Method for producing semiconductor single-walled carbon nanotube dispersion

By using non-ionic polymers in aqueous media for centrifugal separation, the problems of complicated operations and low efficiency in separating semiconductor-type and metal-type single-walled carbon nanotubes in the existing technology are solved, and an efficient and simple separation method is realized. , improving the separability and manufacturing efficiency of semiconductor-type SWCNTs.

CN114728795BActive Publication Date: 2024-10-11KAO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080079242.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-15
Filing Date
2020-11-13
Publication Date
2024-10-11
Estimated Expiration
2040-11-13

AI Technical Summary

Technical Problem

The existing technology has the problems of complex operation, long time consumption, low separation efficiency and the need for expensive separating agents when separating semiconductor type and metal type single-walled carbon nanotubes.

Method used

Using a specific non-ionic polymer in an aqueous medium, semiconductor-type and metallic-type single-walled carbon nanotubes are separated by centrifugal separation. The affinity of the polymer to the aqueous medium and the interaction difference between SWCNTs are used to achieve selectivity. separation.

Benefits of technology

It achieves efficient and simple separation of semiconductor-type SWCNTs in aqueous media, improves separation performance and manufacturing efficiency, and reduces operating costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004717930830000031
    Figure FDA0004717930830000031
  • Figure GDA0003642914490000151
    Figure GDA0003642914490000151
  • Figure GDA0003642914490000271
    Figure GDA0003642914490000271
Patent Text Reader

Abstract

One embodiment of the present invention provides a method for producing a semiconducting single-layer carbon nanotube dispersion that can separate semiconducting single-layer carbon nanotubes from a single-layer carbon nanotube mixture containing semiconducting single-layer carbon nanotubes and metallic single-layer carbon nanotubes in an aqueous medium by using an easily available separation agent and a simple operation. One embodiment of the present invention relates to a method for producing a semiconducting single-layer carbon nanotube dispersion, comprising: step A, preparing a separated single-layer carbon nanotube dispersion containing single-layer carbon nanotubes containing semiconducting single-layer carbon nanotubes and metallic single-layer carbon nanotubes, an aqueous medium, and a nonionic polymer containing a structural unit A derived from a monomer represented by the following formula (1); and step B, after centrifuging the separated single-layer carbon nanotube dispersion, extracting a supernatant containing the semiconducting single-layer carbon nanotubes from the centrifuged separated single-layer carbon nanotube dispersion, wherein the content of the structural unit A in all the structural units of the polymer is 2 mol% or more, and the polymer is water-soluble. CH2=CR 1 -COO-(EO) p (PO) q -R 2 (1).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a semiconductor single-walled carbon nanotube dispersion, a method for producing semiconductor single-walled carbon nanotubes comprising the production method as a process, and a method for separating metallic single-walled carbon nanotubes from semiconductor single-walled carbon nanotubes. Background Art

[0002] In recent years, nano-sized carbon materials are expected to be applied to various fields due to their physical and chemical properties. As one of such materials, there is a carbon nanotube (hereinafter, sometimes referred to as "CNT"). CNT has a structure in which a graphene sheet is rolled into a cylindrical shape, and a CNT consisting of only one layer of the cylinder is called a single-walled carbon nanotube (hereinafter sometimes referred to as "SWCNT").

[0003] It is known that the electrical properties of CNTs vary depending on the winding method and diameter of the graphene sheet. In particular, since SWCNTs are greatly affected by quantum effects, there are those that exhibit metallic properties (metallic CNTs) and those that exhibit semiconductor properties (semiconductor CNTs). As methods for manufacturing SWCNTs, known synthesis methods include high-pressure carbon monoxide disproportionation (HiPco method), improved direct injection pyrolysis synthesis (e-DIPS method), arc discharge method, laser ablation method, etc., but at this stage, there is no established technology for manufacturing only any one type of CNT. When SWCNTs are applied to various purposes, it is necessary to separate the target type of SWCNTs from their mixture. Metallic CNTs are expected to be used in touch panels, transparent electrodes for solar cells, fine wiring of devices, etc. due to their excellent conductivity, and semiconductor CNTs are expected to be used in transistors and sensors, etc.

[0004] Several methods for separating metallic SWCNTs from semiconducting SWCNTs have been reported. For example, the following methods are known: density gradient centrifugation, using a surfactant such as sodium dodecyl sulfate or sodium cholate to disperse SWCNTs, and mixing with a density gradient agent for centrifugal separation (Japanese Patent Publication No. 2010-1162); electric field separation, using a surfactant to apply an electric field to a dispersion in which SWCNTs are dispersed for separation (Japanese Patent Publication No. 2008-55375); mixing with a separation agent such as porphyrin in an organic solvent to form a complex of semiconducting SWCNTs and the separation agent and taking it out (Japanese Patent Publication No. 2007-519594); mixing with a separation agent such as a polythiophene derivative in an organic solvent to separate the semiconducting SWCNTs and the separation agent using ... separate the semiconducting SWCNTs and the separation agent and taking it out (Japanese Patent Publication No. 2007-519594); mixing with a separation agent such as a polythiophene derivative in an organic solvent to separate the semiconducting SWCNTs and the separation agent using a separation agent such as porphyrin in an organic solvent to form a complex of semiconducting SWCNTs and the separation agent and taking it out (Japanese Patent Publication No. 2007-519594). A method for selectively separating semiconductor SWCNTs by using the interaction between semiconductor SWCNTs and a separation agent (Japanese Patent Publication No. 2014-503445); a method for separating semiconductor SWCNTs by mixing with a separation agent such as a flavin derivative in an organic solvent and utilizing the adsorption effect of the separation agent on the semiconductor SWCNTs (WO2014 / 136981); a method for placing a dispersion in which SWCNTs are dispersed using a surfactant into a separation container filled with a separation material such as agar gel, and using an eluent to dissolve the semiconductor SWCNTs adsorbed on the separation material from the separation material (Japanese Patent Publication No. 2012-36041), etc. Summary of the invention

[0005] One embodiment of the present invention relates to a method for producing a semiconductor single-walled carbon nanotube dispersion (hereinafter, also referred to as a "semiconductor SWCNT dispersion"), comprising: a step A of preparing a separated single-walled carbon nanotube dispersion (hereinafter, also referred to as a "separated SWCNT dispersion"), wherein the separated SWCNT dispersion contains single-walled carbon nanotubes including semiconductor single-walled carbon nanotubes (hereinafter, also referred to as "semiconductor SWCNTs") and metallic single-walled carbon nanotubes (hereinafter, also referred to as "metallic SWCNTs"), an aqueous medium, and a nonionic polymer containing a structural unit A derived from a monomer represented by the following formula (1); and a step B of centrifuging the separated SWCNT dispersion, and extracting a supernatant containing the semiconductor SWCNT from the centrifuged separated SWCNT dispersion; the content of the structural unit A in all structural units of the polymer is 2 mol% or more, and the polymer is water-soluble.

[0006] CH2=CR 1 -COO-(EO) p (PO) q -R 2 (1)

[0007] In formula (1), R 1represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average number of added moles of the ethyleneoxy group, which is 4 to 120, and q represents the average number of added moles of the propyleneoxy group, which is 0 to 50.

[0008] One embodiment of the present invention relates to a method for producing a semiconductor SWCNT, comprising the step of filtering a semiconductor SWCNT dispersion obtained by the method for producing a semiconductor SWCNT dispersion of the present invention to extract semiconductor SWCNTs.

[0009] One embodiment of the present invention relates to a method for producing a semiconductor SWCNT, comprising the steps of: drying a semiconductor SWCNT dispersion obtained by the method for producing a semiconductor SWCNT dispersion of the present invention to obtain a mixture containing semiconductor single-layer SWCNTs and the above-mentioned polymer; and removing the above-mentioned polymer from the above-mentioned mixture to extract the semiconductor SWCNT.

[0010] One embodiment of the present invention relates to a method for producing semiconductor SWCNTs, which obtains a semiconductor SWCNT dispersion obtained by the method for producing a semiconductor SWCNT dispersion of the present invention as semiconductor SWCNTs without further performing a separation treatment.

[0011] One embodiment of the present invention relates to a method for separating semiconductor SWCNTs and metallic SWCNTs, comprising: step A of preparing a SWCNT dispersion to be separated, wherein the SWCNT dispersion to be separated contains single-walled carbon nanotubes containing semiconductor SWCNTs and metallic SWCNTs, an aqueous medium, and a nonionic polymer containing a structural unit A derived from a monomer represented by the following formula (1); and step B of centrifuging the SWCNT dispersion to be separated, and then extracting a supernatant containing the semiconductor SWCNTs from the centrifuged SWCNT dispersion to be separated; the content of the structural unit A in all structural units of the polymer is 2 mol% or more, and the polymer is water-soluble.

[0012] CH2=CR 1 -COO-(EO) p (PO) q -R 2 (1)

[0013] In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average number of added moles of the ethyleneoxy group, which is 4 to 120, and q represents the average number of added moles of the propyleneoxy group, which is 0 to 50.

[0014] One embodiment of the present invention relates to a method for producing an ink containing a semiconductor SWCNT, which includes the method for producing a semiconductor SWCNT dispersion liquid of the present invention or the method for producing a semiconductor SWCNT of the present invention as one step.

[0015] One embodiment of the present invention relates to an ink containing a semiconductor SWCNT, comprising: at least one of an organic solvent and water, a semiconductor SWCNT, and a nonionic polymer comprising a structural unit A derived from a monomer represented by the following formula (1); the content of the structural unit A in all structural units of the above polymer is 2 mol% or more, and the above polymer is water-soluble.

[0016] CH2=CR 1 -COO-(EO) p (PO) q -R 2 (1)

[0017] In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average number of added moles of the ethyleneoxy group, which is 4 to 120, and q represents the average number of added moles of the propyleneoxy group, which is 0 to 50.

[0018] One embodiment of the present invention relates to an aqueous dispersion comprising: semiconductor SWCNTs; and a polymer comprising a structural unit A derived from a monomer represented by the following formula (1), wherein the content of the structural unit A in all structural units is 2 mol % or more.

[0019] CH2=CR 1 -COO-(EO) p (PO) q -R 2 (1)

[0020] In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average number of added moles of the ethyleneoxy group, which is 4 to 120, and q represents the average number of added moles of the propyleneoxy group, which is 0 to 50.

[0021] One embodiment of the present invention relates to use of a polymer for separating semiconducting single-walled carbon nanotubes, wherein the polymer comprises a structural unit A derived from a monomer represented by the following formula (1), and the content of the structural unit A in all structural units is 2 mol% or more.

[0022] CH2=CR 1 -COO-(EO) p (PO) q -R 2 (1)

[0023] In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average number of added moles of the ethyleneoxy group, which is 4 to 120, and q represents the average number of added moles of the propyleneoxy group, which is 0 to 50. DETAILED DESCRIPTION

[0024] The separation methods disclosed in Japanese Patent Publication No. 2010-1162 and Japanese Patent Publication No. 2012-36041 require density gradient agents, agar gel, etc., and have many operating steps. The separation method disclosed in Japanese Patent Publication No. 2008-55375 requires an electrophoresis device, and the separation takes time, and the concentration of the separated SWCNT is dilute. The separation methods disclosed in Japanese Patent Publication No. 2007-519594, Japanese Patent Publication No. 2014-503445, and WO2014 / 136981 need to be carried out in a non-polar solvent and require an expensive separation agent, so they are low in practicality.

[0025] The present invention relates to a method for producing a semiconductor SWCNT dispersion liquid capable of separating semiconductor SWCNTs from a SWCNT mixture containing semiconductor SWCNTs and metallic SWCNTs in an aqueous medium using an easily available separating agent and a simple operation, a method for producing semiconductor SWCNTs including the production method as a process, a method for separating semiconductor SWCNTs from metallic SWCNTs, and a method for producing an ink containing semiconductor SWCNTs.

[0026] The present invention is based on the finding that, by including a specific nonionic polymer in a SWCNT dispersion to be separated, separation of metallic SWCNTs and semiconductor SWCNTs in the SWCNT dispersion to be separated can be performed by using an easily available separation agent and by a simple operation.

[0027] According to the present invention, there can be provided a method for producing a semiconductor SWCNT dispersion having excellent separation properties of semiconductor SWCNTs, which can be carried out in an aqueous medium using an easily available separation agent and a simple operation; a method for producing semiconductor SWCNTs including the production method as a process; a method for separating semiconductor SWCNTs from metal SWCNTs; and a method for producing an ink containing semiconductor SWCNTs.

[0028] The details of the mechanism by which the effects of the present invention are exhibited are not clear, but are presumed as follows.

[0029] In the present invention, the SWCNT dispersion to be separated contains a nonionic polymer, and the nonionic polymer contains a structural unit A derived from a monomer represented by the above formula (1). The structural unit A has a high affinity for aqueous media, and the polymer tends to be easily dispersed in the dispersion. On the other hand, the magnitude of the interaction between the polymer and SWCNT is different between semiconductor type and metal type, and it is believed that the degree of dispersion will differ depending on the magnitude of the interaction. As a result, semiconductor type SWCNT is selectively dispersed in the above dispersion, while metal type SWCNT aggregates. Therefore, it is speculated that by subjecting the above dispersion to centrifugal separation, metal type SWCNT and semiconductor type SWCNT can be well separated.

[0030] However, the present invention is not limited to these mechanisms for interpretation.

[0031] [Method for producing semiconductor SWCNT dispersion, method for separating semiconductor SWCNT and metallic SWCNT]

[0032] One embodiment of the present invention relates to a method for producing a semiconductor SWCNT dispersion liquid comprising the following steps A and B (hereinafter also referred to as "the method for producing the dispersion liquid of the present invention"). In addition, another embodiment of the present invention relates to a method for separating semiconductor SWCNTs and metallic SWCNTs comprising the following steps A and B (hereinafter also referred to as "the separation method of the present invention").

[0033] (Step A) A SWCNT dispersion to be separated is prepared, wherein the SWCNT dispersion to be separated contains: single-walled carbon nanotubes including semiconductor-type SWCNTs and metallic-type SWCNTs (hereinafter also referred to as a "SWCNT mixture"), a nonionic polymer containing a structural unit A derived from a monomer represented by the following formula (1) (hereinafter also referred to as "monomer A"), and an aqueous medium.

[0034] (Step B) After centrifuging the separated SWCNT dispersion, a supernatant containing the semiconductor-type SWCNT is extracted from the centrifuged separated SWCNT dispersion.

[0035] CH2=CR 1 -COO-(EO) p (PO) q -R 2 (1)

[0036] In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average number of added moles of the ethyleneoxy group, which is 4 to 120, and q represents the average number of added moles of the propyleneoxy group, which is 0 to 50.

[0037] In the present invention, "extracting a supernatant containing the semiconductor SWCNT" means extracting a supernatant in which the ratio of the semiconductor SWCNT is increased compared to the ratio of the semiconductor SWCNT to the metal SWCNT in the separated SWCNT dispersion obtained in step A; the supernatant is a semiconductor SWCNT dispersion. In the present invention, the supernatant does not exclude the case where a relatively small amount of metal SWCNT is contained in comparison with the semiconductor SWCNT. If the separability of the semiconductor SWCNT is improved, the ratio of the semiconductor SWCNT in the SWCNT in the supernatant becomes higher, which is more useful as a material for semiconductor devices.

[0038] Extraction of the supernatant in step B can be performed, for example, by separating the supernatant from its residue. The residue contains a precipitate, and the precipitate contains a relatively larger amount of metallic SWCNTs than semiconductor SWCNTs.

[0039] [Process A]

[0040] The separated SWCNT dispersion in the step A in the method for producing a dispersion of the present invention and the separation method of the present invention can be obtained, in one or more embodiments, by preparing a mixed solution containing at least a polymer including a structural unit A derived from the monomer A, the SWCNT mixture, and an aqueous medium (hereinafter sometimes referred to as "mixed solution A"), and then dispersing the mixed solution A. The mixed solution A can be prepared, for example, by adding the SWCNT mixture to an aqueous solution of the polymer.

[0041] [Nonionic polymer comprising structural unit A derived from monomer A]

[0042] From the viewpoint of improving the separability of semiconductor SWCNT, the above polymer is water-soluble. In the present invention, the so-called "water-soluble" means that more than 1 g of the polymer is dissolved in 100 g of water at 20°C. In one or more embodiments, the above polymer can be used to separate semiconductor single-layer carbon nanotubes. That is, one embodiment of the present invention relates to the use of a polymer for separating semiconductor single-layer carbon nanotubes, wherein the above polymer comprises a structural unit A derived from a monomer represented by the following formula (1), and the content of the structural unit A in all structural units is 2 mol% or more.

[0043] The structural unit A contained in the above polymer is a structural unit derived from a monomer A represented by the following formula (1). The structural unit A may be one type or a combination of two or more types.

[0044] CH2=CR 1 -COO-(EO) p (PO) q -R 2 (1)

[0045] In the above formula (1), R 1 represents a hydrogen atom or a methyl group, and is preferably a methyl group from the viewpoint of improving the separability of the semiconductor-type SWCNT.

[0046] In the above formula (1), R 2 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms. 2 When R is a hydrocarbon group, from the viewpoint of improving the separability of the semiconductor-type SWCNT and the availability of the monomer, 2 The carbon number of R is 1 or more and 20 or less, preferably 1 or more and 18 or less, more preferably 1 or more and 6 or less, further preferably 1 or more and 4 or less, and still more preferably 1. 2 Examples of the hydrocarbon group include an alkyl group and a phenyl group.

[0047] As R 2 Specific examples include at least one selected from stearyl, lauryl, 2-ethylhexyl, butyl, phenyl, ethyl, methyl, and hydrogen atoms, and from the viewpoint of improving the separability of semiconductor-type SWCNTs, a methyl group or a hydrogen atom is preferred.

[0048] In formula (1), from the viewpoint of improving the separability of semiconductor-type SWCNTs, p is greater than 4, and from the viewpoint of improving the separability of semiconductor-type SWCNTs and the availability of monomers, p is less than 120, preferably less than 90, more preferably less than 45, further preferably less than 25, further more preferably less than 15, and further more preferably less than 10.

[0049] In formula (1), from the viewpoint of water solubility of the polymer, improvement of the separability of the semiconductor-type SWCNT, and availability of the monomer, q is greater than or equal to 0 and less than or equal to 50, preferably greater than or equal to 0 and less than or equal to 30, more preferably greater than or equal to 0 and less than or equal to 10, further preferably greater than or equal to 0 and less than or equal to 3, and still more preferably 0.

[0050] In formula (1), q / (p+q) is preferably 0.7 or less, more preferably 0.4 or less, and even more preferably 0, from the viewpoints of water solubility of the polymer, improvement of separability of semiconductor-type SWCNTs, and availability of monomers.

[0051] In the formula (1), the order of addition of the ethyleneoxy group and the propyleneoxy group is not limited, and when q is 2 or more, either block bonding or random bonding may be used.

[0052] Examples of the monomer A include at least one selected from the group consisting of polyethylene glycol monomethacrylate (PEGMA) and polyethylene glycol monoacrylate (PEGA).

[0053] The polymer may further include a structural unit B derived from a monomer B other than the monomer A. The structural unit B may be one or a combination of two or more. As monomer B, there is no particular limitation if it is a nonionic monomer copolymerizable with monomer A. From the perspective of improving the separability of semiconductor-type SWCNTs, at least one monomer selected from the group consisting of a monomer represented by the following formula (2), a (meth)acrylate monomer, a (meth)acrylamide monomer, a styrene monomer, and a (meth)acrylonitrile monomer can be cited. Among these, a monomer represented by the following formula (2) or a (meth)acrylate monomer is preferred.

[0054] CH2=CR 3 -COO-(EO) r (PO) s -R 4 (2)

[0055] In the above formula (2), R 3 represents a hydrogen atom or a methyl group, R 4 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, r represents the average number of added moles of the ethyleneoxy group, which is 1 to less than 4, and s represents the average number of added moles of the propyleneoxy group, which is 0 to 50. The order of addition of the ethyleneoxy group and the propyleneoxy group is not limited, and when r is 2 or more and s is 2 or more, either a block bond or a random bond may be used.

[0056] In the above formula (2), from the viewpoint of improving the separability of the semiconductor-type SWCNT, R 3It is a hydrogen atom or a methyl group, and is preferably a methyl group.

[0057] In the above formula (2), R 4 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms. 4 In the case of a hydrocarbon group, R 4 The carbon number of R is 1 to 20, preferably 1 to 18, more preferably 1 to 6, further preferably 1 to 4, and even more preferably 1, from the viewpoint of improving the separability of the semiconductor-type SWCNT and the availability of the monomer. 4 In the case of a hydrocarbon group, examples of the hydrocarbon group include an alkyl group and a phenyl group.

[0058] As R 4 Specific examples include at least one selected from stearyl, lauryl, 2-ethylhexyl, butyl, phenyl, ethyl, methyl, and hydrogen atoms, and from the viewpoint of improving the separability of semiconductor-type SWCNTs, a methyl group or a hydrogen atom is preferred.

[0059] In the above formula (2), r is 1 or more and less than 4 from the viewpoint of improving the separability of the semiconductor-type SWCNT.

[0060] In the above formula (2), the order of addition of the ethyleneoxy group and the propyleneoxy group is not limited, and when r is 2 or more and s is 2 or more, either block bonding or random bonding may be used.

[0061] In the above formula (2), from the viewpoint of water solubility of the polymer, separation property of the semiconductor-type SWCNT, and availability of the monomer, s is greater than 0 and less than 50, preferably greater than 0 and less than 30, more preferably greater than 0 and less than 10, further preferably greater than 0 and less than 3, and still more preferably 0.

[0062] When monomer B is a (meth)acrylate monomer, monomer B may be, for example, at least one selected from methyl (meth)acrylate, ethyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and benzyl (meth)acrylate. Of these, monomer B is preferably at least one selected from 2-hydroxyethyl methacrylate (HEMA), lauryl methacrylate (LMA), and benzyl methacrylate (BzMA) from the viewpoint of improving the separability of semiconductor-type SWCNTs.

[0063] The monomer B is a (meth)acrylamide-based monomer, and examples of the monomer B include at least one selected from the group consisting of acrylamide, methacrylamide, dimethylacrylamide, and dimethylmethacrylamide.

[0064] When the monomer B is a styrene-based monomer, examples of the monomer B include styrene and methylstyrene.

[0065] When the monomer B is a (meth)acrylonitrile-based monomer, examples of the monomer B include acrylonitrile and methacrylonitrile.

[0066] Examples of the polymer include polyethylene glycol (23) monomethacrylate polymers (PEG (23) MA), polyethylene glycol (9) monomethacrylate polymers (PEG (9) MA), polyethylene glycol (4) monomethacrylate polymers (PEG (4) MA), polyethylene glycol (23) monoacrylate / polyethylene glycol (2) monomethacrylate copolymers (PEG (23) MA / PEG (2) MA), polyethylene glycol (23) monoacrylate / 2-hydroxyethyl methacrylate (PEG (23) MA), polyethylene glycol (23) monoacrylate / 2-hydroxyethyl methacrylate (PEG (23) MA), polyethylene glycol (23) monometh ... )MA / HEMA), polyethylene glycol (9) monoacrylate / lauryl methacrylate (PEG (9)MA / LMA), polyethylene glycol (9) monoacrylate / benzyl methacrylate (PEG (9)MA / BzMA), polyethylene glycol (23) monoacrylate / polyethylene glycol (23) monoacrylate copolymer (PEG (23)MA / PEG (23)A), and polyethylene glycol (9) monoacrylate / polyethylene glycol (9) monoacrylate copolymer (PEG (9)MA / PEG (9)A). It should be noted that the numerical value in parentheses () represents the average number of added moles.

[0067] From the viewpoint of improving the separability of semiconductor-type SWCNTs, the content (mol %) of structural unit A in all structural units of the above-mentioned polymer is 2 mol % or more, preferably 4 mol % or more, more preferably 5 mol % or more, and from the same viewpoint, it is preferably 100 mol % or less.

[0068] From the viewpoint of improving the separability of the semiconductor-type SWCNT, the content (mol %) of the structural unit A in all the structural units of the polymer is preferably 100 mol %.

[0069] When the above-mentioned polymer contains structural unit B, the content (mol %) of structural unit A in all structural units of the above-mentioned polymer is preferably less than 100 mol %, more preferably 95 mol % or less, further preferably 90 mol % or less, even more preferably 80 mol % or less, further more preferably 70 mol % or less, further more preferably 60 mol % or less, further more preferably 50 mol % or less, further more preferably 40 mol % or less, further more preferably 15 mol % or less, further more preferably 8 mol % or less.

[0070] From the viewpoint of improving the separability of semiconductor-type SWCNTs, the content (mass %) of the structural unit A in all the structural units of the above-mentioned polymer is preferably 10 mass % or more, more preferably 20 mass % or more, and further preferably 30 mass % or more, and from the same viewpoint, it is preferably 100 mass % or less.

[0071] When the polymer contains the structural unit B, the content (mass %) of the structural unit A in all the structural units of the polymer is preferably less than 100 mass %, more preferably 98 mass % or less, and further preferably 96 mass % or less.

[0072] When the above-mentioned polymer contains structural unit B, from the viewpoint of improving the separability of semiconductor-type SWCNTs, the content (mol %) of structural unit B in all structural units of the above-mentioned polymer is preferably 98 mol % or less, more preferably 96 mol % or less, and further preferably 95 mol % or less, and from the same viewpoint, it is preferably greater than 0 mol %, more preferably 5 mol % or more, and further preferably 10 mol % or more.

[0073] When the above-mentioned polymer contains structural unit B, from the viewpoint of improving the separability of semiconductor-type SWCNTs, the content (mass %) of structural unit B in all structural units of the above-mentioned polymer is preferably 90 mass % or less, more preferably 80 mass % or less, and further preferably 70 mass % or less, and from the same viewpoint, it is preferably greater than 0 mass %, more preferably 2 mass % or more, and further preferably 4 mass % or more.

[0074] From the viewpoint of improving the separability of semiconductor-type SWCNTs, the total content (mass %) of structural unit A and structural unit B in all structural units of the above-mentioned polymer is preferably 80 mass % or more, more preferably 90 mass % or more, further preferably 95 mass % or more, and even more preferably 100 mass %.

[0075] When the above-mentioned polymer contains structural unit B, from the viewpoint of improving the separability of semiconductor-type SWCNTs, the mass ratio (A / B) of structural unit A to structural unit B in the above-mentioned polymer is preferably 0.05 or more, more preferably 0.11 or more, and further preferably 0.25 or more, and from the viewpoint of improving the separability of semiconductor-type SWCNTs, it is preferably 99 or less, more preferably 49 or less, and further preferably 33 or less.

[0076] When the above-mentioned polymer contains structural unit B, from the viewpoint of improving the separability of semiconductor-type SWCNTs, the molar ratio of structural unit A to structural unit B in the above-mentioned polymer (A / B) is preferably 0.02 or more, more preferably 0.03 or more, and further preferably 0.04 or more, and from the viewpoint of improving the separability of semiconductor-type SWCNTs, it is preferably 99 or less, more preferably 19 or less, and further preferably 12 or less.

[0077] From the viewpoint of improving the separability of semiconductor-type SWCNTs, the weight average molecular weight of the polymer is preferably 2000 or more, more preferably 5000 or more, further preferably 7000 or more, and even more preferably 8000 or more, and from the same viewpoint, it is preferably 250,000 or less, more preferably 150,000 or less, further preferably 120,000 or less, and even more preferably 110,000 or less. In the present invention, the weight average molecular weight of the polymer is obtained by gel permeation chromatography, and specifically, can be measured by the method described in the Examples.

[0078] From the viewpoint of improving the separability of semiconductor-type SWCNTs, the number of ethyleneoxy groups derived from the structural unit A in each structural unit in the polymer, that is, the value obtained by multiplying the average number of moles of EO added to the structural unit A of the polymer by the molar fraction of the structural unit A is preferably 0.5 or more, more preferably 0.8 or more, and further preferably 1.0 or more, and from the viewpoint of improving the separability of semiconductor-type SWCNTs, it is preferably 120 or less, more preferably 90 or less, further preferably 45 or less, further preferably 25 or less, further more preferably 12 or less, and further more preferably 6 or less. When the structural unit A is a combination of two or more types, the number of ethyleneoxy groups derived from the structural unit A is the total value thereof. In addition, when the structural unit A is a combination of two or more types, the value obtained by multiplying the average number of moles of EO added to the structural unit A of the polymer by the molar fraction of the structural unit A is the total value of the values ​​obtained by multiplying the p of each structural unit A by the respective molar fractions.

[0079] From the viewpoint of improving the separability of the semiconductor-type SWCNT, the molar ratio of the methyl group at the α position (hereinafter also referred to as "α methyl group") to the hydrogen atom at the α position (hereinafter also referred to as "α hydrogen") of all structural units of the above-mentioned polymer (α methyl group / α hydrogen) is preferably 20 / 80 or more and 100 / 0 or less, more preferably 30 / 70 or more and 100 / 0 or less, further preferably 70 / 30 or more and 100 / 0 or less, further more preferably 80 / 20 or more and 100 / 0 or less, and further more preferably 90 / 10 or more and 100 / 0 or less. It should be noted that the so-called α position is, for example, R 1 , R in formula (2) 3The part indicated.

[0080] From the viewpoint of improving the separability of semiconductor-type SWCNTs, the mass ratio of the polymer to SWCNT in the mixed solution A and in the separated SWCNT dispersion (polymer / SWCNT) is preferably 0.5 or more, more preferably 1 or more, further preferably 2 or more, and even more preferably 5 or more, and from the same viewpoint, it is preferably 100 or less, more preferably 70 or less, further preferably 50 or less, further more preferably 30 or less, and even more preferably 20 or less.

[0081] From the viewpoint of improving the separability of semiconductor-type SWCNTs, the content of the above-mentioned polymer in the above-mentioned mixed solution A and the separated SWCNT dispersion is preferably 0.05 mass% or more, more preferably 0.1 mass% or more, further preferably 0.2 mass% or more, and even more preferably 0.5 mass% or more, and from the same viewpoint, it is preferably 10 mass% or less, more preferably 7 mass% or less, further preferably 5 mass% or less, further more preferably 3 mass% or less, and even more preferably 2 mass% or less.

[0082] [SWCNT]

[0083] There is no particular limitation on the SWCNTs used to prepare the mixed solution A and the separated SWCNT dispersion. SWCNTs are synthesized by conventionally known synthesis methods such as the HiPco method and the e-DIPS method, and may include SWCNTs of various winding methods and diameters. Metallic SWCNTs and semiconductor SWCNTs may be included in any proportion, and the synthesized SWCNTs are generally a SWCNT mixture containing about 1 / 3 metallic SWCNTs and about 2 / 3 semiconductor SWCNTs.

[0084] From the viewpoint of improving the separability of semiconductor-type SWCNTs, the average diameter of SWCNTs is preferably 0.5 nm or more, more preferably 0.8 nm or more, and from the same viewpoint, preferably 3 nm or less, more preferably 2 nm or less. The average diameter of SWCNTs can be calculated as follows: based on an image obtained using a transmission electron microscope, the diameters of 10 or more CNTs are measured and averaged.

[0085] From the viewpoint of electrical properties, the average length of SWCNT is preferably 0.1 μm or more, more preferably 0.3 μm or more, and further preferably 0.5 μm or more, and from the viewpoint of improving the separability of semiconductor-type SWCNT and improving productivity, it is preferably 100 μm or less, more preferably 50 μm or less, further preferably 20 μm or less, and further preferably 10 μm or less. The average length of SWCNT can be calculated, for example, by measuring the lengths of 10 or more CNTs based on an image obtained using a transmission electron microscope and averaging the lengths.

[0086] From the viewpoint of improving the separability of semiconductor-type SWCNTs, the content of SWCNTs in the mixed solution A and the content of SWCNTs in the separated SWCNT dispersion is preferably 0.001 mass % or more, more preferably 0.01 mass % or more, and further preferably 0.03 mass % or more, and from the viewpoint of improving the separability of semiconductor-type SWCNTs and improving productivity, it is preferably 5 mass % or less, more preferably 1 mass % or less, and further preferably 0.5 mass % or less.

[0087] [Aqueous medium]

[0088] The mixed solution A and the separated SWCNT dispersion solution contain an aqueous medium as a dispersion medium. The aqueous medium is preferably water, and from the viewpoint of improving the separation of semiconductor-type SWCNTs, the water is preferably pure water, ion-exchanged water, purified water or distilled water, and more preferably pure water.

[0089] The mixed solution A and the separated SWCNT dispersion solution may contain, in addition to water as an aqueous medium, lower alcohols such as methanol, ethanol, and isopropanol, or water-soluble organic solvents such as acetone, tetrahydrofuran, and dimethylformamide.

[0090] When water and a dispersion medium other than water are used in combination as the aqueous medium, the proportion of water in the aqueous medium is preferably 70 mass % or more, more preferably 80 mass % or more, and even more preferably 90 mass % or more from the viewpoint of improving the separability of semiconductor-type SWCNTs.

[0091] From the viewpoint of improving the separability of semiconductor-type SWCNTs and improving productivity, the content of the aqueous medium in the mixed solution A and the aqueous medium in the separated SWCNT dispersion is preferably 85 mass % or more, more preferably 92 mass % or more, and further preferably 96 mass % or more, and from the same viewpoint, it is preferably 99.9 mass % or less, more preferably 99.8 mass % or less, further preferably 99.5 mass % or less, and further preferably 99.0 mass % or less.

[0092] The dispersion treatment of the mixed solution A can be performed using, for example, a dispersing machine such as a bath ultrasonic disperser, a homomixer, a high-pressure homogenizer, an ultrasonic homogenizer, a jet mill, a bead mill, or a pulverizer.

[0093] In step A, before the mixed solution A is subjected to the dispersion treatment, a defoaming treatment may be performed.

[0094] [Process B]

[0095] In step B, the separated SWCNT dispersion obtained in step A is subjected to centrifugal separation, and a supernatant containing semiconductor SWCNTs is extracted from the separated SWCNT dispersion subjected to centrifugal separation. The supernatant is a supernatant in which the ratio of semiconductor SWCNTs is increased relative to the ratio of semiconductor SWCNTs to metal SWCNTs in the separated SWCNT dispersion before being subjected to centrifugal separation. The ratio varies depending on centrifugal separation conditions, etc. From the perspective of improving the separation of semiconductor SWCNTs and the perspective of improving productivity, the rotation speed of the centrifuge is preferably 5,000 rpm or more, more preferably 10,000 rpm or more, and from the same perspective, it is preferably 100,000 rpm or less, and more preferably 70,000 rpm or less. From the perspective of improving the separation of semiconductor SWCNTs and the perspective of improving productivity, the gravitational acceleration of the centrifuge is preferably 10 kG or more, more preferably 50 kG or more, and from the same perspective, it is preferably 1000 kG or less, and more preferably 500 kG or less.

[0096] From the viewpoint of semiconductor properties, the separability of the semiconductor-type SWCNT in the supernatant obtained in step B is preferably 1.1 or more, more preferably 1.3 or more, further preferably 1.4 or more, still more preferably 1.6 or more, and further more preferably 2.0 or more, and from the viewpoint of yield, it is preferably 100 or less. In the present invention, the separability of the semiconductor-type SWCNT is a value obtained by the following formula.

[0097] [Mathematical formula 1]

[0098]

[0099] The supernatant obtained in the step (B) is, in one or more embodiments, an aqueous dispersion containing the semiconductor SWCNT and the polymer. That is, one embodiment of the present invention relates to an aqueous dispersion containing semiconductor SWCNT and a polymer, wherein the polymer contains a structural unit A derived from the monomer A, and the content of the structural unit A in all structural units is 2 mol% or more.

[0100] [Method for producing semiconductor SWCNT and semiconductor SWCNT]

[0101] If semiconductor SWCNTs are extracted from a semiconductor SWCNT dispersion produced by the method for producing a semiconductor SWCNT dispersion of the present invention, semiconductor SWCNTs can be produced. Extraction of semiconductor SWCNTs from a semiconductor SWCNT dispersion can be carried out, for example, in the following manner: filtering out semiconductor SWCNTs from a semiconductor SWCNT dispersion using a membrane filter and then drying it. When filtering semiconductor SWCNTs from a semiconductor SWCNT dispersion, filtration can be performed after pretreatment such as reprecipitation of the semiconductor SWCNTs in the semiconductor SWCNT dispersion. Alternatively, it can be carried out in the following manner: drying the semiconductor SWCNT dispersion and removing the above-mentioned coexisting polymers by washing or thermal decomposition. Alternatively, the semiconductor SWCNT dispersion can be used as a semiconductor SWCNT without further separation treatment.

[0102] Therefore, one embodiment of the present invention relates to a method for producing a semiconductor SWCNT (hereinafter also referred to as "method A for producing a semiconductor SWCNT of the present invention"), which includes the following steps: filtering a semiconductor SWCNT dispersion obtained by the method for producing a semiconductor SWCNT dispersion of the present invention to extract the semiconductor SWCNT.

[0103] In addition, another embodiment of the present invention relates to a method for producing a semiconductor SWCNT (hereinafter also referred to as "method B for producing a semiconductor SWCNT of the present invention"), which comprises the following steps: drying the semiconductor SWCNT dispersion obtained by the method for producing a semiconductor SWCNT dispersion of the present invention to obtain a mixture of semiconductor single-walled carbon nanotubes and the above-mentioned polymer; and removing the above-mentioned polymer from the above-mentioned mixture to extract the semiconductor single-walled carbon nanotubes.

[0104] In addition, another embodiment of the present invention relates to a method for producing a semiconductor single-walled carbon nanotube (hereinafter also referred to as "method C for producing semiconductor SWCNTs of the present invention"), which obtains a semiconductor SWCNT dispersion obtained by the method for producing a semiconductor SWCNT dispersion of the present invention as a semiconductor SWCNT without further separation treatment.

[0105] Another embodiment of the present invention relates to a semiconductor-type SWCNT obtained by the semiconductor-type SWCNT production method A, B, or C of the present invention (hereinafter also referred to as “the semiconductor-type SWCNT of the present invention”).

[0106] [Method for producing ink containing semiconductor SWCNT]

[0107] One embodiment of the present invention relates to a method for producing an ink containing semiconductor SWCNTs (hereinafter, also referred to as "the method for producing an ink containing semiconductor SWCNTs of the present invention"), which includes the method for producing a semiconductor SWCNT dispersion of the present invention or the method for producing a semiconductor SWCNT of the present invention as a process. One embodiment of the method for producing an ink containing semiconductor SWCNTs of the present invention, for example, includes the method for producing semiconductor SWCNTs A, B or C of the present invention as a process, and further includes the step of mixing an organic solvent with at least one of water, the semiconductor SWCNTs, and at least one of a surfactant and a resin as required. In addition, another embodiment of the method for producing an ink containing semiconductor SWCNTs of the present invention, for example, includes the method for producing a semiconductor SWCNT dispersion of the present invention as a process, and includes the step of mixing the semiconductor SWCNT dispersion with an organic solvent, a surfactant and a resin that can be mixed with the dispersion as required.

[0108] Examples of the organic solvent include aliphatic solvents such as n-hexane, n-octane, and n-decane; alicyclic solvents such as cyclohexane; aromatic solvents such as benzene and toluene; alcohol solvents such as methanol and ethanol; glycol ether solvents such as diethylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and butyl cellosolve. From the perspective of improving film-forming properties, the ink containing semiconductor SWCNTs may further include, for example, polystyrene resins, acrylic resins, vinyl resins, etc. as the above-mentioned resins that can be dissolved or dispersed in the solvent, and may also include known surfactants or other additives as dispersants. The content of semiconductor SWCNTs in the ink containing semiconductor SWCNTs can be appropriately set according to the application.

[0109] [Ink containing semiconductor SWCNT]

[0110] One embodiment of the present invention relates to an ink containing a semiconductor SWCNT (hereinafter also referred to as "the ink containing a semiconductor SWCNT of the present invention"), which comprises: at least one of an organic solvent and water, a semiconductor single-layer SWCNT, and a nonionic polymer containing 2 mol% or more of a structural unit A derived from the above-mentioned monomer A; the content of the structural unit A in all the structural units of the above-mentioned polymer is 2 mol% or more, and the above-mentioned polymer is water-soluble.

[0111] One embodiment of the ink containing semiconductor SWCNT of the present invention comprises at least: semiconductor SWCNT of the present invention; a nonionic polymer comprising a structural unit A derived from the above-mentioned monomer A, wherein the content of the structural unit A in all the structural units of the above-mentioned polymer is 2 mol% or more, and the above-mentioned polymer is water-soluble; and at least one of an organic solvent and water; and contains a surfactant and a resin as needed.

[0112] [Method for manufacturing semiconductor device]

[0113] One embodiment of the present invention relates to a method for manufacturing a semiconductor device, including the step of printing or applying a semiconductor-containing SWCNT ink obtained by the method for manufacturing a semiconductor-containing SWCNT ink of the present invention onto a substrate to form a semiconductor layer.

[0114] In addition, another embodiment of the present invention relates to a method for manufacturing a semiconductor element, the semiconductor element having a substrate, and a gate electrode, a source electrode, and a drain electrode disposed on the substrate, the manufacturing method comprising the following steps: forming a semiconductor circuit and a semiconductor film (semiconductor layer) by printing or coating the ink containing the semiconductor type SWCNT. As the printing method of the ink containing the semiconductor type SWCNT, inkjet printing, screen printing, offset printing, relief printing, etc. can be cited. It can also include a step of forming a semiconductor film by printing or coating, and then etching to form a circuit.

[0115] Regarding the above-mentioned embodiments, the present invention also discloses the following method for producing a semiconductor single-walled carbon nanotube dispersion, a method for separating semiconductor single-walled carbon nanotubes from metallic single-walled carbon nanotubes, a method for producing an ink containing semiconductor single-walled carbon nanotubes, and an ink containing semiconductor single-walled carbon nanotubes.

[0116] <1> A method for producing a semiconducting single-walled carbon nanotube dispersion or a method for separating semiconducting single-walled carbon nanotubes from metallic single-walled carbon nanotubes, comprising: step A, preparing a separated single-walled carbon nanotube dispersion, wherein the separated single-walled carbon nanotube dispersion contains single-walled carbon nanotubes including semiconducting single-walled carbon nanotubes and metallic single-walled carbon nanotubes, an aqueous medium, and a nonionic polymer containing a structural unit A derived from a monomer represented by the following formula (1); and

[0117] Step B, after centrifuging the separated single-walled carbon nanotube dispersion, extracting a supernatant containing the following semiconductor single-walled carbon nanotubes from the separated single-walled carbon nanotube dispersion after centrifugation;

[0118] The content of the structural unit A in all structural units of the above-mentioned polymer is 2 mol% or more, and the above-mentioned polymer is water-soluble;

[0119] CH2=CR 1 -COO-(EO) p (PO) q -R 2 (1)

[0120] In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average number of added moles of the ethyleneoxy group, which is 4 to 120, and q represents the average number of added moles of the propyleneoxy group, which is 0 to 50.

[0121] <2> A method for producing a semiconductor single-walled carbon nanotube dispersion or a method for separating semiconductor single-walled carbon nanotubes from metallic single-walled carbon nanotubes as described in <1>, comprising: step A, preparing a separated single-walled carbon nanotube dispersion, wherein the separated single-walled carbon nanotube dispersion contains single-walled carbon nanotubes including semiconductor single-walled carbon nanotubes and metallic single-walled carbon nanotubes, an aqueous medium, and a nonionic polymer containing a structural unit A derived from a monomer represented by the above formula (1); and

[0122] Step B, after centrifuging the separated single-walled carbon nanotube dispersion, extracting a supernatant containing the semiconductor single-walled carbon nanotubes from the separated single-walled carbon nanotube dispersion after centrifugation;

[0123] The content of the structural unit A in all the structural units of the above-mentioned polymer is 100 mol %, and the above-mentioned polymer is water-soluble;

[0124] CH2=CR 1 -COO-(EO) p (PO) q -R 2 (1)

[0125] In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a stearyl group, a lauryl group, a 2-ethylhexyl group, a butyl group, a phenyl group, an ethyl group, a methyl group, and a hydrogen atom, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average added mole number of the ethyleneoxy group, which is 4 to 45, and q represents the average added mole number of the propyleneoxy group, which is 0 to 3.

[0126] <3> A method for producing a semiconductor single-walled carbon nanotube dispersion or a method for separating semiconductor single-walled carbon nanotubes from metallic single-walled carbon nanotubes as described in <1>, comprising: step A, preparing a separated single-walled carbon nanotube dispersion, wherein the separated single-walled carbon nanotube dispersion contains single-walled carbon nanotubes including semiconductor single-walled carbon nanotubes and metallic single-walled carbon nanotubes, an aqueous medium, and a nonionic polymer containing a structural unit A derived from a monomer represented by the following formula (1); and

[0127] Step B, after centrifuging the separated single-walled carbon nanotube dispersion, extracting a supernatant containing the semiconductor single-walled carbon nanotubes from the separated single-walled carbon nanotube dispersion after centrifugation;

[0128] The content of the structural unit A in all the structural units of the above-mentioned polymer is 100 mol %, and the above-mentioned polymer is water-soluble;

[0129] CH2=CR 1 -COO-(EO) p (PO) q -R 2 (1)

[0130] In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a methyl group, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average added mole number of the ethyleneoxy group, which is 4 or more and 25 or less, and q represents the average added mole number of the propyleneoxy group, which is 0.

[0131] <4> A method for producing a semiconductor single-walled carbon nanotube dispersion or a method for separating semiconductor single-walled carbon nanotubes from metallic single-walled carbon nanotubes as described in <1>, comprising: step A, preparing a separated single-walled carbon nanotube dispersion, wherein the separated single-walled carbon nanotube dispersion contains single-walled carbon nanotubes including semiconductor single-walled carbon nanotubes and metallic single-walled carbon nanotubes, an aqueous medium, and a nonionic polymer containing a structural unit A derived from a monomer represented by the following formula (1); and

[0132] Step B, after centrifuging the separated single-walled carbon nanotube dispersion, extracting a supernatant containing the following semiconductor single-walled carbon nanotubes from the separated single-walled carbon nanotube dispersion after centrifugation;

[0133] The content of structural unit A in all structural units of the above-mentioned polymer is greater than 2 mol% and less than 100 mol%. The above-mentioned polymer further contains structural unit B, and the above-mentioned structural unit B is derived from at least one monomer selected from the group consisting of a monomer represented by the following formula (2), a (meth)acrylate monomer, a (meth)acrylamide monomer, a styrene monomer and a (meth)acrylonitrile monomer. The content of structural unit B in all structural units of the above-mentioned polymer is greater than 0 mol% and less than 98 mol%, and the above-mentioned polymer is water-soluble.

[0134] CH2=CR 1 -COO-(EO) p (PO) q -R 2 (1)

[0135] In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average number of added moles of the ethyleneoxy group, which is 4 to 120, and q represents the average number of added moles of the propyleneoxy group, which is 0 to 50.

[0136] CH2=CR 3 -COO-(EO) r (PO) s -R 4 (2)

[0137] In formula (2), R 3 represents a hydrogen atom or a methyl group, R 4 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, r represents the average number of added moles of the ethyleneoxy group, which is 1 to less than 4, and s represents the average number of added moles of the propyleneoxy group, which is 0 to 50.

[0138] <5> A method for producing a semiconductor single-walled carbon nanotube dispersion or a method for separating semiconductor single-walled carbon nanotubes from metallic single-walled carbon nanotubes as described in <1>, comprising: step A, preparing a separated single-walled carbon nanotube dispersion, wherein the separated single-walled carbon nanotube dispersion contains single-walled carbon nanotubes including semiconductor single-walled carbon nanotubes and metallic single-walled carbon nanotubes, an aqueous medium, and a nonionic polymer containing a structural unit A derived from a monomer represented by the following formula (1); and

[0139] Step B, after centrifuging the separated single-walled carbon nanotube dispersion, extracting a supernatant containing the following semiconductor single-walled carbon nanotubes from the separated single-walled carbon nanotube dispersion after centrifugation;

[0140] The content of structural unit A in all structural units of the above-mentioned polymer is greater than 2 mol% and less than 95 mol%, and the above-mentioned polymer further contains structural unit B, and the above-mentioned structural unit B is derived from at least one monomer selected from the monomer represented by the following formula (2) and a (meth)acrylate monomer. The content of structural unit B in all structural units of the above-mentioned polymer is greater than 5 mol% and less than 98 mol%, and the above-mentioned polymer is water-soluble.

[0141] CH2=CR 1 -COO-(EO) p (PO) q -R 2 (1)

[0142] In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a methyl group, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average added mole number of the ethyleneoxy group, which is 4 or more and 25 or less, and q represents the average added mole number of the propyleneoxy group, which is 0.

[0143] CH2=CR 3 -COO-(EO) r (PO) s -R 4 (2)

[0144] In formula (2), R 3 represents a hydrogen atom or a methyl group, R 4 represents a hydrogen atom or a methyl group, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, r represents the average added mole number of the ethyleneoxy group, which is 1 or more and less than 4, and s represents the average added mole number of the propyleneoxy group, which is 0.

[0145] <6> A method for producing a semiconductor single-walled carbon nanotube dispersion or a method for separating semiconductor single-walled carbon nanotubes and metallic single-walled carbon nanotubes as described in <4> or <5>, wherein the total content of structural unit A and structural unit B in all structural units of the above-mentioned polymer is 100% by mass.

[0146] <7> The method for producing a semiconductor single-walled carbon nanotube dispersion or the method for separating semiconductor single-walled carbon nanotubes from metallic single-walled carbon nanotubes as described in any one of <1> to <6>, wherein the weight average molecular weight of the polymer is 5,000 to 150,000.

[0147] <8> A method for producing a semiconductor single-walled carbon nanotube dispersion or a method for separating semiconductor single-walled carbon nanotubes from metallic single-walled carbon nanotubes as described in any one of <1> to <7>, wherein the number of ethyleneoxy groups derived from structural unit A in each structural unit in the above-mentioned polymer is greater than 0.8 and less than 25.

[0148] <9> A method for producing a semiconductor single-walled carbon nanotube dispersion or a method for separating semiconductor single-walled carbon nanotubes and metallic single-walled carbon nanotubes as described in any one of <1> to <8>, wherein the molar ratio of the methyl group at the α-position to the hydrogen atom at the α-position (α methyl / α hydrogen) of all structural units of the above-mentioned polymer is greater than 20 / 80 and less than 100 / 0.

[0149] <10> A method for producing a semiconductor single-layer carbon nanotube dispersion or a method for separating semiconductor single-layer carbon nanotubes from metallic single-layer carbon nanotubes as described in any one of <1> to <9>, wherein the mass ratio of the polymer to the carbon nanotubes in the separated single-layer carbon nanotube dispersion (polymer / carbon nanotube) is greater than 5 and less than 50.

[0150] <11> A method for producing a semiconductor single-walled carbon nanotube dispersion or a method for separating semiconductor single-walled carbon nanotubes from metallic single-walled carbon nanotubes as described in any one of <1> to <10>, wherein the content of the above-mentioned polymer in the above-mentioned separated single-walled carbon nanotube dispersion is greater than 0.5% by mass and less than 5% by mass.

[0151] <12> A method for producing a semiconductor single-walled carbon nanotube dispersion or a method for separating semiconductor single-walled carbon nanotubes from metallic single-walled carbon nanotubes as described in any one of <1> to <11>, wherein the content of the carbon nanotubes in the separated single-walled carbon nanotube dispersion is greater than 0.03 mass % and less than 0.5 mass %.

[0152] <13> A method for producing a semiconductor single-layer carbon nanotube dispersion or a method for separating semiconductor single-layer carbon nanotubes from metallic single-layer carbon nanotubes as described in any one of <1> to <12>, wherein the average diameter of the single-layer carbon nanotubes used to prepare the separated single-layer carbon nanotube dispersion in the above step A is greater than 0.5 nm and less than 2 nm.

[0153] <14> A method for producing a semiconducting single-walled carbon nanotube dispersion, comprising: step A, preparing a separated single-walled carbon nanotube dispersion, wherein the separated single-walled carbon nanotube dispersion contains single-walled carbon nanotubes including semiconducting single-walled carbon nanotubes and metallic single-walled carbon nanotubes, an aqueous medium, and a nonionic polymer containing a structural unit A derived from a monomer represented by the above formula (1); and

[0154] Step B, after centrifuging the separated single-walled carbon nanotube dispersion, extracting a supernatant containing the semiconductor single-walled carbon nanotubes from the separated single-walled carbon nanotube dispersion after centrifugation;

[0155] The average diameter of the single-walled carbon nanotubes used to prepare the separated single-walled carbon nanotube dispersion in the step A is 0.5 nm or more and 2 nm or less.

[0156] The content of the structural unit A in all structural units of the above-mentioned polymer is 2 mol% or more, and the above-mentioned polymer is water-soluble,

[0157] The number of ethyleneoxy groups derived from the structural unit A per structural unit in the polymer is 0.5 or more and 120 or less.

[0158] <15> A method for producing semiconducting single-walled carbon nanotubes, comprising the step of filtering a dispersion of semiconducting single-walled carbon nanotubes obtained by the method of any one of <1> to <14> to extract the semiconducting single-walled carbon nanotubes.

[0159] <16> A method for producing semiconducting single-walled carbon nanotubes, comprising the following steps: a step of drying a semiconducting single-walled carbon nanotube dispersion obtained by any one of the methods <1> to <14> to obtain a mixture containing the semiconducting single-walled carbon nanotubes and the above-mentioned polymer; and a step of removing the above-mentioned polymer from the above-mentioned mixture to extract the semiconducting single-walled carbon nanotubes.

[0160] <17> A method for producing semiconducting single-walled carbon nanotubes, comprising obtaining the semiconducting single-walled carbon nanotube dispersion obtained by the method according to any one of <1> to <14> as semiconducting single-walled carbon nanotubes without further performing a separation treatment.

[0161] <18> A method for producing an ink containing semiconductor single-walled carbon nanotubes, the method comprising the production method according to any one of <1> to <17> as one step.

[0162] <19> An ink containing semiconducting single-walled carbon nanotubes, comprising: at least one of an organic solvent and water, semiconducting single-walled carbon nanotubes, and a nonionic polymer as specified in any one of <1> to <9>; the content of structural unit A in all structural units of the above-mentioned polymer is greater than 2 mol%, and the above-mentioned polymer is water-soluble.

[0163] <20> An aqueous dispersion comprising: semiconductor single-walled carbon nanotubes; and a polymer comprising a structural unit A derived from a monomer represented by the above formula (1), wherein the content of the structural unit A in all structural units is 2 mol % or more.

[0164] <21> Use of a polymer for separating semiconducting single-walled carbon nanotubes, wherein the polymer comprises a structural unit A derived from a monomer represented by the above formula (1), and the content of the structural unit A in all structural units is 2 mol% or more.

[0165] Example

[0166] Hereinafter, the present invention will be described in further detail by way of Examples, but these are merely illustrative and the present invention is not limited to these Examples.

[0167] 1. Determination methods of various parameters

[0168] [Determination of Weight Average Molecular Weight of Polymer]

[0169] The weight average molecular weight of the polymer used for preparing the isolated SWCNT dispersion was measured under the following conditions using gel permeation chromatography (hereinafter also referred to as "GPC") method.

[0170] <GPC conditions>

[0171] Measuring device: HLC-8320GPC (manufactured by Tosoh Corporation)

[0172] Column: α-M+α-M (manufactured by Tosoh Corporation)

[0173] Eluent: 60mmol / L H3PO4 and 50mmol / L LiBr in N,N-dimethylformamide (DMF) solution

[0174] Flow rate: 1.0mL / min

[0175] Column temperature: 40°C

[0176] Detection: RI

[0177] Sample volume: 0.5 mg / mL

[0178] Standard material: Monodisperse polystyrene (manufactured by Tosoh Corporation)

[0179] [Evaluation of water solubility]

[0180] 1 g of polymer (or compound) was added to 100 g of water at 20°C, stirred for 5 minutes, and the presence of insoluble matter was visually observed. The case where no insoluble matter was observed was judged to be water-soluble. In Tables 1 and 2, the case judged to be water-soluble was recorded as A, and the case judged to be water-insoluble was recorded as B.

[0181] [Measurement of average diameter and average length of SWCNT]

[0182] The average diameter and average length of SWCNT can be calculated by measuring the diameters and lengths of 10 or more CNTs from an image obtained using a transmission electron microscope and averaging the measured values.

[0183] 2. Production of polymers 1 to 16

[0184] [Polymer 1]

[0185] 15 g of ethanol was added to a reaction container equipped with a stirrer, a reflux tube, a thermometer, and dropping funnels 1 and 2. The reaction system was replaced with nitrogen while stirring, and then the temperature was raised to 80°C. In a dropping funnel 1, a solution prepared by dissolving 50 g (100 mol%) of methoxypolyethylene glycol (23) methacrylate ("M-230G" manufactured by Shin-Nakamura Chemical Co., Ltd.) as a polymerization monomer and 0.15 g (3.0 mol% relative to the monomer) of 3-mercapto-1,2-propanediol (Fujifilm Wako Pure Chemical Industries, Ltd.) as a chain transfer agent in 23 g of ethanol was prepared, and in a dropping funnel 2, a solution prepared by dissolving 0.06 g (0.5 mol% relative to the monomer) of 2,2'-azobis(2,4-dimethylvaleronitrile) ("V-65B" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a polymerization initiator in 37 g of ethanol was prepared, and the mixture was added dropwise over 1 hour. After the addition was completed, the mixture was aged for 1 hour while stirring, and after the reaction was completed, the ethanol was distilled off by a rotary evaporator to obtain a polymer 1.

[0186] [Polymers 2 to 16]

[0187] Polymers 2 to 16 were obtained by the same method as the method for producing Polymer 1 except that the amounts of monomers, chain transfer agents, and polymerization initiators shown in Table 1 were changed.

[0188] Table 1 shows the physical properties of polymers 1 to 16.

[0189] The monomers used in the production of polymers 1 to 16 are as follows.

[0190] (Monomer A)

[0191] PEG(23)MA: polyethylene glycol (23) monomethacrylate ["NKESTETR M-230G" manufactured by Shin-Nakamura Chemical Co., Ltd.] (in formula (1), R 1 , R 2 = methyl, p = 23, q = 0)

[0192] PEG(9)MA: polyethylene glycol (9) monomethacrylate [“NK ESTETRM-90G” manufactured by Shin-Nakamura Chemical Co., Ltd.] (In the formula (1), R 1, R 2 = methyl, p = 9, q = 0)

[0193] PEG(4)MA: polyethylene glycol (4) monomethacrylate [“NK ESTETRM-40G” manufactured by Shin-Nakamura Chemical Co., Ltd.] (In the formula (1), R 1 , R 2 = methyl, p = 4, q = 0)

[0194] PEG(23)A: polyethylene glycol (23) monoacrylate ["NK ESTETRAM-230G" manufactured by Shin-Nakamura Chemical Co., Ltd.] (in the formula (1), R 1 =H, R 2 = methyl, p = 23, q = 0)

[0195] PEG(9)A: polyethylene glycol (9) monoacrylate [“AM-90G” manufactured by Shin-Nakamura Chemical Co., Ltd.] (in the formula (1), R 1 =H, R 2 = methyl, p = 9, q = 0)

[0196] (Monomer B)

[0197] PEG(2)MA: polyethylene glycol (2) monomethacrylate [“NK ESTETRM-20G” manufactured by Shin-Nakamura Chemical Co., Ltd.] (In formula (2), R 3 , R 4 = methyl, r = 2, s = 0)

[0198] HEMA: 2-Hydroxyethyl methacrylate [manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.]

[0199] LMA: Lauryl methacrylate [manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.]

[0200] BzMA: Benzyl methacrylate [manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.]

[0201] [Table 1]

[0202]

[0203] 3. Preparation of Semiconducting SWCNT Dispersion

[0204] [Examples 1 to 12, Comparative Examples 1 to 2]

[0205] To 30 mL of a 1 mass % aqueous solution prepared by dissolving the polymers shown in Table 2 in ultrapure water (manufactured by Wako Pure Chemical Industries, Ltd.), 30 mg of a SWCNT mixture synthesized by the HiPco method ("HiPco-Raw" manufactured by NanoIntegris; average diameter: 0.8-1.2 nm; average length: 0.4-0.7 μm) was added to obtain a mixed solution.

[0206] Next, while stirring with a stirrer, dispersion was performed with an ultrasonic homogenizer ("450D" manufactured by BRANSON) at an amplitude of 30% and 10°C for 10 minutes to obtain a separated SWCNT dispersion as shown in Table 2. The contents of the SWCNT mixture and the polymer in the separated SWCNT dispersion are shown in Table 2, and the water content is the remainder after removing the SWCNT mixture and the polymer.

[0207] The separated SWCNT dispersion was centrifuged for 60 minutes using an ultracentrifuge ("CS100GXII" manufactured by Hitachi Koki Co., Ltd., rotor S50A) at a rotation speed of 50,000 rpm, a gravitational acceleration of 210 kG, and 20°C. Thereafter, 80% of the supernatant was extracted from the liquid surface on a volume basis in a manner that did not allow the precipitated sediment to float, thereby obtaining semiconductor-type SWCNT dispersions of Examples 1 to 12 and Comparative Examples 1 to 2.

[0208] [Comparative Examples 3 and 4]

[0209] The same procedure as in Example 1 was followed except that the compounds shown in Table 2 were used instead of the polymer to obtain a separated SWCNT dispersion and a supernatant (semiconductor-type SWCNT dispersion) of Comparative Example 3. The contents of the SWCNT mixture and the compound in the separated SWCNT dispersion are shown in Table 2, and the water content is the remainder after removing the SWCNT mixture and the compound.

[0210] The compounds used in the preparation of the semiconductor-type SWCNT dispersions of Comparative Examples 3 and 4 are shown below.

[0211] Polyoxyethylene (100) stearyl ether ("Brij S100" manufactured by Sigma-Aldrich)

[0212] Sodium Lauryl Sulfate

[0213] 4. Evaluation

[0214] [Separability evaluation]

[0215] The absorbance was measured using an ultraviolet-visible near-infrared spectrophotometer ("UV-3600Plus" manufactured by Shimadzu Corporation) that can measure visible light to infrared light. Then, the value obtained by taking the ratio of the peak intensity representing the semiconductor-type SWCNT to the peak intensity representing the metal-type SWCNT was calculated and used as an evaluation criterion for the separation of the metal-type SWCNT and the semiconductor-type SWCNT. The higher the calculated value, the higher the semiconductor-type SCNT separation can be evaluated. The results are shown in Table 2.

[0216] [Mathematical formula 2]

[0217]

[0218] It should be noted that the SWCNT (HIPCO) used has a unique wavelength of semiconductor-type SWCNT at around 730 nm and a unique wavelength of metal-type SWCNT at around 480 nm.

[0219] [Table 2]

[0220]

[0221] As shown in Table 2, the SWCNT dispersions separated in Examples 1 to 12 were superior in the separation properties of semiconductor-type SWCNTs compared to the SWCNT dispersions separated in Comparative Examples 1 to 4.

[0222] Industrial Applicability

[0223] As described above, according to the method for producing a semiconductor SWCNT dispersion of the present invention, metal SWCNTs and semiconductor SWCNTs can be separated in an aqueous medium without using a density gradient forming agent or the like, using an easily available separation agent and a simple operation. Therefore, it is expected that the production efficiency of the method for producing a semiconductor SWCNT dispersion and semiconductor SWCNTs themselves can be improved.

Claims

1. A method for producing a semiconductor single-walled carbon nanotube dispersion, comprising the following steps: Step A, preparing a separated single-walled carbon nanotube dispersion, wherein the separated single-walled carbon nanotube dispersion contains single-walled carbon nanotubes including semiconductor single-walled carbon nanotubes and metallic single-walled carbon nanotubes, an aqueous medium, and a nonionic polymer containing a structural unit A derived from a monomer represented by the following formula (1); and Step B, after centrifuging the separated single-walled carbon nanotube dispersion, extracting a supernatant containing the semiconductor single-walled carbon nanotubes from the separated single-walled carbon nanotube dispersion after centrifugation, The content of the structural unit A in all structural units of the polymer is 2 mol% or more, the polymer is water-soluble, CH 2 =CR 1 -COO-(EO) p (PO) q -R 2 (1) In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average number of added moles of the ethyleneoxy group, which is 4 to 120, and q represents the average number of added moles of the propyleneoxy group, which is 0 to 50.

2. The method for producing a semiconductor single-walled carbon nanotube dispersion according to claim 1, in, In formula (1), p is 4 or more and 25 or less.

3. The method for producing a semiconductor single-walled carbon nanotube dispersion according to claim 1 or 2, in, In formula (1), q is 0 or more and 3 or less.

4. The method for producing a semiconductor single-walled carbon nanotube dispersion according to claim 1 or 2, in, The number of ethylene groups derived from the structural unit A per structural unit in the polymer is 0.5 or more and 120 or less.

5. The method for producing a semiconductor single-walled carbon nanotube dispersion according to claim 1 or 2, in, The number of ethylene groups derived from the structural unit A per structural unit in the polymer is 0.5 or more and 25 or less.

6. The method for producing a semiconductor single-walled carbon nanotube dispersion according to claim 1 or 2, in, The content of the structural unit A in all the structural units of the polymer is, in mol%, 5 mol% or more and 100 mol% or less.

7. The method for producing a semiconductor single-walled carbon nanotube dispersion according to claim 1 or 2, in, The content of the structural unit A in all the structural units of the polymer is, in mass %, 10 mass % or more and 100 mass % or less.

8. The method for producing a semiconductor single-walled carbon nanotube dispersion according to claim 1 or 2, in, The content of the structural unit A in all the structural units of the polymer is 100 mol %.

9. The method for producing a semiconductor single-walled carbon nanotube dispersion according to claim 1 or 2, in, The polymer further comprises a structural unit B, wherein the structural unit B is derived from at least one monomer B selected from the group consisting of a monomer represented by the following formula (2), a (meth)acrylate monomer, a (meth)acrylamide monomer, a styrene monomer, and a (meth)acrylonitrile monomer. CH 2 =CR 3 -COO-(EO) r (PO) s -R 4 (2) In formula (2), R 3 represents a hydrogen atom or a methyl group, R 4 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, r represents the average number of added moles of the ethyleneoxy group, which is 1 to less than 4, and s represents the average number of added moles of the propyleneoxy group, which is 0 to 50.

10. The method for producing a semiconducting single-walled carbon nanotube dispersion according to claim 9, in, The content of the structural unit B in all the structural units of the polymer is greater than 0 mol % and 98 mol % or less.

11. The method for producing a semiconducting single-walled carbon nanotube dispersion according to claim 9, in, The content of the structural unit B in all the structural units of the polymer is, in mol%, 5 mol% or more and 95 mol% or less.

12. The method for producing a semiconducting single-walled carbon nanotube dispersion according to claim 9, in, The content of the structural unit B in all the structural units of the polymer is 4 mass % or more and 80 mass % or less in terms of mass %.

13. The method for producing a semiconducting single-walled carbon nanotube dispersion according to claim 9, in, The mass ratio A / B of the structural unit A to the structural unit B in the polymer is 0.25 or more and 33 or less.

14. The method for producing a semiconducting single-walled carbon nanotube dispersion according to claim 9, in, The monomer B is at least one selected from the group consisting of 2-hydroxyethyl methacrylate (HEMA), lauryl methacrylate (LMA), and benzyl methacrylate (BzMA).

15. The method for producing a semiconductor single-walled carbon nanotube dispersion according to claim 1 or 2, in, The mass ratio of the polymer to the single-walled carbon nanotubes SWCNT in the separated single-walled carbon nanotube dispersion, ie, polymer / SWCNT, is 0.5 or more and 20 or less.

16. The method for producing a semiconductor single-walled carbon nanotube dispersion according to claim 1 or 2, in, The average diameter of the single-walled carbon nanotubes used to prepare the separated single-walled carbon nanotube dispersion in the step A is 0.5 nm or more and 2 nm or less.

17. The method for producing a semiconductor single-walled carbon nanotube dispersion according to claim 1 or 2, in, The separation efficiency of the semiconductor single-walled carbon nanotubes in the supernatant obtained in step B is 1.1 or more; Here, the separability of the semiconductor single-walled carbon nanotube, i.e., the semiconductor SWCNT, is a value obtained according to the following formula:

18. The method for producing a semiconductor single-walled carbon nanotube dispersion according to claim 1 or 2, in, The separation efficiency of the semiconductor single-walled carbon nanotubes in the supernatant obtained in step B is 1.6 or more.

19. A method for producing a semiconductor single-walled carbon nanotube, comprising the following steps: A step of filtering the semiconducting single-walled carbon nanotube dispersion obtained by the method for producing a semiconducting single-walled carbon nanotube dispersion according to any one of claims 1 to 18 to extract the semiconducting single-walled carbon nanotubes.

20. A method for producing a semiconductor single-walled carbon nanotube, comprising the following steps: A step of drying the semiconducting single-walled carbon nanotube dispersion obtained by the method for producing a semiconducting single-walled carbon nanotube dispersion according to any one of claims 1 to 18 to obtain a mixture containing the semiconducting single-walled carbon nanotubes and the polymer; and A step of removing the polymer from the mixture to extract the semiconductor single-walled carbon nanotubes.

21. A method for producing semiconducting single-walled carbon nanotubes, comprising obtaining the semiconducting single-walled carbon nanotube dispersion obtained by the method for producing a semiconducting single-walled carbon nanotube dispersion according to any one of claims 1 to 18 as semiconducting single-walled carbon nanotubes without further separation treatment.

22. A method for separating semiconductor single-walled carbon nanotubes from metallic single-walled carbon nanotubes, comprising the following steps: Step A, preparing a separated single-walled carbon nanotube dispersion, wherein the separated single-walled carbon nanotube dispersion contains single-walled carbon nanotubes including semiconductor single-walled carbon nanotubes and metallic single-walled carbon nanotubes, an aqueous medium, and a nonionic polymer containing a structural unit A derived from a monomer represented by the following formula (1); and Step B, after centrifuging the separated single-walled carbon nanotube dispersion, extracting a supernatant containing the semiconductor single-walled carbon nanotubes from the separated single-walled carbon nanotube dispersion after centrifugation, The content of the structural unit A in all structural units of the polymer is 2 mol% or more, the polymer is water-soluble, CH 2 =CR 1 -COO-(EO) p (PO) q -R 2 (1) In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average number of added moles of the ethyleneoxy group, which is 4 to 120, and q represents the average number of added moles of the propyleneoxy group, which is 0 to 50.

23. A method for producing an ink containing semiconductor single-walled carbon nanotubes, comprising the production method according to any one of claims 1 to 21 as one step.

24. An ink containing semiconducting single-walled carbon nanotubes, comprising: at least one of an organic solvent and water, semiconducting single-walled carbon nanotubes, and a nonionic polymer containing a structural unit A derived from a monomer represented by the following formula (1), The content of the structural unit A in all structural units of the polymer is 2 mol% or more, the polymer is water-soluble, CH 2 =CR 1 -COO-(EO) p (PO) q -R 2 (1) In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average number of added moles of the ethyleneoxy group, which is 4 to 120, and q represents the average number of added moles of the propyleneoxy group, which is 0 to 50.

25. An aqueous dispersion comprising: Semiconducting single-walled carbon nanotubes; and A polymer comprising a structural unit A derived from a monomer represented by the following formula (1), wherein the content of the structural unit A in all structural units is 2 mol% or more, CH 2 =CR 1 -COO-(EO) p (PO) q -R 2 (1) In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average number of added moles of the ethyleneoxy group, which is 4 to 120, and q represents the average number of added moles of the propyleneoxy group, which is 0 to 50.

26. Use of a polymer for separating semiconducting single-walled carbon nanotubes, the polymer comprising a structural unit A derived from a monomer represented by the following formula (1), wherein the content of the structural unit A in all structural units is 2 mol% or more, CH 2 =CR 1 -COO-(EO) p (PO) q -R 2 (1) In formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, EO represents an ethyleneoxy group, PO represents a propyleneoxy group, p represents the average number of added moles of the ethyleneoxy group, which is 4 to 120, and q represents the average number of added moles of the propyleneoxy group, which is 0 to 50.