A method for regulating the oxygen content of sintered NdFeB
By using MgO powder to regulate the oxygen content in the preparation process of the rare earth permanent magnet NdFeB, the problem of large fluctuations in the oxygen content in the existing technology is solved, the flexible regulation of the oxygen content and the improvement of the magnet performance are achieved, ensuring the high quality of the product. Consistency and coercivity.
Patent Information
- Application Number
- CN202210210146.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-04
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-03-04
AI Technical Summary
It is difficult to effectively control the oxygen content of rare earth permanent magnets NdFeB with existing technology, resulting in large fluctuations in the oxygen supply effect and affecting the performance consistency of the product.
MgO powder is used as the oxygen content regulator. During the vacuum smelting and sintering process, the grain boundary oxygen content of the magnet is controlled through the diffusion of Mg element. The excess Mg element is volatilized through the vacuum system to ensure flexible regulation of the oxygen content within the range of 1000-2000ppm. .
It achieves flexible regulation of the oxygen content of the rare earth permanent magnet NdFeB, improves the coercivity and performance consistency of the magnet, avoids excessive introduction of impurity elements, and improves the controllability of the preparation process.
Smart Images

Figure CN114724832B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnet preparation, and in particular to a method for preparing sintered NdFeB by regulating the oxygen content. Background Art
[0002] Rare earth permanent magnet NdFeB is the most powerful permanent magnet so far, and is widely used in air conditioners, automobiles, motors and other fields. The preparation process of sintered NdFeB magnets involves a powder metallurgy process, and rare earth elements are easily oxidized. Therefore, the higher oxygen content in the finished sintered NdFeB magnets initially limits the magnet performance. With the advancement of process technology and equipment, the production control level of rare earth permanent magnet sintered NdFeB is getting higher and higher, and the oxygen content of the finished sintered NdFeB magnets has also been reduced from the initial 5000ppm to about 500ppm, which has promoted the continuous improvement of the magnetic energy product of sintered NdFeB. However, existing studies have shown that when there is an appropriate amount of oxygen in the grain boundary phase of the sintered NdFeB magnet, it can promote the transformation of the Nd-rich phase of the double hexagonal close-packed (dhcp) structure into the Nd-O phase of the cubic crystal structure of FCC or BCC. The Nd-O phase has good wettability with the main phase grains, which can improve the coercive force of the sintered NdFeB magnet without increasing the formulation cost. At present, the main oxygen supplementation process used in the industry is air flow mill oxygen supplementation, that is, a certain amount of oxygen is added during the air flow milling process to slightly passivate the powder and increase the oxygen content of the magnet appropriately. However, the crushing efficiency of coarse powder between batches and within batches of air flow mills is different, and gas oxygen supplementation will lead to different oxygen supplementation effects as the air flow mill efficiency changes. Under the same oxygen supply, when the air flow mill crushing efficiency is high, the average oxygen content is low, and when the crushing efficiency is low, the average oxygen content is high. Especially for the air flow mill process, the material needs to be discharged in batches, which results in a low oxygen content in the powder packaged first and a high oxygen content in the powder packaged later, affecting the performance consistency of the mass production of the product.
[0003] For example, the "High-performance sintered Nd-Fe-B material and its preparation method" disclosed in Chinese patent literature has a publication number of CN110739113A. In terms of mass percentage, the Nd-Fe-B material is composed of the following chemical components: PrNd: 29.5-31%, Ti: 0.05-1%, Zr: 0.05-0.15%, Al: 0.15-0.7%, Ga: 0.1-1%, Co: 0.05-2%, Cu: 0.08-1.5%, B: 0.8-1%, and the balance is Fe. The preparation method of the d-Fe-B material includes: raw material preparation, rapid solidification smelting, hydrogen crushing, air flow milling, orientation molding, sintering, and heat treatment. In the air flow milling stage, a certain concentration of oxygen is added to the inert gas. This method supplements oxygen in the air flow milling stage, and the oxygen supplementation effect fluctuates greatly, resulting in poor product consistency. Summary of the invention
[0004] In order to overcome the problems that it is difficult to control the oxygen content of rare earth permanent magnet NdFeB under the prior art, the oxygen supplementation effect fluctuates greatly, and the consistency of the product is poor, the present invention provides a method for controlling the oxygen content of sintered NdFeB, which can flexibly control the oxygen content of rare earth permanent magnet NdFeB, optimizes the performance of the magnet, and the consistency of the prepared magnet is good.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for regulating the oxygen content of sintered NdFeB comprises the following steps:
[0007] a. The NdFeB magnet raw material is vacuum melted and stripped to obtain NdFeB stripping sheets;
[0008] b. hydrogen-crushing the NdFeB strip to obtain a coarse powder after hydrogen-crushing;
[0009] c. Grind the coarse powder after hydrogen decomposition in a jet mill with an inert gas to obtain fine NdFeB powder;
[0010] d. Adding MgO powder and additives to the NdFeB fine powder, and mixing to obtain a mixed fine powder;
[0011] e. Orienting and isostatically pressing the mixed fine powder to obtain a NdFeB compact;
[0012] f. After vacuum sintering and tempering the NdFeB compact, NdFeB magnets are obtained.
[0013] The present invention adopts MgO as an oxygen content regulator. In the process of melting the O element into the Nd-rich phase, the Mg element diffuses to the surface of the magnet through the gaps and grain boundaries, and volatilizes in a high-temperature vacuum environment and is taken away by the vacuum system, thereby realizing the regulation of the grain boundary oxygen content of the magnet without introducing excessive other elements. The method is suitable for quick-setting sheets with different crushing properties, and for controlling the oxygen content between and within different batches of unified materials.
[0014] Preferably, in step a, the NdFeB magnet raw material comprises, by mass percentage, Pr-Nd: 31.5% to 32.5%; B: 0.92% to 0.98%; Al: 0.1% to 0.2%; Cu: 0.25 to 0.32%; Co: 0 to 0.5%; Ga: 0 to 0.5%; Zr: 0 to 0.15%; and the remainder is Fe.
[0015] Preferably, in step d, the amount of MgO powder added is 0.05-0.25% of the mass of the NdFeB fine powder.
[0016] The amount of oxygen added to the magnet is positively correlated with the amount of MgO powder added, and the final oxygen content of the magnet is related to the magnetic properties of the magnet. When the amount of MgO added is large, MgO is prone to agglomeration and thus affects the performance of the magnet. Therefore, when the amount of MgO powder added is 0.05-0.25% of the mass of the NdFeB fine powder, the magnetic properties of the prepared magnet are better.
[0017] Preferably, in step d, the average particle size of the MgO powder is 1 to 3 μm.
[0018] The particle size of MgO powder will affect the mixing uniformity of MgO and NdFeB fine powder, as well as the difficulty of removing Mg element during sintering. When there is a lot of residual Mg, the composite of Mg and Nd will reduce the magnetic properties of the magnet.
[0019] Preferably, in step d, the proportion of MgO powder with a particle size greater than 5 μm is no greater than 5%.
[0020] For a single MgO powder particle, when the particle size is large, the MgO particle will remain in the magnet after sintering, which will have a negative impact on the magnetic properties of the magnet.
[0021] Preferably, in the step b, the hydrogen pressure during hydrogen rupture is 0.01 to 0.09 MPa.
[0022] Preferably, the particle size of the NdFeB fine powder obtained in step c is 3 to 5 μm.
[0023] Preferably, in step d, the additive comprises one or more of zinc stearate, calcium stearate and polyethylene glycol octane, and the amount of the additive added is 0.03-0.05% of the mass of the NdFeB fine powder.
[0024] Preferably, in step f, the vacuum sintering temperature is not less than 1050°C, the sintering time is not less than 6 hours, and the vacuum degree is not less than 1×10 -3 Pa.
[0025] During sintering, the density of the NdFeB compact increases, and the Mg element in MgO leaves the magnet and evaporates into the vacuum environment. When the sintering temperature is low or the sintering time is short, the Mg element cannot be fully volatilized, and more Mg remains in the magnet.
[0026] Preferably, in step f, the tempering process is to subject the NdFeB magnet obtained by vacuum sintering to a primary heat treatment at 800-900° C. for 2-8 hours, and then to a secondary heat treatment at 400-600° C. for 2-8 hours.
[0027] Therefore, the present invention has the following beneficial effects: (1) the oxygen content of the rare earth permanent magnet NdFeB can be flexibly controlled within the range of 1000-2000 ppm; (2) the coercive force of the sintered NdFeB magnet is effectively improved without excessively increasing the second impurity element, thereby further optimizing the performance of the magnet; (3) the controllability of the preparation process is improved, thereby improving the consistency of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a cross-sectional SEM image of the sintered NdFeB magnet obtained in Example 1.
[0029] Figure 2 This is a cross-sectional SEM image of the sintered NdFeB magnet obtained in Comparative Example 3.
[0030] Figure 3 This is a cross-sectional SEM image of the sintered NdFeB magnet obtained in Comparative Example 4. DETAILED DESCRIPTION
[0031] The present invention is further described below in conjunction with the accompanying drawings and specific implementation methods.
[0032] Examples 1 to 7
[0033] A neodymium iron boron magnet, the preparation steps are as follows:
[0034] a. The raw materials of NdFeB magnets are composed of Pr-Nd: 32%; B: 0.92%; Al: 0.15%; Cu: 0.3%; Co: 0.5%; Ga: 0.5%; Zr: 0.15%; the balance is Fe. Put the raw materials into the crucible in descending order of melting point, and evacuate the furnace through the vacuum system until the vacuum degree reaches 10 -4 Pa, the dew point is lower than -55℃, and it is heated by the medium frequency induction coil. After the raw materials are completely melted, the heating power is adjusted to keep warm for 5 minutes, and then the crucible is rotated to make the molten liquid be transported to the cooling roller through the tundish for solidification and then fall onto the water cooling plate to cool down to obtain an alloy sheet with a thickness of 0.3mm±0.05mm, namely the NdFeB strip sheet;
[0035] b. Place the NdFeB strips in a reactor for hydrogen cracking treatment, evacuate the reactor and fill it with hydrogen until the hydrogen pressure reaches 0.03MPa to start the hydrogen absorption reaction. When the pressure change in the reactor does not exceed 0.5% within 10 minutes, a coarse powder after hydrogen cracking is obtained. Then, the reactor is heated to release the hydrogen adsorbed in the coarse powder after hydrogen cracking, and the hydrogen is extracted through a vacuum system;
[0036] c. Place the coarse powder after hydrogen crushing in a pure argon gas jet mill, drive the coarse powder to collide with each other through high-speed gas to crush, control the sorting wheel and cyclone separator of the jet mill to adjust the particle size of the powder, and optimize the particle size of the powder after jet milling through a powder multi-stage screening device, and finally obtain NdFeB fine powder with a particle size of 5μm;
[0037] d. Add MgO powder and zinc stearate to the NdFeB fine powder. The particle size and addition amount of MgO are shown in Table 1. The addition amount of zinc stearate is 0.05% of the mass of the NdFeB fine powder. Mix and obtain mixed fine powder.
[0038] e. The mixed fine powder is molded in an orientation magnetic field with an orientation magnetic field of 2.0T. The density of the green compact after orientation molding is 3.6-4.0g / cm 3 The green compact after orientation forming is then cold isostatically pressed to further eliminate the internal cracks of the green compact. The density of the green compact after cold isostatic pressing is >4.5g / cm 3 , obtaining a NdFeB compact;
[0039] f. Place the NdFeB compact in a sintering furnace and adjust the vacuum degree in the sintering furnace to 10 -3 The sintering temperature and sintering time are shown in Table 1. The sintered magnet is heat treated at 850°C for 5h, then at 500°C for 4h, and then cooled to room temperature to obtain a NdFeB magnet.
[0040] Comparative Example 1
[0041] A neodymium iron boron magnet, the preparation steps are as follows:
[0042] a. The raw materials of NdFeB magnets are composed of Pr-Nd: 32%; B: 0.92%; Al: 0.15%; Cu: 0.3%; Co: 0.5%; Ga: 0.5%; Zr: 0.15%; the balance is Fe. Put the raw materials into the crucible in descending order of melting point, and evacuate the furnace through the vacuum system until the vacuum degree reaches 10 -4 Pa, the dew point is lower than -55℃, and it is heated by the medium frequency induction coil. After the raw materials are completely melted, the heating power is adjusted to keep warm for 5 minutes, and then the crucible is rotated to make the molten liquid be transported to the cooling roller through the tundish for solidification and then fall onto the water cooling plate to cool down to obtain an alloy sheet with a thickness of 0.3mm±0.05mm, namely the NdFeB strip sheet;
[0043] b. Place the NdFeB strips in a reactor for hydrogen cracking treatment, evacuate the reactor and fill it with hydrogen until the hydrogen pressure reaches 0.03MPa to start the hydrogen absorption reaction. When the pressure change in the reactor does not exceed 0.5% within 10 minutes, a coarse powder after hydrogen cracking is obtained. Then, the reactor is heated to release the hydrogen adsorbed in the coarse powder after hydrogen cracking, and the hydrogen is extracted through a vacuum system;
[0044] c. Place the coarse powder after hydrogen crushing in a pure argon gas jet mill, drive the coarse powder to collide with each other through high-speed gas to crush, control the sorting wheel and cyclone separator of the jet mill to adjust the particle size of the powder, and optimize the particle size of the powder after jet milling through a powder multi-stage screening device, and finally obtain NdFeB fine powder with a particle size of 5μm;
[0045] d. The NdFeB fine powder is molded in an oriented magnetic field with an orientation magnetic field of 2.0T. After orientation molding, the density of the compact is 3.6-4.0g / cm 3 The green compact after orientation forming is then cold isostatically pressed to further eliminate the internal cracks of the green compact. The density of the green compact after cold isostatic pressing is >4.5g / cm 3 , obtaining a NdFeB compact;
[0046] e. Place the NdFeB compact in a sintering furnace and adjust the vacuum degree in the sintering furnace to 10 -3 The sintering temperature and sintering time are shown in Table 1. The sintered magnet is heat treated at 850°C for 5h, then at 500°C for 4h, and then cooled to room temperature to obtain a NdFeB magnet.
[0047] Comparative Example 2
[0048] A neodymium iron boron magnet, the preparation steps are as follows:
[0049] a. The raw materials of NdFeB magnets are composed of Pr-Nd: 32%; B: 0.92%; Al: 0.15%; Cu: 0.3%; Co: 0.5%; Ga: 0.5%; Zr: 0.15%; the balance is Fe. Put the raw materials into the crucible in descending order of melting point, and evacuate the furnace through the vacuum system until the vacuum degree reaches 10 -4 Pa, the dew point is lower than -55℃, and it is heated by the medium frequency induction coil. After the raw materials are completely melted, the heating power is adjusted to keep warm for 5 minutes, and then the crucible is rotated to make the molten liquid be transported to the cooling roller through the tundish for solidification and then fall onto the water cooling plate to cool down to obtain an alloy sheet with a thickness of 0.3mm±0.05mm, namely the NdFeB strip sheet;
[0050] b. Place the NdFeB strips in a reactor for hydrogen cracking treatment, evacuate the reactor and fill it with hydrogen until the hydrogen pressure reaches 0.03MPa to start the hydrogen absorption reaction. When the pressure change in the reactor does not exceed 0.5% within 10 minutes, a coarse powder after hydrogen cracking is obtained. Then, the reactor is heated to release the hydrogen adsorbed in the coarse powder after hydrogen cracking, and the hydrogen is extracted through a vacuum system;
[0051] c. Place the coarse powder after hydrogen crushing in an argon gas jet mill, mix 30ppm of oxygen into the grinding gas, drive the coarse powder to collide with each other through high-speed gas to crush, control the sorting wheel and cyclone separator of the jet mill to adjust the particle size of the powder, and optimize the powder particle size after jet milling through a powder multi-stage screening device, and finally obtain NdFeB fine powder with a particle size of 5μm;
[0052] d. Add MgO powder and zinc stearate to the NdFeB fine powder. The particle size and addition amount of MgO are shown in Table 1. The addition amount of zinc stearate is 0.05% of the mass of the NdFeB fine powder. Mix and obtain mixed fine powder.
[0053] e. The mixed fine powder is molded in an orientation magnetic field with an orientation magnetic field of 2.0T. The density of the green compact after orientation molding is 3.6-4.0g / cm 3 The green compact after orientation forming is then cold isostatically pressed to further eliminate the internal cracks of the green compact. The density of the green compact after cold isostatic pressing is >4.5g / cm 3 , obtaining a NdFeB compact;
[0054] f. Place the NdFeB compact in a sintering furnace and adjust the vacuum degree in the sintering furnace to 10 -3 The sintering temperature and sintering time are shown in Table 1. The sintered magnet is heat treated at 850°C for 5h, then at 500°C for 4h, and then cooled to room temperature to obtain a NdFeB magnet.
[0055] Comparative Examples 3 to 6
[0056] A neodymium iron boron magnet, the preparation steps are the same as those in the embodiment, wherein the particle size and addition amount of MgO in step d and the sintering temperature and sintering time in step f are as shown in Table 1.
[0057] Table 1. Preparation conditions of Examples 1 to 7 and Comparative Examples 1 to 6.
[0058]
[0059]
[0060] The magnetic properties and magnetic components of the magnets obtained in the above embodiments and comparative examples were tested. The testing process is as follows: the magnets obtained in the embodiments and comparative examples were taken, and samples of 10*10 mm in diameter were processed by wire cutting. The magnetic properties of the magnets were tested by NIM16000. Each group of tests was trial-produced 5 times, and 3 samples were taken each time to test the magnetic properties and calculate the average value; the magnets obtained in the embodiments and comparative examples were taken, and they were crushed and sampled in the center. The magnet components were detected by ICP-OES, and the oxygen content was tested by oxygen and nitrogen analyzer. The test results are shown in Table 2.
[0061] Table 2. Test results of Examples 1 to 7 and Comparative Examples 1 to 6.
[0062] project B / KG Br standard deviation / ± HkDJ Hcj standard deviation / ± Magnet Mg content / wt.% O content / ppm Example 1 14.01 0.07 17.5 0.2 Not detected 713 Example 2 13.99 0.09 17.8 0.1 0.003 978 Example 3 13.97 0.10 18.1 0.1 0.007 1498 Example 4 14.02 0.08 17.4 0.1 0.005 1313 Example 5 13.95 0.11 17.7 0.2 0.006 1285 Example 6 14.01 0.08 17.6 0.1 0.006 1269 Example 7 13.99 0.12 17.9 0.2 0.005 1332 Comparative Example 1 14.01 0.21 16.5 0.4 Not detected 532 Comparative Example 2 14.00 0.27 17.2 0.3 Not detected 1108 Comparative Example 3 13.65 0.50 15.7 0.7 0.012 2310 Comparative Example 4 13.36 0.23 16.7 0.5 0.005 1361 Comparative Example 5 13.87 0.57 14.1 1.1 0.09 1357 Comparative Example 6 13.85 0.36 15.5 0.6 0.031 1346
[0063] The cross section of the magnet prepared in Example 1 was observed using SEM. Figure 1 As shown, the grains in the magnet are evenly distributed and there are fewer voids. Examples 1 to 7 use MgO powder to regulate the oxygen content in the rare earth permanent magnet NdFeB. As can be seen from Table 2, compared with Comparative Example 1 which does not use the oxygen supplementation process, the oxygen content of the magnets prepared in Examples 1 to 7 is improved, the coercive force is significantly improved, and the volatility of the remanence and coercive force of Examples 1 to 7 is less than that of Comparative Example 1, and the final magnet has a lower MgO content. Comparative Example 2 uses air flow milling to supplement oxygen, and the magnet prepared therefrom has a large performance volatility, and its coercive force is also lower than that of Examples 1 to 7. This shows that the rare earth permanent magnet NdFeB prepared by the method for regulating the oxygen content of sintered NdFeB according to the present invention has good coercive force, good product uniformity, and less impurities are introduced.
[0064] The mass of MgO added in Example 1, Example 2, Example 6 and Example 3 increases successively, and the final MgO content also increases successively, which shows that the oxygen content in the magnet can be adjusted by the method of the present invention, but the coercive force does not increase with the increase of oxygen content. When the amount of MgO added is 2% of the mass of the NdFeB fine powder, the crystal structure of the magnet is better and the coercive force is large. When the oxygen content is too high, the remanence and coercive force are significantly reduced. For example, in Comparative Example 3, excessive MgO is added, and its magnetic properties are significantly worse than those of Example 6. The cross-section of the magnet obtained in Comparative Example 3 is observed using SEM, as shown in FIG. Figure 2 As shown, the oxides in the magnet agglomerate, affecting the remanence and coercive force.
[0065] The magnetic properties of Example 4 are better than those of Example 5, which indicates that when the amount of MgO added is certain, the smaller the average particle size of MgO is, the easier it is to remove from the magnet during sintering, and the better the effect of improving the coercive force of the magnet. The remanence and coercive force of Comparative Example 4 are both lower. The cross-section of the magnet obtained in Comparative Example 4 is observed using SEM, as shown in FIG. Figure 3As shown, there are reverse magnetization nucleation areas formed by the residual large MgO particles in the magnet, which causes the remanence and coercive force to decrease. This is because the particle size of the MgO particles added in Comparative Example 4 is too large and it is difficult to eliminate them by sintering.
[0066] The sintering temperature and sintering time of Comparative Examples 5 and 6 are not enough, resulting in that the Mg element cannot be fully volatilized during the sintering process. Excessive Mg is easy to form a soft magnetic phase with Nd, resulting in deterioration of magnetic properties.
Claims
1. A method for regulating the oxygen content of sintered NdFeB, characterized in that: The steps include: a. The NdFeB magnet raw material is vacuum melted and stripped to obtain NdFeB stripping sheets; b. hydrogen-crushing the NdFeB strip to obtain a coarse powder after hydrogen-crushing; c. Grind the coarse powder after hydrogen decomposition in a jet mill with an inert gas to obtain fine NdFeB powder; d. Adding MgO powder and additives to the NdFeB fine powder, and mixing to obtain a mixed fine powder; e. Orienting and isostatically pressing the mixed fine powder to obtain a NdFeB compact; f. After vacuum sintering and tempering the NdFeB compact, a NdFeB magnet is obtained. The vacuum sintering temperature is not less than 1050°C and the sintering time is not less than 6 hours; In the step d, the amount of MgO powder added is 0.05-0.25% of the mass of the NdFeB fine powder; and the average particle size of the MgO powder is 1-3 μm.
2. The method for controlling the oxygen content of sintered NdFeB according to claim 1, characterized in that: In the step a, the raw material of the NdFeB magnet comprises Pr-Nd in mass percentage: 31.5% to 32.5%; B: 0.92% ~ 0.98%; Al: 0.1% ~ 0.2%; Cu: 0.25 ~ 0.32%; Co: 0~0.5%; Ga: 0~0.5%; Zr: 0-0.15%; the balance is Fe.
3. The method for controlling the oxygen content of sintered NdFeB according to claim 1, characterized in that: In the step d, the proportion of MgO powder with a particle size greater than 5 μm is no greater than 5%.
4. The method for controlling the oxygen content of sintered NdFeB according to claim 1, characterized in that: In the step b, the hydrogen pressure during hydrogen rupture is 0.01-0.09 MPa.
5. The method for controlling the oxygen content of sintered NdFeB according to claim 1, characterized in that: The particle size of the NdFeB fine powder obtained in step c is 3-5 μm.
6. The method for controlling the oxygen content of sintered NdFeB according to claim 1, characterized in that: In the step d, the additive includes one or more of zinc stearate, calcium stearate and polyethylene glycol octane, and the amount of the additive added is 0.03-0.05% of the mass of the NdFeB fine powder.
7. The method for controlling the oxygen content of sintered NdFeB according to claim 1, characterized in that: In the step f, the vacuum degree of vacuum sintering is not less than 1×10 -3 Pa.
8. The method for controlling the oxygen content of sintered NdFeB according to claim 1, characterized in that: In the step f, the tempering process is to perform a primary heat treatment at 800-900° C. for 2-8 hours on the NdFeB magnet obtained by vacuum sintering, and then perform a secondary heat treatment at 400-600° C. for 2-8 hours.
Citation Information
Patent Citations
High-performance sintered Nd-Fe-B material and preparation method thereof
CN110739113A
Permanent magnetic RE material and preparation thereof
CN101364465A
Method for improving coercivity of sintered neodymium iron boron through compound addition of grain boundary phase
CN106252011A
Preparation method of sintered neodymium-iron-boron material
CN112466643A
Heat-resisting rare earth magnet and its manufacturing method