of the aromatic tetracarboxylic acid residue, a tetracarboxylic acid residue derived from 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA, i.e., a BPDA residue, and a tetracarboxylic acid residue derived from 1,4-phenylenebis(trimellitic acid monoester) dianhydride TAHQ, i.e., a TAHQ residue, and a tetracarboxylic acid residue derived from pyromellitic dianhydride PMDA, i.e., a PMDA residue, and a tetracarboxylic acid residue derived from 2,3,6,7-naphthalenetetracarboxylic dianhydride NTCDA, i.e., a NTCDA residue, in total of 80 parts by mole or more, The molar ratio of at least one of the BPDA residue and the TAHQ residue to at least one of the PMDA residue and the NTCDA residue {(BPDA residue+TAHQ residue) / (PMDA residue+NTCDA residue)} is in the range of 0.6 to 1.3; Condition a-ii: The thermoplastic polyimide constituting the thermoplastic polyimide layer is an aromatic tetracarboxylic acid residue and an aromatic diamine residue, and With respect to 100 parts by mole of the aromatic diamine residue, The diamine residue derived from at least one diamine compound selected from the diamine compounds represented by the following general formula (B1) to (B7) is 70 mol parts or more, and the diamine residue derived from the diamine compound represented by the following general formula (A1) is in the range of 1 mol part to 30 mol parts; Condition a-iii: the thermal expansion coefficient is within the range of 10 ppm / K to 30 ppm / K; Condition a-iv: Dielectric tangent Df at 10 GHz is less than 0.004, In formula (B1) to formula (B7), R1 independently represents a monovalent hydrocarbon group or alkoxy group having 1 to 6 carbon atoms, the linking group A independently represents a divalent group selected from -O-, -S-, -CO-, -SO-, -SO2-, -COO-, -CH2-, -C(CH3)2-, -NH- or -CONH-, and n1 independently represents an integer of 0 to 4; wherein, From formula (B3), remove those that repeat with formula (B2); from formula (B5), remove those that repeat with formula (B4); In formula (A1), the linking group X represents a single bond or -COO-, Y independently represents hydrogen, a monovalent hydrocarbon group having 1 to 3 carbon atoms, or an alkoxy group, n represents an integer of 0 to 2, and p and q independently represent an integer of 0 to 4.

2. The polyimide film according to claim 1, characterized in that The diamine residue derived from the diamine compound represented by the general formula (A1) is 80 mol parts or more per 100 mol parts of the aromatic diamine residue in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer.

3. The polyimide film according to claim 1, wherein the diamine residue derived from at least one diamine compound selected from the diamine compounds represented by the general formula (B1) to the general formula (B7) is in the range of 70 mol parts to 99 mol parts, relative to 100 mol parts of the aromatic diamine residue in the thermoplastic polyimide constituting the thermoplastic polyimide layer.

4. A polyimide film having a thermoplastic polyimide layer containing a thermoplastic polyimide on at least one side of a non-thermoplastic polyimide layer containing a non-thermoplastic polyimide, wherein the polyimide film is characterized by satisfying the following conditions bi to b-iv: Condition bi: The thermal expansion coefficient is within the range of 10ppm / K to 30ppm / K; Condition b-ii: The residue of the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer consists of an aromatic tetracarboxylic acid residue and an aromatic diamine residue, and With respect to 100 parts by mole of the aromatic tetracarboxylic acid residue, The tetracarboxylic acid residue derived from at least one tetracarboxylic acid dianhydride selected from 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA and 1,4-phenylenebis(trimellitic acid monoester) dianhydride TAHQ is within a range of 30 mol parts to 60 mol parts, The tetracarboxylic acid residue derived from pyromellitic dianhydride PMDA is in the range of 40 mol parts or more and 70 mol parts or less; Condition b-iii: relative to 100 parts by mole of the aromatic diamine residue in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer, The diamine residue derived from the diamine compound represented by the following general formula (A1) is 80 mol parts or more; Condition b-iv: The thermoplastic polyimide constituting the thermoplastic polyimide layer comprises an aromatic tetracarboxylic acid residue and an aromatic diamine residue, and relative to 100 parts by mole of the aromatic diamine residue, The diamine residue derived from at least one diamine compound selected from the diamine compounds represented by the following general formula (B1) to (B7) is within a range of 70 parts by mole or more and 99 parts by mole or less, The diamine residue derived from the diamine compound represented by the following general formula (A1) is within a range of 1 mol part or more and 30 mol parts or less, In formula (A1), the linking group X represents a single bond or -COO-, Y independently represents hydrogen, a monovalent hydrocarbon group having 1 to 3 carbon atoms, or an alkoxy group, n represents an integer of 0 to 2, and p and q independently represent an integer of 0 to 4. In formula (B1) to formula (B7), R1 independently represents a monovalent hydrocarbon group or alkoxy group having 1 to 6 carbon atoms, the linking group A independently represents a divalent group selected from -O-, -S-, -CO-, -SO-, -SO2-, -COO-, -CH2-, -C(CH3)2-, -NH- or -CONH-, and n1 independently represents an integer of 0 to 4; wherein, From formula (B3), those that are repeated in formula (B2) are removed, and from formula (B5), those that are repeated in formula (B4) are removed.

5. The polyimide film according to claim 1 or 4, characterized in that: The imide group concentration of the non-thermoplastic polyimide and the thermoplastic polyimide is 33 wt % or less.

6. A polyimide film having at least one non-thermoplastic polyimide layer, wherein the polyimide film is characterized by satisfying the following conditions ci to c-iii: Condition ci: The residue of the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer consists of an aromatic tetracarboxylic acid residue and an aromatic diamine residue, and The present invention relates to 100 parts by mole of the aromatic tetracarboxylic acid residue, wherein the tetracarboxylic acid residue derived from at least one of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride and 1,4-phenylenebis(trimellitic acid monoester) dianhydride is contained in an amount of 30 to 60 parts by mole, and the tetracarboxylic acid residue derived from at least one of pyromellitic acid dianhydride and 2,3,6,7-naphthalenetetracarboxylic acid dianhydride is contained in an amount of 40 to 70 parts by mole, The present invention comprises 70 mol parts or more of diamine residues derived from a diamine compound represented by the following general formula (A1) relative to 100 mol parts of the aromatic diamine residues, and 2 mol parts to 15 mol parts of diamine residues derived from diamine compounds represented by the following general formulas (C1) to (C4); Condition c-ii: glass transition temperature is above 300°C; Condition c-iii: Dielectric tangent Df at 10 GHz is less than 0.004, In formula (A1), the linking group X represents a single bond or -COO-, Y independently represents hydrogen, a monovalent hydrocarbon group having 1 to 3 carbon atoms, or an alkoxy group, n represents an integer of 1 or 2, and p and q independently represent an integer of 0 to 4. In formula (C1) to formula (C4), R2 independently represents a monovalent hydrocarbon group, an alkoxy group or an alkylthio group having 1 to 6 carbon atoms, the linking group A' independently represents a divalent group selected from -O-, -SO2-, -CH2- or -C(CH3)2-, and the linking group X1 independently represents -CH2-, -O-CH2-O-, -O-C2H4-O-, -O-C3H6-O-, -O-C4H8-O-, -O-C5H 10 -O-, -O-CH2-C(CH3)2-CH2-O-, -C(CH3)2-, -C(CF3)2- or -SO2-, n3 independently represents an integer from 1 to 4, and n4 independently represents an integer from 0 to 4, but in formula (C3), when the linking group A' does not contain -CH2-, -C(CH3)2-, -C(CF3)2- or -SO2-, any one of n4 is 1 or more.

7. A copper sheet laminate comprising an insulating layer and copper foil on at least one side of the insulating layer, wherein: The insulating layer includes the polyimide film according to any one of claims 1 , 4 or 6 .

8. A circuit board obtained by processing the copper foil of the copper sheet laminate according to claim 7 into wiring.

Citation Information

Patent Citations

  • Metal plated laminate

    JP2004358961A

  • Method for manufacturing functional plastic lens

    JP2016191786A

  • Image formation apparatus, control method and program of the same

    JP2016191787A

  • Polyimide, resin film, and metal-clad laminate

    CN105339416A

  • polyimide composite sheet

    JP1993271438A