Method for producing (METH) acrylic resin and method for producing adhesive composition
The (meth)acrylic resin prepared by RAFT polymerization and addition reaction combines photopolymerization initiator and crosslinking agent to solve the problem of insufficient adhesion and residual glue in semiconductor manufacturing, and achieve high adhesion Force and easy peeling effect, suitable for cutting-patch integrated film.
Patent Information
- Application Number
- CN202380034013.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-08-03
- Filing Date
- 2023-07-14
- Publication Date
- 2024-11-22
AI Technical Summary
In the semiconductor manufacturing process, especially the adhesive layer of the cutting-patch integrated film, the insufficient adhesive force leads to peeling and residual glue problems, making it difficult to meet the requirements of high adhesion and easy peeling, especially After UV irradiation.
By reversible addition break chain transfer (RAFT) polymerization of hydroxyl-containing (meth)acrylate and alkyl (meth)acrylate, a copolymer is obtained, and an isocyanate-containing olefin is added to the side chain. Saturated compounds, a (meth)acrylic resin having an ethylenically unsaturated group is prepared, and a photopolymerization initiator and a crosslinking agent are combined to form a binder composition.
It provides sufficient adhesion to the bonding agent layer, and achieves excellent peeling after UV irradiation, reduces the occurrence of residual glue, and is suitable for the manufacturing of semiconductor chips.
Smart Images

Figure BDA0005082733860000061 
Figure BDA0005082733860000062 
Figure BDA0005082733860000063
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for producing a (meth)acrylic resin for an adhesive composition and a method for producing the adhesive composition. Background Art
[0002] In the past, various adhesive sheets were used in the manufacturing steps of semiconductors. Specifically, there are protective sheets (back grinding tape) used to protect the wafer in the back grinding step of the semiconductor wafer, and fixing sheets (dicing tape) used in the dicing step from the semiconductor wafer to the component chips. These adhesive sheets are removable adhesive sheets that are attached to the semiconductor wafer as the attached body and are peeled off from the attached body after the completion of a specific processing step.
[0003] As an adhesive composition used for the adhesive layer of a removable adhesive sheet, it is known that an adhesive composition containing a resin having an ethylenically unsaturated group capable of UV (ultraviolet) curing is introduced into the side chain of a (meth) acrylic resin. Such an adhesive composition is cured by a cross-linking reaction caused by UV irradiation, and the adhesive force is reduced. For example, Patent Document 1 (Japanese Patent Publication No. 2018-138682) describes an adhesive tape containing an active free radical polymerized polymer with a molecular weight distribution (Mw / Mn) of 1.05 to 2.5, especially a (meth) acrylic polymer having a UV-curable polymerizable group introduced into the side chain of a polymer obtained by active free radical polymerization using an organic tellurium polymerization initiator.
[0004] [Prior art literature]
[0005] [Patent Document]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2018-138682 Summary of the invention
[0007] [Problems to be Solved by the Invention]
[0008] In order to shorten the semiconductor manufacturing steps, a dicing tape as a re-peelable adhesive sheet and a film (adhesive layer) are integrated into a dicing-die bonding intergration film. The film is used, for example, by attaching the adhesive layer to the back of the semiconductor wafer and attaching the adhesive layer from the dicing tape to the dicing ring. Then, the semiconductor wafer is cut by a dicing knife to obtain a singulated semiconductor chip. Therefore, the adhesive layer from the dicing tape is required to have high adhesion to the adhesive layer and the dicing ring in the cutting step. On the other hand, in the pickup step of the semiconductor chip, it is required that no adhesive remains (residual adhesive) on each semiconductor chip, and the semiconductor chip with the adhesive sheet can be easily picked up. If the adhesive layer has insufficient adhesion to the adhesive layer, peeling occurs between the adhesive layer and the adhesive layer due to the high-speed rotation of the dicing knife, and the adhesive layer breaks, and the cutting end of the adhesive layer scatters (DAF (Die attach film) scatters). If the adhesive force of the adhesive layer to the dicing ring is insufficient, a phenomenon occurs in which the dicing ring is peeled off from the adhesive layer by the flow of cutting water (ring peeling).
[0009] In recent years, stealth dicing has attracted attention as a dicing method that does not use a dicing knife. In stealth dicing, laser light is focused inside the wafer to form a starting point (modified layer) for division, and a removable adhesive sheet is attached to the back of the wafer. The sheet is cooled and expanded to obtain a single-piece semiconductor chip. When a dicing-and-chip integrated film is used in stealth dicing, the wafer and the adhesive layer are singulated by cooling and expansion. If the adhesive force of the adhesive layer is insufficient in the cooling and expansion step, the outer periphery of the adhesive layer breaks due to the impact and stress during expansion, causing the cutting end to scatter (DAF scattering), or the end of the chip with the adhesive sheet attached to the adhesive layer to peel off from the adhesive layer (chip edge peeling), and a bad situation may occur in the subsequent steps.
[0010] Thus, the adhesive layer used in the dicing-patch integrated film is required to have high adhesion to the adhesive layer, no adhesive residue after UV irradiation, and be easily peeled off from the adhesive layer, which are characteristics not required in other removable adhesive sheets. Therefore, it is difficult to directly apply the acrylic adhesive used in the conventional removable adhesive sheet to the dicing-patch integrated film.
[0011] The present invention provides a method for producing a (meth)acrylic resin or an adhesive composition containing the (meth)acrylic resin, wherein the resin or the composition can provide an adhesive layer having sufficient adhesive strength to an adhesive layer, and when an adhesive sheet is peeled off from the adhesive layer after UV irradiation, an excellent peeling property is obtained, and an adhesive layer is not prone to residual adhesive.
[0012] [Methods to solve the problem]
[0013] The inventors and others have discovered that a copolymer obtained by reversible addition-fragmentation chain transfer (RAFT) polymerization of a hydroxyl-containing (meth)acrylate and an alkyl (meth)acrylate and modified with an ethylenically unsaturated compound containing an isocyanate group can be suitable for the adhesive layer of a cutting-and-sticking integrated film.
[0014] That is, the present disclosure includes the following aspects.
[0015] [1]. A method for producing a (meth)acrylic resin, comprising:
[0016] Step (i) of subjecting a raw material monomer group (M) containing a hydroxyl-containing (meth)acrylate (m-1) and an alkyl (meth)acrylate (m-2) to reversible addition fragmentation chain transfer (RAFT) polymerization to obtain a copolymer (A-0); and
[0017] Step (ii) of adding an isocyanate group-containing ethylenically unsaturated compound (a) to a part of the side chain hydroxyl groups of the copolymer (A-0) to obtain a (meth)acrylic resin (A) having an ethylenically unsaturated group.
[0018] [2] The method for producing a (meth)acrylic resin according to [1], wherein the raw monomer group (M) further contains a carboxyl group-containing monomer (m-3).
[0019] [3] The method for producing a (meth)acrylic resin according to [1] or [2], wherein the (meth)acrylic resin (A) having an ethylenically unsaturated group has a molecular weight distribution Mw / Mn of 2.4 to 10.0.
[0020] [4] A method for producing an adhesive composition, comprising the step (iii) of mixing a (meth)acrylic resin (A) having an ethylenically unsaturated group obtained by the production method described in any one of [1] to [3], a photopolymerization initiator (B) and a crosslinking agent (C).
[0021] [5] The method for producing an adhesive composition according to [4], wherein the crosslinking agent (C) is at least one selected from polyisocyanates and polyepoxy compounds.
[0022] [6] A method for producing an adhesive layer, comprising the step of forming a crosslinked structure in the adhesive composition obtained by the production method according to [4] or [5].
[0023] [7] A method for producing a PSA sheet, comprising applying the PSA composition obtained by the production method described in [4] or [5] onto a sheet-like substrate to form a PSA layer.
[0024] [8] A method for producing a pressure-sensitive adhesive sheet, comprising the step of forming a cross-linked structure in the pressure-sensitive adhesive layer obtained by the production method described in [7].
[0025] [9] A method for producing a dicing-and-sticking integrated film, comprising laminating an adhesive layer on a pressure-sensitive adhesive layer having a cross-linked structure obtained by the production method described in [8].
[0026]
[10] . A method for producing a dicing-and-sticking integrated film, comprising applying an adhesive composition obtained by the production method described in any one of [4] or [5] onto an adhesive layer.
[0027] [Effects of the invention]
[0028] By using the (meth)acrylic resin obtained by the method disclosed in the present invention in the adhesive layer of the dicing-and-sticking integrated film, it is possible to provide an adhesive layer that has sufficient adhesion to the adhesive layer and has excellent removability when the adhesive sheet is peeled off from the adhesive layer after UV irradiation, while being less likely to produce residual adhesive. DETAILED DESCRIPTION
[0029] Hereinafter, embodiments of the present invention will be described in detail. However, the present invention is not limited to the embodiments described below.
[0030] In the present specification, when "to" is used for a numerical range, the numerical values at both ends are the upper limit and the lower limit, respectively, and are included in the numerical range.
[0031] In the present specification, “(meth)acrylic acid” means methacrylic acid or acrylic acid, “(meth)acrylate” means acrylate or methacrylate, and “(meth)acryloyloxy” means acryloyloxy or methacryloyloxy.
[0032] In this specification, the “weight average molecular weight” and the “number average molecular weight” are values obtained by measuring at room temperature (23° C.) using gel permeation chromatography (GPC) under the following conditions using a standard polystyrene calibration curve.
[0033] Device: Shodex (trademark) GPC-101 (Showa Denko K.K.)
[0034] Column: Shodex (trademark) LF-804 (Showa Denko K.K.)
[0035] Column temperature: 40℃
[0036] Sample: 0.2 mass% tetrahydrofuran solution of the sample
[0037] Flow rate: 1mL / min
[0038] Eluent: Tetrahydrofuran
[0039] Detector: Shodex (trademark) RI-71S (Showa Denko K.K.)
[0040] In this specification, "glass transition temperature (Tg)" is the endothermic start temperature of the glass transition observed by taking 10 mg of a sample and measuring the sample by differential scanning calorimetry (DSC) at a heating rate of 10°C / min from -100°C to 200°C. When two or more endothermic start temperatures are observed, Tg is a simple average of the two or more endothermic start temperatures.
[0041] [Method for producing (meth)acrylic resin (A) having ethylenically unsaturated group]
[0042] The method for producing a (meth)acrylic resin (A) having an ethylenically unsaturated group (hereinafter referred to as "(meth)acrylic resin (A)") comprises: a step (i) of polymerizing a raw monomer group (M) containing a hydroxyl group-containing (meth)acrylic ester (m-1) and an alkyl (meth)acrylic ester (m-2) by reversible addition-fragmentation chain transfer (RAFT) to obtain a copolymer (A-0); and a step (ii) of adding an isocyanate group-containing ethylenically unsaturated compound (a) to a part of the side chain hydroxyl groups of the copolymer (A-0) to obtain the (meth)acrylic resin (A). The raw monomer group (M) may contain a carboxyl group-containing monomer (m-3).
[0043] <Step (i)>
[0044] Copolymer (A-0) is obtained by RAFT polymerization of a raw monomer group (M) containing a hydroxyl-containing (meth) acrylate (m-1), an alkyl (meth) acrylate (m-2) and an arbitrarily selected carboxyl-containing monomer (m-3) in the presence of a reversible addition-fragmentation chain transfer agent (RAFT agent). In this specification, the so-called RAFT polymerization refers to a free radical polymerization carried out in the presence of a RAFT agent. RAFT polymerization is a type of living free radical polymerization. Living free radical polymerization is generally known as a polymerization method that can obtain a polymer with a small molecular weight distribution. As specific examples thereof, atom transfer radical polymerization, free radical polymerization via organic tellurium, RAFT polymerization, etc. can be cited. Among these, RAFT polymerization does not use halogens and heavy metals, so the environmental load is low and it is suitable for semiconductor applications. Without being bound by any theory, the copolymer (A-0) obtained by RAFT polymerization has a more appropriate molecular weight distribution than the (meth)acrylic copolymer obtained by other active free radical polymerizations. Therefore, the adhesive composition produced using the (meth)acrylic resin (A) obtained from the copolymer (A-0) has excellent wettability to the adhesive layer and high adhesion to the adhesive layer. This is because the low molecular weight components of the (meth)acrylic resin (A) contribute to the wettability and fluidity of the adhesive composition. When the molecular weight distribution of the (meth)acrylic copolymer is too narrow, the fluidity and wettability of the obtained adhesive composition to the adhesive layer are low, and sufficient adhesion cannot be obtained.
[0045] As the polymerization method, solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, alternating copolymerization, etc. can be used. Among these polymerization methods, considering the addition reaction of step (ii), solution polymerization is preferably used in terms of the ease of reaction.
[0046] (Hydroxy-containing (meth)acrylate (m-1))
[0047] The hydroxyl-containing (meth)acrylate (m-1) is not particularly limited as long as it has a hydroxyl group and a (meth)acryloyloxy group. Specifically, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2,3-dihydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; (meth)acrylates having an aromatic ring and a hydroxyl group such as hydroxyphenyl (meth)acrylate and 2-hydroxy-3-phenoxypropyl (meth)acrylate, etc. are listed. Among them, from the viewpoint of the releasability of the adhesive sheet after UV irradiation, hydroxyalkyl (meth)acrylates are preferred, and hydroxyalkyl (meth)acrylates having a hydroxyalkyl group with 1 to 6 carbon atoms are more preferred, and 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate are particularly preferred.
[0048] Relative to 100 mol% of the raw material monomer group (M), the content of the hydroxyl-containing (meth)acrylate (m-1) is preferably 5 to 50 mol%, more preferably 10 to 40 mol%, and particularly preferably 15 to 35 mol%. If the content of the hydroxyl-containing (meth)acrylate (m-1) is 5 mol% or more, the (meth)acrylic resin (A) has sufficient hydroxyl groups to ensure the amount of crosslinking with the crosslinking agent (C), so that an adhesive layer with sufficient cohesive force can be obtained. In addition, the reaction point for introducing ethylenically unsaturated groups can also be ensured, and when the adhesive sheet is peeled off from the attached body after UV irradiation, a better peelability can be obtained. On the other hand, if the content of the hydroxyl-containing (meth)acrylate (m-1) is 50 mol% or less, the occurrence of unexpected reactions in the adhesive composition can be suppressed, and the storage stability is good.
[0049] (Alkyl (meth)acrylate (m-2))
[0050] The (meth) alkyl ester (m-2) is not particularly limited as long as it does not have a hydroxyl group and a carboxyl group but has an alkyl group and a (meth) acryloyloxy group. Specifically, alkyl (meth) acrylates such as methyl (meth) acrylate, ethyl (meth) acrylate, n-propyl (meth) acrylate, isopropyl (meth) acrylate, n-butyl (meth) acrylate, tert-butyl (meth) acrylate, pentyl (meth) acrylate, neopentyl (meth) acrylate, 2-ethylhexyl (meth) acrylate, isopentyl (meth) acrylate, and dodecyl (meth) acrylate; and alicyclic alkyl (meth) acrylates such as cyclopentyl (meth) acrylate, cyclohexyl (meth) acrylate, ethylcyclohexyl (meth) acrylate, norbornyl (meth) acrylate, dicyclopentyl (meth) acrylate, isobornyl (meth) acrylate, and adamantyl (meth) acrylate. The alkyl group in the alkyl (meth) acrylate (m-2) may have a substituent. As a substituent, alkoxy groups such as methoxy and ethoxy groups may be listed. Among them, from the viewpoint of the releasability of the adhesive sheet after UV irradiation, alkyl (meth)acrylates having an alkyl group with 1 to 20 carbon atoms and alicyclic alkyl (meth)acrylates are preferred, and one or more selected from methyl (meth)acrylate, ethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate and dicyclopentanyl (meth)acrylate are more preferred.
[0051] The content of the (meth) alkyl acrylate (m-2) is preferably 10 to 94 mol%, more preferably 30 to 85 mol%, and particularly preferably 50 to 80 mol%, relative to 100 mol% of the raw monomer group (M). If the content of the (meth) alkyl acrylate (m-2) is 10 mol% or more, excellent adhesion can be obtained. If the content of the (meth) alkyl acrylate (m-2) is 94 mol% or less, the content of the hydroxyl group and the ethylenically unsaturated group of the (meth) acrylic resin (A) can be fully ensured, so that from the perspective of the cohesive force of the adhesive layer and the peelability of the adhesive sheet after UV irradiation, an adhesive layer with balanced physical properties can be obtained.
[0052] (Carboxyl group-containing monomer (m-3))
[0053] The carboxyl-containing monomer (m-3) is not particularly limited as long as it is a monomer having a carboxyl group and an ethylenically unsaturated group but having no hydroxyl group. For example, unsaturated monobasic acids such as (meth)acrylic acid, crotonic acid, vinylbenzoic acid, α-halogenated alkyl, alkoxy, halogen, nitro or cyano substituents of acrylic acid, and unsaturated dibasic acids such as itaconic acid can be cited. Among them, (meth)acrylic acid is preferred from the perspective of ease of manufacturing the adhesive.
[0054] When a carboxyl-containing monomer (m-3) is used, the content of the carboxyl-containing monomer (m-3) is preferably 0.1 to 10 mol%, more preferably 0.5 to 8.0 mol%, and particularly preferably 1.0 to 5.0 mol%, relative to 100 mol% of the raw monomer group (M). If the content of the carboxyl-containing monomer (m-3) is 0.1 mol% or more, when the crosslinking agent (C) is a polyepoxy compound, a sufficient amount of crosslinking can be ensured, and sufficient cohesion of the adhesive can be obtained. If the content of the carboxyl-containing monomer (m-3) is 10 mol% or less, the content of the hydroxyl group and the ethylenically unsaturated group of the (meth) acrylic resin (A) can be fully ensured, so that from the perspective of the cohesion of the adhesive layer and the peelability of the adhesive sheet after UV irradiation, an adhesive layer with balanced physical properties can be obtained.
[0055] In the raw material monomer group (M), the molar ratio of the hydroxyl-containing (meth)acrylate (m-1), the (meth)acrylate alkyl ester (m-2) and the carboxyl-containing monomer (m-3) is preferably (m-1): (m-2): (m-3) = 10 to 70: 30 to 90: 0 to 10, and more preferably (m-1): (m-2): (m-3) = 15 to 35: 65 to 85: 0 to 5.
[0056] (Other monomers (m-4))
[0057] The raw material monomer group (M) may contain other monomers (m-4) in addition to (m-1) to (m-3). Specific examples include dienes such as butadiene and dicyclopentadiene, styrenes, unsaturated dicarboxylic acid diesters, and other vinyl compounds.
[0058] Specific examples of styrenes include styrene and α-, o-, m- or p-alkyl derivatives of styrene.
[0059] Specific examples of the unsaturated dicarboxylic acid diester include diethyl citraconic acid, diethyl maleate, diethyl fumarate, and diethyl itaconate.
[0060] Specific examples of other vinyl compounds include norbornene (bicyclo[2.2.1]hept-2-ene), 5-methylbicyclo[2.2.1]hept-2-ene, 5-ethylbicyclo[2.2.1]hept-2-ene, tetracyclo[4.4.0.1 2,5 .1 7,10 ]Dodec-3-ene, 8-methyltetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, 8-ethyltetracyclo[4.4.0.1 2,5 .1 7 ,10 ] dodec-3-ene, tricyclo[5.2.1.0 2,6 ]dec-8-ene, tricyclo[5.2.1.0 2,6 ]De-3-ene, tricyclo[4.4.0.1 2 ,5 ] undec-3-ene, tricyclo[6.2.1.0 1,8 ]Undec-9-ene, tricyclo[6.2.1.01 ,8 ]undec-4-ene, tetracyclo[4.4.0.1 2,5 .1 7,10 .0 1,6 ]Dodec-3-ene, 8-methyltetracyclo[4.4.0.1 2,5 .1 7,10 .0 1,6 ] dodec-3-ene, 8-ethylenetetracyclo[4.4.0.1 2,5 .1 7,12 ] dodec-3-ene, 8-ethylenetetracyclo[4.4.0.1 2,5 .1 7,10 .0 1,6 ] dodec-3-ene, pentacyclic [6.5.1.1 3,6 .0 2,7 .0 9,13 ]pentadeca-4-ene, pentacyclo[7.4.0.1 2,5 .19,12 .0 8,13 ]pentadeca-3-ene, (meth)acrylic acid aniline, vinyl pyridine, ethyl acetate, etc.
[0061] (Reversible addition fragmentation chain transfer agent (RAFT agent))
[0062] As the RAFT agent, a well-known one can be used without particular limitation. For example, sulfur compounds (trithiocarbonates, dithioesters, dithiocarbonates, and dithiocarbamates) represented by the following formula (1), formula (2), formula (3), or formula (4) are preferred.
[0063] 《Trithiocarbonate》
[0064]
Chemistry 1
[0065]
[0066] (In formula (1), R 1a With R 1b are the same or different, representing a hydrogen atom, a hydrocarbon group, a carboxyl group or a cyano group, R 1c represents a cyano group, a saturated or unsaturated aliphatic hydrocarbon group which may be substituted with a cyano group or a carboxyl group, or a phenyl group which may be substituted, R 2 It represents a saturated or unsaturated aliphatic hydrocarbon group in which a part of hydrogen atoms may be substituted by a carboxyl group, or a benzyl group which may be substituted).
[0067] Dithioesters
[0068]
Chemistry 2
[0069]
[0070] (In formula (2), R 3 a and R 3b are the same or different, representing a hydrogen atom, a hydrocarbon group or a cyano group, R 3 c represents a carboxyl group, an acetoxymethyl group, or a hydrocarbon group which may be substituted with a cyano group or a carboxyl group, R 4 represents a hydrocarbon group).
[0071] Dithiocarbonates
[0072]
Chemistry 3
[0073]
[0074] (In formula (3), R 5a With R 5b are the same or different and represent a hydrogen atom, a hydrocarbon group, a carboxyl group which may be substituted by a saturated aliphatic hydrocarbon group having 1 to 3 carbon atoms, or a cyano group, R 5c represents a hydrocarbon group which may be substituted by an alkoxy group, R 6represents a hydrocarbon group).
[0075] Dithiocarbamates
[0076]
Chemistry 4
[0077]
[0078] (In formula (4), R 7a With R 7b The same or different, representing a hydrogen atom or a hydrocarbon group, R 7c Represents cyano, R 8 With R 9 The same or different, representing a hydrocarbon group, or R 8 With R 9 bonded to form a saturated aliphatic hydrocarbon group having 1 to 3 carbon atoms or a pyrazole ring which may be substituted by a chlorine atom).
[0079] In formula (1), as R 1a and R 1b The hydrocarbon group shown in the formula (1) may be a linear, branched or cyclic saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, preferably a linear, branched or cyclic saturated or unsaturated hydrocarbon group having 1 to 12 carbon atoms. Examples of the hydrocarbon group include a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclohexyl, dodecyl, octadecyl, etc.; an aryl group having 6 to 12 carbon atoms, such as phenyl; and an arylalkyl group having 7 to 10 carbon atoms, such as benzyl and phenethyl. In formula (1), R 1c The saturated or unsaturated aliphatic hydrocarbon group shown in the formula (1) may be a linear, branched or cyclic saturated or unsaturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, preferably a linear, branched or cyclic saturated or unsaturated aliphatic hydrocarbon group having 1 to 12 carbon atoms. Examples of the aliphatic hydrocarbon group include a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclohexyl, dodecyl, octadecyl, etc. In formula (1), R 1c The saturated or unsaturated aliphatic hydrocarbon group shown in the formula (1) may have 1 to 3 hydrogen atoms substituted by, for example, a carboxyl group or a cyano group, and the carboxyl group may be further substituted by a saturated aliphatic hydrocarbon group having 1 to 3 carbon atoms. 1c The substituents of the phenyl group which may be substituted as shown in the formula (1) include substituted carbamoyl, alkoxycarbonyl having 2 to 5 carbon atoms which may be substituted with a hydroxyl group, alkenyloxycarbonyl having 3 to 5 carbon atoms, and the like. The substituents of the substituted carbamoyl group include saturated aliphatic hydrocarbon groups having 1 to 3 carbon atoms which may be substituted with a hydroxyl group or an acetoxy group, and the like. 2The saturated or unsaturated aliphatic hydrocarbon group shown in the formula (1) may be, for example, a linear, branched or cyclic saturated or unsaturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, preferably an aliphatic hydrocarbon group having 1 to 12 carbon atoms. Examples of the aliphatic hydrocarbon group include a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclohexyl, dodecyl, octadecyl, etc. In formula (1), R 2 The saturated or unsaturated aliphatic hydrocarbon group shown may have 1 to 3 hydrogen atoms substituted by carboxyl groups. 2 The substituents of the substituted benzyl group shown in the figure include substituted carbamoyl groups, alkoxycarbonyl groups having 2 to 5 carbon atoms which may be substituted with a hydroxyl group, alkenyloxycarbonyl groups having 3 to 5 carbon atoms, etc. As the substituents of the substituted carbamoyl group, saturated aliphatic hydrocarbon groups having 1 to 3 carbon atoms which may be substituted with a hydroxyl group or an acetoxy group, etc. can be mentioned. Among these, R 1a and R 1b are the same or different and are a hydrogen atom, a hydrocarbon group having 1 to 4 carbon atoms, or a carboxyl group, R 1c is a hydrocarbon group having 1 to 4 carbon atoms or a phenyl group which may be substituted, R 2 The compound represented by the formula (1) is preferably a linear, branched or cyclic saturated or unsaturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, or a benzyl group which may be substituted, wherein R 1a and R 1b is a hydrogen atom, a combination of a methyl group or an ethyl group and a carboxyl group, or a hydrogen atom, R 1c is methyl, ethyl or phenyl which may be substituted, R 2 The compound represented by the formula (1) which is a linear saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms or an optionally substituted benzyl group is more preferred.
[0080] In formula (2), as R 3a , R 3b , R 3c and R 4 The hydrocarbon group shown in , for example, can be a linear, branched or cyclic saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, preferably a linear, branched or cyclic saturated or unsaturated hydrocarbon group having 1 to 12 carbon atoms. Examples of the above hydrocarbon group include a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclohexyl, dodecyl, octadecyl, etc.; an aryl group having 6 to 12 carbon atoms, such as phenyl; an arylalkyl group having 7 to 10 carbon atoms, such as benzyl, phenethyl, etc. In formula (2), R 3cThe hydrocarbon group which may be substituted with a cyano group or a carboxyl group as shown in the above-mentioned hydrocarbon group includes, for example, a group in which 1 to 3 hydrogen atoms of the above-mentioned hydrocarbon group are substituted with a cyano group or a carboxyl group. 3a With R 3b are the same or different, and are straight-chain saturated hydrocarbon groups having 1 to 4 carbon atoms, R 3c is an aryl group, R 4 The compound represented by formula (2) is preferably an aryl group or a benzyl group, wherein R 3a With R 3b The same or different, methyl or ethyl, R 3c is phenyl, R 4 The compound represented by formula (2) which is a phenyl group or a benzyl group is more preferred.
[0081] In formula (3), as R 5a , R 5b , R 5c and R 6 The hydrocarbon group shown in , for example, can be a linear, branched or cyclic saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, preferably a linear, branched or cyclic saturated or unsaturated hydrocarbon group having 1 to 12 carbon atoms. Examples of the above hydrocarbon group include a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclohexyl, dodecyl, octadecyl, etc.; an aryl group having 6 to 12 carbon atoms, such as phenyl; an arylalkyl group having 7 to 10 carbon atoms, such as benzyl, phenethyl, etc. In formula (3), R 5c Examples of the hydrocarbon group which may be substituted with an alkoxy group include groups in which 1 to 3 hydrogen atoms possessed by the above hydrocarbon groups are substituted with an alkoxy group.
[0082] In formula (4), as R 7a , R 7b , R 8 and R 9 The hydrocarbon group shown in , for example, can be a linear, branched or cyclic saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, preferably a linear, branched or cyclic saturated or unsaturated hydrocarbon group having 1 to 12 carbon atoms. Examples of the hydrocarbon group include a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclohexyl, dodecyl, octadecyl, etc.; an aryl group having 6 to 12 carbon atoms such as phenyl; an arylalkyl group having 7 to 10 carbon atoms such as benzyl, phenethyl, etc. 8 and R 9 It may form a pyrazole ring together with the nitrogen atom of formula (4). The pyrazole ring may be substituted with a saturated aliphatic hydrocarbon group having 1 to 3 carbon atoms or a chlorine atom.
[0083] When polymerization is carried out in the presence of a RAFT agent represented by formulae (1) to (4), radical species undergo a chain reaction between the sulfur atom in the RAFT agent and the carbon atom adjacent to the sulfur atom, and polymerization proceeds. Among them, RAFT agents represented by formulae (1) and (2) are preferred from the viewpoint of ease of polymerization.
[0084] Most of the RAFT agents are commercially available. Those that are not commercially available can be easily synthesized by well-known or customary methods.
[0085] Specific examples of the RAFT agent include S-cyanomethyl-S-dodecyl trithiocarbonate, 2-[(dodecylsulfinylthiocarbonyl)sulfinyl]propionic acid, 2-{[(2-carboxyethyl)sulfinylthiocarbonyl]sulfinyl}propionic acid, bis{4-[ethyl-(2-hydroxyethyl)carbamoyl]benzyl}trithiocarbonate, 4-[(2-carboxyethylsulfinylthiocarbonyl)sulfinyl]-4-cyanovaleric acid, 4-cyano-4-[(dodecylsulfinylthiocarbonyl)sulfinyl]propionic acid, 4-[(dodecylsulfinylthiocarbonyl)sulfinyl]pentanoate, 2-cyano-2-propyldodecyl trithiocarbonate, bis[4-(allyloxycarbonyl)benzyl]trithiocarbonate, bis[4-(2,3-dihydroxypropoxycarbonyl)benzyl]trithiocarbonate, bis{4-[ethyl-(2-acetoxyethyl)carbamoyl]benzyl}trithiocarbonate, bis[4-(2-hydroxyethoxycarbonyl)benzyl]trithiocarbonate trithiocarbonates of carbonates, etc.; dithioesters of cyanoethyl dithiopropionate, benzyl dithiopropionate, benzyl dithiobenzoate, acetoxyethyl dithiobenzoate, 2-phenyl-2-propyl dithiobenzoic acid, 2-cyano-2-propyl dithiobenzoic acid, 4-cyano-4-(phenylthiocarbonylthio) pentanoic acid, S-(thiobenzoyl) thioglycolic acid, etc.; ethyl 2-[(ethoxythiocarbonyl)thio] propionate, O-ethyl-S-(2-propoxyethyl) dithiocarbonate, O-ethyl-S-( dithiocarbamates such as 2-cyano-2-propyldiethyldithiocarbamate, 2'-cyanobutane-2'-yl 4-chloro-3,5-dimethylpyrazole-1-dithiocarbamate, 2'-cyanobutane-2'-yl 3,5-dimethylpyrazole-1-dithiocarbamate, cyanomethyl 3,5-dimethylpyrazole-1-dithiocarbamate, cyanomethyl N-methyl-N-phenyldithiocarbamate, and the like. Among these, from the viewpoint of the ease of polymerization of the (meth)acrylic resin (A), trithiocarbonates and dithioesters are preferred, and 2-[(dodecylsulfinylthiocarbonyl)sulfinyl]propionic acid, 2-{[(2-carboxyethyl)sulfinylthiocarbonyl]sulfinyl}propionic acid, 2-phenyl-2-propyldithiobenzoic acid, S,S-dibenzyl trithiocarbonate, and bis{4-[ethyl-(2-acetoxyethyl)carbamoyl]benzyl}trithiocarbonate are more preferred.
[0086] The RAFT agent may be used alone or in combination of two or more.
[0087] (Free Radical Polymerization Initiator)
[0088] RAFT polymerization is preferably carried out in the presence of a free radical polymerization initiator. Examples of the free radical polymerization initiator include conventional organic free radical polymerization initiators, and specifically, examples include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2 ,4,4-trimethylpentane), dimethyl-2,2'-azobis(2-methylpropionate), etc.; and oil-soluble polymerization initiators such as peroxide-based polymerization initiators such as benzoyl peroxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, tert-butyl peroxybenzoate, diisopropyl peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, and 1,1-bis(tert-butylperoxy)cyclododecane.
[0089] The radical polymerization initiator may be used alone or in combination of two or more.
[0090] The amount of the radical polymerization initiator used is preferably 0.001 to 5 parts by mass, more preferably 0.005 to 3 parts by mass, and particularly preferably 0.01 to 1 part by mass, based on 100 parts by mass of the total amount of the raw material monomer group (M).
[0091] (Solvent)
[0092] As the solvent used in RAFT polymerization, a common solvent can be used. Examples of the solvent include esters such as ethyl acetate, propyl acetate, and butyl acetate; aromatic hydrocarbons such as toluene, xylene, and benzene; aliphatic hydrocarbons such as hexane and heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; ketones such as methyl ethyl ketone and methyl isobutyl ketone; glycols such as ethylene glycol, propylene glycol, and dipropylene glycol; glycol ethers such as methyl cellosolve, propylene glycol monomethyl ether, and dipropylene glycol monomethyl ether; and glycol esters such as ethylene glycol diacetate and propylene glycol monomethyl ether acetate. The solvent may be used alone or in combination of two or more.
[0093] (Reaction Conditions)
[0094] The reaction temperature of RAFT polymerization depends on the type of radical polymerization initiator used, but is usually 30° C. to 130° C., preferably 40° C. to 120° C., and more preferably 50° C. to 110° C. If the temperature during RAFT polymerization is 30° C. or higher, a sufficient reaction rate can be obtained. If the temperature during RAFT polymerization is 130° C. or lower, there is less risk during production.
[0095] The reaction time of RAFT polymerization also depends on the types of the raw monomer group (M), RAFT agent and free radical polymerization initiator used, but is generally 3 to 30 hours, preferably 4 to 20 hours, and more preferably 5 to 15 hours. If the reaction time is 3 hours or more, copolymer (A-0) can be produced from the raw monomer group (M) with an appropriate degree of polymerization, and if the reaction time is 30 hours or less, the production can be carried out efficiently.
[0096] <Step (ii)>
[0097] (Meth) acrylic resin (A) is obtained by adding an isocyanate group-containing ethylenically unsaturated compound (a) to a part of the side chain hydroxyl groups of the hydroxyl-containing (meth) acrylic ester (m-1) possessed by the copolymer (A-0). If the isocyanate group-containing ethylenically unsaturated compound (a) is added to all the side chain hydroxyl groups of the copolymer (A-0), the reaction site with the crosslinking agent (C) described later disappears, so the addition stays on a part of the side chain hydroxyl groups. Specifically, the side chain hydroxyl group is regarded as 100 mol%, and the addition reaction is preferably 5.0 to 99 mol%. There is no particular limitation on the method of adding the isocyanate group-containing ethylenically unsaturated compound (a), and methods well known in the technical field of this specification can be used. Since the (meth) acrylic resin (A) has an ethylenically unsaturated group in the side chain, the length of the molecular chain between the crosslinking points is relatively short compared to the (meth) acrylic copolymer having an ethylenically unsaturated group introduced at the end, and the adhesive force can be greatly reduced after UV irradiation. Therefore, the adhesive sheet using the (meth)acrylic resin (A) has excellent peelability from the attached body. In addition, since the (meth)acrylic resin (A) has an appropriate molecular weight distribution, the adhesive composition manufactured using the methacrylic resin (A) has excellent adhesion to the adhesive layer. Therefore, the adhesive composition manufactured using the (meth)acrylic resin (A) is suitable for the adhesive layer of the dicing-patch integrated film.
[0098] The molecular weight distribution (Mw / Mn) of the (meth)acrylic resin (A) is preferably 2.4 or more, more preferably 2.5 or more, and particularly preferably 3.0 or more. The molecular weight distribution of the (meth)acrylic resin (A) is preferably 10.0 or less, more preferably 6.0 or less, particularly preferably 5.8 or less, and particularly preferably 5.6 or less. Any combination of these lower limits and upper limits may be used.
[0099] The molecular weight distribution of the (meth)acrylic resin (A) is preferably 2.4 to 10.0, more preferably 2.4 to 6.0, particularly preferably 2.5 to 5.8, and particularly preferably 3.0 to 5.6. If the molecular weight distribution is 2.4 or more, the wettability of the adhesive composition containing the (meth)acrylic resin (A) is improved, and the adhesion to the attached body, especially the adhesive layer, is good. If the molecular weight distribution is 10.0 or less, the (meth)acrylic resin (A) in the high molecular weight region is controlled within an appropriate range, so the viscosity of the adhesive composition is easy to control, and since the (meth)acrylic resin (A) in the low molecular weight region is controlled within an appropriate range, it is possible to suppress residual adhesive when peeling the adhesive sheet from the attached body.
[0100] The weight average molecular weight (Mw) of the (meth)acrylic resin (A) is preferably 100,000 or more, more preferably 150,000 or more, particularly preferably 200,000 or more, and particularly preferably 300,000 or more. The weight average molecular weight of the (meth)acrylic resin (A) is preferably 800,000 or less, more preferably 700,000 or less, and particularly preferably 650,000 or less. Any combination of these lower limits and upper limits may be used.
[0101] The weight average molecular weight (Mw) of the (meth)acrylic resin (A) is preferably 100,000 to 800,000, more preferably 150,000 to 700,000, particularly preferably 200,000 to 650,000, and particularly preferably 300,000 to 650,000. If the weight average molecular weight is 100,000 or more, the peelability after UV irradiation is improved. If the weight average molecular weight is 800,000 or less, the viscosity of the adhesive composition containing the (meth)acrylic resin (A) can be appropriately suppressed, and the workability of the adhesive composition can be improved.
[0102] The ethylenically unsaturated group equivalent of the (meth)acrylic resin (A) is preferably 100 to 3,000 g / mol, more preferably 300 to 2,500 g / mol, and particularly preferably 500 to 2,000 g / mol. If it is within the above range, the crosslinking amount of the adhesive composition during UV irradiation is sufficient, and excellent peeling property when peeling the adhesive sheet produced using the (meth)acrylic resin (A) from the attached body and excellent pickup property of the small-piece element are obtained. In this specification, the ethylenically unsaturated group equivalent of the (meth)acrylic resin (A) is the mass of the (meth)acrylic resin (A) per mole of ethylenically unsaturated bonds. The ethylenically unsaturated group equivalent of the (meth)acrylic resin (A) in one embodiment is a calculated value calculated from the feed amount when it is assumed that each raw material used in the production of the (meth)acrylic resin (A) reacts 100%. The ethylenically unsaturated group equivalent of the (meth)acrylic resin (A) can be calculated from the binding amount of halogen to the (meth)acrylic resin (A). The bonding amount of halogen to the (meth)acrylic resin (A) can be evaluated in accordance with JIS K 0070:1992.
[0103] The glass transition temperature (Tg) of the (meth)acrylic resin (A) is preferably -80°C to 0°C, more preferably -70°C to -10°C, and particularly preferably -60°C to -30°C. If the glass transition temperature (Tg) is -80°C or higher, the cohesive force of the adhesive composition increases, and residual adhesive is suppressed. If the glass transition temperature (Tg) is 0°C or lower, sufficient fixation and bonding strength are obtained during the attached body processing.
[0104] When the raw material monomer group (M) contains a carboxyl group-containing monomer (m-3), the acid value of the (meth)acrylic resin (A) is preferably 0.5 to 100 mgKOH / g, more preferably 1.0 to 50 mgKOH / g, and particularly preferably 3.0 to 25 mgKOH / g. If the acid value is 0.5 mgKOH / g or more, when a polyepoxide is used as a crosslinking agent (C), a sufficient amount of crosslinking can be ensured, and the cohesive force of the adhesive layer can be sufficiently ensured. If the acid value is 100 mgKOH / g or less, the storage stability of the adhesive composition is good. The acid value in this specification is a value measured in accordance with JIS K 0070:1992.
[0105] (Isocyanate group-containing ethylenically unsaturated compound (a))
[0106] The isocyanate group-containing ethylenically unsaturated compound (a) is not particularly limited as long as it is a compound having an isocyanate group and an ethylenically unsaturated group but having no hydroxyl group and a carboxyl group. Specifically, (meth)acryloyloxyalkyl isocyanates such as 2-isocyanate ethyl (meth)acrylate, 2-isocyanate propyl (meth)acrylate, 3-isocyanate propyl (meth)acrylate, 2-isocyanate-1-methylethyl (meth)acrylate, 2-isocyanate-1,1-dimethylethyl (meth)acrylate, and 4-isocyanate cyclohexyl (meth)acrylate; 2-(2-isocyanate ethoxy)ethyl (meth)acrylate; 1,1-(bis (meth)acryloyloxymethyl)ethyl isocyanate, etc. Among them, from the viewpoint of the ease of synthesis of the (meth)acrylic resin (A), preferably (meth)acryloyloxyalkyl isocyanate, more preferably 2-isocyanate ethyl (meth)acrylate.
[0107] The content of the ethylenically unsaturated compound (a) containing an isocyanate group is preferably 0.25 mol or more, more preferably 0.50 mol or more, and particularly preferably 1.0 or more relative to 100 mol of the raw monomer group (M). The content of the ethylenically unsaturated compound (a) containing an isocyanate group is preferably 49 mol or less, more preferably 47 mol or less, and particularly preferably 45 mol or less. The combination of these lower limits and upper limits may be any combination.
[0108] The content of the isocyanate group-containing ethylenically unsaturated compound (a) is preferably 0.25 to 49 mol, more preferably 0.50 to 47 mol, and particularly preferably 1.0 to 45 mol relative to 100 mol of the raw monomer group (M). If the content of the isocyanate group-containing ethylenically unsaturated compound (a) is 0.25 mol or more, a sufficient amount of ethylenically unsaturated groups are introduced into the (meth)acrylic resin (A), and a better peelability can be obtained when the adhesive sheet is peeled off from the attached body after UV irradiation. If the content of the isocyanate group-containing ethylenically unsaturated compound (a) is 49 mol or less, the hydroxyl content of the (meth)acrylic resin (A) can be fully ensured, and excellent cohesion of the adhesive layer can be obtained. In addition, since the amount of unreacted isocyanate group-containing ethylenically unsaturated compound (a) can be reduced, an adhesive sheet with less residual adhesive can be obtained.
[0109] (catalyst)
[0110] In the addition reaction of step (ii), a well-known catalyst may be used as necessary. As the catalyst, for example, a urethanization catalyst such as dibutyltin dilaurate, bis(ethylacetoacetate)titanium diisopropoxyester, tetrakis(2,4-pentanedione)zirconium, tris(2-ethylhexanoate)bismuth may be used.
[0111] When a catalyst is used in step (ii), the amount of the catalyst used is preferably 0.01 to 10 parts by mass, more preferably 0.02 to 5 parts by mass, and particularly preferably 0.03 to 1 part by mass, based on 100 parts by mass of the total of the copolymer (A-0) and the isocyanate group-containing ethylenically unsaturated compound (a).
[0112] (Polymerization Inhibitor)
[0113] In the addition reaction of step (ii), a well-known polymerization inhibitor may be used as needed. As the polymerization inhibitor, well-known ones may be used without particular limitation, and examples thereof include 4-methoxyphenol, hydroquinone, p-methoxyphenol, 2,6-di-tert-butylphenol, 2,2'-methylenebis(4-methyl-6-tert-butylphenol) and phenothiazine. The polymerization inhibitor may be used alone or in combination of two or more.
[0114] When a polymerization inhibitor is used in step (ii), the amount of the polymerization inhibitor used is preferably 0.005 to 5 parts by mass, more preferably 0.03 to 3 parts by mass, and particularly preferably 0.05 to 1.5 parts by mass, relative to 100 parts by mass of the total of the copolymer (A-0) and the isocyanate group-containing ethylenically unsaturated compound (a). If the amount of the polymerization inhibitor used is 0.005 parts by mass or more, gelation during the addition reaction can be prevented. On the other hand, if the amount of the polymerization inhibitor used is 5 parts by mass or less, sufficient exposure sensitivity of the (meth)acrylic resin (A) during UV irradiation is obtained.
[0115] (Reaction Conditions)
[0116] The temperature of the addition reaction is preferably 25° C. to 130° C., particularly preferably 40° C. to 120° C. If the temperature of the addition reaction is 25° C. or higher, a sufficient reaction rate can be obtained. If the temperature of the addition reaction is 130° C. or lower, crosslinking of double bond portions due to free radical polymerization caused by heat and generation of gel can be prevented.
[0117] During the addition reaction, a gas having a polymerization inhibiting effect may be introduced into the reaction system. By introducing a gas having a polymerization inhibiting effect into the reaction system, gelation during the addition reaction can be prevented.
[0118] Examples of the gas having a polymerization inhibitory effect include a gas containing oxygen to a degree that is not within the explosion range of the substances in the system, such as air.
[0119] It is more preferable to use a gas having a polymerization inhibitory effect in combination with a polymerization inhibitor, because this can reduce the amount of the polymerization inhibitor to be used or enhance the polymerization inhibitory effect.
[0120] [Method for producing adhesive composition]
[0121] The adhesive composition can be prepared by a method comprising the step (iii) of mixing a (meth)acrylic resin (A), a photopolymerization initiator (B), a crosslinking agent (C) and other components added as needed. The adhesive composition comprising the (meth)acrylic resin (A) is suitable for a removable adhesive sheet, especially a dicing-and-sticking integrated film.
[0122] The method for mixing the components contained in the adhesive composition is not particularly limited, and the mixing can be performed using, for example, a homodispersor or a stirring device equipped with a stirring blade such as a paddle blade.
[0123] <Photopolymerization initiator (B)>
[0124] Examples of the photopolymerization initiator (B) include benzophenone, diphenylethanedione, benzoin, ω-bromoacetophenone, chloroacetone, acetophenone, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, p-dimethylaminoacetophenone, p-dimethylaminopropiophenone, 2-chlorobenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bisdiethylaminobenzophenone, Michler's ketone, benzoin methyl ether, Carbonyl photopolymerization initiators such as benzoin isobutyl ether, benzoin n-butyl ether, benzyl methyl ketal, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, methyl benzoylformate, 4'-dimethylaminoacetophenone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one.
[0125] Examples of the photopolymerization initiator (B) include sulfide-based photopolymerization initiators such as diphenyl disulfide, dibenzyl disulfide, tetraethylthiuram disulfide, and tetramethylammonium monosulfide; acylphosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 2,4,6-trimethylbenzoylphenylethoxyphosphine oxide; quinone-based photopolymerization initiators such as benzoquinone and anthraquinone; sulfonyl chloride-based photopolymerization initiators; and thioxanthone-based photopolymerization initiators such as thioxanthone, 2-chlorothioxanthone, and 2-methylthioxanthone.
[0126] Among these photopolymerization initiators (B), carbonyl photopolymerization initiators and acylphosphine oxides are preferred from the viewpoint of solubility in the adhesive composition, and at least one selected from 1-hydroxycyclohexyl phenyl ketone and 2,4,6-trimethylbenzoyldiphenylphosphine oxide is more preferred.
[0127] The photopolymerization initiator (B) may be used alone or in combination of two or more.
[0128] The photopolymerization initiator (B) is preferably 0.1 to 5.0 parts by mass, more preferably 0.5 to 2.0 parts by mass, relative to 100 parts by mass of (meth) acrylic resin (A). If the content of the photopolymerization initiator (B) is 0.1 parts by mass or more relative to 100 parts by mass of (meth) acrylic resin (A), the adhesive composition can be cured at a sufficiently fast curing speed during UV irradiation, so the adhesive force of the adhesive layer after UV irradiation can be sufficiently reduced. If the content of the photopolymerization initiator (B) is 5.0 parts by mass or less relative to 100 parts by mass of (meth) acrylic resin (A), the adhesive layer is not likely to remain on the attached body when the adhesive sheet having an adhesive layer containing the adhesive composition is attached to the attached body and then peeled off. Even if the content of the photopolymerization initiator (B) exceeds 5.0 parts by mass relative to 100 parts by mass of (meth) acrylic resin (A), the effect commensurate with the content of the photopolymerization initiator (B) is not seen, so by setting the content to 5.0 parts by mass or less, the adhesive composition can be economically manufactured.
[0129] <Crosslinking agent (C)>
[0130] By mixing the crosslinking agent (C), an adhesive composition having a good balance between the adhesive strength before UV irradiation and the adhesive strength after UV irradiation can be obtained. The crosslinking agent (C) is a compound having no ethylenically unsaturated bond and having two or more functional groups that can react with the hydroxyl group contained in the (meth)acrylic resin (A) and / or the carboxyl group as an optional functional group contained.
[0131] As crosslinking agent (C), there is no particular limitation, but preferably a compound having two or more functional groups reactive to hydroxyl groups. When (meth) acrylic resin (A) has a carboxyl group, a compound having two or more functional groups reactive to carboxyl groups can be used. As a functional group reactive to hydroxyl groups, isocyanate groups, epoxy groups, carboxyl groups, anhydride groups, aziridine groups, etc. can be listed, but from the viewpoint of reactivity, isocyanate groups and epoxy groups are preferred, and isocyanate groups are particularly preferred. As a functional group reactive to carboxyl groups, epoxy groups, hydroxyl groups, aziridine groups, etc. can be listed, but from the viewpoint of reactivity, epoxy groups and aziridine groups are preferred.
[0132] Examples of the crosslinking agent (C) include 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, hydrogenated toluene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, diphenylmethane-4,4′-diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, isocyanurate of hexamethylene diisocyanate, tetramethylxylylene diisocyanate, 1,5-naphthalene diisocyanate, toluene diisocyanate adduct of trimethylolpropane, xylylene diisocyanate adduct of trimethylolpropane, and triphenylmethane. Polyisocyanates such as methane triisocyanate, methylene bis(4-phenylmethane) triisocyanate, etc.; 1,3-bis(N,N'-diepoxypropylaminomethyl)cyclohexane, bisphenol A-epichlorohydrin type epoxy resin, N,N'-[1,3-phenylenebis(methylene)]bis[bis(oxiran-2-ylmethyl)amine], ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerol diglycidyl ether, glycerol triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polycyclopentyl Polyepoxy compounds such as propylene glycol, diglycerol polyglycidyl ether, etc.; aziridine compounds such as tetramethylolmethane-tri-β-aziridine propionate, trimethylolpropane-tri-β-aziridine propionate, N,N'-diphenylmethane-4,4'-bis(1-aziridine carboxylic acid amide), N,N'-hexamethylene-1,6-bis(1-aziridine carboxylic acid amide); melamine compounds such as hexamethoxymethyl melamine, hexaethoxymethyl melamine, hexapropoxymethyl melamine, hexabutoxymethyl melamine, hexapentoxymethyl melamine, hexahexyloxymethyl melamine; ethylene glycol-bis(ethylene glycol)-tri-β-aziridine propionate, trimethylolpropane-tri-β-aziridine propionate, N,N'-diphenylmethane-4,4'-bis(1-aziridine carboxylic acid amide), N,N'-hexamethylene-1,6-bis(1-aziridine carboxylic acid amide); [3-(2-aziridinyl)propionate], trimethylolpropane-tris[3-(2-aziridinyl)propionate], trimethylolpropane-tris[3-(1-aziridinyl)propionate], trimethylolpropane-tris[3-(2-methyl-1-aziridinyl)propionate], tetramethylolmethane-tris[3-(2-aziridinyl)propionate], pentaerythritol-tris[3-(1-aziridinyl)propionate], N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide), and the like.
[0133] Among these crosslinking agents (C), at least one selected from polyisocyanates and polyepoxy compounds is preferably used, and polyisocyanates are more preferably used, because of good reactivity with the (meth)acrylic resin (A).
[0134] The cross-linking agent (C) may be used alone or in combination of two or more.
[0135] The amount of the crosslinking agent (C) is preferably 0.1 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, particularly preferably 0.1 to 10 parts by mass, and particularly preferably 0.1 to 5 parts by mass relative to 100 parts by mass of the (meth)acrylic resin (A). If the amount of the crosslinking agent (C) is 0.1 parts by mass or more relative to 100 parts by mass of the (meth)acrylic resin (A), a three-dimensional crosslinked structure is fully formed in the adhesive composition during UV irradiation, thereby sufficiently reducing the adhesive force of the adhesive composition after UV irradiation. If the amount of the crosslinking agent (C) is 30 parts by mass or less relative to 100 parts by mass of the (meth)acrylic resin (A), the adhesive force of the adhesive composition before UV irradiation is good.
[0136] (Other ingredients)
[0137] In the method for producing the pressure-sensitive adhesive composition, other components other than the (meth)acrylic resin (A), the photopolymerization initiator (B) and the crosslinking agent (C) may be mixed as necessary. Examples of other components include a thickener, a solvent and various additives.
[0138] (Thickener)
[0139] As the thickener, any known thickener can be used without particular limitation. As the thickener, for example, terpene thickener resins, phenol thickener resins, rosin thickener resins, aliphatic petroleum resins, aromatic petroleum resins, copolymerized petroleum resins, alicyclic petroleum resins, xylene resins, epoxy thickener resins, polyamide thickener resins, ketone thickener resins and elastic thickener resins can be listed. These thickeners can be used alone or in combination of two or more.
[0140] When the thickener is mixed, the amount thereof added is preferably 30 parts by mass or less, more preferably 5 to 20 parts by mass, based on 100 parts by mass of the (meth)acrylic resin (A).
[0141] (Solvent)
[0142] The solvent is used to adjust the viscosity of the adhesive composition and can be used to dilute the adhesive composition. For example, when applying the adhesive composition, the solvent can be used to adjust the viscosity of the adhesive composition to an appropriate viscosity.
[0143] Examples of the solvent include organic solvents such as methyl ethyl ketone, methyl isobutyl ketone, acetone, ethyl acetate, propyl acetate, tetrahydrofuran, dioxane, dicyclohexanone, hexane, toluene, xylene, n-propanol, and isopropanol. These solvents may be used alone or in combination of two or more.
[0144] (additive)
[0145] Examples of the additives include plasticizers, surface lubricants, leveling agents, softeners, antioxidants, anti-aging agents, light stabilizers, ultraviolet absorbers, polymerization inhibitors, benzotriazole-based light stabilizers, phosphate-based and other flame retardants, surfactants, and antistatic agents.
[0146] [Method for producing adhesive sheet]
[0147] The pressure-sensitive adhesive sheet can be produced, for example, by the method described below.
[0148] First, a pressure-sensitive adhesive solution is prepared by dissolving or dispersing the pressure-sensitive adhesive composition in a solvent. The pressure-sensitive adhesive composition may be used as the pressure-sensitive adhesive solution as it is.
[0149] Next, the adhesive solution is applied to the substrate, and when it contains a solvent, it is heated and dried to remove the solvent to form an adhesive layer. Then, a peeling sheet is attached to the adhesive layer as needed. Furthermore, the obtained sheet is aged in an oven for a certain period of time as needed to form a cross-linked structure, thereby obtaining an adhesive sheet.
[0150] The adhesive sheet can also be manufactured by the method shown below. When an adhesive solution is applied to a release sheet and contains a solvent, the solvent is removed by heating and drying to form an adhesive layer. Then, the release sheet having the adhesive layer is placed on a substrate so that the surface of the adhesive layer side faces the substrate, and the adhesive layer is transferred to the substrate (transfer attachment). Furthermore, the obtained sheet can be cured in an oven for a certain period of time as needed to form a cross-linked structure, thereby obtaining an adhesive sheet.
[0151] In the above method, a substrate having an adhesive layer is used as the substrate, and a dicing-bonding integrated film can be obtained by coating the adhesive composition on the adhesive layer or laminating the adhesive layer with the adhesive layer facing each other.
[0152] As a method for applying the adhesive solution on a substrate (or on a release sheet), a well-known method can be used. Specifically, a method for applying using a conventional coating machine, such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a rod coater, a knife coater, a spray coater, a notch wheel coater, a direct coater, etc. can be listed.
[0153] There are no particular restrictions on the conditions for heating and drying the applied adhesive solution, but it is usually heated and dried at 25 to 180°C, preferably at 60 to 150°C, usually for 1 to 20 minutes, preferably for 1 to 10 minutes. By heating and drying within the above range, the solvent contained in the adhesive solution can be removed. There are no particular restrictions on the conditions for aging the heat-dried sheet in an oven for a certain period of time, but it is usually aged at 25 to 100°C, preferably at 30 to 80°C, usually for 1 to 30 days, preferably for 1 to 14 days. By aging under the above conditions, the (meth)acrylic resin (A) can be cross-linked by the cross-linking agent (C), and the gel fraction of the adhesive layer can be adjusted to the desired range.
[0154] [Application of adhesive sheet]
[0155] The adhesive sheet can be used as a removable adhesive sheet, for example, in the manufacture of electronic parts. Specifically, the removable adhesive sheet is used to fix the attached body in each step of the manufacture of electronic parts, and after various processing steps, it is irradiated with UV (ultraviolet rays) and peeled from the attached body. Therefore, the adhesive sheet can be used as a back grinding tape, a dicing tape, etc. when processing semiconductor wafers. The adhesive sheet can also be used as a supporting tape for fragile components such as extremely thin glass substrates and components that are easily warped such as FPC substrates. In particular, the adhesive sheet is suitable for the dicing tape used in the manufacture of dicing-chip integrated films because it has excellent adhesion to the adhesive layer and excellent peelability after UV irradiation.
[0156] When using an adhesive sheet as a dicing tape for a wafer, an adhesive sheet is attached to a wafer forming a plurality of parts before the dicing step is performed. Next, the wafer is cut and cut (cut) into individual parts to form component pieces (chips). Then, the adhesive sheet attached to each component piece is irradiated with UV. In this way, UV is irradiated through the substrate of the adhesive sheet to the adhesive layer, and the unsaturated bonds in the adhesive form a three-dimensional cross-linked structure and solidify. As a result, the adhesive force of the adhesive layer is reduced. Then, the adhesive sheet is peeled off from each component piece.
[0157] Examples of the light source used for UV irradiation include a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a carbon arc lamp, a xenon lamp, a metal halide lamp, a chemical lamp, and a black light lamp.
[0158] The UV irradiation dose irradiated to the adhesive sheet is preferably 50 to 3,000 mJ / cm 2 , more preferably 100 to 600 mJ / cm 2 If the UV radiation dose irradiated to the adhesive sheet is 50mJ / cm 2If the UV irradiation is above 3,000 mJ / cm, the adhesive layer can be cured at a sufficiently fast curing speed by UV irradiation, so the adhesive force of the adhesive layer after UV irradiation can be sufficiently reduced. 2 Therefore, the UV irradiation dose to the adhesive sheet was set to 3,000 mJ / cm 2 In the following, the pressure-sensitive adhesive sheet can be peeled off economically while reducing the influence of UV irradiation on the adherend.
[0159] [Example]
[0160] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0161] The raw materials used for the synthesis of the (meth)acrylic resins (A) and (cA) are shown below.
[0162] Hydroxyl-containing (meth)acrylate (m-1):
[0163] 2-hydroxyethyl acrylate, Nippon Shokubai Co., Ltd.
[0164] 2-hydroxyethyl methacrylate, Nippon Shokubai Co., Ltd.
[0165] 4-Hydroxybutyl acrylate, Osaka Organic Chemical Industry Co., Ltd.
[0166] (Meth) acrylate alkyl ester (m-2):
[0167] 2-Ethylhexyl acrylate, Osaka Organic Chemical Industry Co., Ltd.,
[0168] n-Butyl acrylate, Osaka Organic Chemical Industry Co., Ltd.,
[0169] Lauryl acrylate, Osaka Organic Chemical Industry Co., Ltd.,
[0170] 2-Methoxyethyl acrylate, Osaka Organic Chemical Industry Co., Ltd.,
[0171] Ethyl acrylate, Nippon Shokubai Co., Ltd.
[0172] Methyl methacrylate, Nippon Shokubai Co., Ltd.
[0173] Carboxyl-containing monomer (m-3):
[0174] Acrylic, Nippon Shokubai Co., Ltd.
[0175] Methacrylic acid, Nippon Shokubai Co., Ltd.
[0176] Free Radical Polymerization Initiator:
[0177] 2,2'-Azobis(isobutyronitrile), Fujifilm Wako Pure Chemical Industries, Ltd.
[0178] RAFT agent:
[0179] 2-[(Dodecylsulfinylthiocarbonyl)sulfinyl]propionic acid, Fujifilm Wako Pure Chemical Industries, Ltd.,
[0180] Bis{4-[ethyl-(2-hydroxyethyl)carbamoyl]benzyl}trithiocarbonate, Fujifilm Wako Pure Chemical Industries, Ltd., S,S-dibenzyl trithiocarbonate, Fujifilm Wako Pure Chemical Industries, Ltd.,
[0181] 2-Phenyl-2-propyldithiobenzoic acid, Ouchi Shinko Chemical Industry Co., Ltd.
[0182] additive:
[0183] 2-Methyl-2-n-butyltelluryl-propionic acid ethyl ester, Otsuka Chemical Co., Ltd.
[0184] Isocyanate group-containing ethylenically unsaturated compound (a):
[0185] Karenz (trademark) MOI, 2-isocyanate ethyl methacrylate, Showa Denko K.K.,
[0186] AOI-VM (trademark), 2-isocyanate ethyl acrylate, Showa Denko K.K.
[0187] The following is a synthesis example of (meth)acrylic resins (A) and (cA). The weight average molecular weight, molecular weight distribution, acid value and glass transition temperature of (meth)acrylic resins (A) and (cA) were measured and calculated by the above-mentioned method. The ethylenically unsaturated group equivalent of (meth)acrylic resins (A) and (cA) was calculated from the feed amount as described above. The hydroxyl value is the mass (mg) of potassium hydroxide required to neutralize the acetic acid bonded to the hydroxyl group when 1 g of the resin is acetylated in accordance with JIS K0070:1992. Table 1 shows the weight average molecular weight, molecular weight distribution, ethylenically unsaturated group equivalent, hydroxyl value, acid value and glass transition temperature of (meth)acrylic resins (A) and (cA).
[0188] [Synthesis Example 1 (Example 1-1)]
[0189] In a reaction apparatus equipped with a stirrer, a temperature regulator, a reflux cooler, a dropping funnel, and a thermometer, 132 parts by mass (71.6 mol) of 2-ethylhexyl acrylate, 33 parts by mass (28.4 mol) of 2-hydroxyethyl acrylate, 0.23 parts by mass of 2-[(dodecylsulfinylthiocarbonyl)sulfinyl]propionic acid, 0.05 parts by mass of 2,2'-azobis(isobutyronitrile), and 471 parts by mass of ethyl acetate as a solvent were added. After the start of heating reflux, the reaction was carried out for 10 hours. Next, the temperature of the reactant was lowered to 60°C, and a mixed solution of 24.7 parts by mass (15.9 mol) of 2-isocyanate ethyl methacrylate and 0.19 parts by mass of dibutyltin dilaurate as a urethanization catalyst was added dropwise through a dropping funnel. After the addition was completed, the reaction system was kept at 70°C for 4 hours to eliminate the isocyanate group. In this way, a solution containing 35% by mass of a (meth)acrylic resin (A1) having a weight average molecular weight of 300,000, a glass transition temperature of −50° C., and an ethylenically unsaturated group equivalent of 1,189 g / mol was obtained.
[0190] [Synthesis Examples 2 to 4 (Examples 1-2 to 1-4)]
[0191] (Meth)acrylic resins (A2) to (A4) were obtained in the same manner as in Synthesis Example 1 except that the compositions shown in Table 1 were used.
[0192] [Comparative Synthesis Example 1 (Comparative Example 1-1)]
[0193] In a reaction apparatus equipped with a stirrer, a temperature regulator, a reflux cooler, a dropping funnel, and a thermometer, 132 parts by mass (71.6 mol) of 2-ethylhexyl acrylate, 33 parts by mass (28.4 mol) of 2-hydroxyethyl acrylate, 0.08 parts by mass of 2,2'-azobis(isobutyronitrile), and 471 parts by mass of ethyl acetate as a solvent were added. After the start of heating and reflux, the reaction was carried out for 10 hours. Next, the temperature of the reactant was lowered to 60°C, and a mixed solution of 16.5 parts by mass (10.6 mol) of 2-isocyanate ethyl methacrylate and 0.18 parts by mass of dibutyltin dilaurate as a urethanization catalyst was added dropwise through a dropping funnel. After the addition was completed, the reaction system was kept at 70°C for 4 hours to eliminate the isocyanate group. Thus, a solution containing 35% by mass of a (meth)acrylic resin (cA1) having a weight average molecular weight of 600,000, a glass transition temperature of −45° C., and an ethylenically unsaturated group equivalent of 1,707 g / mol was obtained.
[0194] [Comparative Synthesis Example 2 (Comparative Example 1-2)]
[0195] A (meth)acrylic resin (cA2) was obtained in the same manner as in Synthesis Example 1 except that 2-methyl-2-n-butyltelluryl-propionic acid ethyl ester was used instead of 2-[(dodecylsulfinylthiocarbonyl)sulfinyl]propionic acid and the composition shown in Table 1 was used.
[0196] [Comparative Synthesis Example 3 (Comparative Example 1-3)]
[0197] Except having used the composition shown in Table 1, it carried out similarly to Synthesis Example 1, and obtained the (meth)acrylic resin (cA3).
[0198]
[0199] The raw materials used for preparing the adhesive composition are shown below.
[0200] Photopolymerization initiator (B):
[0201] TPO: 2,4,6-trimethylbenzoyldiphenylphosphine oxide (BASF, trade name: L-TPO)
[0202] Crosslinking agent (C)
[0203] L-45E: trimethylolpropane toluene diisocyanate adduct (Tosoh Corporation, trade name: Coronate L-45E),
[0204] TETRAD-X: N,N'-[1,3-phenylenebis(methylene)]bis[bis(oxiran-2-ylmethyl)amine] (Mitsubishi Gas Chemical Co., Ltd., trade name: TETRAD-X)
[0205] [Preparation of Adhesive Composition]
[0206] Ethyl acetate was added as a diluent to the solution containing the (meth)acrylic resins (A1) to (A4) and (cA1) to (cA3) obtained in Synthesis Examples 1 to 4 and Comparative Synthesis Examples 1 to 3, and the content of each of the (meth)acrylic resins (A1) to (A4) and (cA1) to (cA3) was adjusted to 30% by mass. Using this solution, an adhesive composition was obtained by the method shown below.
[0207] In a room where active lines are blocked, in a plastic container, the (meth)acrylic resin (A) or (cA) shown in Table 2, a photopolymerization initiator (B) and a crosslinking agent (C) are added in the contents (parts by mass) shown in Table 2, respectively, and stirred to obtain adhesive compositions (B1) to (B4) and (cB1) to (cB3). The values of (meth)acrylic resins (A1) to (A4) and (meth)acrylic resins (cA1) to (cA3) in Table 2 are the solid content of the solution used, that is, the usage amount (parts by mass) of (meth)acrylic resins (A1) to (A4) and (cA1) to (cA3). The value of the photopolymerization initiator (B) is the usage amount (parts by mass) of the photopolymerization initiator (B) relative to 100 parts by mass of the (meth)acrylic resin (A) or (cA). The value of the crosslinking agent (C) is the usage amount (parts by mass) of the crosslinking agent (C) relative to 100 parts by mass of the (meth)acrylic resin (A) or (cA).
[0208] [Example 2-1] Preparation of adhesive sheet
[0209] As a spacer, a polysiloxane-based light-peel PET film (Toyobo Co., Ltd., product name: E7006, thickness 25 μm) was prepared. For the surface subjected to the demolding treatment, the adhesive composition (B1) was applied using an applicator in such a way that the thickness after curing became 20 μm, and heated and dried at 100°C for 2 minutes to form an adhesive layer. Next, as a sheet substrate, a PO film with a thickness of 90 μm was prepared. The PO film was attached to the adhesive layer using a rubber roller in such a way that the corona-treated surface of the PO film was bonded to the exposed surface of the adhesive layer. The adhesive layer was cross-linked and cured in an oven at 40°C for 3 days to obtain the adhesive sheet of Example 2-1.
[0210] [Examples 2-2 to 2-4 and Comparative Examples 2-1 to 2-3] Preparation of Adhesive Sheets
[0211] PSA sheets of Examples 2-2 to 2-4 and Comparative Examples 2-1 to 2-3 were obtained in the same manner as in Example 2-1 except that the PSA compositions described in Table 2 were used instead of the PSA composition (B1).
[0212]
[0213] [Production of cutting-chip integrated film]
[0214] The cover film on one side of the patch film (FH-D25T-50, Showa Denko Materials Co., Ltd.) whose two sides of the adhesive layer are protected by the cover film was peeled off to expose the adhesive layer. The adhesive layer and the PET film were peeled off to expose the adhesive layer, and the adhesive layer of the adhesive sheet of Examples 2-1 to 2-4 and Comparative Examples 2-1 to 2-3 was attached with a rubber roller. It was left at room temperature for 1 day to obtain a dicing-patch integrated film.
[0215] [evaluate]
[0216] (1) Determination of adhesion (30° peel strength) before UV irradiation
[0217] As follows, the adhesion of the adhesive sheet of the embodiment and the comparative example to the patch film is evaluated by measuring the 30° peel strength. A sample with a width of 25 mm and a length of 100 mm is cut from the cutting-patch integrated film. The cover film on the side of the cutting-patch integrated film to which the adhesive sheet is not attached is peeled off, and the adhesive layer is attached to the polycarbonate plate using double-sided tape to obtain a sample for adhesion measurement. The peel strength of the adhesive sheet to the patch film is measured using a tensile testing machine (VPA-H200, Kyowa Interface Science Co., Ltd.). The measurement conditions are set to a peel angle of 30° and a tensile speed of 600 mm / min. Furthermore, the storage of the sample and the determination of the peel strength are carried out in an environment of a temperature of 23°C and a relative humidity of 40%. The results are shown in Table 2.
[0218] (2) Determination of adhesion (30° peel strength) after UV irradiation
[0219] For the dicing-bonding integrated film, irradiation was performed from the substrate side of the adhesive sheet at a dose of 300 mJ / cm 2 The adhesive sheet was irradiated with ultraviolet light (UV) under the conditions of , and a sample for measuring the adhesive strength after UV irradiation was obtained. During UV irradiation, a conveyor type ultraviolet irradiation device (EYEGRAPHICS Co., Ltd., 2KW lamp, 80W / cm) was used. Then, the peel strength of the adhesive sheet to the patch film was measured in the same manner as the measurement of the adhesive strength (30° peel strength) before UV irradiation. The results are shown in Table 2.
[0220] (3) Processability evaluation
[0221] (i) Preparation of samples for processability evaluation
[0222] A protective tape (BG tape) is attached to the surface of a silicon wafer (diameter: 12 inches, thickness: 775 μm). Then, invisible dicing of the silicon wafer is performed. That is, laser light is irradiated on the side (back side) of the silicon wafer opposite to the side on which the BG tape is attached under the following conditions to form a modified layer inside the silicon wafer.
[0223] <Stealth cutting conditions>
[0224] Stealth cutting device: DFL7361 (DISCO Co., Ltd.)
[0225] Laser oscillator model: Q-switched semiconductor excited solid laser
[0226] Wavelength: 1342nm
[0227] Frequency: 90kHz
[0228] Output: 1.7W
[0229] Number of passes: 2
[0230] Chip size: 10mm×10mm
[0231] Cutting speed: 700mm / sec
[0232] The silicon wafer after stealth dicing was ground until the thickness reached 30 μm. A grinding and polishing device (DGP8761, DISCO Co., Ltd.) was used for grinding. Under the following conditions, a bonding agent layer of a dicing-chip integrated film was attached to the ground silicon wafer, with the substrate side of the dicing tape facing the dicing ring. Then, the BG tape was peeled off from the surface of the silicon wafer.
[0233] <Attachment Conditions>
[0234] ·Attachment device: DFM2800 (DISCO Co., Ltd.)
[0235] Attachment temperature: 70℃
[0236] Attachment speed: 10mm / s
[0237] Attachment tension level: Level 6
[0238] Next, a die separator (DDS2300, DISCO Co., Ltd.) was used to cool and expand the wafer under the following conditions. Then, the substrate layer (PO film) of the dicing-bonding integrated film was thermally shrunk under the following conditions. After these steps, the silicon wafer and the bonding layer were singulated into a plurality of chips (size 10 mm×10 mm) with bonding sheets.
[0239] <Cooling expansion conditions>
[0240] Cooling temperature: -15℃
[0241] Cooldown: 120 seconds
[0242] ·Push up amount: 12mm
[0243] Pushing speed: 200mm / sec
[0244] Hold time after push-up: 3 seconds
[0245] <Heat shrinkage conditions>
[0246] Heater temperature: 220℃
[0247] Heater rotation speed: 5° / sec
[0248] ·Push up amount: 8mm
[0249] ·Tape cooling waiting time: 10 seconds
[0250] After the silicon wafer and the adhesive layer were separated into individual pieces, the adhesive layer was irradiated with ultraviolet rays from the substrate side of the adhesive sheet under the following conditions. This cured the adhesive layer and reduced the adhesive force to the adhesive layer.
[0251] <Ultraviolet irradiation conditions>
[0252] UV illumination: 100mW / cm 2
[0253] ·Ultraviolet radiation: 150mJ / cm 2
[0254] (ii) Evaluation of processability
[0255] (DAF scattering)
[0256] After cooling expansion and heat shrinkage, DAF scattering was evaluated based on the following criteria. Table 2 shows the results.
[0257] A: DAF scattering does not occur at all.
[0258] B: DAF scattering did not occur, but peeling or lifting was observed at the interface between the adhesive layer and the pressure-sensitive adhesive layer.
[0259] C: DAF scattering occurs at least one place.
[0260] (Chip edge peeling)
[0261] After the cooling expansion and the heat shrinkage, the peeling of the adhesive layer and the pressure-sensitive adhesive layer at the edge of the chip with the adhesive sheet was evaluated based on the following criteria.
[0262] A: No peeling was observed at all in the edge portion.
[0263] B: Peeling was observed at a length of 1 mm or more and less than 2 mm from the edge.
[0264] C: Peeling was observed at a length of 2 mm or more and less than 3 mm from the edge.
[0265] D: Peeling was observed at a length of 3 mm or more from the edge.
[0266] (Separability of adhesive layer)
[0267] The entire surface of the silicon wafer after cooling expansion and heat shrinkage was observed with a microscope, and the splitting properties of the adhesive layer were evaluated according to the following criteria.
[0268] A: The adhesive layer is completely divided.
[0269] D: There is an undivided portion in at least one location of the adhesive layer.
[0270] (Incision Width)
[0271] Using a microscope, measure the spacing (cut width) of the chips with adhesive sheets after singulation. Measure the cut width in the MD / TD direction at two locations (up, down, left, and right) and one location in the center of the silicon wafer (18 points in total) and find the average value. Evaluate using the following criteria. The results are shown in Table 2.
[0272] S: The average value of the slit width is 100 μm or more and less than 150 μm.
[0273] A: The average value of the incision width is 70 μm or more and less than 100 μm.
[0274] B: The average value of the incision width is 50 μm or more and less than 70 μm.
[0275] (Pickup)
[0276] After the above evaluation was performed, 100 chips with a binder were picked up under the following conditions and evaluated based on the following criteria. Table 2 shows the results.
[0277] <Pickup conditions>
[0278] ·Patch device: DB-830P (FASFORD TECHNOLOGY Co., Ltd.)
[0279] · Top push pin: EJECTOR NEEDLE SEN2-83-05 (diameter: 0.7 mm, tip shape: hemisphere with a radius of 350 μm, MICROMECHANICS)
[0280] Push-up height: 250μm
[0281] Pushing speed: 1mm / sec
[0282] Number of push pins: 9
[0283] <Evaluation Criteria>
[0284] A: The success rate of picking up is 100%.
[0285] B: The success rate of picking up is 80% or more and less than 100%.
[0286] C: The success rate of picking up is 60% or more and less than 80%.
[0287] The results of the processability evaluation of the dicing-chip integrated film made using the adhesive sheets of Examples 2-1 to 2-3 are all good. In particular, the incision width of Examples 2-1, 2-2 and 2-4 was evaluated as "S". From the perspective of achieving excellent pickup, the incision width is considered one of the important items in the process of invisible dicing. On the other hand, the incision width of the comparative examples was evaluated as "B". In addition, the comparative examples all experienced chip edge peeling after cooling expansion and thermal contraction, and poor pickup also occurred. Comparative Example 2-2, which uses a (meth) acrylic resin obtained from a copolymer manufactured by organic tellurium free radical polymerization, has a small amount of low molecular weight components and insufficient propagation of the fracture stress, so the splitting property of the adhesive layer is D.
[0288] Industrial Availability
[0289] According to the present disclosure, a (meth)acrylic resin suitable for an adhesive composition can be provided. An adhesive layer formed by using an adhesive composition produced using a (meth)acrylic resin can be preferably used as an adhesive layer of a removable adhesive sheet, especially a dicing-and-sticking integrated film.
Claims
1. A method for producing a (meth)acrylic resin, comprising: Step (i) of subjecting a raw material monomer group (M) containing a hydroxyl-containing (meth)acrylate (m-1) and an alkyl (meth)acrylate (m-2) to reversible addition fragmentation chain transfer (RAFT) polymerization to obtain a copolymer (A-0); and Step (ii) of adding an isocyanate group-containing ethylenically unsaturated compound (a) to a part of the side chain hydroxyl groups of the copolymer (A-0) to obtain a (meth)acrylic resin (A) having an ethylenically unsaturated group. 2 . The method for producing a (meth)acrylic resin according to claim 1 , wherein the raw monomer group (M) further contains a carboxyl group-containing monomer (m-3). 3 . The method for producing a (meth)acrylic resin according to claim 1 , wherein the (meth)acrylic resin (A) having an ethylenically unsaturated group has a molecular weight distribution Mw / Mn of 2.4 to 10.
0.
4. A method for producing an adhesive composition, comprising the step (iii) of mixing the (meth)acrylic resin (A) having an ethylenically unsaturated group obtained by the production method according to claim 1 or 2, a photopolymerization initiator (B) and a crosslinking agent (C). 5 . The method for producing an adhesive composition according to claim 4 , wherein the crosslinking agent (C) is at least one selected from the group consisting of polyisocyanates and polyepoxides. 6 . A method for producing an adhesive layer, comprising the step of forming a crosslinked structure in the adhesive composition obtained by the production method according to claim 4 . 7 . A method for producing a pressure-sensitive adhesive sheet, comprising applying the pressure-sensitive adhesive composition obtained by the production method according to claim 4 onto a sheet-like substrate to form a pressure-sensitive adhesive layer. 8 . A method for producing a pressure-sensitive adhesive sheet, comprising the step of forming a crosslinked structure in the pressure-sensitive adhesive layer obtained by the production method according to claim 7 . 9 . A method for producing a dicing-and-sticking integrated film, comprising laminating an adhesive layer on the pressure-sensitive adhesive layer having a cross-linked structure obtained by the production method according to claim 8 . 10 . A method for producing a dicing-and-bonding integrated film, comprising applying the adhesive composition obtained by the production method according to claim 4 onto an adhesive layer.