Semiconductor processing tape
By forming an antistatic layer on a substrate and preparing a single-layer adhesive layer, the problems of complex manufacturing and residual adhesive residue in the prior art are solved, achieving simplified manufacturing and efficient protection of the tape used in semiconductor processing.
Patent Information
- Application Number
- CN202080078579.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-17
- Filing Date
- 2020-12-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-12-15
AI Technical Summary
Existing adhesive films for semiconductor processing involve complex manufacturing processes and are prone to adhesive layer transfer residue during peeling, making it difficult to simultaneously achieve sufficient surface absorption, antistatic properties, and appropriate adhesion.
An antistatic layer is formed on a sheet substrate, and an adhesive layer is prepared on it. The adhesive layer is composed of polyurethane, (meth)acrylate monomer, chain transfer agent and photopolymerization initiator, with a thickness of 50-500 μm and a single-layer structure to ensure antistatic performance and adhesion.
It achieves effective protection of surface irregularities in semiconductor processing, reduces residual adhesive during peeling, simplifies manufacturing processes, and maintains good surface irregularity absorption and antistatic properties.
Smart Images

Figure BDA0003638697750000291 
Figure BDA0003638697750000341
Abstract
Description
Technical Field
[0001] The present invention relates to tapes for semiconductor processing. Background Art
[0002] As semiconductor devices are required to be thinner, a back grinding process of a semiconductor wafer is performed in the manufacturing process of semiconductor devices. In the back grinding process of a semiconductor wafer, the surface of the semiconductor wafer is protected with a back grinding tape, and then the back side is ground to thin the semiconductor wafer.
[0003] This application claims priority based on Japanese Patent Application No. 2019-227280 filed in Japan on December 17, 2019, the contents of which are incorporated herein by reference.
[0004] Various back grinding tapes have been proposed for protecting the surface of semiconductor wafers. In recent years, back grinding tapes have been required to have sufficient unevenness absorption even for semiconductor wafers having uneven surfaces, such as semiconductor wafers having bumps (electrodes) formed of solder or the like on the surface.
[0005] Furthermore, conventionally, when the back grinding tape is peeled off from the semiconductor wafer, static electricity called peeling electrification may be generated, which may damage the circuit of the semiconductor wafer or cause foreign matter to adhere to the semiconductor wafer. Therefore, the back grinding tape is required to have sufficient antistatic properties.
[0006] It can be considered that the treatment for preventing peeling electrification is effective when applied to the adhesive side. However, if a material with an antistatic effect such as a surfactant, a conductive filler, and carbon black is added to the adhesive itself, the physical properties of the adhesive change. In addition, it becomes difficult to adjust or suppress the physical properties of the adhesive and its changes over time. Furthermore, when the adhesive tape is peeled off, the adhesive and the added antistatic material itself may move to the adherend and contaminate the adherend. In this case, residual glue visible to the naked eye, adhesion of granular materials at the microscope level, or adhesion of liquid materials that cannot be observed optically occur on the surface of the adherend, which may cause adverse effects such as poor bonding of components in subsequent processes.
[0007] Based on such a background, for example, in Patent Document 1, an adhesive film for semiconductor wafer processing is disclosed, which sequentially comprises a base layer, a bump-absorbing resin layer, an antistatic layer, and an adhesive resin layer, as a back grinding tape having both bump-absorbing and antistatic properties.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2018-6540 Summary of the invention
[0011] Problems to be solved by the invention
[0012] However, the adhesive film for semiconductor wafer processing described in Patent Document 1 needs to be manufactured by laminating each layer after being sliced. Therefore, the manufacturing steps are complicated. In addition, the back grinding tape is required to have an adhesive force that can fix the adherend such as the semiconductor wafer to the back grinding tape with sufficient strength. However, if the back grinding tape with high adhesive force is pasted to the adherend and then the adherend is processed, and then the back grinding tape is peeled off, sometimes the adhesive layer of the back grinding tape is transferred to the adherend and residual glue occurs.
[0013] The present invention is proposed in view of the above situation, and its purpose is to provide a semiconductor processing tape that has sufficient unevenness absorption, appropriate adhesion, antistatic performance, is unlikely to have residual adhesive after peeling off the semiconductor processing tape, and can be manufactured with a small number of manufacturing steps.
[0014] Methods for solving problems
[0015] The present invention includes the following aspects.
[0016] [1] A tape for semiconductor processing, comprising a sheet-like substrate and an adhesive layer,
[0017] The sheet-like substrate comprises a substrate main body and an antistatic layer provided on at least one surface of the substrate main body.
[0018] The adhesive layer is formed on the antistatic layer;
[0019] The antistatic layer contains a polypyrrole compound.
[0020] The adhesive layer is a cured product of the adhesive composition.
[0021] The thickness of the adhesive layer is 50 to 500 μm.
[0022] The adhesive composition comprises polyurethane (A), (meth)acrylate monomer (B), chain transfer agent (C), and photopolymerization initiator (D).
[0023] The polyurethane (A) contains polyurethane (a1),
[0024] The polyurethane (a1) has a skeleton including a structure derived from a polyoxyalkylene polyol and a structure derived from a polyisocyanate, and has (meth)acryloyl groups at a plurality of terminals.
[0025] The (meth)acrylate monomer (B) includes monofunctional (meth)acrylate and polyfunctional (meth)acrylate.
[0026] [2] The semiconductor processing tape according to [1], wherein the adhesive layer has a single-layer structure.
[0027] [3] The semiconductor processing tape according to [1] or [2], wherein the chain transfer agent (C) is a polyfunctional thiol.
[0028] [4] The semiconductor processing tape according to any one of [1] to [3], wherein the adhesive layer has a gel fraction of 50 to 65% by mass.
[0029] [5] The semiconductor processing tape according to any one of [1] to [4], wherein the surface resistivity of the adhesive layer is less than 1×10 12 Ω / □.
[0030] [6] The semiconductor processing tape according to any one of [1] to [5], wherein the (meth)acrylate monomer (B) contains 85 to 99 mol % of the monofunctional (meth)acrylate and 1 to 15 mol % of the polyfunctional (meth)acrylate.
[0031] [7] The semiconductor processing tape according to any one of [1] to [6], wherein the adhesive composition comprises:
[0032] 20 to 50% by mass of the polyurethane (A),
[0033] 35 to 79% by mass of the (meth)acrylate monomer (B),
[0034] The chain transfer agent (C) is 0.5 to 8% by mass,
[0035] The photopolymerization initiator (D) is contained in an amount of 0.01 to 5% by mass.
[0036] [8] The tape for semiconductor processing according to any one of [1] to [7], wherein the adhesive composition further contains a fatty acid ester (E).
[0037] Effects of the Invention
[0038] According to the present invention, it is possible to provide a semiconductor processing tape which has sufficient unevenness absorption, appropriate adhesive strength, and antistatic performance, and which is unlikely to leave adhesive residue after the semiconductor processing tape is peeled off.
[0039] Moreover, the semiconductor processing tape of the present invention has sufficient unevenness absorption and adhesiveness because the adhesive layer is a cured product of the adhesive composition, so it is not necessary to separately provide a layer having unevenness absorption and a layer having adhesiveness, and can be manufactured with a minimum number of manufacturing steps. Furthermore, by forming the adhesive layer on the substrate having the antistatic layer, it can have sufficient antistatic performance.
[0040] Therefore, the semiconductor processing tape of the present invention is suitable as a back grinding tape used to protect the surface when performing a back grinding step of an adherend having uneven surfaces such as a semiconductor wafer having bumps formed on the surface. DETAILED DESCRIPTION
[0041] Hereinafter, embodiments of the present invention will be described in detail. However, the present invention is not limited to the embodiments described below.
[0042] <Tape for semiconductor processing>
[0043] The semiconductor processing tape in the present embodiment has a sheet-like substrate and an adhesive layer formed on one side of the substrate. The substrate has a substrate body and an antistatic layer provided on at least one side of the substrate body. The antistatic layer contains a polypyrrole compound. The adhesive layer is a cured product of the adhesive composition described later. The thickness of the adhesive layer is 50 to 500 μm. The adhesive composition contains polyurethane (A), (meth)acrylate monomer (B), chain transfer agent (C), and photopolymerization initiator (D). The polyurethane (A) contains polyurethane (a1). The polyurethane (a1) has a skeleton containing a structure derived from a polyoxyalkylene polyol and a structure derived from a polyisocyanate, and has a (meth)acryloyl group at multiple ends. The (meth)acrylate monomer (B) contains a monofunctional (meth)acrylate and a polyfunctional (meth)acrylate.
[0044] The "belt" referred to here is not limited to a belt-shaped piece, but also includes a rectangular or disk-shaped piece.
[0045] (Material body)
[0046] The material of the substrate body can be appropriately selected, and for example, resin materials can be cited. As resin materials, polyolefins such as polyethylene (PE) and polypropylene (PP) can be cited; polyester sheets such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyethylene naphthalate; polyvinyl chloride (PVC); polyimide (PI); polyphenylene sulfide (PPS); ethylene vinyl acetate (EVA); polytetrafluoroethylene (PTFE), etc. Among these resin materials, in order to obtain a sheet with appropriate flexibility, PE, PP, and PET are preferably used. The resin material can be used alone or in combination with two or more.
[0047] When a resin sheet formed of a resin material is used as the substrate body, the resin sheet may be a single layer or a multilayer structure having two or more layers (e.g., a three-layer structure). In a resin sheet having a multilayer structure, the resin material constituting each layer may be a resin material containing only one type alone or a resin material containing two or more types.
[0048] Furthermore, the surface of the substrate body on which the antistatic layer is to be formed may be subjected to an adhesion-facilitating treatment such as acid treatment, alkali treatment, primer treatment, corona treatment, plasma treatment, ultraviolet treatment, ozone treatment, etc., as necessary.
[0049] The thickness of the substrate body can be appropriately selected according to the material of the substrate body, etc. In the case where the semiconductor processing tape is pasted on a semiconductor wafer having a concave-convex portion on the surface and then peeled off, in addition, in the case where the semiconductor processing tape uses a resin sheet as the substrate body, the thickness of the substrate body is preferably 10 to 1000 μm, and more preferably 50 to 300 μm. If the thickness of the substrate body is 10 μm or more, the rigidity (toughness) of the semiconductor processing tape becomes higher. Therefore, when the semiconductor processing tape is pasted on a semiconductor wafer as an adherend or peeled off, there is a tendency that the semiconductor processing tape is not easy to wrinkle and float. In addition, if the thickness of the substrate body is less than 1000 μm, it is easy to peel off the semiconductor processing tape pasted on the semiconductor wafer from the semiconductor wafer, and the workability (handling, operation) becomes good.
[0050] (Antistatic layer)
[0051] At least one side of the substrate body has an antistatic layer. The antistatic layer contains a polypyrrole compound. The polypyrrole compound is not particularly limited as long as it is a polymer of pyrrole and / or pyrrole derivatives, and as a polymer component, it can contain a small amount of other monomers other than pyrrole and pyrrole derivatives. As pyrrole derivatives, N-alkylpyrrole, 3-alkylpyrrole, 3,4-dialkylpyrrole, 3-alkoxypyrrole, 3,4-dialkoxypyrrole, 3-chloropyrrole, 3,4-dichloropyrrole, etc. can be cited. By having an antistatic layer containing a polypyrrole compound, the time stability and non-contamination of the antistatic effect of the semiconductor processing belt become good.
[0052] The means for providing the antistatic layer is not particularly limited, and various known methods can be adopted. For example, the following methods (i) to (vi) can be mentioned.
[0053] (i) A method in which pyrrole and / or a pyrrole derivative is dissolved in an organic solvent such as diethyl ether, methanol, tetrahydrofuran (THF), applied to the substrate body, and then the organic solvent is dried and removed (e.g., Japanese Patent Application Laid-Open No. 3-122115);
[0054] (ii) a method in which pyrrole and / or a pyrrole derivative is applied to a substrate body, the substrate body is doped by immersing the substrate body in an organic solvent of a salt or an acid, water or a mixture thereof, and the solvent is then removed by drying (e.g., Japanese Patent Application Laid-Open No. 4-285626);
[0055] (iii) A method in which a pyrrole monomer is polymerized in a treatment solution to which a substrate body has been added in the presence of a chemical oxidation polymerization catalyst and a dopant, thereby coating the surface of the substrate body with polypyrrole (e.g., Japanese Patent Application Laid-Open No. 2000-280335);
[0056] (iv) A method in which an aqueous solution containing fine particles coated with pyrrole and / or a pyrrole derivative is applied to the surface of the substrate body, and then stretched after drying (e.g., Japanese Patent Laid-Open No. 8-58044);
[0057] (v) A method in which a layer containing polypyrrole and / or a polypyrrole derivative, an organic electron acceptor, and a thermoplastic resin is laminated on the surface of a substrate body (e.g., Japanese Patent Application Laid-Open No. 10-278188);
[0058] (vi) A method in which microparticles of polypyrrole and / or polypyrrole derivatives are dispersed in a hydrophilic solvent using a polymer dispersant and / or a dopant, and further mixed with a hydrophilic binder resin to prepare a resin composition; the resin composition is applied to a substrate such as a polymer film, and then the solvent is dried and removed (e.g., Japanese Patent Application Laid-Open No. 2001-334598).
[0059] Among them, from the viewpoint of adhesion to the substrate body and adhesion to the adhesive layer, "(vi) fine particles of polypyrrole and / or polypyrrole derivative are dispersed in a hydrophilic solvent using a polymer dispersant and / or a dopant, and further mixed with a water-soluble or water-dispersible binder resin to prepare a resin composition; the resin composition is applied to the substrate body and then the solvent is dried and removed to form the method". It is preferable to use a known coating method such as a rod coater, an air knife coater, a blade coater, a rod coater, a gravure coater, a size press coater, a horizontal roll coater (gate roll coater) or the like.
[0060] As the film thickness of the antistatic layer, preferably 0.1 to 20 μm, more preferably 0.5 to 10 μm. If the thickness of the antistatic layer is within this range, sufficient antistatic performance is exerted. The content of the polypyrrole compound in the antistatic layer is preferably 5 to 80% by mass, more preferably 10 to 70% by mass. If it is 5% by mass or more, sufficient antistatic performance can be obtained, and if it is 80% by mass or less, the economy is also good.
[0061] As the polymer dispersant, specifically, polymer acids, salts of these polymer acids, and esters of these polymer acids can be cited, and they can be used alone or in combination of two or more. Specific examples of polymer acids include polymer acids such as polystyrene sulfonic acid, polyacrylic acid, polyallyl sulfonic acid, and alginic acid. Specific examples of salts of polymer acids include neutralized salts such as sodium salts, potassium salts, and ammonium salts.
[0062] As dopant, it is not particularly limited, preferably molecular iodine and / or iodide ion are used. When iodide ion is used, the iodide ion valence is not particularly specified. By using iodine and / or iodide ion, the conductivity and the adhesion to the substrate body are further improved.
[0063] As water-soluble or water-dispersible binder resins, for example, polyester, polyurethane, acrylic resin, vinyl resin, epoxy resin, amide resin, etc. can be cited. Their respective skeleton structures can substantially have a composite structure by copolymerization, etc. As binder resins with a composite structure, for example, acrylic resin grafted polyester, acrylic resin grafted polyurethane, vinyl resin grafted polyester, vinyl resin grafted polyurethane, etc. can be cited. By containing these resins, the strength of the antistatic layer and the adhesion to the substrate body can be improved. One water-soluble or water-dispersible binder resin can be used alone, or two or more can be used in combination.
[0064] In addition, the resin composition may contain a crosslinking reactive compound as required. The crosslinking reactive compound can improve the cohesion, surface hardness, scratch resistance, solvent resistance, and water resistance of the coating layer mainly through crosslinking reaction with other resins and functional groups contained in the compound or self-crosslinking. As the crosslinking reactive compound that can be used, amino resins such as melamine-based, benzoguanamine-based, and urea-based resins, Oxazoline-based, epoxy-based, glyoxal-based, etc. It also includes polymer-type cross-linking reactive compounds that allow other polymer skeletons to have reactive groups.
[0065] The resin composition may contain additives such as surfactants, defoamers, coating improvers, thickeners, organic lubricants, organic particles, inorganic particles, antioxidants, ultraviolet absorbers, dyes, pigments, etc. These additives may be used alone or in combination of two or more as needed.
[0066] (adhesive layer)
[0067] The adhesive layer is formed on the antistatic layer of the substrate.
[0068] When the antistatic layer is formed on both surfaces of the substrate body, the adhesive layer is formed on any one surface thereof.
[0069] The adhesive layer is a cured product of the adhesive composition described later. The adhesive layer is particularly a photocured product of the adhesive composition described later. The semiconductor processing tape is sometimes used in applications where it is pasted to an adherend such as a semiconductor wafer having concave-convex portions on the surface and then peeled off. In this case, the adhesive layer has the effect of protecting the surface of the adherend in the back grinding process by fixing the semiconductor processing tape to the surface of the adherend with sufficient adhesive force. In addition, the adhesive layer has the effect of smoothing the concave-convex portions on the adherend surface by absorbing them, thereby improving the accuracy of the back grinding process. Further, the adhesive layer reduces the peeling charge generated when the semiconductor processing tape is peeled off from the adherend. In addition, the adhesive layer possessed by the semiconductor processing tape of the present embodiment does not produce residual adhesive when the semiconductor processing tape is peeled off.
[0070] The thickness of the adhesive layer of the present embodiment is 50 to 500 μm, preferably 60 to 400 μm, and more preferably 70 to 300 μm. If the thickness of the adhesive layer is 50 μm or more, the concave-convex absorption and adhesive force of the semiconductor processing tape become good. In addition, if the thickness of the adhesive layer is 500 μm or less, the film thickness control of the adhesive layer becomes easy.
[0071] In the case where the semiconductor processing tape of the present embodiment is pasted to an adherend having a concave-convex portion on the surface, the thickness of the adhesive layer depends greatly on the height of the concave-convex portion on the adherend surface. In order to obtain sufficient concave-convex absorption, the thickness of the adhesive layer is preferably greater than or equal to the height of the concave-convex portion on the surface. Therefore, for example, in the case where the concave-convex on the surface is a bump formed on a semiconductor wafer, it is preferred that the thickness of the adhesive layer is more than twice the height dimension of the bump. The height of the bump is generally 30 to 200 μm. For example, in the case where the height of the bump is 100 μm, the thickness of the adhesive layer is preferably 200 μm or more. In the case where the height of the bump is 200 μm, the thickness of the adhesive layer is preferably 400 μm or more.
[0072] The adhesive layer can be a single-layer structure, or a multilayer structure formed by laminating the adhesive layer of the present embodiment with more than one other adhesive layers different from the adhesive layer of the present embodiment. As other adhesive layers, adhesive layers known in the past can be used. In the present embodiment, when the adhesive layer is a multilayer structure, it is necessary for the adhesive layer of the present embodiment to be present on the outermost surface. In addition, in the semiconductor processing tape of the present embodiment, a layer other than the adhesive layer can be present between the adhesive layer and the substrate within the range of not hindering the curing of the adhesive layer. From the perspective of shortening the process, the adhesive layer is preferably a single-layer structure.
[0073] The gel fraction of the adhesive layer is preferably 50 to 65% by mass. If the gel fraction is 50% by mass or more, the occurrence of residual adhesive caused by peeling off the semiconductor processing tape attached to the adherend can be more effectively suppressed. In addition, if the gel fraction is 65% by mass or less, the adhesive layer has sufficient fluidity, and the bump absorption of the semiconductor processing tape becomes better. The gel fraction of the adhesive layer is more preferably 52% by mass or more. In addition, the gel fraction of the adhesive layer is more preferably 63% by mass or less.
[0074] The preferred range of the gel fraction of the adhesive layer can be achieved, for example, by adjusting the composition of the adhesive composition described below to a preferred range.
[0075] (Measurement of Gel Fraction of Adhesive Layer)
[0076] The gel fraction of the adhesive layer is determined by the following method. First, a piece of about 1 g is cut from a semiconductor processing tape, and the adhesive layer is peeled off from the substrate as a sample for measurement, and its mass is measured. Next, the sample for measurement is immersed in 50 ml of toluene and left to stand at room temperature for 72 hours. Then, the sample for measurement is taken out of toluene, dried at 80°C for 5 hours, and the mass is measured again. Furthermore, the gel fraction is calculated based on the following formula.
[0077] Gel fraction (%) = [A / B] × 100
[0078] A: Mass of the measurement sample after immersion in toluene (mass excluding toluene)
[0079] B: Mass of the measurement sample before immersion in toluene
[0080] The surface resistivity of the adhesive layer is preferably less than 1×10 12 Ω / □, more preferably less than 1×10 11 Ω / □. If the surface resistivity is less than 1×10 12 Ω / □, the peeling electrification when peeling the semiconductor processing tape affixed to the adherend is reduced, and the semiconductor processing tape has a more excellent antistatic performance.
[0081] In the semiconductor processing tape, for the purpose of protecting the adhesive layer, a transparent spacer can be provided on the surface of the adhesive layer. The spacer is preferably laminated on the surface of the adhesive layer. As the material of the spacer, for example, paper, plastic film, etc. can be used. From the perspective of excellent surface smoothness, plastic film is preferably used. As the plastic film that can be used as a spacer, as long as it can protect the above-mentioned adhesive layer, there is no particular limitation, and for example, polyethylene, polypropylene, polyethylene terephthalate, polybutylene, etc. can be cited.
[0082] <Adhesive composition>
[0083] The adhesive layer of the semiconductor processing tape of the present embodiment is a cured product of the adhesive composition. Hereinafter, the adhesive composition used as a material of the adhesive layer in the semiconductor processing tape of the present embodiment will be described in detail.
[0084] The adhesive composition of the present embodiment contains polyurethane (A), a (meth)acrylate monomer (B), a chain transfer agent (C), and a photopolymerization initiator (D).
[0085] (Polyurethane (A))
[0086] Polyurethane (A) includes polyurethane (a1) described later. In polyurethane (A), for the purpose of adjusting the cohesive force in the cured product of the adhesive composition, it may include not only polyurethane (a1) but also polyurethane (a2) described later. In polyurethane (A), it is preferred not to include components other than polyurethane (a1) and polyurethane (a2) contained as required.
[0087] [Polyurethane (a1)]
[0088] The polyurethane (a1) has a skeleton including a structure derived from a polyoxyalkylene polyol and a structure derived from a polyisocyanate. In addition, the polyurethane (a1) has a (meth)acryloyl group at a plurality of terminals. The terminal (meth)acryloyl group of the polyurethane (a1) is preferably a part of a (meth)acryloyloxy group.
[0089] In the present invention, the so-called "plurality of terminals" of the polyurethane refers to two terminals when the polyurethane is a linear polymer, and refers to two or more terminals among the terminals having the same number as the number of branches when the polyurethane is a branched polymer.
[0090] In the present invention, the (meth)acryloyl group refers to one or more functional groups selected from the group consisting of a functional group represented by the chemical formula CH2=CH-CO- and a functional group represented by the chemical formula CH2=C(CH3)-CO-.
[0091] [Polyurethane (a2)]
[0092] Polyurethane (a2) has a skeleton containing a structure derived from polyoxyalkylene polyol and a structure derived from polyisocyanate, similarly to polyurethane (a1). Polyurethane (a2) is different from polyurethane (a1) in that it has a (meth)acryloyl group only at one end. The (meth)acryloyl group at the end possessed by polyurethane (a2) is preferably a part of a (meth)acryloyloxy group. The end without a (meth)acryloyl group in polyurethane (a2) preferably has one selected from an isocyanate group, a structure derived from an alkyl alcohol, and a structure derived from an alkyl isocyanate, and more preferably has a structure derived from an alkyl alcohol.
[0093] "Structure derived from polyoxyalkylene polyol"
[0094] The polyoxyalkylene polyol that forms the polyoxyalkylene polyol-derived structure contained in the skeleton of polyurethane (a1) and polyurethane (a2) is preferably a polyoxyalkylene polyol having an alkylene chain having 2 to 4 carbon atoms. Specific examples thereof include polyoxyethylene polyol, polyoxypropylene polyol, polyoxybutylene polyol, and the like.
[0095] The polyoxyalkylene polyol forming the structure derived from the polyoxyalkylene polyol may contain one type of alkylene chain, or may contain two or more types of alkylene chains.
[0096] The polyoxyalkylene polyol forming the structure derived from the polyoxyalkylene polyol preferably has two or three hydroxyl groups at the terminal (diol-type or triol-type polyoxyalkylene polyol), more preferably polyoxyalkylene glycol (diol-type), and particularly preferably polypropylene glycol having an alkylene chain having 3 carbon atoms.
[0097] For example, when the polyoxyalkylene polyol is polypropylene glycol, the hydroxyl value is preferably 20 to 120 mgKOH / g, more preferably 30 to 100 mgKOH / g, and further preferably 40 to 80 mgKOH / g. Specific examples of polypropylene glycol include polypropylene glycol having a hydroxyl group at the end and a hydroxyl value of 56 mgKOH / g (Actocol D-2000; manufactured by Mitsui Chemicals, number average molecular weight 2000, diol type).
[0098] Here, the hydroxyl value of the polyoxyalkylene polyol is the hydroxyl value of the polyoxyalkylene polyol measured in accordance with JIS K0070. That is, it refers to the number of mg of potassium hydroxide required to neutralize the free acetic acid when 1 g of the polyoxyalkylene polyol is acetylated. Specifically, it can be obtained by acetylation of the hydroxyl groups in the sample (polyoxyalkylene polyol) with acetic anhydride and titration of the free acetic acid generated at this time with a potassium hydroxide solution.
[0099] The number average molecular weight of the polyoxyalkylene polyol is preferably 500 to 5,000, more preferably 800 to 4,000, and further preferably 1,000 to 3,000. If the number average molecular weight of the polyoxyalkylene polyol is 500 or more, the peel strength of the semiconductor processing tape having an adhesive layer as a cured product of an adhesive composition containing a polyurethane (A) synthesized using the polyoxyalkylene polyol is high. In addition, if the number average molecular weight of the polyoxyalkylene polyol is 5,000 or less, the polyurethane (A) synthesized using the polyoxyalkylene polyol contains a sufficient amount of urethane bonds. Therefore, the cohesive force of the cured product obtained by curing the adhesive composition containing the polyurethane (A) is good.
[0100] The structure derived from the polyoxyalkylene polyol contained in the skeleton of each of the polyurethane (a1) and the polyurethane (a2) may be only one type, or may be a structure containing two or more types.
[0101] The polyurethane (a1) and the polyurethane (a2) may have a structure in which two or more different structures derived from polyoxyalkylene polyol are bonded to each other with a structure derived from polyisocyanate interposed therebetween.
[0102] The structure derived from the polyoxyalkylene polyol contained in the skeleton of the polyurethane (a1) and the structure derived from the polyoxyalkylene polyol contained in the skeleton of the polyurethane (a2) may be the same as or different from each other.
[0103] "Structure derived from polyisocyanate"
[0104] As the polyisocyanate forming the polyisocyanate-derived structure contained in the skeleton of the polyurethane (a1) and the polyurethane (a2), a compound having a plurality of isocyanate groups can be used, and diisocyanate is preferably used.
[0105] Examples of the diisocyanate include toluene diisocyanate and hydrogenated products thereof, xylylene diisocyanate and hydrogenated products thereof, diphenylmethane diisocyanate and hydrogenated products thereof, 1,5-naphthalene diisocyanate and hydrogenated products thereof, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, tetramethylxylylene diisocyanate, isophorone diisocyanate, 4,4′-dicyclohexyl diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, and norbornane diisocyanate.
[0106] Among these polyisocyanates, isophorone diisocyanate or a hydrogenated product of diphenylmethane diisocyanate is preferably used from the viewpoint of the light resistance of the polyurethane (A) synthesized using the same and the control of the reactivity with the polyoxyalkylene polyol. In addition, the hydrogenated product of diphenylmethane diisocyanate is more preferably used from the viewpoint of the reactivity with the polyoxyalkylene polyol.
[0107] Specific examples of the polyisocyanate forming a polyisocyanate-derived structure include a hydrogenated product of diphenylmethane diisocyanate (Desmodium W, manufactured by Sumika Combustion Laboratory Co., Ltd.) and isophorone diisocyanate (Desmodium I, manufactured by Sumika Combustion Laboratory Co., Ltd.).
[0108] The polyisocyanate-derived structure contained in the skeleton of each of the polyurethane (a1) and the polyurethane (a2) may be only one type or may be a structure containing two or more types.
[0109] Furthermore, the structure derived from polyisocyanate contained in the skeleton of polyurethane (a1) and the structure derived from polyisocyanate contained in the skeleton of polyurethane (a2) may be the same as or different from each other.
[0110] It is preferred that the polyisocyanate-derived structure and the polyoxyalkylene polyol-derived structure contained in the skeletons of polyurethane (a1) and polyurethane (a2) are the same, because in this case, polyurethane (a1) and polyurethane (a2) can be synthesized simultaneously, and polyurethane (A) can be produced efficiently.
[0111] The ratio of the polyurethane (a1) contained in the polyurethane (A) is preferably 80 to 100% of the polyurethane (A) based on the number of molecules, more preferably 90 to 100%, and even more preferably 100%.
[0112] The ratio of the polyurethane (a2) contained in the polyurethane (A) is preferably 0 to 20% of the polyurethane (A) based on the number of molecules, more preferably 0 to 10%, and even more preferably 0%.
[0113] When the ratio of the polyurethane (a1) contained in the polyurethane (A) is 80% or more, the cohesive force of the cured product of the adhesive composition containing the polyurethane (A) is sufficiently large, which is preferable.
[0114] The (meth)acryloyl group is preferably introduced in 90 to 100% of the total number of terminals contained in the polyurethane (A) (the total number of terminals of the polyurethane (a1) and the number of terminals of the polyurethane (a2) contained as required), more preferably in 95 to 100%, and even more preferably in 100%, based on the number of molecules. If the amount of (meth)acryloyl group introduced in the total number of terminals contained in the polyurethane (A) is 90% or more based on the number of molecules, the cohesive force of the cured product obtained by curing the adhesive composition containing the polyurethane (A) is sufficiently high.
[0115] The ratio of the number of terminals into which the (meth)acryloyl group is introduced, based on the number of molecules, among all the terminals contained in the polyurethane (A) can be calculated using the results of analyzing the polyurethane (A). Examples of the analysis method include infrared absorption spectroscopy (IR) and nuclear magnetic resonance spectroscopy (NMR).
[0116] The ratio of the content of the polyurethane (a1) and the polyurethane (a2) contained in the polyurethane (A), that is, the ratio of the number of terminals into which a (meth)acryloyl group is introduced based on the number of molecules among all the terminals contained in the polyurethane (A), can be adjusted by the method for producing the polyurethane (A) described below.
[0117] The mass average molecular weight of polyurethane (A) is preferably 30,000 to 200,000, more preferably 50,000 to 150,000, and further preferably 60,000 to 100,000. If the mass average molecular weight of polyurethane (A) is 30,000 or more, the cured product obtained by curing the adhesive composition containing polyurethane (A) has good flexibility. In addition, if the mass average molecular weight of polyurethane (A) is 200,000 or less, the adhesive composition containing polyurethane (A) is easy to handle and has good workability.
[0118] (Method for measuring mass average molecular weight of polyurethane (A))
[0119] The mass average molecular weight of the polyurethane (A) is a value in terms of polystyrene measured by gel permeation chromatography (GPC-101; Shodex (registered trademark) manufactured by Showa Denko K.K.) (hereinafter referred to as GPC). The measurement conditions of GPC are as follows.
[0120] Column: LF-804 (Showa Denko K.K.)
[0121] Column temperature: 40°C
[0122] Sample: 0.2 mass % tetrahydrofuran solution of polyurethane (A)
[0123] Flow rate: 1ml / min
[0124] Eluent: Tetrahydrofuran
[0125] Detector: RI detector (differential refractive index detector)
[0126] The content of the polyurethane (A) in the adhesive composition of the present embodiment is preferably 20 to 50% by mass, more preferably 25 to 45% by mass, and further preferably 30 to 40% by mass. If the content of polyurethane (A) is more than 20% by mass, the cured product obtained by curing the adhesive composition has sufficient cohesive force, and excellent adhesion can be obtained. In addition, the cured product is used as a semiconductor processing tape for the adhesive layer, and the flexibility of the adhesive layer becomes an appropriate range, and it is not easy to sandwich bubbles between the adhesive layer and the adherend. In addition, if the content of polyurethane (A) is less than 50% by mass, the cured product obtained by curing the adhesive composition has sufficient flexibility. Therefore, the cured product is used as a semiconductor processing tape for the adhesive layer, and the wettability to the adherend is good.
[0127] ((Meth)acrylate monomer (B))
[0128] The (meth)acrylate monomer (B) is a substance other than the polyurethane (A), and contains a monofunctional (meth)acrylate and a polyfunctional (meth)acrylate.
[0129] In the present invention, the term “monofunctional” in the monofunctional (meth)acrylate refers to a (meth)acrylate having only one (meth)acryloyloxy group.
[0130] In the present invention, the term “multifunctional” in the multifunctional (meth)acrylate refers to a (meth)acrylate having two or more (meth)acryloyloxy groups.
[0131] As the (meth)acrylate monomer (B), from the viewpoint of the cohesive force of the cured product obtained by curing the adhesive composition and the curability of the adhesive composition, it is preferred to use a monofunctional (meth)acrylate in combination with a multifunctional (meth)acrylate. It is more preferred to contain a monofunctional (meth)acrylate and a trifunctional or higher (meth)acrylate. In particular, it is most preferred to contain a monofunctional (meth)acrylate and a trifunctional (meth)acrylate having three (meth)acryloyloxy groups.
[0132] As monofunctional (meth)acrylate, for example, (meth)acrylate alkyl ester, (meth)acrylate cyclic alkyl esters such as isobornyl (meth)acrylate, (meth)acrylate alkoxyalkyl ester, alkoxy (poly) alkylene glycol (meth)acrylate, hydroxyl group-containing (meth)acrylate, carboxyl group-containing (meth)acrylate, (meth)acrylate fluorinated alkyl ester, (meth)acrylate dialkylaminoalkyl ester, (meth)acrylamide, epoxy group-containing (meth)acrylate, (meth)acryloyl morpholine, etc. These may be used alone or in combination of two or more.
[0133] Among these monofunctional (meth)acrylates, it is preferred to contain alkyl (meth)acrylates. The reason is that, when a cured product is used as an adhesive layer of a semiconductor processing tape, the adhesion (peel force) and gel fraction of the cured product obtained by curing the adhesive composition are easily changed to a more appropriate range. As the alkyl (meth)acrylate, it is more preferred to use an alkyl (meth)acrylate having an alkyl group with 4 to 10 carbon atoms. Specifically, as the alkyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc. can be cited. Among them, 2-ethylhexyl (meth)acrylate and / or n-butyl (meth)acrylate are particularly preferably used.
[0134] The polyfunctional (meth)acrylate is a compound other than the polyurethane (A) and having a plurality of (meth)acryloyloxy groups. As the polyfunctional (meth)acrylate, it is preferable to use a poly(meth)acrylate of a polyol compound.
[0135] Specific examples of the polyfunctional (meth)acrylate include polyethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, hydroxypivalate neopentyl glycol di(meth)acrylate, 1,3-bis(hydroxyethyl)-5,5-dimethylhydantoin di(meth)acrylate, α,ω-di(meth)acrylate bis(diethylene glycol phthalate), trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, diacryloyloxyethyl phosphate, and pentaerythritol tetra(meth)acrylate. Among them, trimethylolpropane tri(meth)acrylate is preferably used as the polyfunctional (meth)acrylate from the viewpoint of curability of the adhesive composition. These polyfunctional (meth)acrylates may be used alone or in combination of two or more.
[0136] Regarding the ratio of monofunctional (meth)acrylate and polyfunctional (meth)acrylate, when the total amount of (meth)acrylate monomer (B) is 100 mol%, it is preferred to contain 85 to 99 mol% of monofunctional (meth)acrylate and 1 to 15 mol% of polyfunctional (meth)acrylate. In this case, the content of monofunctional (meth)acrylate is more preferably 90 to 99 mol%, and further preferably 95 to 98 mol%. In addition, the content of polyfunctional (meth)acrylate is more preferably 1 to 10 mol%, and further preferably 2 to 5 mol%.
[0137] If the content of monofunctional (meth) acrylate is 85 mol% or more, the fluidity of the cured product obtained by curing the adhesive composition becomes a preferred range when the cured product is used as the adhesive layer of the semiconductor processing tape. Therefore, the semiconductor processing tape using the cured product as the adhesive layer can obtain sufficient concave-convex absorption, and when it is attached to an adherend having a concave-convex portion on the surface, it is not easy to generate a gap between the concave-convex portion of the adherend, which is preferred. In addition, if the content of monofunctional (meth) acrylate is 99 mol% or less, it is not easy to leave residual glue when the semiconductor processing tape using the cured product of the adhesive composition as the adhesive layer is peeled off from the adherend, which is preferred.
[0138] If the content of the multifunctional (meth) acrylate is 1 mol% or more, the fluidity of the cured product obtained by curing the adhesive composition will not become too large, which is preferred. In addition, if the content of the multifunctional (meth) acrylate is 15 mol% or less, the fluidity of the cured product obtained by curing the adhesive composition becomes a preferred range when the cured product is used as the adhesive layer of the semiconductor processing tape. Therefore, the semiconductor processing tape using the cured product as the adhesive layer has sufficient concave-convex absorption, and when it is attached to an adherend having a concave-convex portion on the surface, it is not easy to generate a gap between the concave-convex portion of the adherend, which is preferred.
[0139] The content of the (meth) acrylate monomer (B) in the adhesive composition of the present embodiment is preferably 35 to 79% by mass, more preferably 40 to 73% by mass, and further preferably 45 to 66% by mass. If the content of the (meth) acrylate monomer (B) is 35% by mass or more, the viscosity of the adhesive composition will not become too high, and the coating property is excellent, so it is preferred. In addition, if the content of the (meth) acrylate monomer (B) is 79% by mass or less, the viscosity of the adhesive composition will not become too low, and it is easy to control the thickness of the coating film formed by the adhesive composition, which is preferred.
[0140] (Chain transfer agent (C))
[0141] The pressure-sensitive adhesive composition contains a chain transfer agent (C) for the purpose of controlling the unevenness absorbency and gel fraction of a cured product obtained by curing the pressure-sensitive adhesive composition.
[0142] As the chain transfer agent (C), a thiol compound is preferably used. In particular, a polyfunctional thiol can be preferably used. A polyfunctional thiol is a compound having two or more mercapto groups in the molecule.
[0143] The polyfunctional thiol is not particularly limited, and examples thereof include 1,2-ethanedithiol, 1,4-bis(3-mercaptobutyryloxy)butane, tetraethylene glycol bis(3-mercaptopropionate), trimethylolethane tris(3-mercaptobutyrate), trimethylolpropane tris(3-mercaptobutyrate), trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), pentaerythritol tetrakis(3-mercaptopropionate), 1,3,5-tris(3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, dipentaerythritol hexa(3-mercaptopropionate), etc. As the chain transfer agent (C), among the above, pentaerythritol tetrakis(3-mercaptobutyrate) is preferably used from the viewpoint of the reactivity of the adhesive composition.
[0144] The content of the chain transfer agent (C) in the adhesive composition of the present embodiment is preferably 0.5 to 8% by mass, more preferably 1 to 5% by mass, and further preferably 3 to 4.5% by mass. If the content of the chain transfer agent (C) is 0.5% by mass or more, the fluidity of the cured product obtained by curing the adhesive composition becomes a preferred range when the cured product is used as the adhesive layer of the semiconductor processing tape. Therefore, the semiconductor processing tape using the cured product as the adhesive layer has sufficient concave-convex absorption, and it is not easy to produce a gap between the concave-convex part of the adherend, which is preferred. If the content is 8% by mass or less, it is not easy to leave residual glue when the semiconductor processing tape using the cured product of the adhesive composition as the adhesive layer is peeled off from the adherend, which is preferred.
[0145] (Photopolymerization initiator (D))
[0146] Photopolymerization initiator (D) is not particularly limited, but is preferably a photo radical polymerization initiator. As photopolymerization initiator (D), for example, carbonyl-based photopolymerization initiators, sulfide-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, quinone-based photopolymerization initiators, sulfonyl chloride-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, etc. can be used. Among these photopolymerization initiators (D), from the perspective of the transparency of the cured product obtained by photocuring the adhesive composition, carbonyl-based photopolymerization initiators and / or acylphosphine oxide-based photopolymerization initiators are preferably used. Specifically, 2,4,6-trimethylbenzoyl diphenylphosphine oxide agent and / or 1-hydroxycyclohexyl-phenyl ketone are more preferably used.
[0147] The content of the photopolymerization initiator (D) in the adhesive composition of the present embodiment is preferably 0.01 to 5% by mass, more preferably 0.05 to 3% by mass, and further preferably 0.1 to 2% by mass. If the content of the photopolymerization initiator (D) is 0.01% by mass or more, the photocuring of the adhesive composition is fully carried out. In addition, if the content of the photopolymerization initiator (D) is 5% by mass or less, the low molecular weight component will not become too much during the photocuring of the adhesive composition. Therefore, it is preferred that the semiconductor processing tape using the cured product of the adhesive composition as the adhesive layer is not easy to be peeled off from the adherend.
[0148] (Fatty acid ester (E))
[0149] The adhesive composition of the present embodiment contains polyurethane (A), a (meth)acrylate monomer (B), a chain transfer agent (C), and a photopolymerization initiator (D), and may further contain a fatty acid ester (E) as necessary.
[0150] The adhesive composition contains a fatty acid ester (E) for the purpose of controlling the adhesive force in a semiconductor processing tape using a cured product of the adhesive composition as an adhesive layer and improving the lamination properties (wettability) and degassing properties (ease of removing bubbles trapped when the semiconductor processing tape is attached to an adherend) of the adhesive layer.
[0151] As the fatty acid ester (E), an ester formed by a fatty acid and an alkyl alcohol can be used. In addition, from the viewpoint of compatibility with other components, it is preferred to use a fatty acid ester selected from esters formed by fatty acids having 8 to 18 carbon atoms and monofunctional alcohols having branched hydrocarbon groups having 3 to 18 carbon atoms, and esters formed by unsaturated fatty acids having 14 to 18 carbon atoms and 2 to 4 functional alcohols.
[0152] Examples of the esters of fatty acids having 8 to 18 carbon atoms and monofunctional alcohols having branched hydrocarbon groups having 3 to 18 carbon atoms include isostearyl laurate, isopropyl myristate, isocetyl myristate, octyldodecyl myristate, isopropyl palmitate, isostearyl palmitate, isocetyl stearate, 2-ethylhexyl stearate, octyldodecyl oleate, diisostearyl adipate, diisocetyl sebacate, trioleyl trimellitate, and triisocetyl trimellitate. Among them, isopropyl myristate, isopropyl palmitate, and 2-ethylhexyl stearate are preferably used, and isopropyl myristate and / or 2-ethylhexyl stearate are particularly preferably used.
[0153] Examples of the esters of unsaturated fatty acids having 14 to 18 carbon atoms and difunctional to tetrafunctional alcohols include esters of unsaturated fatty acids such as myristic acid, oleic acid, linoleic acid, linolenic acid, isopalmitic acid, and isostearic acid with alcohols such as ethylene glycol, propylene glycol, glycerol, trimethylolpropane, pentaerythritol, and sorbitan.
[0154] The content of the fatty acid ester (E) in the adhesive composition of the present embodiment is preferably 3 to 18% by mass, more preferably 5 to 15% by mass.
[0155] If the content of fatty acid ester (E) is 3% by mass or more, the adhesive force in the semiconductor processing tape using the cured product of the adhesive composition as the adhesive layer becomes a preferred range, and the lamination and degassing properties of the adhesive layer become good. If the content of fatty acid ester (E) is 18% by mass or less, when the semiconductor processing tape using the cured product of the adhesive composition as the adhesive layer is peeled off from the adherend, residual adhesive containing fatty acid ester (E) is not easy to occur, which is preferred.
[0156] (Solvent)
[0157] The adhesive composition of the present embodiment may contain a solvent, but is more preferably a solvent-free adhesive composition containing substantially no solvent.
[0158] When the adhesive composition of the present embodiment contains a solvent, for example, a leveling agent and / or a softener can be used as the solvent.
[0159] When the adhesive composition of the present embodiment is solvent-free, when the adhesive layer of the semiconductor processing tape is formed using the adhesive composition, the step of heating and drying the solvent can be omitted, so that excellent productivity can be obtained. In particular, when the adhesive composition of the present embodiment is used to manufacture a semiconductor processing tape having an adhesive layer having a thickness of more than 50 μm, the productivity improvement effect brought about by omitting the step of heating and drying the solvent becomes significant, so it is preferably solvent-free.
[0160] In the present invention, the adhesive composition “does not substantially contain a solvent” means that the content of the solvent in the adhesive composition is 0 to 1% by mass, preferably 0 to 0.5% by mass, and more preferably 0 to 0.1% by mass.
[0161] (other)
[0162] The adhesive composition of the present embodiment may contain other additives as required within the scope of not impairing the effect of the present invention. As additives, for example, plasticizers, surface lubricants, antioxidants, anti-aging agents, light stabilizers, ultraviolet absorbers, polymerization inhibitors, light stabilizers such as benzotriazole, phosphates and other flame retardants, dyes, etc. can be cited.
[0163] <Method for producing adhesive composition>
[0164] Next, the manufacturing method of the adhesive composition of the present embodiment is described in detail with examples. Below, among the components contained in the adhesive composition of the present embodiment, about polyurethane (A), a preferred synthesis method is described with examples. Among the components contained in the adhesive composition of the present embodiment, about each component other than polyurethane (A) such as (meth) acrylate monomer (B), chain transfer agent (C), photopolymerization initiator (D), fatty acid ester (E), commercial products can be easily purchased. In addition, the synthesis method is different according to the type of compound used as each component. Therefore, the description of the synthesis method is omitted.
[0165] <Method for synthesizing polyurethane (A)>
[0166] Hereinafter, an example of a preferred synthesis method of the polyurethane (A) included in the adhesive composition of the present embodiment is described. In addition, the synthesis method of the polyurethane (A) is not limited to the synthesis method shown below, and can be appropriately changed according to the conditions such as the raw materials and equipment used for the synthesis.
[0167] In the synthesis method of polyurethane (A) shown below, the reaction of hydroxyl group and isocyanate group is carried out in the presence of an organic solvent inert to isocyanate group in any process, using a carbamate catalyst. The carbamate catalyst can be, for example, dibutyltin dilaurate, dibutyltin diethylhexanoate, dioctyltin dilaurate, etc. In addition, the reaction of hydroxyl group and isocyanate group is preferably carried out continuously at 30 to 100° C. for 1 to 5 hours in any process. The amount of the carbamate catalyst used is preferably 50 to 500 mass ppm relative to the total mass of the reactants (raw materials).
[0168] In order to synthesize polyurethane (A), first, polyoxyalkylene polyol and polyisocyanate are added in a ratio in which the amount of isocyanate groups (based on the number of molecules, the same below) is greater than the amount of hydroxyl groups (based on the number of molecules, the same below). Then, polyoxyalkylene polyol and polyisocyanate are reacted to synthesize a polyurethane having an isocyanate group at the end as a precursor of polyurethane (A). Specific examples of polyoxyalkylene polyol and polyisocyanate used as raw materials are as exemplified in the section of polyurethane (A).
[0169] At this time, by adjusting the ratio of the amount of isocyanate groups contained in the raw materials to the amount of hydroxyl groups, the molecular weight (polymerization degree) of the polyurethane with isocyanate groups at the end can be adjusted. Specifically, the less the excess amount of isocyanate groups relative to the amount of hydroxyl groups, the greater the molecular weight of the polyurethane with isocyanate groups at the end. In addition, the more the excess amount of isocyanate groups relative to the amount of hydroxyl groups, the smaller the molecular weight of the polyurethane with isocyanate groups at the end. In the present embodiment, by adjusting the molecular weight of the polyurethane with isocyanate groups at the end, the mass average molecular weight of the polyurethane (A) as the target substance is adjusted.
[0170] Next, a polyurethane having an isocyanate group at the end is reacted with a compound having a hydroxyl group and a (meth)acryloyl group to generate a polyurethane (A) including a polyurethane (a1). The polyurethane (a1) has a skeleton including a structure derived from a polyoxyalkylene polyol and a structure derived from a polyisocyanate, and has (meth)acryloyl groups at multiple ends. The terminal (meth)acryloyl group of the generated polyurethane (A) is preferably a part of a (meth)acryloyloxy group.
[0171] As the compound having a hydroxyl group and a (meth) acryloyl group, there is no particular limitation, and examples include (meth) alkyl acrylates such as 2-hydroxyethyl (meth) acrylate, 2-hydroxypropyl (meth) acrylate, and 4-hydroxybutyl (meth) acrylate; monoalcohols having (meth) acryloyl groups derived from various polyols such as 1,3-butanediol mono(meth) acrylate, 1,4-butanediol mono(meth) acrylate, 1,6-hexanediol mono(meth) acrylate, and 3-methylpentanediol mono(meth) acrylate. These compounds having a hydroxyl group and a (meth) acryloyl group can be used alone or in combination of two or more. Among these compounds having a hydroxyl group and a (meth) acryloyl group, 2-hydroxyethyl (meth) acrylate is preferably used in terms of the reactivity with the isocyanate group of the polyurethane having an isocyanate group at the end and the photocurability of the adhesive composition.
[0172] The polyurethane (A) can be produced by reacting a polyurethane having an isocyanate group at the terminal with an alkyl alcohol having one hydroxyl group and a compound having a hydroxyl group and a (meth)acryloyl group.
[0173] As the alkyl alcohol, any alkyl alcohol may be used without particular limitation, as long as it has no (meth)acryloyl group and has one hydroxyl group, and linear, branched, alicyclic alkyl alcohols and the like may be used. The alkyl alcohols may be used alone or in combination of two or more.
[0174] By reacting a compound having a hydroxyl group and a (meth)acryloyl group, an alkyl alcohol having no (meth)acryloyl group and one hydroxyl group, and a polyurethane having an isocyanate group at a terminal, polyurethane (A) is produced, and the amount of the (meth)acryloyl group introduced into the polyurethane having an isocyanate group at a terminal can be adjusted.
[0175] In more detail, if the above reaction is adopted, as polyurethane (A), a substance including a plurality of polyurethanes having different amounts of (meth)acryloyl groups introduced at the terminals is generated. Among the plurality of polyurethanes, a polyurethane (a1) having a (meth)acryloyl group at a plurality of terminals is included. Furthermore, among the plurality of polyurethanes, not only polyurethane (a1) is included, but also polyurethanes in which at least a portion of the plurality of terminals have a structure derived from the above-mentioned alkyl alcohol are included. Therefore, among the plurality of polyurethanes generated, a polyurethane in which at least a portion of the plurality of terminals do not have a (meth)acryloyl group is included. Furthermore, among the plurality of polyurethanes generated, a polyurethane (a2) having a (meth)acryloyl group only at one terminal can also be included.
[0176] <Other examples of the synthesis method of polyurethane (A)>
[0177] Next, another example of a preferred synthesis method of polyurethane (A) will be described.
[0178] In the synthesis method of polyurethane (A) shown below, similarly to the example of the above synthesis method, the reaction between the hydroxyl group and the isocyanate group is carried out in any process in the presence of an organic solvent inert to the isocyanate group using a carbamate catalyst. Examples of carbamate catalysts include dibutyltin dilaurate, dibutyltin diethylhexanoate, dioctyltin dilaurate, etc. In addition, the reaction between the hydroxyl group and the isocyanate group is preferably carried out continuously at 30 to 100° C. for 1 to 5 hours in any process. The amount of the carbamate catalyst used is preferably 50 to 500 mass ppm relative to the total mass of the reactants (raw materials).
[0179] When the polyurethane (A) is synthesized using this synthesis method, unlike the above-mentioned example of the synthesis method, a polyurethane having a hydroxyl group at a terminal is synthesized as a precursor of the polyurethane (A).
[0180] Specifically, first, polyoxyalkylene polyol and polyisocyanate are added in a ratio such that the amount of hydroxyl groups (based on the number of molecules, the same below) is greater than the amount of isocyanate groups (based on the number of molecules, the same below). Then, polyoxyalkylene polyol and polyisocyanate are reacted to synthesize a polyurethane having a hydroxyl group at the end as a precursor of polyurethane (A).
[0181] At this time, by adjusting the ratio of the hydroxyl amount contained in the raw material to the isocyanate group amount, the molecular weight (polymerization degree) of the polyurethane with hydroxyl at the end can be adjusted. Specifically, the less the excess amount of the hydroxyl amount relative to the isocyanate group amount, the larger the molecular weight of the polyurethane with hydroxyl at the end. In addition, the more the excess amount of the hydroxyl amount relative to the isocyanate group amount, the smaller the molecular weight of the polyurethane with hydroxyl at the end. In the present embodiment, by adjusting the molecular weight of the polyurethane with hydroxyl at the end, the mass average molecular weight of the polyurethane (A) as the target substance is adjusted.
[0182] Next, a polyurethane having a hydroxyl group at a terminal is reacted with a compound having an isocyanate group and a (meth)acryloyl group to generate a polyurethane (A) including a polyurethane (a1) having a skeleton including a structure derived from a polyoxyalkylene polyol and a structure derived from a polyisocyanate and having (meth)acryloyl groups at a plurality of terminals. The terminal (meth)acryloyl group of the generated polyurethane (A) is preferably a part of a (meth)acryloyloxy group.
[0183] As the compound with isocyanate group and (meth) acryloyl group, it is not particularly limited, and 2-(meth) acryloyloxyethyl isocyanate, 2-(meth) acryloyloxypropyl isocyanate, 1,1-bis(acryloyloxymethyl) ethyl isocyanate, etc. can be cited. In addition, as a commercial product of a compound with isocyanate group and (meth) acryloyl group, examples can be given such as, Karens MOI (registered trademark) and Karens AOI (registered trademark) made by Showa Denko K.K., etc. These compounds with isocyanate group and (meth) acryloyl group can be used alone, or two or more kinds can be used in combination. Among these compounds with isocyanate group and (meth) acryloyl group, from the reactivity of the hydroxyl group of the polyurethane having a hydroxyl group at the end and the light curing property of the adhesive composition, it is preferred to use 2-(meth) acryloyloxyethyl isocyanate.
[0184] The polyurethane (A) can be produced by reacting a polyurethane having a terminal hydroxyl group with an alkyl isocyanate having no (meth)acryloyl group and one isocyanate group together with a compound having an isocyanate group and a (meth)acryloyl group.
[0185] As the alkyl isocyanate, there is no particular limitation as long as it has no (meth)acryloyl group and has one isocyanate group, and linear, branched, alicyclic alkyl isocyanates and the like can be used. The above alkyl isocyanates can be used alone or in combination of two or more.
[0186] By reacting a compound having an isocyanate group and a (meth)acryloyl group, an alkyl isocyanate having no (meth)acryloyl group and one isocyanate group, and a polyurethane having a hydroxyl group at the terminal, a polyurethane (A) is produced, whereby the amount of the (meth)acryloyl group introduced into the polyurethane having a hydroxyl group at the terminal can be adjusted.
[0187] In more detail, if the above reaction is adopted, as polyurethane (A), a material of multiple polyurethanes having different amounts of (meth)acryloyl groups introduced at the terminals is generated. Among the multiple polyurethanes, polyurethane (a1) having (meth)acryloyl groups at multiple terminals is included. Further, among the multiple polyurethanes, not only polyurethane (a1) is included, but also polyurethanes having a structure derived from the above-mentioned alkyl isocyanate at at least a portion of the multiple terminals are included. Therefore, among the multiple polyurethanes generated, polyurethanes having at least a portion of the multiple terminals not having (meth)acryloyl groups are included. Further, among the multiple polyurethanes generated, polyurethanes having (meth)acryloyl groups only at one terminal can also be included (a2).
[0188] <Method of mixing components included in adhesive composition>
[0189] The adhesive composition of this embodiment can be produced by mixing the polyurethane (A) obtained by the above-mentioned synthesis method, the (meth)acrylate monomer (B), the chain transfer agent (C), the photopolymerization initiator (D), and the fatty acid ester (E) and other additives added as needed.
[0190] The method for mixing the components contained in the adhesive composition of the present embodiment is not particularly limited, and for example, the method can be carried out using a homodispersor or a stirring device equipped with stirring blades such as paddle blades.
[0191] <Method for manufacturing semiconductor processing tape>
[0192] Next, a method for producing the semiconductor processing tape according to the present embodiment will be described.
[0193] The method for producing the semiconductor processing tape according to the present embodiment is not particularly limited, and the tape can be produced using a known method.
[0194] For example, microparticles of polypyrrole and / or polypyrrole derivatives are dispersed in a hydrophilic solvent using a polymer dispersant and / or a dopant, and further mixed with a water-soluble or water-dispersible binder resin to modulate a resin composition; after the resin composition is applied to a substrate body such as a polymer film, the solvent is dried and removed to obtain a substrate having an antistatic layer. Next, an adhesive composition is applied to the antistatic layer of the substrate, and a transparent spacer film is laminated to form a laminate. Then, ultraviolet rays are irradiated to the adhesive composition via the spacer to photocure the adhesive composition. Thus, a semiconductor processing tape having an adhesive layer as a cured product of the adhesive composition formed on a substrate having an antistatic layer can be obtained.
[0195] The method for applying the adhesive composition on the substrate is not particularly limited and can be appropriately selected. For example, as the method for applying the adhesive composition on the substrate, methods using various coating machines such as a gravure roll coater, a reverse roll coater, a touch roll coater, a dip roll coater, a rod coater, a blade coater, a spray coater, a comma coater (commacoater,), a direct coater, and screen printing methods can be cited.
[0196] Examples of a light source for photocuring the adhesive composition include black light, a low-pressure mercury lamp, a high-pressure mercury lamp, an ultrahigh-pressure mercury lamp, a metal halide lamp, and a xenon lamp.
[0197] The light irradiation intensity is preferably such that the adhesive composition can be sufficiently cured and the gel fraction of the cured product can be within a range of 50 to 65% by mass, for example, preferably 50 to 3000 mW / cm 2In addition, if the light irradiation intensity is weak, curing takes time and productivity decreases.
[0198] In the present embodiment, the adhesive composition is irradiated with ultraviolet rays through a transparent spacer. However, when the substrate is transparent, ultraviolet rays may be irradiated from the substrate side, or an opaque substance may be used as the spacer.
[0199] <Applications and required performance of semiconductor processing tape>
[0200] The semiconductor processing tape of this embodiment can be used, for example, in applications where it is attached to an adherend having concavo-convex portions on the surface and then peeled off. Specifically, it can be used as a back grinding tape for semiconductor wafer processing that is attached to the surface of a semiconductor wafer with bumps formed thereon to protect the surface of the semiconductor wafer and is peeled off after a predetermined wafer processing step.
[0201] When the semiconductor processing tape of the present embodiment is used for protecting the surface of a semiconductor wafer having bumps formed on the surface, the peel strength (adhesion) of the semiconductor processing tape needs to be such that the semiconductor processing tape is firmly fixed to the semiconductor wafer in, for example, a back grinding step in a semiconductor device processing step. On the other hand, the peel strength of the semiconductor processing tape needs to be such that the semiconductor device components are not damaged when the semiconductor processing tape is peeled off from the semiconductor wafer after a predetermined processing step.
[0202] From these viewpoints, when the peeling speed is 0.3 m / min and the thickness of the adhesive layer is 50 to 200 μm, the peel strength of the semiconductor processing tape used in the above-mentioned application is preferably 10 to 300 gf / 25 mm, more preferably 15 to 200 gf / 25 mm, and further preferably 20 to 150 gf / 25 mm. When the thickness of the adhesive layer is 200 to 500 μm, it is preferably 50 to 500 gf / 25 mm, more preferably 60 to 400 gf / 25 mm, and further preferably 70 to 300 gf / 25 mm. The specific method for measuring the peel strength of the semiconductor processing tape is described below in the examples.
[0203] The semiconductor processing tape of this embodiment has an adhesive layer which is a cured product of the adhesive composition of this embodiment on one side of the substrate on which the antistatic layer is formed. Therefore, the semiconductor processing tape of this embodiment has sufficient adhesive force, and is unlikely to have residual adhesive of the adhesive layer transferred to the adherend after the semiconductor processing tape is peeled off, and has excellent concavo-convex absorption and antistatic performance. Therefore, the semiconductor processing tape of this embodiment is suitable for being attached to an adherend having concavo-convex parts on the surface and then peeled off.
[0204] The semiconductor processing tape of the present embodiment can be used, for example, as a semiconductor processing tape that is pasted during the back grinding process of a semiconductor wafer having a concave-convex portion formed by a bump on the surface and is peeled off after the back grinding process. In this case, the semiconductor wafer is fixed with sufficient adhesive force by the semiconductor processing tape of the present embodiment. Moreover, since the semiconductor processing tape has sufficient concave-convex absorption, it is not easy to generate a gap between the semiconductor processing tape pasted to the semiconductor wafer and the bump. Therefore, it is possible to prevent the water used in the back grinding process from invading the gap between the semiconductor processing tape and the bump and contaminating the semiconductor wafer. In addition, since the semiconductor processing tape of the present embodiment has sufficient antistatic performance, it is possible to suppress the peeling electrification when the semiconductor processing tape pasted to the semiconductor wafer is peeled off after the back grinding process. Furthermore, after the back grinding process, it is not easy for residual glue to occur around the bump of the semiconductor wafer from which the semiconductor processing tape has been peeled off, which is preferred.
[0205] The semiconductor processing tape of the present embodiment may be a single-layer structure in which the adhesive layer is a cured product of the adhesive composition. In this case, the adhesive layer can be formed by only performing a step of forming one layer. Therefore, the semiconductor processing tape of the present embodiment can be easily manufactured with fewer manufacturing steps, for example, compared with the case of forming a semiconductor processing tape having a layer with uneven absorption and a layer with adhesive force.
[0206] Example
[0207] Hereinafter, the present invention will be described in more detail by way of Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0208] (Production Example 1)
[0209] <Manufacturing of Sheet-like Base Material 1 Having Antistatic Layer>
[0210] 9.4 parts by mass of polypyrrole dispersion (PPY-12 manufactured by Maru Ryo Chemical Industry Co., Ltd., solid content 8%), 5.0 parts by mass of polyester adhesive (BI-12 manufactured by Maru Ryo Chemical Industry Co., Ltd., solid content 30%), 2.6 parts by mass of melamine crosslinking agent (CL-12 manufactured by Maru Ryo Chemical Industry Co., Ltd., solid content 25%), 0.05 parts by mass of polyoxyethylene lauryl ether, and 830.0 parts by mass of water were mixed to prepare an aqueous dispersion. Next, as a substrate body, the resin composition was applied to one side of a 50 μm thick PET film (manufactured by Toyobo Co., Ltd., trade name: Esther (trademark) film E5100) using a gravure coater in such a manner that the film thickness after heat curing became 1.0 μm. Next, curing was performed at 130° C. for 1 minute to obtain a sheet-like substrate 1. The resistance of the substrate 1 measured by a low resistivity meter (Lorest-AX manufactured by Mitsubishi Chemical Analytic Co., Ltd.) was 8×10 5 Ω·cm.
[0211] (Comparative Manufacturing Example 1)
[0212] <Manufacturing of Sheet-like Base Material 2 Having Antistatic Layer>
[0213] 93.0 parts by mass of polythiophene (Clevios (trademark) P manufactured by Echi-Stellk Co., Ltd., solid content 1%), 6.8 parts by mass of polyester resin (Bialonal (trademark) MD-1930 manufactured by Toyobo Co., Ltd., solid content 31%), 2.4 parts by mass of melamine crosslinking agent (CL-12 manufactured by Maru-Ryo Oil Chemical Industry Co., Ltd., solid content 25%), 0.05 parts by mass of polyoxyethylene lauryl ether, and 900.0 parts by mass of water were mixed to prepare an aqueous dispersion. Next, as a substrate body, the resin composition was applied to one side of a 50 μm thick PET film (manufactured by Toyobo Co., Ltd., trade name: Esther (trademark) film E5100) using a gravure coater in such a manner that the film thickness after heat curing was 1.0 μm. Next, curing was performed at 130° C. for 1 minute to obtain a sheet-like substrate 2. The resistance of the substrate 2 measured by a low resistivity meter (Lorestad-AX manufactured by Mitsubishi Chemical Analytic Co., Ltd.) was 4×10 5 Ω·cm.
[0214] (Synthesis example 1)
[0215] <Synthesis of polyurethane (A-1)>
[0216] In a reactor equipped with a thermometer, a stirrer, a dropping funnel, and a cooling tube with a drying tube, 0.55 kg (2.1 mol) of a hydrogenated product of diphenylmethane diisocyanate (Desmogel W, manufactured by Sumika Chemical Corporation), 4.01 kg (2.0 mol) of a polypropylene glycol having a hydroxyl group at the end and a hydroxyl value of 56 mgKOH / g (Actocol D-2000; manufactured by Mitsui Chemicals, number average molecular weight 2000), and 0.8 g of dioctyltin (Neostan U-810, manufactured by Nitto Kasei Co., Ltd.) as a urethanization catalyst were added.
[0217] Then, the reactor was heated to 60°C and reacted for 4 hours to obtain a polyurethane having isocyanate groups at both ends as a precursor of polyurethane (A). Next, 23.22 g (0.2 mol) of 2-hydroxyethyl acrylate was added to the reactor, and the temperature was raised to 70°C and reacted for 2 hours to obtain 4.58 kg of polyurethane (A-1) having a mass average molecular weight of 67,000.
[0218] The obtained polyurethane (A-1) was analyzed by infrared absorption spectroscopy (IR). As a result, no peak derived from isocyanate groups was observed. Therefore, it was confirmed that polyurethane (A-1) was a polyurethane (a1) having acryloyloxy groups introduced at all ends.
[0219] (Synthesis example 2)
[0220] <Synthesis of polyurethane (A-2)>
[0221] A polyurethane (A-2) having a mass average molecular weight of 66,000 was obtained in the same manner as in the synthesis of polyurethane (A-1), except that 2.1 mol of isophorone diisocyanate (Desmodium I, manufactured by Sumika Combustion Laboratories) was used instead of the hydrogenated product of diphenylmethane diisocyanate.
[0222] The obtained polyurethane (A-2) was analyzed by infrared absorption spectroscopy (IR). As a result, no peak derived from isocyanate groups was observed. Therefore, it was confirmed that polyurethane (A-2) was polyurethane (a1) having acryloyloxy groups introduced at all ends.
[0223] (Mixing Examples 1 to 3, Comparative Mixing Examples 1 to 4)
[0224] <Preparation of adhesive composition>
[0225] The polyurethane (A) obtained by the above-mentioned synthesis method, the (meth)acrylate monomer (B) shown in Table 1, the chain transfer agent (C), the photopolymerization initiator (D), and the fatty acid ester (E) were mixed in the proportions described in Table 1, and mixed using a disperser at 25°C to obtain adhesive compositions c1 to c7 of Mixing Examples 1 to 3 and Comparative Mixing Examples 1 to 4.
[0226]
[0227] The following symbols described in Table 1 indicate the compounds shown below.
[0228] 2EHA: 2-ethylhexyl acrylate (manufactured by Toagosei Co., Ltd.)
[0229] BUA: n-butyl acrylate (manufactured by Toagosei Co., Ltd.)
[0230] ACMO: Acryloylmorpholine (manufactured by Shin-Nakamura Chemical Co., Ltd.)
[0231] TMPTA: trimethylolpropane triacrylate (manufactured by Toagosei Co., Ltd.)
[0232] PE1: Pentaerythritol tetrakis(3-mercaptobutyrate) (manufactured by Showa Denko K.K.)
[0233] NR1: 1,3,5-Tris(3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by Showa Denko K.K.)
[0234] TPO (Omnirad TPO H): 2,4,6-trimethylbenzoyldiphenylphosphine oxide (manufactured by IGM Resins BV)
[0235] 184 (Omnirad 184): 1-hydroxycyclohexyl-phenyl ketone (manufactured by IGM Resins BV)
[0236] Ecosper IPM: Isopropyl myristate (manufactured by Kao Corporation)
[0237] Ekisepal EH-S: 2-Ethylhexyl stearate (manufactured by Kao Corporation)
[0238] (Example 1)
[0239] The adhesive composition c1 of Mixing Example 1 in Table 1 was applied on the antistatic layer side of the substrate 1 using an applicator so that the thickness after curing would be 150 μm.
[0240] Next, a 75 μm-thick silicone-based ultralight release PET film (manufactured by Toyobo Co., Ltd., product name: E7006) was laminated onto the surface coated with the adhesive composition as a separator using a rubber roller.
[0241] Then, the adhesive composition was irradiated with ultraviolet light (manufactured by Igfraflex Corporation, UV irradiation device 3 kW, high pressure mercury lamp) through the spacer at an irradiation distance of 25 cm, a lamp moving speed of 1.0 m / min, and an irradiation dose of 1000 mJ / cm 2 The adhesive composition was photocured by irradiating ultraviolet rays under the conditions of . Thus, a semiconductor processing tape of Example 1 in which an adhesive layer as a cured product of the adhesive composition and a spacer were laminated on a substrate was obtained.
[0242] (Example 2 to Example 3 and Comparative Example 1 to Comparative Example 6)
[0243] Semiconductor processing tapes were prepared in the same manner as in Example 1 except that the substrates and adhesive compositions c2 to c7 described in Table 2 were used and the adhesive layer had the film thickness described in Table 2. As a result, semiconductor processing tapes of Examples 2 to 3 and Comparative Examples 1 to 6 were obtained.
[0244] Next, the items shown below were evaluated for the tapes for semiconductor processing of Examples 1 to 3 and Comparative Examples 1 to 4. The results are shown in Table 2.
[0245] <Measurement of surface resistivity>
[0246] The semiconductor processing tape was cut into a size of 120 mm in length and 120 mm in width, and placed in an environment of 23 ° C and 50% RH for 3 hours for humidity adjustment. Then, the peeling PET film was peeled off to expose the adhesive layer, and the surface resistivity of the adhesive layer side was measured using a high resistivity meter (made by Mitsubishi Chemical Analytic Co., Ltd., HiResta-UX) under the condition of applying a voltage of 100V×60 seconds. Then, the evaluation was performed according to the following criteria. The smaller the surface resistivity, the less likely it is to cause peeling electrification when peeling the semiconductor processing tape attached to the semiconductor wafer, and it can be said that the semiconductor processing tape has better antistatic performance.
[0247] Evaluation Benchmarks
[0248] ◎: Surface resistivity is less than 1×10 11 Ω / □
[0249] ○: Surface resistivity is 1×10 11 Ω / □ or more and less than 1×10 12 Ω / □
[0250] △: Surface resistivity is 1×10 12 Ω / □ or more and less than 1×10 13 Ω / □
[0251] ×: Surface resistivity is 1×10 13 Ω / □ or more
[0252] <Peel force (peel strength)>
[0253] The semiconductor processing tape was cut into a size of 25 mm in length and 150 mm in width, and the spacer was peeled off to expose the adhesive layer. Then, the entire surface of the exposed adhesive layer was laminated to a glass plate, and a rubber roller (diameter: 85 mm, width: 50 mm) with a mass of 2 kg (load 19.6 N) was reciprocated once to obtain a measurement sample. The obtained measurement sample was placed in an environment of temperature 23 ° C and relative humidity 50% RH for 30 minutes. Then, according to JIS K 6854-2, a tensile test in the 180 ° direction was performed at a peeling speed of 0.3 m / min, and the peel strength (gf / 25mm) relative to the glass plate was measured.
[0254] <Absorption of unevenness>
[0255] The semiconductor processing tape was cut into a size of 25 mm in length and 50 mm in width, and the spacer was peeled off to expose the adhesive layer. Then, the surface of the exposed adhesive layer was placed opposite to the bumps of a wafer with bumps (WALTS-TEG FC150SCJYLF (PI), bump height: 75 μm, bump size: 90 μm in diameter). Furthermore, a rubber roller (diameter: 85 mm, width: 50 mm) with a mass of 2 kg (load 19.6 N) was reciprocated 3 times at a speed of 10 mm / sec on the substrate of the semiconductor processing tape to bond the semiconductor processing tape to the wafer with bumps.
[0256] The wafer with bumps bonded to the semiconductor processing tape was observed from the substrate side of the semiconductor processing tape using a digital optical microscope (RH-2000 manufactured by Hilock Co., Ltd.), and the unevenness absorption property for the bumps was evaluated according to the following criteria.
[0257] "Benchmark"
[0258] ◯: There is no gap between the adhesive layer of the semiconductor processing tape and the periphery of the bumps of the wafer with bumps.
[0259] ×: There is a gap between the adhesive layer of the semiconductor processing tape and the periphery of the bump of the wafer with bumps.
[0260] <Pollution caused by residual adhesive>
[0261] The semiconductor processing tape was cut into a size of 25 mm in length and 50 mm in width, and the spacer was peeled off to expose the adhesive layer. Then, the surface of the exposed adhesive layer was placed opposite to the bumps of a wafer with bumps (WALTS-TEG FC150SCJYLF (PI), bump height: 75 μm, bump size: 90 μm in diameter). Furthermore, a rubber roller (diameter: 85 mm, width: 50 mm) with a mass of 2 kg (load 19.6 N) was reciprocated 3 times at a speed of 10 mm / sec on the substrate of the semiconductor processing tape to bond the semiconductor processing tape to the wafer with bumps.
[0262] After the wafer with bumps attached to the semiconductor processing tape was placed at 23°C for 24 hours, the semiconductor processing tape was peeled off by hand at a speed of about 2 m / min. Furthermore, the surface of the wafer with bumps was observed by a digital optical microscope (manufactured by Hilox Co., Ltd., RH-2000), and the presence or absence of contamination caused by residual adhesive was evaluated according to the following criteria. In addition, the so-called "residual adhesive" refers to the state in which the adhesive layer itself remains attached to the surface of the wafer, and the surface of the wafer is sticky.
[0263] "Benchmark"
[0264] ○: There is no contamination caused by residual adhesive around the bump.
[0265] ×: There is contamination around the bump caused by residual adhesive.
[0266] <Measurement of gel fraction>
[0267] The adhesive composition was applied to a 75 μm thick peelable PET film (manufactured by Toyama Film Co., Ltd., trade name: Clear Sera (trademark) HY-S10-2) using an applicator so that the thickness after curing was 150 μm. In addition, for Comparative Example 4, the thickness after curing was adjusted to 30 μm. Next, the coated surface of the adhesive composition was covered with a 75 μm thick silicone ultra-light peelable PET film (manufactured by Toyobo Co., Ltd., product name: E7006).
[0268] Next, an ultraviolet irradiation device (manufactured by Igfraflex Corporation, UV irradiation device 3 kW, high pressure mercury lamp) was used at an irradiation distance of 25 cm, a lamp moving speed of 1.0 m / min, and an irradiation dose of 1000 mJ / cm 2 Under the conditions of , the adhesive composition was cured by irradiating ultraviolet rays through an ultralight peeling PET film to obtain a cured product (adhesive layer).
[0269] Next, the solidified product (adhesive layer) was cut into a size of about 1 g, and the PET films on both sides were peeled off to prepare a sample for measurement, and its mass was measured. Next, the sample for measurement was immersed in 50 ml of toluene and left to stand at room temperature for 72 hours. Then, the sample for measurement was taken out of toluene, dried at 80°C for 5 hours, and the mass was measured again. Furthermore, the gel fraction was measured based on the following formula.
[0270] Gel fraction (%) = [A / B] × 100
[0271] A: Mass of the measurement sample after immersion in toluene (mass excluding toluene)
[0272] B: Mass of the measurement sample before immersion in toluene
[0273]
[0274] As shown in Table 2, the semiconductor processing tapes of Examples 1 to 3 have low surface resistivity and excellent antistatic properties. In addition, they have high peeling strength (adhesive strength) and excellent unevenness absorption, and no contamination due to residual adhesive occurs when peeling from a wafer with bumps.
[0275] In contrast, in Comparative Example 1 using a substrate 2 in which the antistatic layer does not contain a polypyrrole compound, the surface resistivity is high, showing poor antistatic performance. In Comparative Examples 2, 3 and 6, which are adhesive compositions but do not use a chain transfer agent (C), the gel fraction of the adhesive layer cannot be controlled within an appropriate range, resulting in poor results in any of the selected peeling force, bump absorption, and residual adhesive. In Comparative Example 4, in which the thickness of the adhesive layer is thin, sufficient bump absorption cannot be obtained. In Comparative Example 5, compared with the adhesive composition c1, an adhesive composition c6 in which the photopolymerization initiator (D) is increased without using a chain transfer agent (C) is used. As a result, although a gel fraction equivalent to that of Example 1 is obtained, the bump absorption is insufficient, and contamination caused by residual adhesive also occurs.
[0276] Industrial Availability
[0277] According to the present invention, there is provided a semiconductor processing tape which has sufficient concavo-convex absorption, antistatic performance, and adhesive force, is not prone to residual adhesive, and can be manufactured with a few manufacturing processes. The semiconductor processing tape can be preferably used as a back grinding tape used to protect the surface of the semiconductor wafer in the semiconductor wafer processing process and to be peeled off after the processing process. In particular, it is suitable as a back grinding tape used to protect the surface when performing a back grinding process of an adherend having concavo-convex parts on the surface, such as a semiconductor wafer with bumps formed on the surface.
Claims
1. A semiconductor processing tape, characterized in that: It has a sheet-like substrate and an adhesive layer, The sheet-like substrate comprises a substrate body and an antistatic layer provided on at least one side of the substrate body. The adhesive layer is formed on the antistatic layer; The antistatic layer contains a polypyrrole compound, The adhesive layer is a cured product of the adhesive composition. The thickness of the adhesive layer is 50 to 500 μm. The adhesive composition comprises 20 to 50% by mass of a polyurethane (A), 35 to 79% by mass of a (meth)acrylate monomer (B), 0.5 to 8% by mass of a chain transfer agent (C), and 0.01 to 5% by mass of a photopolymerization initiator (D). The polyurethane (A) contains polyurethane (a1), The polyurethane (a1) has a skeleton including a structure derived from a polyoxyalkylene polyol and a structure derived from a polyisocyanate, and has (meth)acryloyl groups at a plurality of terminals. The (meth)acrylate monomer (B) contains 85 to 99 mol % of a monofunctional (meth)acrylate and 1 to 15 mol % of a multifunctional (meth)acrylate. 2 . The semiconductor processing tape according to claim 1 , wherein the adhesive layer has a single-layer structure. 3 . The semiconductor processing tape according to claim 1 , wherein the chain transfer agent (C) is a polyfunctional thiol. 4 . The tape for semiconductor processing according to claim 1 , wherein the gel fraction of the adhesive layer is 50 to 65% by mass.
5. The semiconductor processing tape according to claim 1 or 2, wherein the surface resistivity of the adhesive layer is less than 1×10 12 Ω / □. 6 . The semiconductor processing tape according to claim 1 , wherein the adhesive composition further contains a fatty acid ester (E).