Polycarbonate-polyorganosiloxane copolymer and resin composition containing the copolymer

By preparing polycarbonate-polyorganosiloxane copolymers with specific structures and fully introducing siloxane blocks into the polymer backbone using melt polymerization, the problem of insufficient mechanical properties in existing technologies is solved, achieving high transparency and excellent mechanical properties, while reducing environmental and economic burdens.

CN114746473BActive Publication Date: 2024-11-15IDEMITSU KOSAN CO LTD
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202080083822.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-06
Filing Date
2020-12-07
Publication Date
2024-11-15
Estimated Expiration
2040-12-07

AI Technical Summary

Technical Problem

Existing technologies, other than interfacial polymerization, make it difficult to fully introduce siloxane blocks into the polymer backbone, leading to a decrease in the mechanical properties of polycarbonate-polyorganosiloxane copolymers.

Method used

By preparing polycarbonate-polyorganosiloxane copolymers with specific structures, polymers that meet specific conditions, containing polyorganosiloxane blocks and polycarbonate blocks with specific structures, are synthesized using melt polymerization, avoiding the use of toxic solvents and high-energy-consuming equipment.

Benefits of technology

This method enables the full introduction of siloxane blocks into the polymer backbone, improving the mechanical properties and transparency of the copolymer while reducing the environmental burden and economic costs of the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003674616100000051
    Figure BDA0003674616100000051
  • Figure BDA0003674616100000061
    Figure BDA0003674616100000061
  • Figure BDA0003674616100000062
    Figure BDA0003674616100000062
Patent Text Reader

Abstract

A polycarbonate-polyorganosiloxane copolymer, comprising a polycarbonate block (A-1) containing a specific structural unit and a polycarbonate block (A-2) containing a specific repeating unit, which satisfies the following conditions (A) or (B): Condition (A): The hexane extraction amount of the above-mentioned polycarbonate-polyorganosiloxane copolymer is less than 150 ppm; Condition (B): The average weight of the polycarbonate-polyorganosiloxane block contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the above-mentioned polycarbonate-polyorganosiloxane copolymer by gel permeation chromatography satisfies a specific formula.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polycarbonate-polyorganosiloxane copolymer, a method for producing the copolymer and a resin composition containing the copolymer. Background Art

[0002] Polycarbonate resin is an engineering plastic with excellent transparency and mechanical properties and very high impact resistance. It is known that polycarbonate-polyorganosiloxane copolymers obtained by copolymerizing polysiloxane and polycarbonate have excellent low-temperature impact resistance and excellent chemical resistance while maintaining high transparency.

[0003] Generally, as a method for producing a polycarbonate resin, there are known methods of directly reacting an aromatic dihydroxy compound with phosgene (interfacial polycondensation method) or transesterifying an aromatic dihydroxy compound with a carbonic acid diester in a molten state (melt polymerization method).

[0004] In many cases, interfacial polymerization is used to manufacture polycarbonate-polyorganosiloxane copolymers. For example, it is known that diaryl glycol compounds such as bisphenols and phosgene can be reacted in the presence of an organic solvent to generate a polycarbonate oligomer with a reactive chloroformate group, and the generation of the polycarbonate oligomer is simultaneously or sequentially further contacted with polycarbonate oligomers, bisphenols and polysiloxanes having hydroxyl-containing aryls at both ends in a dichloromethane / water medium to manufacture (patent document 1). Generally speaking, in the polymerization reaction, homocoupled products formed by bonding the same raw material components to each other are sometimes produced, and a part of the raw materials do not participate in the polymerization reaction and produce unreacted raw material components. These components are present in the polymer without being uniformly introduced into the polymer main chain, and therefore, the transparency and mechanical properties of the polymer significantly decrease. In the above-mentioned interfacial polymerization method, there are few situations in which such problems are generated, and polycarbonate-polyorganosiloxane copolymers with excellent transparency and mechanical properties can be obtained.

[0005] On the other hand, the interfacial polymerization method needs to use phosgene with high toxicity as a carbonate source. In addition, the polymerization reaction system needs to use methylene dichloride with large environmental burden as a solvent, which removes the need for large-scale degassing devices and a large amount of energy, which is disadvantageous in terms of economy. In order to avoid this problem, the manufacture method other than the interfacial polymerization method, for example, the melt polymerization method, has been studied to manufacture polycarbonate-polyorganosiloxane copolymers.

[0006] Patent document 2 discloses a method for producing a polycarbonate-polyorganosiloxane copolymer by melt polymerization from a bisphenol compound, a carbonate aromatic diester, a silanol-terminated polysiloxane and a catalyst. Patent document 3 discloses a method for producing a block copolymerized siloxane carbonate in the presence of a carbonate-terminated polyorganosiloxane, a dihydroxy aromatic compound, a diaryl carbonate and a carbonate exchange catalyst. Patent document 4 discloses a method for producing a polysiloxane / polycarbonate block cocondensation product, which comprises reacting a hydroxyaryloxy-terminated dimethylsiloxane and an oligocarbonate having a specific weight average molecular weight and a specific terminal ratio (OH terminal group and aryl terminal group) in a molten state in the presence of a catalyst.

[0007] Patent document 5 discloses a method for producing a poly(diorganosiloxane) / polycarbonate block copolymer, wherein a polydiorganosiloxane containing a polydiorganosiloxane component having a specific terminal structure, a bisphenol not containing Si, and a diaryl carbonate are melt polymerized in the presence of a specific catalyst. Patent document 6 discloses a method for producing a modified polycarbonate resin by solid phase polymerization, which describes the use of a polysiloxane compound as a starting material. Patent documents 7 to 9 disclose methods for producing polycarbonate-polyorganosiloxane block co-condensation products by an ester exchange method.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2015-189953

[0011] Patent Document 2: U.S. Patent No. 5,227,449

[0012] Patent Document 3: Japanese Patent Application Laid-Open No. 8-311206

[0013] Patent Document 4: Japanese Patent Application Laid-Open No. 10-251408

[0014] Patent Document 5: Japanese Patent Application Publication No. 2008-248262

[0015] Patent Document 6: Japanese Patent Application No. 2008-513594

[0016] Patent Document 7: Japanese Patent Application No. 2017-505841

[0017] Patent Document 8: Japanese Patent Application No. 2016-532734

[0018] Patent Document 9: Japanese Patent Application No. 2016-532733 Summary of the invention

[0019] Problem that the invention aims to solve

[0020] Although patent documents 2 to 7 disclose methods for producing polycarbonate-polyorganosiloxane copolymers based on melt polymerization, they are still insufficient in terms of obtaining polycarbonate-polyorganosiloxane copolymers with good mechanical properties. Although patent document 2 uses silanol-terminated siloxane, it is known that the lower the molecular weight of silanol-terminated dimethylsiloxane, the more it tends to undergo intramolecular condensation. The cyclic siloxane generated by intramolecular condensation remains in the obtained polycarbonate-polysiloxane copolymer, which may not only adversely affect its mechanical properties, but also cause adverse effects such as poor relay contacts in the field of electrical and electronic applications.

[0021] Although Patent Document 3 discloses that the amount of polydimethylsiloxane introduced into the polymer main chain increases, the appearance of carbonate-terminated polysiloxane and other raw materials in the molten state is described as "milky white", which suggests that carbonate-terminated polysiloxane is separated from other raw materials, and components generated by homocoupling and unreacted carbonate-terminated polysiloxane still remain in the polymer. These components significantly reduce the mechanical properties of polycarbonate-polysiloxane copolymers. In Patent Document 3, even in the manufacturing examples where the amount of siloxane introduced into the polymer main chain is large, a molar amount of 10×10 bisphenol A is used. -6 In the case of using an excessive amount of catalyst, the increase in the amount of residual catalyst components induces hydrolysis of the polycarbonate chain, and therefore, it is inferred that the obtained polymer does not have heat resistance and weather resistance that can withstand actual use conditions. The present inventors have confirmed that the mechanical properties of the allylphenol-terminated polyorganosiloxane copolymer disclosed in Patent Document 3 are also reduced.

[0022] The method disclosed in Patent Document 4 requires the preparation of oligocarbonates having a specific weight average molecular weight and a specific terminal ratio (OH terminal group and aryl terminal group) in advance in order to obtain a polycarbonate-polysiloxane copolymer. Therefore, it cannot be said to be a practical production method from the viewpoint of economic efficiency.

[0023] The copolymer disclosed in Patent Document 5 has a large micro-domain structure, and it cannot be said that siloxane has been uniformly introduced into the polymer main chain. Although Patent Document 6 discloses a method for producing a polycarbonate-polyorganosiloxane copolymer using a solid phase reaction, it does not mention the uniformity of the reaction and the physical properties of the polymer. Although Patent Documents 7 to 9 produce copolymers containing polysiloxane blocks having the same structure by an ester exchange method (melt polymerization method), in these methods, a polycarbonate of a specific structure containing a structure in which a carbonyl group is directly bonded to a benzene ring is required as a raw material. In order to obtain the desired polycarbonate-polysiloxane copolymer, it is necessary to produce the polycarbonate of the above-mentioned specific structure in advance, which is disadvantageous in terms of economic efficiency.

[0024] As described in detail above, although attempts have been made to obtain polycarbonate-polyorganosiloxane copolymers by methods other than interfacial polymerization, the current situation is that the introduction of siloxane blocks into the polymer backbone is insufficient. The subject of the present invention is to obtain a polycarbonate-polyorganosiloxane copolymer in which a sufficient amount of siloxane blocks can be introduced into the polymer backbone by methods other than interfacial polymerization, resulting in high mechanical properties.

[0025] Means used to solve problems

[0026] The present inventors have conducted intensive studies and have found that a polycarbonate-polyorganosiloxane copolymer having a specific structure and satisfying specific conditions can be produced to obtain a polycarbonate-polyorganosiloxane copolymer having a sufficient amount of siloxane blocks introduced into the polymer main chain and having high mechanical properties.

[0027] That is, the present invention relates to the following contents.

[0028] [1] A polycarbonate-polyorganosiloxane copolymer comprising a polyorganosiloxane block (A-1) containing a structural unit represented by the following general formula (1) and a polycarbonate block (A-2) containing a repeating unit represented by the following general formula (2), wherein the copolymer satisfies the following conditions (A) or (B):

[0029] Condition (A): The hexane extract of the polycarbonate-polyorganosiloxane copolymer is 150 ppm by mass or less;

[0030] Condition (B): The average weight of the polyorganosiloxane blocks contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the polycarbonate-polyorganosiloxane copolymer by gel permeation chromatography satisfies the following formula (B1).

[0031] [Mathematical formula 1]

[0032] 0.3≤[POS-Mh] / [POS-M1]≤3 (B1)

[0033] [In formula (B1), [POS-Mh] represents the average weight of the polyorganosiloxane block contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the components corresponding to the retention time range T1 to T2 using gel permeation chromatography. [POS-M1] represents the average weight of the polyorganosiloxane block contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the components corresponding to the retention time range T1 to T2 using gel permeation chromatography.

[0034] T1: Retention time of the peak top in the gel permeation chromatogram of standard polystyrene with Mw / Mn=1.01 and Mw=98900

[0035] T2: Retention time of the peak top in the gel permeation chromatogram of standard polystyrene with Mw / Mn=1.01 and Mw=13700

[0036] T3: retention time of the peak top in the gel permeation chromatogram of standard polystyrene with Mw / Mn=1.03 and Mw=3120]

[0037] [Chemical formula 1]

[0038]

[0039] [Where R 1 ~R 4 R may be the same or different and each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkylaryl group having 1 to 10 carbon atoms in the alkyl moiety. 6 represents an arylene group having 6 to 20 carbon atoms, an alkylene group having 1 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl moiety, and may contain -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -. R 111 represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms. 40 A divalent aliphatic hydrocarbon group having 3 to 400 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 400 carbon atoms, or a divalent aromatic hydrocarbon group having 8 to 400 carbon atoms, which may be substituted with a substituent. The divalent aliphatic hydrocarbon group, the divalent alicyclic hydrocarbon group, or the divalent aromatic hydrocarbon group may contain at least one heteroatom selected from oxygen atoms, nitrogen atoms, and sulfur atoms, and at least one halogen atom selected from fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms. a represents an integer of 2 to 500, and u represents 0 or 1. R 10represents a divalent aliphatic hydrocarbon group having 2 to 40 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 40 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, which may be substituted by a substituent. The divalent aliphatic hydrocarbon group, the divalent alicyclic hydrocarbon group, or the divalent aromatic hydrocarbon group may contain at least one hetero atom selected from oxygen atoms, nitrogen atoms, and sulfur atoms, and at least one halogen atom selected from fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms. y represents an integer of 10 to 500.]

[0040] [2] The polycarbonate-polyorganosiloxane copolymer according to [1] above, wherein the polyorganosiloxane block (A-1) has a structure represented by the following general formula (1′).

[0041] [Chemical formula 2]

[0042]

[0043] [Where R 1 ~R 4 , R 6 and a as described above. 8 The alkylene groups may be the same or different and are independent of each other and represent an arylene group having 6 to 20 carbon atoms, an alkylene group having 2 to 10 carbon atoms, a branched alkylene group having 3 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl portion. As a functional group, -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -. R 111 represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms. z represents 0 or 1. b represents an integer of 2 to 200.]

[0044] [3] The polycarbonate-polyorganosiloxane copolymer according to [1] or [2] above, wherein the polycarbonate block (A-2) has a structure represented by the following general formula (111) or a structure represented by the following general formula (112).

[0045] [Chemical formula 3]

[0046]

[0047] [Where R 55 and R 56 Each independently represents a halogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. X represents a single bond, an alkylene group having 1 to 8 carbon atoms, an alkylidene group having 2 to 8 carbon atoms, a cycloalkylene group having 5 to 15 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, a fluorenediyl group, an arylalkylene group having 7 to 15 carbon atoms, an arylalkylidene group having 7 to 15 carbon atoms, -S-, -SO-, -SO2-, -O-, or -CO-. R 100It represents a divalent aliphatic hydrocarbon group having 2 to 40 carbon atoms, which may have a branched structure or a cyclic structure. 100 It may contain at least one hetero atom selected from oxygen, nitrogen and sulfur atoms, and at least one halogen atom selected from fluorine, chlorine, bromine and iodine atoms. y represents an integer of 10 to 500. s and t each independently represent an integer of 0 to 4.]

[0048] [4] The polycarbonate-polyorganosiloxane copolymer according to any one of [1] to [3], wherein the polycarbonate block (A-2) comprises a member selected from the group consisting of 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3-methylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5 A structural unit derived from an aromatic bisphenol selected from the group consisting of trimethylcyclohexane and 1,1-bis(4-hydroxyphenyl)cyclododecene, or a structural unit derived from an aliphatic diol selected from the group consisting of isosorbide, cyclohexane-1,4-dimethanol, tricyclodecane dimethanol, 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 1,3-propylene glycol and 1,4-butanediol.

[0049] [5] The polycarbonate-polysiloxane copolymer according to any one of [1] to [4] above, wherein the polycarbonate block (A-2) has one or more selected from the group consisting of repeating units represented by the following general formulae (ai) to (av).

[0050] [Chemical formula 4]

[0051]

[0052] [6] The polycarbonate-polyorganosiloxane copolymer according to any one of [1] to [5] above, wherein in the general formula (1), a is an integer of 2 to 300.

[0053] [7] The polycarbonate-polyorganosiloxane copolymer according to any one of [1] to [6] above, wherein the polyorganosiloxane block (A-1) comprises at least one selected from the group consisting of structural units represented by the following general formulae (1-1) to (1-3).

[0054] [Chemical formula 5]

[0055]

[0056] [Where R 1 ~R 4 , R6 , R 8 , z, a, b are as described above. 5 represents an arylene group having 6 to 20 carbon atoms, an alkylene group having 1 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl moiety, and may contain -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -. R 7 represents an arylene group having 6 to 20 carbon atoms, an alkylene group having 2 to 10 carbon atoms, a branched alkylene group having 3 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl portion, and may contain -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -. R 111 represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms. z1 represents 0 or 1. b1 represents an integer of 2 to 200. β represents a divalent group derived from a diisocyanate compound, or a divalent group derived from a dicarboxylic acid or a halide of a dicarboxylic acid.]

[0057] [8] The polycarbonate-polyorganosiloxane copolymer according to any one of [1] to [7], wherein in the general formula (1), R 1 ~R 4 All represent methyl.

[0058] [9] The polycarbonate-polyorganosiloxane copolymer according to any one of [1] to [8], wherein in the general formula (1), R 6 It is trimethylene (-(CH2)3-).

[0059]

[10] The polycarbonate-polyorganosiloxane copolymer according to any one of [2] to [9], wherein in the general formula (1'), R 8 It is any structure selected from the group consisting of dimethylene (-(CH2)2-), methyl-substituted dimethylene (-CH2CHMe-), trimethylene (-(CH2)3-), and tetramethylene (-(CH2)4-).

[0060]

[11] The polycarbonate-polyorganosiloxane copolymer according to any one of [1] to

[10] above, wherein the content of the polyorganosiloxane block represented by the general formula (1) in the polycarbonate-polyorganosiloxane copolymer is 0.1% by mass or more and 60% by mass or less.

[0061]

[12] The polycarbonate-polyorganosiloxane copolymer according to any one of [1] to

[11] above, which has a viscosity average molecular weight (Mv) of 5,000 to 50,000.

[0062]

[13] The polycarbonate-polyorganosiloxane copolymer according to any one of [1] to

[12] above, wherein a 1 mm thick plate obtained by molding the polycarbonate-polyorganosiloxane copolymer has a haze value of 40 or less as measured in accordance with ISO 14782:1999.

[0063]

[14] The polycarbonate-polyorganosiloxane copolymer according to any one of [1] to

[13] above, which is obtained by a melt polymerization method.

[0064]

[15] The polycarbonate-polyorganosiloxane copolymer according to any one of [1] to

[14] above, which is obtained using a diol monomer (a1).

[0065]

[16] A polycarbonate resin composition comprising the polycarbonate-polyorganosiloxane copolymer described in any one of [1] to

[15] .

[0066]

[17] The polycarbonate resin composition according to

[16] above, further comprising an inorganic filler.

[0067]

[18] The polycarbonate resin composition according to

[17] , wherein the inorganic filler is contained in an amount of 1 to 150 parts by mass based on 100 parts by mass of the polycarbonate-polyorganosiloxane copolymer.

[0068]

[19] The polycarbonate resin composition according to

[17] or

[18] above, wherein the inorganic filler is glass fiber or carbon fiber.

[0069]

[20] A molded article formed from the polycarbonate resin composition described in any one of

[16] to

[19] .

[0070] Effects of the Invention

[0071] According to the present invention, a sufficient amount of siloxane blocks can be introduced into the polymer main chain, and thus a polycarbonate-polyorganosiloxane copolymer having excellent mechanical properties can be obtained. DETAILED DESCRIPTION

[0072] Hereinafter, the polycarbonate-polyorganosiloxane copolymer of the present invention and the polycarbonate resin composition containing the copolymer are described in detail. In this specification, any of the provisions considered as preferred can be adopted, and the combination of preferred provisions can be said to be more preferred. In this specification, the description of "XX to YY" means "XX or more and YY or less".

[0073] <Polycarbonate-polyorganosiloxane copolymer>

[0074] The polycarbonate-polyorganosiloxane copolymer of the present invention is characterized in that it comprises a polyorganosiloxane block (A-1) comprising a structural unit represented by the following general formula (1) and a polycarbonate block (A-2) comprising a repeating unit represented by the following general formula (2), and satisfies the following conditions (A) or (B):

[0075] Condition (A): The amount of hexane extract of the polycarbonate-polyorganosiloxane copolymer is 150 ppm by mass or less;

[0076] Condition (B): The average weight of the polyorganosiloxane blocks contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the polycarbonate-polyorganosiloxane copolymer by gel permeation chromatography satisfies the following formula (B1).

[0077] [Mathematical formula 2]

[0078] 0.3≤[POS-Mh] / [POS-M1]≤3 (B1)

[0079] [In formula (B1), [POS-Mh] represents the average weight of the polyorganosiloxane block contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the components corresponding to the retention time range T1 to T2 using gel permeation chromatography. [POS-M1] represents the average weight of the polyorganosiloxane block contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the components corresponding to the retention time range T1 to T2 using gel permeation chromatography.

[0080] T1: Retention time of the peak top in the gel permeation chromatogram of standard polystyrene with Mw / Mn=1.01 and Mw=98900

[0081] T2: Retention time of the peak top in the gel permeation chromatogram of standard polystyrene with Mw / Mn=1.01 and Mw=13700

[0082] T3: retention time of the peak top in the gel permeation chromatogram of standard polystyrene with Mw / Mn=1.03 and Mw=3120]

[0083] [Chemical formula 6]

[0084]

[0085] [Where R 1 ~R 4 R may be the same or different and each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkylaryl group having 1 to 10 carbon atoms in the alkyl moiety. 6represents an arylene group having 6 to 20 carbon atoms, an alkylene group having 1 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl moiety, and may contain -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -. R 111 represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms. 40 A divalent aliphatic hydrocarbon group having 3 to 400 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 400 carbon atoms, or a divalent aromatic hydrocarbon group having 8 to 400 carbon atoms, which may be substituted with a substituent. The divalent aliphatic hydrocarbon group, the divalent alicyclic hydrocarbon group, or the divalent aromatic hydrocarbon group may contain at least one heteroatom selected from oxygen atoms, nitrogen atoms, and sulfur atoms, and at least one halogen atom selected from fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms. a represents an integer of 2 to 500, and u represents 0 or 1. R 10 represents a divalent aliphatic hydrocarbon group having 2 to 40 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 40 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, which may be substituted by a substituent. The divalent aliphatic hydrocarbon group, the divalent alicyclic hydrocarbon group, or the divalent aromatic hydrocarbon group may contain at least one hetero atom selected from oxygen atoms, nitrogen atoms, and sulfur atoms, and at least one halogen atom selected from fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms. y represents an integer of 10 to 500.]

[0086] In R 6 In the case of an alkylene group, the carbon number is preferably 1 to 5.

[0087] From the viewpoint of improving affinity with the diol monomer (a1) and performing uniform polymerization, R 40, preferably comprising a repeating chain structure formed by connecting at least two structures comprising at least one hydrocarbon group selected from a divalent aliphatic hydrocarbon group having 2 to 20 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms and at least one heteroatom selected from the group consisting of an oxygen atom, a nitrogen atom and a sulfur atom. As a structure containing at least one hydrocarbon group selected from a divalent aliphatic hydrocarbon group having 2 to 20 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, and at least one heteroatom selected from the group consisting of an oxygen atom, a nitrogen atom, and a sulfur atom, a structure containing at least one structure selected from the group consisting of -OH, -O-, -(C=O)-, -O(C=O)-, -O(C=O)O-, -NH2, -NRH, -NR-, -NR-(C=O)-, -N=CR-, -SH, -S-, -SS-, and -(S=O)- is preferred. R represents a hydrogen atom, a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, and these may be substituted with a substituent. Preferred examples of the repeating chain structure include polyether, polyacetal, polylactone, polyacrylate, polyester, polycarbonate, polyketone, polysulfide, polysulfone, polyamide, and polyimide.

[0088] Among them, at least one selected from the group consisting of polyethers, polyacrylates and polycarbonates is preferred, and polyethers are most preferred. As the polyether, polyalkylene ethers are preferred, and among them, polyethylene glycol, polypropylene glycol, polytrimethylene glycol and polytetramethylene glycol are preferred.

[0089] As described above, the polycarbonate-polyorganosiloxane copolymer of the present invention comprises a polyorganosiloxane block (A-1) comprising a structural unit represented by the general formula (1) and a polycarbonate block (A-2) comprising a repeating unit represented by the general formula (2).

[0090] The polyorganosiloxane block constituting the polycarbonate-polyorganosiloxane copolymer contains the structural unit represented by the general formula (1) and satisfies the specific conditions (A) or (B), so that a sufficient amount of siloxane blocks can be introduced into the main chain of the obtained polycarbonate-polyorganosiloxane copolymer. 6 , R 40 , a and / or the polycarbonate block (A-2) containing the repeating unit represented by the general formula (2) wherein R 10 The option of can provide higher transparency.

[0091] As described below, the polycarbonate-polyorganosiloxane copolymer of the present invention can also be obtained by melt polymerization. The melt polymerization does not require solvents such as methylene chloride, so it is advantageous in terms of environmental protection and economy. In addition, phosgene with high toxicity is not used as a carbonate source, so it is also advantageous in terms of manufacturing.

[0092] The polyorganosiloxane block (A-1) containing the structural unit represented by the general formula (1) preferably has a structure represented by the following general formula (1A).

[0093] [Chemical formula 7]

[0094]

[0095] In the above general formula (1A), R 1 ~R 4 , R 6 , a and u are as described above.

[0096] R 40’ represents a divalent aliphatic hydrocarbon group having 2 to 380 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 380 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 380 carbon atoms, which may be substituted with a substituent. The divalent aliphatic hydrocarbon group, the divalent alicyclic hydrocarbon group, or the divalent aromatic hydrocarbon group may contain at least one hetero atom selected from an oxygen atom, a nitrogen atom, and a sulfur atom, and at least one halogen atom selected from a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. 40” represents a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, which may be substituted with a substituent. e represents 0 or 1.

[0097] As R 40’, preferably comprising: a repeating chain structure formed by connecting at least 2 structures comprising at least one hydrocarbon group selected from a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms and at least one heteroatom selected from the group consisting of an oxygen atom, a nitrogen atom and a sulfur atom. As a structure containing at least one hydrocarbon group selected from a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, and at least one heteroatom selected from the group consisting of an oxygen atom, a nitrogen atom, and a sulfur atom, a structure containing at least one structure selected from the group consisting of -OH, -O-, -(C=O)-, -O(C=O)-, -O(C=O)O-, -NH2, -NRH, -NR-, -NR--(C=O)-, -N=CR-, -SH, -S-, -SS-, and -(S=O)- is preferred. R represents a hydrogen atom, a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, and these may be substituted with a substituent. Preferred examples of the repeating chain structure include polyether, polyacetal, polylactone, polyacrylate, polyester, polycarbonate, polyketone, polysulfide, polysulfone, polyamide, and polyimide.

[0098] Among them, at least one selected from the group consisting of polyether, polyacrylate and polycarbonate is preferred, and polyether is most preferred. As the polyether, polyalkylene ether is preferred, and among them, polyethylene glycol, polypropylene glycol, polytrimethylene glycol and polytetramethylene glycol are preferred. The above structure is preferred from the viewpoint of improving affinity with the diol monomer (a1) and performing uniform polymerization.

[0099] The polyorganosiloxane block (A-1) containing the structural unit represented by the general formula (1) further preferably has a structure represented by the following general formula (1′).

[0100] [Chemical formula 8]

[0101]

[0102] [Where R 1 ~R 4 , R 6 and a as described above. 8 The alkylene groups may be the same or different and are independent of each other and represent an arylene group having 6 to 20 carbon atoms, an alkylene group having 2 to 10 carbon atoms, a branched alkylene group having 3 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl portion. As a functional group, -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -. R 111 represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms. z represents 0 or 1. b represents an integer of 2 to 200.]

[0103] R 8 The preferred embodiments are described below.

[0104] The polyorganosiloxane block (A-1) containing the structural unit represented by the general formula (1) preferably contains at least one selected from the group consisting of structural units represented by the following general formulae (1-1) to (1-3).

[0105] [Chemical formula 9]

[0106]

[0107] [Where R 1 ~R 4 , R 6 , R 8 , z, a and b are as described above. 5 represents an arylene group having 6 to 20 carbon atoms, an alkylene group having 1 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl moiety, and may contain -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -. R 7 represents an arylene group having 6 to 20 carbon atoms, an alkylene group having 2 to 10 carbon atoms, a branched alkylene group having 3 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl portion, and may contain -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -. R 111 represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms. z1 represents 0 or 1. b1 represents an integer of 2 to 200. β represents a divalent group derived from a diisocyanate compound, or a divalent group derived from a dicarboxylic acid or a halide of a dicarboxylic acid.]

[0108] In R 5 In the case of an alkylene group, the carbon number is preferably 1 to 5.

[0109] In the formula, as R 1 ~R 4 Examples of the halogen atom represented by R include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom. 1 ~R 4 The alkyl group having 1 to 10 carbon atoms represented by R includes methyl, ethyl, n-propyl, isopropyl, various butyl groups, various pentyl groups, and various hexyl groups. 1 ~R 4 The alkoxy group represented by can be exemplified by the case where the alkyl moiety is the above-mentioned alkyl group. 1 ~R 4 The aryl group represented by R includes phenyl, naphthyl and the like. 1 ~R4 The alkylaryl group shown in the figure includes a case where the alkyl part is the above-mentioned alkyl group and the aryl part is the above-mentioned aryl group.

[0110] As R 1 ~R 4 , are preferably a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an aralkyl group having 1 to 10 carbon atoms, and are more preferably methyl groups.

[0111] As R in the general formula (1), (1A) or (1'): 6 , or R in the general formula (1-1) to (1-3) 5 and R 6 The arylene group having 6 to 20 carbon atoms represented by , for example, phenylene, naphthylene, etc. As R in the above general formula (1), (1A) or (1'), 6 , or R in the general formula (1-1) to (1-3) 5 and R 6 The alkylene group having 1 to 10 carbon atoms as represented by the formula (1) may be a methylene group, a dimethylene group, a trimethylene group, a methyl-substituted dimethylene group, a tetramethylene group (the tetramethylene group may have a branched structure), or the like. 6 , or R in the general formula (1-1) to (1-3) 5 and R 6 The alkylarylene group shown in the figure includes a case where the alkyl part is the above-mentioned alkyl group and the arylene part is the above-mentioned arylene group.

[0112] In the above general formula (1), (1A) or (1'), R 6 , or R in the general formula (1-1) to (1-3) 5 and R 6 are preferably alkylene groups having 1 to 10 carbon atoms, more preferably dimethylene, methyl-substituted dimethylene or trimethylene. 6 It is trimethylene (-(CH2)3-).

[0113] As R in the above general formula (1') 8 , or R in the general formula (1-1) to (1-3) 7 and R 8 The arylene group having 6 to 20 carbon atoms represented by ' includes phenylene and naphthylene. 8 , or R in the general formula (1-1) to (1-3) 7 and R 8Examples of the alkylene group having 2 to 10 carbon atoms include methylene, dimethylene, trimethylene, methyl-substituted dimethylene, tetramethylene (the tetramethylene group may have a branched structure), and the like. 8 , or R in the general formula (1-1) to (1-3) 7 and R 8 The alkylarylene group shown in the figure includes a case where the alkyl part is the above-mentioned alkyl group and the arylene part is the above-mentioned arylene group.

[0114] In the above general formula (1'), R 8 , or R in the general formula (1-1) to (1-3) 7 and R 8 Preferably, the alkylene group has 1 to 10 carbon atoms, and more preferably, any one of the structures selected from the group consisting of dimethylene (-(CH2)2-), methyl-substituted dimethylene (-CH2CHMe-), trimethylene (-(CH2)3-) and tetramethylene (-(CH2)4-). The above structure is preferred from the viewpoint of improving affinity with the diol monomer (a1) and performing uniform polymerization.

[0115] It is particularly preferred that in the above general formula (1), (1A) or (1') or general formulas (1-1) to (1-3), R 1 ~R 4 are all methyl, R in the above general formula (1), (1A) or (1') 6 or R in the general formula (1-1) to (1-3) 5 and R 6 are all trimethylene groups, and R in the above general formula (1') 8 or R in the general formula (1-1) to (1-3) 7 and R 8 All of them are dimethylene polyorganosiloxanes.

[0116] β in the general formulae (1-1) and (1-2) represents a divalent group derived from a diisocyanate compound or a divalent group derived from a dicarboxylic acid or a dicarboxylic acid halide, and examples thereof include divalent groups represented by the following general formulae (iii) to (vii).

[0117] [Chemical formula 10]

[0118]

[0119] In the above general formula (1), (1A) or (1'), or general formulas (1-1) to (1-3), a represents the chain length of the polyorganosiloxane, and represents an integer of 2 to 500, preferably 2 to 300, more preferably 10 to 120, further preferably 15 to 100, and further preferably 20 to 90. When a is within the above range, a polycarbonate-polyorganosiloxane copolymer having excellent mechanical properties can be obtained, which is preferred. When a represents an integer of, for example, 20 to 65, transparency is also excellent in addition to the excellent mechanical properties, which is more preferred.

[0120] In the above general formula (1') or general formulas (1-1) to (1-3), b and b1 each independently represent an integer preferably from 0 to 200, more preferably from 2 to 100, further preferably from 5 to 50, further preferably from 8 to 25. The above range is preferred due to the availability of raw materials. If b and b1 are 100 or less, it is possible to suppress the decrease in operability due to the increase in the viscosity and melting point of the polyorganosiloxane, which is more preferred. If b and b1 are 50 or less, it is possible to maintain the polyorganosiloxane block content in the resin at an amount that can maintain the effect of improving physical properties, which is more preferred.

[0121] In the above general formula (1′) or general formulae (1-1) to (1-3), z and z1 each independently represent 0 or 1, and preferably 0.

[0122] The polycarbonate-polyorganosiloxane copolymer of the present invention contains a polycarbonate block (A-2) comprising a repeating unit represented by the above-mentioned general formula (2).

[0123] As R in the above general formula (2) 10 As the divalent aliphatic hydrocarbon group having 2 to 40 carbon atoms, for example, ethylene, n-propylene, isopropylene, n-butylene, isobutylene, n-pentylene, n-hexylene, n-heptylene, n-octylene, 2-ethylhexylene, n-nonylene, n-decylene, n-undecylene, n-dodecylene, n-tridecylene, n-tetradecylene, n-pentadecanylene, n-hexadecylene, n-heptadecanylene, n-octadecylene, etc. As the alicyclic hydrocarbon group having 3 to 40 carbon atoms, for example, cyclopentylene, cyclohexylene, cyclooctylene, cyclodecylene, cyclotetradecylene, adamantylene, bicycloheptylene, bicyclodecylene, tricyclodecylene, etc. can be mentioned.

[0124] As R in the above general formula (2) 10The divalent aromatic hydrocarbon group having 6 to 20 carbon atoms represented by bisphenol A may include various groups. In particular, divalent aromatic hydrocarbon groups derived from 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), 2,2-bis(4-hydroxy-3-methylphenyl)propane (bisphenol C), 1,1-bis(4-hydroxyphenyl)cyclohexane (bisphenol Z), 1,1-bis(4-hydroxyphenyl)-3-methylcyclohexane (bisphenol 3MZ), 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (bisphenol HTG), and 1,1-bis(4-hydroxyphenyl)cyclododecene may be mentioned. In addition, divalent aromatic hydrocarbon groups derived from at least one selected from the group consisting of hydroquinone, resorcinol, and catechol may also be mentioned.

[0125] The polycarbonate block (A-2) having a structure represented by the above general formula (2) preferably has a structure represented by the following general formula (111) or a structure represented by the following general formula (112).

[0126] [Chemical formula 11]

[0127]

[0128] [Where R 55 and R 56 Each independently represents a halogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. X represents a single bond, an alkylene group having 1 to 8 carbon atoms, an alkylidene group having 2 to 8 carbon atoms, a cycloalkylene group having 5 to 15 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, a fluorenediyl group, an arylalkylene group having 7 to 15 carbon atoms, an arylalkylidene group having 7 to 15 carbon atoms, -S-, -SO-, -SO2-, -O-, or -CO-. R 100 It represents a divalent aliphatic hydrocarbon group having 2 to 40 carbon atoms, which may have a branched structure or a cyclic structure. 100 It may contain at least one hetero atom selected from oxygen, nitrogen and sulfur atoms, and at least one halogen atom selected from fluorine, chlorine, bromine and iodine atoms. y represents an integer of 10 to 500. s and t each independently represent an integer of 0 to 4.]

[0129] In the above general formula (111), R 55 and R 56 Examples of the halogen atom independently represented include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0130] As R 55 and R 56 The alkyl groups independently represented by each of them include methyl, ethyl, n-propyl, isopropyl, various butyl groups ("various" means including straight-chain and all branched groups, the same below), various pentyl groups, and various hexyl groups. 55 and R56 The alkoxy groups independently represented include the case where the alkyl moiety is the above-mentioned alkyl group.

[0131] As the alkylene group represented by X, for example, methylene, ethylene, trimethylene, tetramethylene, hexamethylene, etc. can be mentioned, and preferably an alkylene group having 1 to 5 carbon atoms. As the alkylidene group represented by X, ethylidene, isopropylidene, etc. can be mentioned. As the cycloalkylene group represented by X, cyclopentanediyl, cyclohexanediyl, cyclooctanediyl, etc. can be mentioned, and preferably a cycloalkylene group having 5 to 10 carbon atoms can be mentioned. As the arylene group represented by X, phenylene, naphthylene, biphenylene, etc. can be mentioned. As the cycloalkylidene group represented by X, for example, cyclohexylidene, 3,5,5-trimethylcyclohexylidene, 2-adamantanylidene, etc. can be mentioned, and preferably a cycloalkylene group having 5 to 10 carbon atoms can be mentioned, and more preferably a cycloalkylene group having 5 to 8 carbon atoms can be mentioned. As the aryl moiety of the arylalkylene group represented by X, aryl groups having 6 to 14 ring carbon atoms such as phenyl, naphthyl, biphenyl, anthracenyl, etc. can be mentioned. Examples of the aryl moiety of the arylalkylidene group represented by X include aryl groups having 6 to 14 ring carbon atoms, such as phenyl, naphthyl, biphenylyl and anthracenyl.

[0132] s and t each independently represent an integer of 0 to 4, preferably 0 to 2, more preferably 0 or 1. Among them, it is suitable that s and t are 0 and X is a single bond or an alkylene group having 1 to 8 carbon atoms, or that s and t are 0 and X is an alkylidene group, particularly an isopropylidene group.

[0133] R 100 The divalent aliphatic hydrocarbon group having 2 to 40 carbon atoms represented by is specifically preferably an alkylene group having 2 to 18 carbon atoms, more preferably 2 to 10 carbon atoms, and further preferably 3 to 6 carbon atoms, preferably a cycloalkylene group having 4 to 20 carbon atoms, and more preferably 5 to 20 carbon atoms, or preferably a divalent oxygen- or nitrogen-containing saturated heterocyclic group having 4 to 20 carbon atoms, and more preferably 5 to 20 carbon atoms.

[0134] Examples of the alkylene groups having 2 to 18 carbon atoms include ethylene, n-propylene, isopropylene, n-butylene, isobutylene, n-pentylene, n-hexylene, n-heptylene, n-octylene, 2-ethylhexylene, n-nonylene, n-decylene, n-undecylene, n-dodecylene, n-tridecylene, n-tetradecylene, n-pentadecanylene, n-hexadecylene, n-heptadecylene, n-octadecylene, etc. Examples of the cycloalkylene groups having 4 to 20 carbon atoms include cyclopentylene, cyclohexylene, cyclooctylene, cyclodecylene, cyclotetradecylene, adamantylene, bicycloheptylene, bicyclodecylene, tricyclodecylene, etc. Examples of the divalent oxygen- or nitrogen-containing heterocyclic groups include groups containing oxygen or nitrogen atoms in the above-mentioned cycloalkylene skeletons.

[0135] Specifically, the polycarbonate block (A-2) comprising a repeating unit represented by the general formula (2) preferably has at least one unit selected from the group consisting of repeating units represented by the following general formulae (ai) to (a-xiii), more preferably has at least one unit selected from the group consisting of the following general formulae (ai) to (av), and from the perspective of high transparency, it is further preferred to have one or more units selected from the group consisting of repeating units represented by (ai), (a-ii) and (av).

[0136] [Chemical formula 12]

[0137]

[0138] [Chemical formula 13]

[0139]

[0140] [Chemical formula 14]

[0141]

[0142] The polycarbonate block (A-2) represented by the general formula (2) preferably contains a structural unit derived from an aromatic bisphenol selected from the group consisting of 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3-methylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane and 1,1-bis(4-hydroxyphenyl)cyclododecene, or an aliphatic diol selected from the group consisting of isosorbide, cyclohexane-1,4-dimethanol, tricyclodecane dimethanol, 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 1,3-propylene glycol and 1,4-butanediol.

[0143] Among them, the polycarbonate block (A-2) comprising a repeating unit represented by the general formula (2) more preferably has one or more selected from the group consisting of repeating units represented by the following general formulae (ai) to (av).

[0144] [Chemical formula 15]

[0145]

[0146] The number of units of the polycarbonate block (A-2) represented by the general formula (2) y is preferably 20 to 200, and more preferably 40 to 100. By setting y to 20 or more, the increase of low molecular weight components in the copolymer can be suppressed, which is preferred. By setting y to 40 or more, the toughness of the copolymer is improved, which is preferred. By setting y to 200 or less, appropriate fluidity can be obtained during molding, which is preferred. If it is 100 or less, the reaction mixture during production has appropriate fluidity, thereby improving productivity, which is preferred.

[0147] The content of the polyorganosiloxane block represented by the general formula (1) in the polycarbonate-polyorganosiloxane copolymer is preferably 0.1 to 60% by mass, more preferably 0.5 to 50% by mass, further preferably 1 to 30% by mass, and further preferably 3 to 20% by mass.

[0148] When the content of the polyorganosiloxane block in the polycarbonate-polyorganosiloxane copolymer is within the above range, more excellent impact resistance and transparency can be obtained.

[0149] The polycarbonate-polyorganosiloxane copolymer of the present invention needs to have the above-mentioned specific structure and satisfy the condition (A) or the condition (B). The polycarbonate-polyorganosiloxane copolymer can also satisfy both the condition (A) and the condition (B).

[0150] The polycarbonate-polyorganosiloxane copolymer satisfying condition (A) or condition (B) can be obtained, for example, by introducing a substituent having a repeating chain structure including a polar functional group as a substituent having high affinity for the hydroxyl group of a diol monomer into the terminal of the polyorganosiloxane.

[0151] It is inferred that the substituent having a repeating chain structure can contact with more diol monomers than the substituent not having a repeating chain structure, and thus can be strongly compatible with the diol monomer. Therefore, it is inferred that if the substituent having a repeating chain is introduced to the terminal of the polyorganosiloxane, the affinity of the polyorganosiloxane with the diol monomer can be improved compared to the case where the substituent having a repeating chain structure is not introduced to the terminal.

[0152] <Condition(A)>

[0153] This condition requires that the hexane extract of the polycarbonate-polyorganosiloxane copolymer is 150 mass ppm or less. "Hexane extract of 150 mass ppm or less" means that the amount of homocoupled components formed by bonding the same raw materials to each other during the production of the polycarbonate-polyorganosiloxane copolymer, cyclic components generated by the reaction of unreacted raw materials or oligomers within their molecules, unreacted diol monomers, and unreacted terminal-modified polyorganosiloxane is low, which means that the polyorganosiloxane block has been sufficiently introduced.

[0154] The hexane extraction amount of the polycarbonate-polyorganosiloxane copolymer in condition (A) is preferably 100 mass ppm or less, more preferably 80 mass ppm or less, further preferably 70 mass ppm or less, and further preferably 60 mass ppm or less. When condition (A) is met, the lower limit of the above-mentioned hexane extraction amount is not particularly limited. From the perspective of synthesis, it is, for example, 10 mass ppm or more, and in one embodiment, 20 mass ppm or more. When the polycarbonate-polyorganosiloxane copolymer is manufactured by interfacial polymerization, the hexane extraction amount can be further suppressed compared with the melt polymerization method. The reason is that the interfacial polymerization method using dichloromethane and water as solvents can make the raw materials and the growing ends of the polymer contact more efficiently compared with the melt polymerization method carried out under solvent-free conditions. Therefore, the conversion rate of the raw materials to the polymer is high, and it is not easy to produce unreacted raw materials and low molecular weight by-products that can be extracted by hexane. However, when the melt polymerization method is selected, it is usually difficult to set the hexane extraction amount as condition (A). The present invention has a solution that the above conditions can be satisfied even when the copolymer is produced by a melt polymerization method by forming a polycarbonate-polyorganosiloxane copolymer having a specific structure.

[0155] The above hexane extraction conditions are described in detail in the Examples.

[0156] <Condition (B)>

[0157] The condition (B) requires that the average weight of the polyorganosiloxane blocks contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the polycarbonate-polyorganosiloxane copolymer by gel permeation chromatography satisfy the following formula (B1).

[0158] [Mathematical formula 3]

[0159] 0.3≤[POS-Mh] / [POS-M1]≤3 (B1)

[0160] In formula (B1), [POS-Mh] represents the average weight of the polyorganosiloxane block contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the components corresponding to the retention time range T1 to T2 using gel permeation chromatography. [POS-M1] represents the average weight of the polyorganosiloxane block contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the components corresponding to the retention time range T1 to T2 using gel permeation chromatography.

[0161] T1: Retention time of the peak top in the gel permeation chromatogram of standard polystyrene with Mw / Mn=1.01 and Mw=98900

[0162] T2: Retention time of the peak top in the gel permeation chromatogram of standard polystyrene with Mw / Mn=1.01 and Mw=13700

[0163] T3: Retention time of the peak top in the gel permeation chromatogram of standard polystyrene with Mw / Mn=1.03 and Mw=3120

[0164] The measurement based on gel permeation chromatography (GPC) can be specifically carried out under the conditions described in the examples. When the [POS-Mh] / [POS-M1] value is outside the range of the above formula (B1), it means that the siloxane is not uniformly introduced into the polymer main chain. The lower limit of the above [POS-Mh] / [POS-M1] is preferably 0.35 or more, more preferably 0.5 or more, and further preferably 0.8 or more, and the upper limit is preferably 2.8 or less, more preferably 2 or less, further preferably 1.4 or less, further preferably 1.25 or less, and particularly preferably 1.2 or less.

[0165] The viscosity average molecular weight of the polycarbonate-polyorganosiloxane copolymer of the present invention is preferably 5,000 to 50,000, more preferably 12,000 or more, further preferably 14,000 or more, particularly preferably 16,000 or more, more preferably 30,000 or less, further preferably 23,000 or less, particularly preferably 21,000 or less.

[0166] The viscosity average molecular weight (Mv) is a value calculated from the following Schnell's equation by measuring the intrinsic viscosity [η] of a dichloromethane solution (concentration: g / L) at 20°C.

[0167] [η] = 1.23 × 10 -5 Mv 0.83

[0168] The refractive index of the polycarbonate-polyorganosiloxane copolymer of the present invention is not particularly limited, but is preferably 1.430 to 1.590, more preferably 1.450 to 1.570, and even more preferably 1.470 to 1.550 for light of a wavelength of 589.3 nm.

[0169] The difference (nF-nC) between the refractive index (nF) of the polycarbonate resin for light of a wavelength of 486.1 nm and the refractive index (nC) for light of a wavelength of 656.3 nm is preferably 0.015 or less, more preferably 0.013 or less, and further preferably 0.011 or less.

[0170] <Method for producing polycarbonate-polyorganosiloxane copolymer>

[0171] The polycarbonate-polyorganosiloxane copolymer of the present invention can be produced by using a diol monomer (a1) and a polyorganosiloxane (a2) as raw material monomers.

[0172] <<Diol Monomer (a1)>>

[0173] The diol monomer (a1) is not particularly limited as long as it has a structure represented by the following general formula (a1). As the diol monomer (a1), an aromatic dihydroxy compound or an aliphatic dihydroxy compound can be used.

[0174] [Chemical formula 16]

[0175] HO—R 10 -OH (a1)

[0176] In the above general formula (a1), R 10 As above, the preferred embodiment is also the same.

[0177] Examples of the aliphatic dihydroxy compound include: dihydroxy compounds having a chain aliphatic hydrocarbon group such as ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,10-decanediol, 2,2-dimethylpropane-1,3-diol, diethylene glycol, triethylene glycol, tetraethylene glycol, octaethylene glycol, dipropylene glycol, N-methyldiethanolamine, and p-terephthalic acid; 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 2,6-decahydronaphthalene diol, 1,5-decahydronaphthalene diol, 2,3-decahydronaphthalene diol, 2,6-decahydronaphthalene diol, 1,5-decahydronaphthalene diol, 2,3-decahydronaphthalene diol, 2,3-norbornane diol, 2,5-norbornane diol, 2,3-norbornane diol, 2,5-norbornane diol, 2,2-bis(4-hydroxycyclohexyl)-propane, 1,3-adamantanediol, 1 , 3-adamantanedimethanol, tricyclodecane dimethanol and other dihydroxy compounds having an alicyclic hydrocarbon group; condensed polycyclic ether diols such as isosorbide, 3,9-bis(2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 3,9-bis(2-hydroxy-1,1-diethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 3,9-bis(2-hydroxy-1,1-diethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, Heterocyclic spiro compounds such as cyclic ether diols such as (1,1-dipropylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane and 1,4-anhydroerythritol; cyclic acetal diols such as 2-(5-ethyl-5-hydroxymethyl-1,3-dioxane-2-yl)-2-methylpropane-1-aldehyde; N-heterocyclic diols such as 3,4-pyrrolidinediol, 3,4-dimethylpiperidinediol, N-ethyl-3,4-piperidinediol and N-ethyl-3,5-piperidinediol; S-heterocyclic diols such as deoxythiofructose, etc.

[0178] Specifically, the aliphatic dihydroxy compound may preferably be an aliphatic diol selected from isosorbide, cyclohexane-1,4-dimethanol, tricyclodecane dimethanol, 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 1,3-propylene glycol and 1,4-butanediol.

[0179] Examples of the aromatic dihydroxy compound include aromatic bisphenol compounds, and specifically, particularly preferably, an aromatic bisphenol selected from bisphenol A, bisphenol C, bisphenol Z, and a compound represented by the following general formula.

[0180] [Chemical formula 17]

[0181]

[0182] Specifically, bisphenol A (2,2-bis(4-hydroxyphenyl)propane), bisphenol C (2,2-bis(4-hydroxy-3-methylphenyl)propane), bisphenol Z (1,1-bis(4-hydroxyphenyl)cyclohexane), bisphenol 3MZ (1,1-bis(4-hydroxyphenyl)-3-methylcyclohexane), bisphenol HTG (1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane), and bisphenol-CDE (1,1-bis(4-hydroxyphenyl)cyclododecene) are more preferably used.

[0183] Among them, when an aliphatic diol is used as the diol monomer (a1), the obtained polycarbonate-polyorganosiloxane copolymer can obtain high transparency, which is preferred.

[0184] <<Polyorganosiloxane (a2)>>

[0185] The polyorganosiloxane (a2) preferably has a structure represented by the following general formula (a2-0).

[0186] [Chemical formula 18]

[0187]

[0188] [Where R 1 ~R 4 R may be the same or different and each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkylaryl group having 1 to 10 carbon atoms in the alkyl moiety. 5 and R 6 The alkylene groups may be the same or different and are independent of each other and represent an arylene group having 6 to 20 carbon atoms, an alkylene group having 1 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl moiety. As a functional group, the alkylene groups may include -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -. R 111 represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms. a represents an integer of 2 to 500.

[0189] R 40’ represents a divalent aliphatic hydrocarbon group having 2 to 380 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 380 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 380 carbon atoms, which may be substituted with a substituent. The divalent aliphatic hydrocarbon group, the divalent alicyclic hydrocarbon group, or the divalent aromatic hydrocarbon group may contain at least one hetero atom selected from an oxygen atom, a nitrogen atom, and a sulfur atom, and at least one halogen atom selected from a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.40” represents a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, which may be substituted by a substituent. e and u represent 0 or 1.]

[0190] As R 40’ , preferably comprising: a repeating chain structure formed by connecting at least two structures comprising at least one hydrocarbon group selected from a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms and at least one hetero atom selected from the group consisting of an oxygen atom, a nitrogen atom, and a sulfur atom. As the repeating chain structure, polyether, polyacetal, polylactone, polyacrylate, polyester, polycarbonate, polyketone, polythioether, polysulfone, polyamide, or polyimide can be cited as a preferred structure.

[0191] Among them, at least one selected from the group consisting of polyether, polyacrylate and polycarbonate is preferred, and polyether is most preferred. As the polyether, polyalkylene ether is preferred, and among them, polyethylene glycol, polypropylene glycol, polytrimethylene glycol and polytetramethylene glycol are preferred. The above structure is preferred from the viewpoint of improving affinity with the diol monomer (a1) and performing uniform polymerization.

[0192] As the polyorganosiloxane (a2), a monomer having any structure represented by the following general formulae (a2-1) to (a2-3) can be used.

[0193] [Chemical formula 19]

[0194]

[0195] In the above formula, R 1 ~R 4 , R 5 and R 6 , R 7 and R 8 , z, z1, β, a, b and b1 are as described above. The preferred embodiments are also the same, and the combination of the preferred embodiments is also preferred.

[0196] In the above-mentioned general formulas (a2-0) and (a2-1) to (a2-3), a represents the chain length of the polyorganosiloxane, and from the viewpoint of improving the affinity with the diol monomer (a1) and performing uniform polymerization, it represents an integer of 2 to 500, preferably 2 to 300, more preferably 10 to 100, further preferably 15 to 70, and further preferably 20 to 65.

[0197] In the above general formulae (a2-1) to (a2-3), b represents an integer of 2 to 200, preferably 2 to 100, more preferably 5 to 50, and even more preferably 8 to 25. The above range is preferred from the viewpoint of improving affinity with the diol monomer (a1) and performing uniform polymerization.

[0198] The polycarbonate-polyorganosiloxane copolymer of the present invention can be manufactured by polymerizing the raw material monomers by using an interfacial polymerization method or a melt polymerization method (ester exchange method). When manufactured by the interfacial polymerization method, reference can be made to the method described in, for example, Japanese Patent Publication No. 2014-80462. The polycarbonate-polyorganosiloxane copolymer of the present invention is preferably manufactured by reacting the polyorganosiloxane (a2), the diol monomer (a1) and the carbonate compound as the raw material monomers by a melt polymerization method under an alkaline catalyst in the presence of an end-capping agent.

[0199] (Carbonate Diester)

[0200] The carbonic acid diester is at least one compound selected from the group consisting of a diaryl carbonate compound, a dialkyl carbonate compound, and an alkyl aryl carbonate compound.

[0201] The diaryl carbonate compound is a compound represented by the following general formula (11) or a compound represented by the following general formula (12).

[0202] [Chemical formula 20]

[0203]

[0204] [In formula (11), Ar 1 and Ar 2 Each represents an aryl group and may be the same as or different from each other. 3 and Ar 4 Each represents an aryl group, and may be the same as or different from each other, D 1 It represents the residue after removing two hydroxyl groups from the above aromatic dihydroxy compound or aliphatic dihydroxy compound.]

[0205] The dialkyl carbonate compound is a compound represented by the following general formula (13) or a compound represented by the following general formula (14).

[0206] [Chemical formula 21]

[0207]

[0208] [In formula (13), R 21 and R 22Each represents an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 4 to 20 carbon atoms, and may be the same as or different from each other. 23 and R 24 Each represents an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 4 to 20 carbon atoms, and they may be the same as or different from each other. 2 It represents the residue after removing two hydroxyl groups from the above aromatic dihydroxy compound or aliphatic dihydroxy compound.]

[0209] The alkyl aryl carbonate compound is a compound represented by the following general formula (15) or a compound represented by the following general formula (16).

[0210] [Chemical formula 22]

[0211]

[0212] [In formula (15), Ar 5 Represents an aryl group, R 25 represents an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 4 to 20 carbon atoms. 6 Represents an aryl group, R 26 represents an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 4 to 20 carbon atoms, D 1 It represents the residue after removing two hydroxyl groups from the above aromatic dihydroxy compound or aliphatic dihydroxy compound.]

[0213] Examples of the diaryl carbonate compound include diphenyl carbonate, ditolyl carbonate, bis(chlorophenyl) carbonate, di(m-tolyl) carbonate, dinaphthyl carbonate, bis(biphenyl) carbonate, and bisphenol A bisphenyl carbonate.

[0214] Examples of the dialkyl carbonate compound include diethyl carbonate, dimethyl carbonate, dibutyl carbonate, dicyclohexyl carbonate, and bisphenol A bismethyl carbonate.

[0215] Examples of the alkyl aryl carbonate compound include methyl phenyl carbonate, ethyl phenyl carbonate, butyl phenyl carbonate, cyclohexyl phenyl carbonate, and bisphenol A methyl phenyl carbonate.

[0216] When the polycarbonate-polyorganosiloxane copolymer of the present invention is produced, one or more of the above-mentioned compounds may be appropriately selected and used as the carbonic acid diester. Among them, diphenyl carbonate is preferably used.

[0217] (Capping agent)

[0218] When the polycarbonate-polyorganosiloxane copolymer of the present invention is manufactured, an end-capping agent may be used as required. As the end-capping agent, any known end-capping agent in the manufacture of polycarbonate resins may be used, and for example, specific compounds thereof include phenol, p-cresol, p-tert-butylphenol, p-tert-octylphenol, p-cumylphenol, p-nonylphenol, and p-tert-amylphenol. Each of these monohydric phenols may be used alone, or two or more may be used in combination.

[0219] (Branching Agent)

[0220] When the polycarbonate-polyorganosiloxane copolymer of the present invention is produced, a branching agent may also be used. Examples of the branching agent include: phloroglucinol; trimellitic acid; 1,1,1-tri(4-hydroxyphenyl)ethane; 1-[α-methyl-α-(4'-hydroxyphenyl)ethyl]-4-[α',α'-bis(4"-hydroxyphenyl)ethyl]benzene; α,α',α"-tri(4-hydroxyphenyl)-1,3,5-triisopropylbenzene; indigo carmine di(o-cresol) and the like.

[0221] Specifically, for example, the polycarbonate-polyorganosiloxane copolymer of the present invention can be produced by the melt polymerization method through the following steps.

[0222] The diol monomer (a1), the polyorganosiloxane (a2) and the carbonate compound are subjected to an ester exchange reaction. The carbonate compound is preferably present in an amount of 0.9 to 1.2 times, more preferably 0.98 to 1.02 times, the molar amount of the diol monomer.

[0223] In the above-mentioned transesterification reaction, if the amount of the end-capping agent is in the range of 0.05 to 10 mol% relative to the diol monomer (a1) and the polyorganosiloxane (a2), the hydroxyl terminal of the obtained polycarbonate-polyorganosiloxane copolymer is capped, and thus a polycarbonate resin having sufficiently excellent heat resistance and water resistance can be obtained, which is preferred. The amount of the end-capping agent is more preferably 1 to 6 mol% relative to the diol monomer (a1) and the polyorganosiloxane (a2). The end-capping agent may be added in full to the reaction system in advance, or a portion may be added to the reaction system in advance and the remainder may be added as the reaction proceeds.

[0224] Preferably, an antioxidant is added into a reactor together with the diol monomer (a1), the polyorganosiloxane (a2) and the carbonate compound, and the transesterification reaction is carried out in the presence of the antioxidant.

[0225] When the transesterification reaction is carried out, the reaction temperature is not particularly limited, and is generally selected from the range of 100 to 330° C., preferably from the range of 180 to 300° C., and more preferably from the range of 200 to 240° C., and a method of gradually raising the temperature to 180 to 300° C. as the reaction proceeds is particularly preferred. If the temperature of the transesterification reaction is 100° C. or higher, the reaction rate is accelerated, while if it is 330° C. or lower, no side reaction occurs, and the generated polycarbonate-polyorganosiloxane copolymer is less likely to be colored.

[0226] The reaction pressure is set according to the vapor pressure of the monomers used and the reaction temperature. There is no particular limitation if it is set in a manner that allows the reaction to proceed efficiently. In many cases, in the initial stage of the reaction, the atmospheric pressure (normal pressure) or pressurized state is set to 1 to 50 atm (760 to 38,000 torr), and in the later stage of the reaction, the pressure is set to a reduced pressure state, preferably 1.33 to 1.33×10 4 pa (0.01~100torr).

[0227] The reaction time may be any time until the target molecular weight is reached, and is generally about 0.2 to 10 hours.

[0228] The above-mentioned transesterification reaction is usually carried out in the absence of an inert solvent, and can be carried out in the presence of 1 to 150 parts by mass of an inert solvent based on 100 parts by mass of the obtained polycarbonate resin as required. Examples of the inert solvent include aromatic compounds such as diphenyl ether, halogenated diphenyl ether, benzophenone, polyphenylene ether, dichlorobenzene, and methylnaphthalene; tricyclic [5.2.1.0 2,6 ] cycloalkanes such as decane, cyclooctane, cyclodecane, etc.

[0229] The reaction may be carried out in an inert gas atmosphere as required. Examples of the inert gas include various gases such as argon, carbon dioxide, nitrous oxide, nitrogen, chlorofluorocarbons, alkanes such as ethane and propane, and olefins such as ethylene and propylene.

[0230] In the melt polymerization method, a basic catalyst is preferably used as a catalyst. As the basic catalyst, at least one selected from the group consisting of metal catalysts such as alkali metal compounds and alkaline earth metal compounds, organic catalysts such as nitrogen-containing compounds and quaternary phosphonium salts containing aromatic groups, and metal compounds can be cited. These compounds can be used alone or in combination.

[0231] As the basic catalyst, organic acid salts, inorganic salts, oxides, hydroxides, hydrides and alkoxides of alkali metals or alkaline earth metals; quaternary ammonium hydroxides; quaternary phosphonium salts containing an aromatic group, etc. The basic catalyst may be used alone or in combination of two or more.

[0232] Examples of the alkali metal compound include sodium hydroxide, potassium hydroxide, cesium hydroxide, lithium hydroxide, sodium bicarbonate, sodium carbonate, potassium carbonate, cesium carbonate, lithium carbonate, sodium acetate, potassium acetate, cesium acetate, lithium acetate, sodium stearate, potassium stearate, cesium stearate, lithium stearate, sodium borohydride, sodium benzoate, potassium benzoate, cesium benzoate, lithium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, disodium phenyl phosphate, disodium salt, dipotassium salt, dicesium salt, dilithium salt of bisphenol A, sodium salt, potassium salt, cesium salt, lithium salt of phenol, and the like.

[0233] Examples of the alkaline earth metal compound include magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, magnesium diacetate, calcium diacetate, strontium diacetate, and barium diacetate.

[0234] Examples of the nitrogen-containing compound include quaternary ammonium hydroxides having an alkyl group, an aryl group, and the like such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, and trimethylbenzylammonium hydroxide. In addition, examples include tertiary amines such as triethylamine, dimethylbenzylamine, and triphenylamine, and imidazoles such as 2-methylimidazole, 2-phenylimidazole, and benzimidazole. In addition, examples include bases or basic salts such as ammonia, tetramethylammonium borohydride, tetrabutylammonium borohydride, tetrabutylammonium tetraphenylborate, and tetraphenylammonium tetraphenylborate.

[0235] Examples of the metal compound include zinc-aluminum compounds, germanium compounds, organic tin compounds, antimony compounds, manganese compounds, titanium compounds, and zirconium compounds.

[0236] Specific examples of the quaternary phosphonium salt containing an aromatic group include tetraphenylphosphonium hydroxide, tetranaphthylphosphonium hydroxide, tetra(chlorophenyl)phosphonium hydroxide, tetra(biphenyl)phosphonium hydroxide, tetratolylphosphonium hydroxide, tetramethylphosphonium hydroxide, tetraethylphosphonium hydroxide, tetrabutylphosphonium hydroxide and the like tetra(aryl or alkyl)phosphonium hydroxides, tetramethylphosphonium tetraphenylborate, tetraphenylphosphonium bromide, tetraphenylphosphonium phenolate, tetraphenylphosphonium tetraphenylborate, methyltriphenylphosphonium tetraphenylborate, benzyltriphenylphosphonium tetraphenylborate, biphenyltriphenylphosphonium tetraphenylborate, tetratolylphosphonium tetraphenylborate, tetraphenylphosphonium phenolate, tetra(p-tert-butylphenyl)phosphonium diphenyl phosphate, triphenylbutylphosphonium phenolate, triphenylbutylphosphonium tetraphenylborate and the like.

[0237] The aromatic group-containing quaternary phosphonium salt is preferably combined with a nitrogen-containing organic basic compound, for example, a combination of tetramethylammonium hydroxide and tetraphenylphosphonium tetraphenylborate is preferred.

[0238] The amount of the basic catalyst used is preferably 1×10 -9 ~1×10 -2moles, preferably 1×10 -8 ~1×10 -2 moles, more preferably 1×10 -7 ~1×10 -3 moles are selected within the range.

[0239] A catalyst deactivator may also be added in the later stage of the reaction. As the catalyst deactivator to be used, known catalyst deactivators can be effectively used. Among them, ammonium salts and phosphonium salts of sulfonic acids are preferred. In addition, salts of dodecylbenzenesulfonic acid such as tetrabutylphosphonium dodecylbenzenesulfonate and salts of p-toluenesulfonic acid such as tetrabutylammonium p-toluenesulfonate are preferred.

[0240] As esters of sulfonic acids, methyl benzenesulfonate, ethyl benzenesulfonate, butyl benzenesulfonate, octyl benzenesulfonate, phenyl benzenesulfonate, methyl p-toluenesulfonate, ethyl p-toluenesulfonate, butyl p-toluenesulfonate, octyl p-toluenesulfonate, phenyl p-toluenesulfonate, etc. are also preferably used. Among them, tetrabutylphosphonium dodecylbenzenesulfonate or butyl p-toluenesulfonate is most preferably used.

[0241] Regarding the amount of the catalyst deactivator used, when using at least one polymerization catalyst selected from alkali metal compounds and alkaline earth metal compounds, it can be used in a proportion of preferably 0.5 to 50 moles, more preferably 0.5 to 10 moles, and further preferably 0.8 to 5 moles relative to 1 mole of the catalyst.

[0242] Preferably, an antioxidant is mixed after adding the catalyst deactivator to end the polymerization reaction.

[0243] The reaction in the melt polymerization method can be carried out in either a continuous or batch mode. The reaction apparatus used in the melt polymerization can be any of a vertical reaction apparatus equipped with an anchor stirrer, a maximum blade type (MAXBLEND) stirrer, or a helical ribbon type (HELICAL RIBBON) stirrer, or a horizontal reaction apparatus equipped with a paddle type stirrer, a grid type paddle (Japanese: lattice wing), or a spectacle type paddle (Japanese: メガ礻 wing). In addition, it can also be an extruder type equipped with a screw. In the case of continuous operation, it is preferred to appropriately combine and use these reaction apparatuses.

[0244] The polycarbonate-polyorganosiloxane copolymer of the present invention is preferably manufactured using raw materials that satisfy the following conditions.

[0245] Condition (i): The haze value measured according to ISO14782:1999 under the conditions of 23°C and a light path length of 10 mm of the mixture obtained by contacting the raw material diol monomer (a1), the raw material polyorganosiloxane (a2), the carbonic acid diester, and the basic catalyst at 100 to 250°C for 0.5 to 5 hours is 30 or less.

[0246] The haze value is a value measured at 23° C. using a haze measuring device in accordance with ISO 14782:1999 using a glass cell with an optical path length of 10 mm filled with the mixture. It should be noted that the haze value measurement conditions of the raw material mixture are different from the polymerization conditions and are only used when selecting the raw materials.

[0247] When the haze value of the raw material mixture after the heat treatment is within the above range, the obtained polycarbonate-polyorganosiloxane copolymer has high transparency, which is preferred.

[0248] The haze value of the raw material mixture after the heat treatment is more preferably 20 or less, further preferably 10 or less, further preferably 5 or less, further preferably 1 or less.

[0249] The conditions for obtaining the mixture for measuring the haze value are the same as those described in the above (i). In addition, the temperature condition in condition (i) is preferably 150 to 250° C., more preferably 180 to 250° C., and the contact time is preferably 0.7 to 4 hours, more preferably 0.7 to 2 hours. When the temperature condition and the contact time in condition (i) are within the above-mentioned appropriate ranges and the obtained mixture has the haze value specified in condition (i), a polycarbonate-polyorganosiloxane copolymer with higher transparency can be obtained.

[0250] <Polycarbonate resin composition>

[0251] The polycarbonate resin composition of the present invention contains the above-mentioned polycarbonate-polyorganosiloxane copolymer (polycarbonate-polyorganosiloxane copolymer (A)).

[0252] The polycarbonate resin composition of the present invention may contain known additives within a range not impairing the properties of the polycarbonate-polyorganosiloxane copolymer (A).

[0253] (additive)

[0254] The polycarbonate resin composition of the present invention may be formulated with known additives according to the application and needs. Examples of the additives include various fillers, antioxidants, heat stabilizers, plasticizers, light stabilizers, polymer metal deactivators, flame retardants, lubricants, antistatic agents, surfactants, antibacterial agents, ultraviolet absorbers, release agents, and the like.

[0255] The antioxidant can suppress the decomposition of the thermoplastic resin composition during production and molding.

[0256] [filler]

[0257] Examples of fillers that can be incorporated into the polycarbonate resin composition of the present invention include inorganic fillers such as spherical fillers, plate-like fillers, and fibrous fillers.

[0258] Examples of the spherical filler include calcium carbonate, kaolin (aluminum silicate), silicon dioxide, perlite, volcanic ash microspheres (SHIRASU BALLOON), sericite, diatomaceous earth, calcium sulfite, calcined alumina, calcium silicate, crystalline zeolite, and amorphous zeolite.

[0259] Examples of the plate-like filler include talc, mica, and wollastonite.

[0260] Examples of the fibrous filler include glass fiber, carbon fiber, needle-shaped filler such as wollastonite, magnesium oxysulfate, potassium titanate fiber, and fibrous calcium carbonate. The inorganic filler is preferably glass fiber or carbon fiber.

[0261] As the glass fiber, any type of glass fiber made of alkali-containing glass, low-alkali glass, alkali-free glass, or the like can be suitably used.

[0262] The form of these glass fibers is not particularly limited, and glass fibers in any form such as rovings, milled fibers, and chopped strands may be used.

[0263] Examples of commercially available glass fibers include CSH-3PA (manufactured by Nitto Bosho Co., Ltd.), T511 (manufactured by Nippon Electric Glass Co., Ltd.), and MA409C (manufactured by Asahi Fiber Glass Co., Ltd.).

[0264] The polycarbonate resin composition of the present invention preferably contains a glass filler from the viewpoint of strengthening the resin composition.

[0265] [Composition ratio]

[0266] The polycarbonate resin composition of the present invention may contain an inorganic filler in an amount of preferably 1 to 150 parts by mass, more preferably 11 to 100 parts by mass, further preferably 15 to 60 parts by mass, and further preferably 15 to 40 parts by mass, relative to 100 parts by mass of the polycarbonate-polyorganosiloxane copolymer (A). By setting the amount within the above range, various mechanical properties effects due to the inorganic filler, such as an improvement in strength such as elastic modulus, can be achieved without impairing the properties of the polycarbonate-polyorganosiloxane copolymer (A).

[0267] The method for producing the polycarbonate resin composition of the present invention is not particularly limited as long as it has a step of mixing the polycarbonate-polyorganosiloxane copolymer and the optional additive. For example, the polycarbonate-polyorganosiloxane copolymer and the optional additive can be mixed using a mixer or the like, and melt-kneaded to thereby produce the polycarbonate-polyorganosiloxane copolymer. The melt-kneading can be carried out by a commonly used method, such as a method using a ribbon blender, a Henschel mixer, a Banbury mixer, a drum mixer, a single-screw extruder, a twin-screw extruder, a co-kneader, a multi-screw extruder, etc. The heating temperature during melt-kneading is usually appropriately selected within the range of 150°C to 300°C, preferably 220°C to 300°C.

[0268] [Molding products]

[0269] The molded article of the present invention comprises the polycarbonate resin composition of the present invention. The molded article can be manufactured by injection molding, injection compression molding, extrusion molding, blow molding, stamping molding, vacuum forming, foaming, etc., using the melt-kneaded product of the polycarbonate resin composition or the pellets obtained by melt-kneading as raw materials. It is particularly preferred that the molded article is manufactured by injection molding or injection compression molding using the obtained pellets.

[0270] The thickness of the molded product can be arbitrarily set according to the application. In particular, when transparency of the molded product is required, it is preferably 0.2 to 4.0 mm, more preferably 0.3 to 3.0 mm, and further preferably 0.3 to 2.0 mm. If the thickness of the molded product is 0.2 mm or more and 4.0 mm or less, good mechanical strength can be obtained.

[0271] The molded article may be coated with a hard coat film, an anti-fogging film, an antistatic film, or an anti-reflection film as required, or may be a composite coating of two or more types.

[0272] Among them, a coating having a hard coating film is particularly preferred because it has good weather resistance and can prevent the wear of the surface of the molded product over time. The material of the hard coating film is not particularly limited, and known materials such as acrylate hard coating agents, silicone hard coating agents, and inorganic hard coating agents can be used.

[0273] In the case of a molded product containing a glass filler, since at least a portion of the glass filler exists on the outermost surface of the molded product, the surface roughness of the molded product increases, the diffuse reflection on the surface of the molded product increases, and as a result, the transparency of the molded product is sometimes deteriorated. Therefore, as a method for reducing the surface roughness of the molded product, there is a method of reducing the surface roughness of the molded product by forming a layer (skin layer) with a high presence ratio of resin on the outermost surface of the molded product. As a method for forming the skin layer, in the case of injection molding, by setting the temperature of the mold to a temperature higher than the general conditions, the resin contacting the mold flows easily, and the surface roughness of the outermost surface of the molded product can be reduced. In addition, in the case of compression molding, by setting the pressure during molding to a pressure higher than the general conditions, the surface roughness of the outermost surface of the molded product can be reduced. By using these methods to reduce the surface roughness of the molded product, the diffuse reflection on the surface of the molded product is reduced, and the haze is reduced, and as a result, the transparency of the molded product can be improved.

[0274] When the molded article thus obtained is molded into a flat plate, when the content of the polyorganosiloxane block represented by formula (1) in the polycarbonate-polyorganosiloxane copolymer is less than 5% by mass and the average chain length a of the polyorganosiloxane block (A-2) in the polycarbonate-polyorganosiloxane copolymer is less than 70, the total light transmittance to visible light is preferably 60% or more. The total light transmittance is more preferably 70% or more, further preferably 80% or more, further preferably 85% or more, and further preferably 90% or more. When the content of the polyorganosiloxane block represented by formula (1) in the polycarbonate-polyorganosiloxane copolymer is 5% or more by mass, the total light transmittance to visible light is preferably 25% or more. The haze during the flat plate molding is preferably 40 or less, more preferably 30 or less, further preferably 15 or less, and further preferably 5 or less, when the content of the polyorganosiloxane block represented by formula (1) in the polycarbonate-polyorganosiloxane copolymer is less than 5% by mass and the average chain length a of the polyorganosiloxane block (A-2) in the polycarbonate-polyorganosiloxane copolymer is less than 70.

[0275] The molded article having the above optical properties has excellent transparency and can be used in applications requiring high transparency. It should be noted that the total transmittance of visible light can be measured in accordance with ISO13468-1:1996, and the haze can be measured in accordance with ISO14782:1999.

[0276] The molded article containing the polycarbonate resin according to the present invention can be suitably used for parts requiring transparency and rigidity as well as scratch resistance and weather resistance, for example: 1) automotive parts such as sunroofs, door visors, rear windows, and side windows, 2) architectural parts such as architectural glass, soundproof walls, carports, sunrooms, and grilles, 3) windows for railway vehicles and ships, 4) various parts for televisions, radio recorders, cameras, video recorders, audio players, DVD players, telephones, monitors, computers, cash registers, copiers, printers, fax machines, etc., various parts for outer panels and housings, etc., for electrical equipment, 5) precision equipment parts such as shells and covers of precision machinery such as mobile phones, PDAs, cameras, slide projectors, clocks, calculators, measuring instruments, and display devices, 6) agricultural parts such as plastic greenhouses and greenhouses, 7) furniture parts such as lighting covers, blinds, and indoor appliances, etc.

[0277] Example

[0278] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0279] The characteristic values ​​in each example were obtained according to the procedure shown below.

[0280] <Method for measuring hexane extraction amount>

[0281] The hexane extraction amount was measured by the following method.

[0282] The particles of the polycarbonate-polysiloxane copolymer obtained in the following examples and comparative examples are crushed using a crusher, and the obtained sample is passed through a 20-mesh mesh (mesh opening 0.84 mm) to remove large pieces that are not crushed enough. Then, it is sieved on a 300-mesh mesh (mesh opening 0.055 mm), and the sample remaining on the mesh is collected as a sample for hexane extraction, thereby removing fine powder formed by excessive crushing.

[0283] Next, accurately weigh about 15 g of the sample for hexane extraction obtained by the above method, put it into a cylindrical filter paper (No. 84, inner diameter 28 mm × total length 100 mm) and install it in a Soxhlet extractor. Next, use 300 mL of n-hexane to reflux for 8 hours at a reflux rate of once every 3 to 4 minutes (70 mL / time) for extraction. Afterwards, use an evaporator to remove the n-hexane from the obtained n-hexane extract while contacting it with a 40°C hot water bath. Afterwards, vacuum dry it at room temperature for 2.5 hours, and calculate the hexane extraction amount (mass ppm) according to the mass (g) of the components remaining in the eggplant-shaped flask using the following formula.

[0284] Hexane extraction amount (mass ppm) = 1000000 × H / sample amount used in extraction

[0285] (H: the mass of the hexane extract remaining in the eggplant-shaped flask, unit: g)

[0286] <Quantitative Method for Polydimethylsiloxane Content>

[0287] Example) Quantitative method for polydimethylsiloxane contained in the polycarbonate-polyorganosiloxane copolymer obtained in Example 3

[0288] NMR equipment: ECA-500 manufactured by JEOL Resonance Co., Ltd.

[0289] Probe: Corresponding to TH5 Sample tube

[0290] Observation range: -5~15ppm

[0291] Observation center: 5ppm

[0292] Pulse repetition time: 9 seconds

[0293] Pulse width: 45°

[0294] Total times: 256 times

[0295] NMR sample tube:

[0296] Sample amount: 30-40 mg

[0297] Solvent: deuterated chloroform

[0298] Measuring temperature: room temperature

[0299] A: Integrated value of the meta position of the phenyl moiety observed at δ7.3 to 7.5

[0300] B: Integrated value of the methyl group of the dimethylsiloxane part observed at δ -0.02 to 0.3

[0301] C: Integrated value of methine groups in the ISB (isosorbide) moiety observed around δ 4.8 to 5.3

[0302] D: Integrated value of the methylene group of the PEG part observed at around δ 3.3 to 3.8

[0303] E: Integrated value of methine and methylene groups in the CHDM part observed around δ0.8 to 2.0

[0304] F: Integrated value of the methylene group at the terminal of dimethylsiloxane observed at δ 0.4 to 0.6

[0305] a=A / 2

[0306] b=B / 6

[0307] c=C / 3

[0308] d=D / 4

[0309] e=(EF) / 10

[0310] T=a+b+c+d+e

[0311] f=a / T×100

[0312] g=b / T×100

[0313] h=c / T×100

[0314] i=d / T×100

[0315] j=e / T×100

[0316] TW=f×93+g×74.1+h×172+i×44+j×170

[0317] PDMS (wt%) = g × 74.1 / TW × 100

[0318] <Measurement method of [POS-Mh] and [POS-M1]>

[0319] Regarding various polycarbonate-polyorganosiloxane copolymers shown in the following Examples and Comparative Examples, the average weight (wt%) of the polyorganosiloxane blocks contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the components corresponding to the retention time range T1 to T2 by gel permeation chromatography (GPC) is determined by the above-mentioned measurement method, and this value is referred to as [POS-Mh]. Similarly, the average weight (wt%) of the polyorganosiloxane blocks contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the components corresponding to the retention time range T2 to T3 is referred to as [POS-M1]. The GPC measurement method and the method for determining T1, T2, and T3 are described below.

[0320] GPC-based separation conditions of polycarbonate-polyorganosiloxane copolymers

[0321] Test equipment: Separation GPC [SPD-M20A] manufactured by Shimadzu Corporation

[0322] Solvent: Chloroform

[0323] Column: JAIGEL-4H, JAIGEL-2H

[0324] Column temperature: room temperature

[0325] Flow rate: 3.8 mL / min

[0326] Detector: RI

[0327] Injection concentration:

[0328] In the case of polystyrene standards: 3 mg / mL

[0329] In the case of polycarbonate-polyorganosiloxane copolymer: 30 mg / mL

[0330] Injection volume: 3mL

[0331] T1 to T3 are determined based on the peak tops of the chromatogram obtained by measuring the polystyrene standard sample by the above-mentioned GPC.

[0332] Polystyrene standard: The following standard polystyrene manufactured by Tosoh Corporation was used.

[0333] F-10: Mw / Mn=1.01, Mw=98900

[0334] F-2: Mw / Mn=1.01, Mw=13700

[0335] A-2500: Mw / Mn=1.03, Mw=3120

[0336] <Viscosity Average Molecular Weight of Polycarbonate-Polyorganosiloxane Copolymer>

[0337] The viscosity of a dichloromethane solution (concentration: g / L) at 20° C. was measured using an Ubbelohde viscometer to determine the intrinsic viscosity [η], and the viscosity average molecular weight (Mv) was calculated using the following formula (Schnell formula).

[0338] [η] = 1.23 × 10 -5 Mv 0.83

[0339] [Evaluation test]

[0340] <Total light transmittance of resin molded products: Tt (%), haze value>

[0341] The evaluation pellets obtained in each example and comparative example were injected into a mold using an injection molding machine ("MD50XB" manufactured by NIIGATA MACHINETECHNO CO., LTD., with a screw diameter of ) was made into three-stage plates for transparency evaluation (90mm×50mm, 3mm thick part 45mm×50mm, 2mm thick part 22.5mm×50mm, 1mm thick part 22.5mm×50mm) at a barrel temperature of 240°C and a mold temperature of 80°C. The total light transmittance was measured on the 1mm thick part of the three-stage plates according to ISO13468-1:1996. The haze value was measured on the 1mm thick part of the sample according to ISO14782:1999. Both values ​​were measured using NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.

[0342] The smaller the haze value, the higher the transparency of the sample.

[0343] Haze = Td / Tt×100

[0344] (Where Td: diffuse transmittance, Tt: total transmittance)

[0345] <Total light transmittance (%), haze value of raw material mixture>

[0346] The total light transmittance and haze value of the raw material mixture were determined using the following measuring device, glass colorimetric cell, and measuring method.

[0347] Measuring device: NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.

[0348] Glass colorimetric cell: optical path length: 10mm

[0349] Dimensions: External dimensions 14mm (depth) x 40mm (width) x 55mm (height)

[0350] Glass thickness on each side: 2mm

[0351] Before measuring the haze of the raw material mixture, the glass colorimetric cell is filled with pure water for zero point correction. Specifically, the measured value in the state where the pure water is filled in the colorimetric cell is corrected to a state where the total light transmittance is 100% and the haze value is 0.00. Then, the pure water is removed from the glass colorimetric cell, and the liquid mixture obtained by the method described below is filled therein and measured, and the haze value at 23°C is obtained in accordance with ISO14782:1999.

[0352] Haze = Td / Tt×100

[0353] (Where Td: diffuse transmittance, Tt: total transmittance)

[0354] Preparation Example 1: Preparation of PDMS-1

[0355] Under nitrogen atmosphere, polyorganosiloxane (100 g) having an average siloxane chain length of 24 represented by the following formula was added.

[0356] [Chemical formula 23]

[0357]

[0358] Polyethylene glycol having an average oxyethylene chain length of 15 as shown in the following formula was added in an amount twice the molar amount (82.3 g) based on the polyorganosiloxane.

[0359] [Chemical formula 24]

[0360] H2C=CH-CH2-O-(CH2CH2O) 15 -H

[0361] After adding 455 g of isopropyl alcohol (2.5 parts relative to the total mass of polyorganosiloxane and polyethylene glycol), the mixture was stirred at 80°C. Then, a toluene solution of a platinum vinylsiloxane complex was added in an amount of 5 ppm by mass of platinum atoms relative to siloxane, and stirred for 10 hours. By removing isopropyl alcohol and the platinum catalyst from the obtained mixture, a polyether-modified polyorganosiloxane PDMS-1 was obtained.

[0362] Preparation Example 2: Preparation of PDMS-2

[0363] The production was carried out in the same manner as in Production Example 1 except that α,ω-dihydroorganopolysiloxane having an average siloxane chain length of 61 was used.

[0364] Preparation Example 3: Preparation of PDMS-3

[0365] The production was carried out in the same manner as in Production Example 1 except that α,ω-dihydrogenorganopolysiloxane having an average siloxane chain length of 88 was used.

[0366] Preparation Example 4: Preparation of PDMS-4

[0367] The production was carried out in the same manner as in Production Example 1 except that the average oxyethylene chain length of the polyethylene glycol used was 12.

[0368] Preparation Example 5: Preparation of PDMS-5

[0369] Under a nitrogen atmosphere, 2-allylphenol was added to a polyorganosiloxane having an average siloxane chain length of 39 represented by the following formula in an amount 2 times the molar amount of the polyorganosiloxane.

[0370] [Chemical formula 25]

[0371]

[0372] The mixture was stirred well while the temperature was controlled at 100° C. Next, a toluene solution of a platinum vinylsiloxane complex was added in an amount of 5 ppm by mass of platinum atoms relative to siloxane, and stirred for 10 hours. Isopropyl alcohol and the platinum catalyst were removed from the obtained mixture to obtain allylphenol-modified polyorganosiloxane PDMS-5.

[0373] Preparation Example 6: Preparation of PDMS-6

[0374] The production was carried out in the same manner as in Production Example 5, except that eugenol was used instead of 2-allylphenol.

[0375] Preparation Example 7: Preparation of PDMS-7

[0376] The preparation was carried out in the same manner as in Preparation Example 1 except that ethylene glycol monoallyl ether (CH2=CHCH2-O-CH2CH2-OH) was used instead of polyethylene glycol.

[0377] Preparation Example 8: Preparation of PDMS-8

[0378] The production was carried out in the same manner as in Production Example 1 except that the average siloxane chain length of the polyorganosiloxane used was 45, the average oxyethylene chain length of the polyethylene glycol used was 8, toluene was used as the solvent, and the reaction temperature was 110°C.

[0379] Preparation Example 9: Preparation of PDMS-9

[0380] The production was carried out in the same manner as in Production Example 8 except that the average oxyethylene chain length of the polyethylene glycol used was 38, toluene was used as the solvent, and the reaction temperature was 110°C.

[0381] Preparation Example 10: Preparation of PDMS-10

[0382] The production was carried out in the same manner as in Production Example 1 except that the average siloxane chain length of the polyorganosiloxane used was 5, toluene was used as the solvent, and the reaction temperature was 110°C.

[0383] Preparation Example 11: Preparation of PDMS-11

[0384] Under a nitrogen atmosphere, 350 mL of dichloromethane was added to a flask, and 21.5 g of 2,6-di-tert-butylpyridine and 21 g of trifluoromethanesulfonic anhydride were added thereto, and the mixture was cooled to below 15°C. 4.3 g of allyl alcohol was added dropwise thereto to form a reaction initiator. After stirring for about 15 minutes, 1 L of dehydrated tetrahydrofuran was added and stirred at 20-23°C for 5 minutes, and then 30 mL of ion exchange water was added to stop the reaction. Extraction was performed with heptane, and the mixture was washed with 10% hydrochloric acid. After the water layer was separated, it was then washed twice with ion exchange water, and the water layer was separated. Afterwards, the solvent was distilled off under reduced pressure to obtain 120 g of single-end allyl-modified polytetramethylene glycol (chain length of tetramethylene glycol part = 20) shown in the following formula.

[0385] [Chemical formula 26]

[0386] H2C=CH-CH2-(OCH2CH2CH2CH2) 20 -OH

[0387] The preparation was carried out in the same manner as in Preparation Example 8 except that the single-end allyl-modified polytetramethylene glycol obtained by the above reaction was used instead of polyethylene glycol, the solvent was changed to a 1:1 (mass ratio) mixed solution of toluene and isopropanol, the amount of the solvent used was set to 3 times the volume of the total volume of the polyorganosiloxane and the single-end allyl-modified polytetramethylene glycol, and the reaction temperature was controlled at 80-90°C.

[0388] Preparation Example 12: Preparation of PDMS-12

[0389] In a flask in a nitrogen atmosphere, polydimethylsiloxane (average number of chains of SiMe2O units: 40) having -C3H6OC2H4OH groups at both ends and trimethylene carbonate in a molar amount of 25 times the hydroxyl group of the above-mentioned polyorganosiloxane were added, and dehydrated dichloromethane was added to make these raw materials have a concentration of 10wt%. In the obtained transparent reaction solution, 1,8-diazabicycloundecene in an amount of 3 equivalents relative to the terminal OH group of the polydimethylsiloxane was added as a catalyst, and the reaction was directly carried out at room temperature for 48 hours. After that, benzoic acid was added to stop the reaction, and the reaction mixture after the reaction was stopped was reprecipitated in a mixed solvent formed by a mixed solution of methanol, 2-propanol, and hexane (volume ratio of 10:1:10, respectively), and the obtained precipitate was vacuum dried, thereby obtaining PDMS-12 (number of chains of polytrimethylene carbonate at each end: 18).

[0390] Preparation Example 13: Preparation of PDMS-13

[0391] Under nitrogen atmosphere, 450 mL of dichloromethane was added to a flask, 45.0 g of 3-iodo-1-propanol was added thereto, and the mixture was cooled in an ice bath. 40.1 g of tert-butyldimethylsilyl chloride was added thereto, and the mixture was stirred at room temperature for 20 hours. The resulting mixture was quenched with a 5% aqueous sodium bicarbonate solution, and the product was extracted with ethyl acetate / ion exchange water. The resulting product was refined with a silica gel column to obtain a TBS protected form of 3-iodo-1-propanol (yield 67.7 g).

[0392] Under a nitrogen atmosphere, 2.9 g of the TBS protected body of the above 3-iodo-1-propanol and 270 mL of tetrahydrofuran were mixed in a flask and cooled to below -65°C. 12.5 mL of 1.6 mol / L tert-butyl lithium (pentane solution) was added dropwise and stirred directly for 15 minutes. 2.5 mL of diphenylethylene was added dropwise and stirred directly for 30 minutes. After that, 55 mL of 0.52 mol / L lithium chloride THF solution was added and stirred for 10 minutes. Then 10.1 mL of methyl methacrylate was added and stirred for 10 minutes. Then 3.36 mL of allyl bromide was added to quench the reaction, and then mixed at room temperature for 12 hours. After the obtained reaction mixture was concentrated under reduced pressure, it was reprecipitated in a THF / heptane system, and then refined on a silica gel column to remove the solvent, thereby obtaining a TBS protected body of single-end allyl-modified PMMA. The product was dissolved in THF, deprotected with 2 mol / L hydrochloric acid aqueous solution, and the obtained reaction mixture was put into heptane to separate the target product (deprotected product). The deprotected product was purified by silica gel column, and the solvent was removed to obtain a single-terminal allyl-modified PMMA (the number of chains in the PMMA part = 20) shown in the following formula.

[0393] [Chemical formula 27]

[0394]

[0395] The production was carried out in the same manner as in Production Example 8 except that the above-mentioned PMMA modified with one terminal allyl group was used instead of polyethylene glycol.

[0396] Preparation Example 14: Preparation of PDMS-14

[0397] The production was carried out in the same manner as in Production Example 1 except that polypropylene glycol having an average oxypropylene group chain length of 15 represented by the following formula was used as polyethylene glycol.

[0398] [Chemical formula 28]

[0399]

[0400] Table 1 shows PDMS-1 to PDMS-14 obtained in Production Examples 1 to 14.

[0401] [Table 1]

[0402]

[0403] [other]

[0404] BisP-A: Bisphenol A [manufactured by Idemitsu Kosan Co., Ltd.]

[0405] 1,4-CHDM: 1,4-cyclohexanedimethanol [manufactured by Tokyo Chemical Industry Co., Ltd.]

[0406] TCDDM: tricyclodecane dimethanol [manufactured by OXEA GmbH]

[0407] 1,3-PG: 1,3-propylene glycol [manufactured by Tokyo Chemical Industry Co., Ltd.]

[0408] PEG400: polyethylene glycol 400 [average molecular weight 380-420 g / mol, manufactured by Tokyo Chemical Industry Co., Ltd.]

[0409] DPC: diphenyl carbonate [manufactured by MITSUI FINE CHEMICALS Co., Ltd.]

[0410] 0.01N sodium hydroxide aqueous solution [manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.]

[0411] Example 1

[0412] <Evaluation of transparency of raw material mixture after heating>

[0413] In a 10L stainless steel reactor equipped with a double helical blade as a stirring device, BisP-A (2489.9g) and DPC (2500g) (mol ratio of each raw material: BisP-A / DPC = 100 / 107) and 28.2g of polyether-modified polyorganosiloxane PDMS-1 were added. After these raw material monomers were completely melted at 150°C, stirring was started at 70rpm, and the inside of the reactor was replaced with nitrogen. Next, 1.64mL of 0.01N sodium hydroxide (1.5×10 mol relative to the total diol monomer) was added as a catalyst. -6 The mixture was heated to 200°C and kept at this temperature for 60 minutes while maintaining the nitrogen pressure of 101 kPa, which was the same as the atmospheric pressure. Next, the contents were discharged from the valve at the bottom of the reactor to obtain a liquid and transparent raw material mixture. The total light transmittance of the liquid raw material mixture after heating was 98.4, and the haze value was 0.5, showing high transparency.

[0414] <Production of Polycarbonate-Polysiloxane (PC-POS) Copolymer>

[0415] A polycarbonate-polyorganosiloxane copolymer was produced using the following raw materials and conditions. The same raw materials as those used in the above transparency evaluation were used, and the polymerization conditions were as follows.

[0416] In a 10L stainless steel reactor equipped with a stirring device, a trapping device (Japanese: Tratpu) for capturing distilled phenol, and a decompression device, BisP-A (2,489.9 g) and DPC (2,500 g) as diol monomers (mol ratio of each raw material: BisP-A / DPC=100 / 107) and 28.2 g of polyether-modified polyorganosiloxane PDMS-1 were added, and these raw material monomers were completely melted at 150°C, and the inside of the reactor was replaced with nitrogen. 1.64 mL of 0.01N sodium hydroxide (1.5×10 mol relative to the total diol monomer molar amount) was added as a catalyst. -6 The reaction mixture was heated and depressurized until the reactor temperature reached 180°C and the pressure reduction reached 200 mmHg (26.6 kPa) over about 60 minutes, and the reaction conditions were maintained until the phenol distillation amount reached 0.2 L. Thereafter, the reaction mixture was heated and depressurized until the reactor internal temperature reached 200°C and the pressure reduction reached 10 mmHg (1.3 kPa) over about 60 minutes, and the conditions were maintained until 1.0 L of phenol was distilled out.

[0417] Next, the internal temperature of the reactor was raised to 240°C in about 120 minutes, and the condition was maintained until 1.5L of phenol was distilled out. Next, the internal temperature of the reactor was adjusted to 280°C and the degree of decompression was below 1mmHg (0.1kPa) in about 120 minutes, and more than 2L of phenol was distilled out, and the reaction was continued until the specified stirring torque was reached. After that, nitrogen was used for re-pressure, and 0.037g of butyl p-toluenesulfonate (10 times the mol amount relative to NaOH) as a deactivator was added. Irganox1010 and Irgafos168 were added respectively so that the content in the obtained polymer reached 1500ppm, and fully stirred. After that, the resin strands were unloaded from the bottom of the reactor by nitrogen pressure, and they were cut by a granulator to obtain a granular polycarbonate-polyorganosiloxane copolymer with high transparency. The evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer are shown in Table 2.

[0418] Example 2

[0419] Except for using BisP-A (1293.3 g), 1,4-CHDM (817.0 g), and DPC (2,500 g) as diol monomers (mol ratio of each raw material: BisP-A / 1,4-CHDM / DPC = 50 / 50 / 103), and 24.4 g of polyether-modified polyorganosiloxane PDMS-1, the transparency evaluation of the heat-treated raw material mixture was carried out in the same manner as in Example 1. The heat-treated liquid raw material mixture had high transparency, with a total light transmittance of 98.5% and a haze value of 0.5.

[0420] Except for using BisP-A (1293.3 g), 1,4-CHDM (817.0 g), and DPC (2,500 g) as diol monomers (mol ratio of each raw material: BisP-A / 1,4-CHDM / DPC = 50 / 50 / 103), and 24.4 g of polyether-modified polyorganosiloxane PDMS-1, polymerization was carried out under the same conditions as in Example 1, thereby obtaining a granular polycarbonate-polyorganosiloxane copolymer with high transparency. The evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer are shown in Table 2.

[0421] Example 3

[0422] <Transparency evaluation of the heat-treated raw material mixture>

[0423] Using isosorbide (ISB) (1193.8 g), 1,4-CHDM (504.9 g), DPC (2500 g) (mol ratio of each raw material: ISB / 1,4-CHDM / DPC = 70∶30∶100), and 20.2 g of polyether-modified polyorganosiloxane PDMS-1, the heat treatment of the raw materials was carried out in the same manner as in Example 1. The heat-treated liquid raw material mixture had high transparency, with a total light transmittance of 99.5% and a haze value of 0.4.

[0424] <Manufacture of PC-POS copolymer>

[0425] In a 10 L stainless steel reactor equipped with a stirring device, a trapping device for capturing distilled phenol, and a decompression device, isosorbide (ISB) (1193.8 g), 1,4-CHDM (504.9 g), DPC (2,500 g) as diol monomers (mol ratio of each raw material: ISB / 1,4-CHDM / DPC = 70∶30∶100), and 20.2 g of polyether-modified polyorganosiloxane PDMS-1 were charged. These raw material monomers were completely melted at 100 °C, and the inside of the reactor was purged with nitrogen. 1.64 mL of 0.01 N sodium hydroxide as a catalyst was charged (relative to the total mol amount of all diol monomers was 1.5×10 -6The reaction mixture was heated and depressurized until the reactor temperature reached 180°C and the pressure was reduced to 200 mmHg (26.6 kPa) over 50 to 100 minutes, and the conditions were maintained until the phenol distillation amount reached 0.2 L. Thereafter, the reaction mixture was heated and depressurized until the reactor internal temperature reached 200°C and the pressure was reduced to 10 mmHg (1.3 kPa) over 150 minutes, and the conditions were maintained until 1.8 L of phenol was distilled.

[0426] Next, the temperature in the reactor was adjusted to 220°C and the degree of decompression was below 1 mmHg (0.1 kPa) for about 60 minutes, and more than 2 L of phenol was distilled out, and the reaction was continued until the specified stirring torque was reached. Afterwards, nitrogen was used for re-pressure, and 0.037 g of butyl p-toluenesulfonate (10 times the molar amount relative to NaOH) was added as a deactivator. Irganox1010 and Irgafos168 were added respectively so that the content in the resulting polymer reached 1500 ppm, and the mixture was stirred thoroughly. Afterwards, the resin strands were unloaded from the bottom of the reactor by nitrogen pressure, and the strands were cut by a granulator to obtain a granular polycarbonate-polyorganosiloxane copolymer with high transparency. The evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer are shown in Table 2.

[0427] Example 4

[0428] Except for using 20.2 g of PDMS-2 as polyorganosiloxane, the transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 3. The liquid raw material mixture after the heat treatment had high transparency, with a total light transmittance of 98.4% and a haze value of 0.8.

[0429] The polymerization was carried out under the same conditions as in Example 3 except that 20.2 g of PDMS-2 was used as the polyorganosiloxane, thereby obtaining a highly transparent granular polycarbonate-polyorganosiloxane copolymer. Table 2 shows the evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer.

[0430] Example 5

[0431] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 3 except that 20.2 g of PDMS-3 was used as the polyorganosiloxane. The liquid raw material mixture after the heat treatment had high transparency, with a total light transmittance of 98.1% and a haze value of 1.3.

[0432] The polymerization was carried out under the same conditions as in Example 3 except that 20.2 g of PDMS-3 was used as the polyorganosiloxane, thereby obtaining a highly transparent granular polycarbonate-polyorganosiloxane copolymer. Table 2 shows the evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer.

[0433] Example 6

[0434] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 3 except that 20.2 g of PDMS-4 was used as polyorganosiloxane. The liquid raw material mixture after the heat treatment had high transparency, with a total light transmittance of 97.9% and a haze value of 0.7.

[0435] The polymerization was carried out under the same conditions as in Example 3 except that 20.2 g of PDMS-4 was used as the polyorganosiloxane, thereby obtaining a highly transparent granular polycarbonate-polyorganosiloxane copolymer. Table 2 shows the evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer.

[0436] Example 7

[0437] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 3 except that 105.4 g of PDMS-1 was used as the polyorganosiloxane. The liquid raw material mixture after the heat treatment had high transparency, with a total light transmittance of 97.5% and a haze value of 0.9.

[0438] The polymerization was carried out under the same conditions as in Example 3 except that 105.4 g of PDMS-1 was used as the polyorganosiloxane, thereby obtaining a highly transparent granular polycarbonate-polyorganosiloxane copolymer. Table 2 shows the evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer.

[0439] Example 8

[0440] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 3 except that 222.5 g of PDMS-1 was used as the polyorganosiloxane. The liquid raw material mixture after the heat treatment had high transparency, with a total light transmittance of 97.1% and a haze value of 1.1.

[0441] The polymerization was carried out under the same conditions as in Example 3 except that 222.5 g of PDMS-1 was used as the polyorganosiloxane, thereby obtaining a highly transparent granular polycarbonate-polyorganosiloxane copolymer. Table 2 shows the evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer.

[0442] Example 9

[0443] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 3 except that ISB (1193.8 g), TCDDM (687.2 g), and DPC (2,500 g) (mol ratio of each raw material: ISB / TCDDM / DPC=70:30:100) as diol monomers and 22.1 g of polyether-modified polyorganosiloxane PDMS-1 were used. The liquid raw material mixture after the heat treatment had high transparency, with a total light transmittance of 98.5% and a haze value of 0.4.

[0444] Polymerization was carried out under the same conditions as in Example 3 except that ISB (1193.8 g), TCDDM (687.2 g), DPC (2,500 g) (mol ratio of each raw material: ISB / TCDDM / DPC=70:30:100) and 22.1 g of polyether-modified polyorganosiloxane PDMS-1 were used as diol monomers to obtain a highly transparent granular polycarbonate-polyorganosiloxane copolymer. The evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer are shown in Table 2.

[0445] Example 10

[0446] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 3 except that ISB (1193.8 g), 1,4-CHDM (420.7 g), 1,3-PG (44.4 g), DPC (2,500 g) (mol ratio of each raw material: ISB / 1,4-CHDM / 1,3-PG / DPC=70:25:5:100) as diol monomers and 19.8 g of polyether-modified polyorganosiloxane PDMS-1 were used. The liquid raw material mixture after the heat treatment had high transparency, with a total light transmittance of 98.3% and a haze value of 0.4.

[0447] Polymerization was carried out under the same conditions as in Example 3 except that ISB (1193.8 g), 1,4-CHDM (420.7 g), 1,3-PG (44.4 g), DPC (2,500 g) (mol ratio of each raw material: ISB / 1,4-CHDM / 1,3-PG / DPC=70:25:5:100) and 19.8 g of polyether-modified polyorganosiloxane PDMS-1 were used as diol monomers to obtain a highly transparent granular polycarbonate-polyorganosiloxane copolymer. The evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer are shown in Table 2.

[0448] Embodiment 11

[0449] Using ISB (1193.8 g), 1,4-CHDM (504.9 g), PEG400 (93.4 g), DPC (2500 g) as diol monomers [mol ratio of each raw material: ISB / 1,4-CHDM / PEG400 / DPC = 70:28:2:100 (the mol amount of PEG400 uses the value obtained by dividing the used mass by the average molecular weight of 400)], 21.3 g of polyether-modified polysiloxane PDMS-1, and otherwise evaluating the transparency of the raw material mixture after heat treatment in the same manner as in Example 3. The liquid raw material mixture after heat treatment has high transparency, with a total light transmittance of 98.3% and a haze value of 0.4.

[0450] Using ISB (1193.8 g), 1,4-CHDM (504.9 g), PEG400 (93.4 g), DPC (2500 g) as diol monomers [mol ratio of each raw material: ISB / 1,4-CHDM / PEG400 / DPC = 70:28:2:100 (the mol amount of PEG400 uses the value obtained by dividing the used mass by the average molecular weight of 400)], 21.3 g of polyether-modified polysiloxane PDMS-1, and otherwise polymerizing under the same conditions as in Example 3, thereby obtaining a granular polycarbonate-polysiloxane copolymer with high transparency. The evaluation results of the obtained polycarbonate-polysiloxane copolymer are shown in Table 2.

[0451] Example 12

[0452] <Transparency evaluation of the raw material mixture after heat treatment>

[0453] Using 179.7 g of PDMS-8 as the polysiloxane, and otherwise evaluating the transparency of the raw material mixture after heat treatment in the same manner as in Example 1. The liquid raw material mixture after heat treatment has high transparency, with a total light transmittance of 90.8% and a haze value of 2.5.

[0454] <Manufacture of PC-POS copolymer>

[0455] Using 179.7 g of PDMS-8 as the polysiloxane, and otherwise polymerizing under the same conditions as in Example 1, thereby obtaining a granular polycarbonate-polysiloxane copolymer with high transparency. The obtained polycarbonate-polysiloxane copolymer has a viscosity-average molecular weight of 20100, a polydimethylsiloxane content of 5.00% by mass, a total light transmittance of 33.7%, a haze value of 97.0, an amount of hexane extractable components of 653 ppm, [POS-Mh] / [POS-M1] = 1.47, and a Charpy impact strength (notched) of 81.0 kJ / m 2 .

[0456] Example 13

[0457] <Evaluation of transparency of raw material mixture after heat treatment>

[0458] Using 312.8 g of PDMS-8 as the polyorganosiloxane, the transparency of the raw material mixture after heat treatment was evaluated in the same manner as in Example 1. The liquid raw material mixture after heat treatment had high transparency, with a total light transmittance of 89.1% and a haze value of 2.6.

[0459] <Manufacture of PC-POS copolymer>

[0460] Using 312.8 g of PDMS-8 as the polyorganosiloxane, polymerization was carried out under the same conditions as in Example 1, thereby obtaining a granular polycarbonate-polyorganosiloxane copolymer with high transparency. The obtained polycarbonate-polyorganosiloxane copolymer had a viscosity-average molecular weight of 20,100, a polydimethylsiloxane content of 8.30% by mass, a total light transmittance of 28.3%, a haze value of 98.1, an amount of hexane extractable components of 714 ppm, [POS-Mh] / [POS-M1] = 1.23, and a Charpy impact strength (notched) of 85.0 kJ / m 2 。

[0461] Example 14

[0462] <Evaluation of transparency of raw material mixture after heat treatment>

[0463] Using 179.7 g of PDMS-9 as the polyorganosiloxane, the transparency of the raw material mixture after heat treatment was evaluated in the same manner as in Example 1. The liquid raw material mixture after heat treatment had high transparency, with a total light transmittance of 90.1% and a haze value of 2.0.

[0464] <Manufacture of PC-POS copolymer>

[0465] Using 179.7 g of PDMS-9 as the polyorganosiloxane, polymerization was carried out under the same conditions as in Example 1, thereby obtaining a granular polycarbonate-polyorganosiloxane copolymer with high transparency. The obtained polycarbonate-polyorganosiloxane copolymer had a viscosity-average molecular weight of 20,000, a polydimethylsiloxane content of 3.10% by mass, a total light transmittance of 62.0%, a haze value of 89.4, an amount of hexane extractable components of 663 ppm, [POS-Mh] / [POS-M1] = 1.13, and a Charpy impact strength (notched) of 75.0 kJ / m 2 。

[0466] Example 15

[0467] <Evaluation of transparency of the raw material mixture after heat treatment>

[0468] Using 179.7 g of PDMS-10 as the polyorganosiloxane, the transparency of the raw material mixture after heat treatment was evaluated in the same manner as in Example 1. The liquid raw material mixture after heat treatment had high transparency, with a total light transmittance of 91.0% and a haze value of 1.3.

[0469] <Manufacture of PC-POS copolymer>

[0470] Using 179.7 g of PDMS-10 as the polyorganosiloxane, polymerization was carried out under the same conditions as in Example 1, thereby obtaining a granular polycarbonate-polyorganosiloxane copolymer with high transparency. The obtained polycarbonate-polyorganosiloxane copolymer had a viscosity-average molecular weight of 20150, a polydimethylsiloxane content of 0.90 mass%, a total light transmittance of 86.1%, a haze value of 6.8, an amount of hexane extractable components of 585 ppm, [POS-Mh] / [POS-M1]=1.09, and a Charpy impact strength (notched) of 76.0 kJ / m 2 。

[0471] Example 16

[0472] <Evaluation of transparency of the raw material mixture after heat treatment>

[0473] Using 28.2 g of PDMS-11 as the polyorganosiloxane, the transparency of the raw material mixture after heat treatment was evaluated in the same manner as in Example 1. The liquid raw material mixture after heat treatment had high transparency, with a total light transmittance of 89.9% and a haze value of 7.3.

[0474] <Manufacture of PC-POS copolymer>

[0475] Using 28.2 g of PDMS-11 as the polyorganosiloxane, polymerization was carried out under the same conditions as in Example 1, thereby obtaining a granular polycarbonate-polyorganosiloxane copolymer with high transparency. The obtained polycarbonate-polyorganosiloxane copolymer had a viscosity-average molecular weight of 20200, a polydimethylsiloxane content of 0.53 mass%, a total light transmittance of 65.1%, a haze value of 83.5, an amount of hexane extractable components of 83 ppm, and [POS-Mh] / [POS-M1]=1.20.

[0476] Example 17

[0477] <Evaluation of transparency of the raw material mixture after heat treatment>

[0478] 57.1 g of PDMS-11 was used as the polyorganosiloxane, and the transparency of the raw material mixture after heat treatment was evaluated in the same manner as in Example 1. The liquid raw material mixture after heat treatment had high transparency, with a total light transmittance of 78.6% and a haze value of 12.0.

[0479] <Manufacture of PC-POS copolymer>

[0480] 57.1 g of PDMS-11 was used as the polyorganosiloxane, and polymerization was carried out under the same conditions as in Example 1, thereby obtaining a granular polycarbonate-polyorganosiloxane copolymer with high transparency. The obtained polycarbonate-polyorganosiloxane copolymer had a viscosity-average molecular weight of 20,100, a polydimethylsiloxane content of 1.10% by mass, a total light transmittance of 48.1%, a haze value of 87.5, an amount of hexane extractable components of 143 ppm, and [POS-Mh] / [POS-M1] = 1.23.

[0481] Example 18

[0482] <Transparency evaluation of raw material mixture after heat treatment>

[0483] 28.2 g of PDMS-12 was used as the polyorganosiloxane, and the transparency of the raw material mixture after heat treatment was evaluated in the same manner as in Example 1. The liquid raw material mixture after heat treatment had high transparency, with a total light transmittance of 97.9% and a haze value of 0.9.

[0484] <Manufacture of PC-POS copolymer>

[0485] 28.2 g of PDMS-12 was used as the polyorganosiloxane, and polymerization was carried out under the same conditions as in Example 1, thereby obtaining a granular polycarbonate-polyorganosiloxane copolymer with high transparency. The obtained polycarbonate-polyorganosiloxane copolymer had a viscosity-average molecular weight of 19,900, a polydimethylsiloxane content of 0.45% by mass, a total light transmittance of 81.0%, a haze value of 11.3, an amount of hexane extractable components of 49 ppm, and [POS-Mh] / [POS-M1] = 1.20.

[0486] Example 19

[0487] <Transparency evaluation of raw material mixture after heat treatment>

[0488] 179.7 g of PDMS-12 was used as the polyorganosiloxane, and the transparency of the raw material mixture after heat treatment was evaluated in the same manner as in Example 1. The liquid raw material mixture after heat treatment had high transparency, with a total light transmittance of 91.3% and a haze value of 2.1.

[0489] <Manufacture of PC-POS Copolymer>

[0490] Using 179.7 g of PDMS-12 as the polysiloxane, polymerization was carried out under the same conditions as in Example 1 except for this, and thus a granular polycarbonate-polysiloxane copolymer with high transparency was obtained. The obtained polycarbonate-polysiloxane copolymer had a viscosity-average molecular weight of 20,100, a polydimethylsiloxane content of 2.70% by mass, a total light transmittance of 61.0%, a haze value of 82.1, an amount of hexane extractable components of 550 ppm, and [POS-Mh] / [POS-M1]=1.41.

[0491] Example 20

[0492] <Transparency Evaluation of the Raw Material Mixture after Heat Treatment>

[0493] Using 28.2 g of PDMS-13 as the polysiloxane, the transparency evaluation of the raw material mixture after heat treatment was carried out in the same manner as in Example 1 except for this. The liquid raw material mixture after heat treatment had high transparency, a total light transmittance of 91.5%, and a haze value of 8.5.

[0494] <Manufacture of PC-POS Copolymer>

[0495] Using 28.2 g of PDMS-13 as the polysiloxane, polymerization was carried out under the same conditions as in Example 1 except for this, and thus a granular polycarbonate-polysiloxane copolymer with high transparency was obtained. The obtained polycarbonate-polysiloxane copolymer had a viscosity-average molecular weight of 20,050, a polydimethylsiloxane content of 0.42% by mass, a total light transmittance of 63.5%, a haze value of 81.2, an amount of hexane extractable components of 75 ppm, and [POS-Mh] / [POS-M1]=1.22.

[0496] Example 21

[0497] <Transparency Evaluation of the Raw Material Mixture after Heat Treatment>

[0498] Using 20.2 g of PDMS-14 as the polysiloxane, the transparency evaluation of the raw material mixture after heat treatment was carried out in the same manner as in Example 3 except for this. The liquid raw material mixture after heat treatment had high transparency, a total light transmittance of 98.1%, and a haze value of 1.0.

[0499] <Manufacture of PC-POS Copolymer>

[0500] Using 20.2 g of PDMS-14 as the polyorganosiloxane, polymerization was carried out under the same conditions as in Example 2, whereby a granular polycarbonate-polyorganosiloxane copolymer with high transparency was obtained. The obtained polycarbonate-polyorganosiloxane copolymer had a viscosity-average molecular weight of 15,000, a polydimethylsiloxane content of 0.68% by mass, a total light transmittance of 69.7%, a haze value of 84.0, an amount of hexane extractable components of 55 ppm, and [POS-Mh] / [POS-M1]=1.31.

[0501] Example 22

[0502] <Transparency evaluation of the raw material mixture after heat treatment>

[0503] Using 19.7 g of PDMS-1 as the polyorganosiloxane, the transparency of the raw material mixture after heat treatment was evaluated in the same manner as in Example 1. The liquid raw material mixture after heat treatment had high transparency, with a total light transmittance of 99.2% and a haze value of 0.4.

[0504] <Manufacture of PC-POS copolymer>

[0505] Using 19.7 g of PDMS-1 as the polyorganosiloxane, polymerization was carried out under the same conditions as in Example 1, whereby a granular polycarbonate-polyorganosiloxane copolymer with high transparency was obtained. The obtained polycarbonate-polyorganosiloxane copolymer had a viscosity-average molecular weight of 15,600, a polydimethylsiloxane content of 0.43% by mass, a total light transmittance of 86.8%, a haze value of 3.9, an amount of hexane extractable components of 55 ppm, [POS-Mh] / [POS-M1]=1.09, and a Charpy impact strength (notched) of 19.5 kJ / m 2 。

[0506] Comparative Example 1

[0507] Using 24.4 g of PDMS-5 as the polyorganosiloxane, the transparency of the raw material mixture after heat treatment was evaluated in the same manner as in Example 2. The liquid raw material mixture after heat treatment was turbid, with a total light transmittance of 78.5% and a haze value of 93.2.

[0508] Using 24.4 g of PDMS-5 as the polyorganosiloxane, polymerization was carried out under the same conditions as in Example 2, whereby a granular polycarbonate-polyorganosiloxane copolymer with significant turbidity was obtained. The evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer are shown in Table 3.

[0509] Comparative Example 2

[0510] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 3 except that 20.2 g of PDMS-5 was used as the polyorganosiloxane. The liquid raw material mixture after the heat treatment was turbid, had a total light transmittance of 79.1%, and a haze value of 92.1.

[0511] The polymerization was carried out under the same conditions as in Example 3 except that 20.2 g of PDMS-5 was used as the polyorganosiloxane, thereby obtaining a significantly turbid granular polycarbonate-polyorganosiloxane copolymer. Table 3 shows the evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer.

[0512] Comparative Example 3

[0513] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 3 except that 105.4 g of PDMS-5 was used as the polyorganosiloxane. The liquid raw material mixture after the heat treatment was turbid, had a total light transmittance of 63.2%, and a haze value of 95.5.

[0514] The polymerization was carried out under the same conditions as in Example 3 except that 105.4 g of PDMS-5 was used as the polyorganosiloxane, thereby obtaining a significantly turbid granular polycarbonate-polyorganosiloxane copolymer. Table 3 shows the evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer.

[0515] Comparative Example 4

[0516] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 3 except that 20.2 g of PDMS-6 was used as the polyorganosiloxane. The liquid raw material mixture after the heat treatment was turbid, had a total light transmittance of 79.5%, and a haze value of 93.1.

[0517] The polymerization was carried out under the same conditions as in Example 3 except that 20.2 g of PDMS-6 was used as the polyorganosiloxane, thereby obtaining a significantly turbid granular polycarbonate-polyorganosiloxane copolymer. Table 3 shows the evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer.

[0518] Comparative Example 5

[0519] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 3 except that 20.2 g of PDMS-7 was used as the polyorganosiloxane. The liquid raw material mixture after the heat treatment was turbid, with a total light transmittance of 81.1% and a haze value of 88.9.

[0520] The polymerization was carried out under the same conditions as in Example 3 except that 20.2 g of PDMS-7 was used as the polyorganosiloxane, thereby obtaining a significantly turbid granular polycarbonate-polyorganosiloxane copolymer. Table 3 shows the evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer.

[0521] Comparative Example 6

[0522] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 9 except that 22.1 g of PDMS-5 was used as the polyorganosiloxane. The liquid raw material mixture after the heat treatment was turbid, with a total light transmittance of 80.1% and a haze value of 90.1.

[0523] The polymerization was carried out under the same conditions as in Example 9 except that 22.1 g of PDMS-5 was used as the polyorganosiloxane, thereby obtaining a significantly turbid granular polycarbonate-polyorganosiloxane copolymer. Table 3 shows the evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer.

[0524] Comparative Example 7

[0525] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 10 except that 19.8 g of PDMS-5 was used as the polyorganosiloxane. The liquid raw material mixture after the heat treatment was turbid, with a total light transmittance of 78.5% and a haze value of 89.9.

[0526] The polymerization was carried out under the same conditions as in Example 10 except that 19.8 g of PDMS-5 was used as the polyorganosiloxane, thereby obtaining a significantly turbid granular polycarbonate-polyorganosiloxane copolymer. Table 3 shows the evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer.

[0527] Comparative Example 8

[0528] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 11 except that 21.3 g of PDMS-5 was used as the polyorganosiloxane. The liquid raw material mixture after the heat treatment was turbid, had a total light transmittance of 79.9%, and a haze value of 88.5.

[0529] The polymerization was carried out under the same conditions as in Example 11 except that 21.3 g of PDMS-5 was used as the polyorganosiloxane, thereby obtaining a significantly turbid granular polycarbonate-polyorganosiloxane copolymer. Table 3 shows the evaluation results of the obtained polycarbonate-polyorganosiloxane copolymer.

[0530] Comparative Example 9

[0531] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 1 except that 19.8 g of PDMS-5 was used as the polyorganosiloxane. The liquid raw material mixture after the heat treatment was turbid, had a total light transmittance of 78.1%, and a haze value of 94.5.

[0532] The polymerization was carried out under the same conditions as in Example 1 except that 19.8 g of PDMS-5 was used as the polyorganosiloxane, thereby obtaining a significantly turbid granular polycarbonate-polyorganosiloxane copolymer. The obtained polycarbonate-polyorganosiloxane copolymer had a viscosity average molecular weight of 15100, a polydimethylsiloxane content of 0.62% by mass, a total light transmittance of 53.1%, a haze value of 98.5, a hexane extract component content of 175 ppm, [POS-Mh] / [POS-M1]=1.1, and a Charpy impact strength (notched) of 15.8 kJ / m 2 .

[0533] Comparative Example 10

[0534] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 1 except that 179.7 g of PDMS-5 was used as the polyorganosiloxane. The liquid raw material mixture after the heat treatment was turbid, had a total light transmittance of 65.1%, and a haze value of 97.5.

[0535] The polymerization was carried out under the same conditions as in Example 1 except that 179.7 g of PDMS-5 was used as the polyorganosiloxane, thereby obtaining a significantly turbid granular polycarbonate-polyorganosiloxane copolymer. The obtained polycarbonate-polyorganosiloxane copolymer had a viscosity average molecular weight of 20,000, a polydimethylsiloxane content of 5.30% by mass, a total light transmittance of 19.3%, a haze value of 99.6, a hexane extract component amount of 1351 ppm, [POS-Mh] / [POS-M1]=1.4, and a Charpy impact strength (notched) of 61.0 kJ / m 2 .

[0536] Comparative Example 11

[0537] The transparency of the raw material mixture after the heat treatment was evaluated in the same manner as in Example 1 except that 179.7 g of PDMS-7 was used as the polyorganosiloxane. The liquid raw material mixture after the heat treatment was turbid, had a total light transmittance of 66.5%, and a haze value of 96.2.

[0538] The polymerization was carried out under the same conditions as in Example 1 except that 179.7 g of PDMS-7 was used as the polyorganosiloxane, thereby obtaining a significantly turbid granular polycarbonate-polyorganosiloxane copolymer. The obtained polycarbonate-polyorganosiloxane copolymer had a viscosity average molecular weight of 20100, a polydimethylsiloxane content of 5.50% by mass, a total light transmittance of 17.5%, a haze value of 99.5, a hexane extract component amount of 1416 ppm, [POS-Mh] / [POS-M1]=1.3, and a Charpy impact strength (notched) of 61.0 kJ / m 2 .

[0539] [Table 2]

[0540]

[0541] [Table 3]

[0542]

Claims

1. A polycarbonate-polyorganosiloxane copolymer comprising: A polyorganosiloxane block (A-1) containing a structural unit represented by the following general formula (1), and A polycarbonate block (A-2) comprising a repeating unit represented by the following general formula (2), The polyorganosiloxane block (A-1) comprises at least one selected from the group consisting of structural units represented by the following general formulae (1-1) to (1-3), It satisfies the following conditions (A) or (B), Condition (A): The hexane extract amount of the polycarbonate-polyorganosiloxane copolymer is 150 ppm by mass or less, Condition (B): The average weight of the polyorganosiloxane blocks contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the polycarbonate-polyorganosiloxane copolymer by gel permeation chromatography satisfies the following formula (B1): 0.3≤[POS-Mh] / [POS-M1]≤3 (B1) In formula (B1), [POS-Mh] represents the average weight of the polyorganosiloxane block contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the components corresponding to the retention time range T1 to T2 using gel permeation chromatography, and [POS-Ml] represents the average weight of the polyorganosiloxane block contained in the polycarbonate-polyorganosiloxane copolymer obtained by separating the components between the retention times T2 and T3 using gel permeation chromatography. T1: Retention time of the peak top in the gel permeation chromatogram of standard polystyrene with Mw / Mn=1.01 and Mw=98900 T2: Retention time of the peak top in the gel permeation chromatogram of standard polystyrene with Mw / Mn=1.01 and Mw=13700 T3: Retention time of the peak top in the gel permeation chromatogram of standard polystyrene with Mw / Mn=1.03 and Mw=3120 In the formula, R 1 ~R 4 are optionally the same or different, and each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkylaryl group having 1 to 10 carbon atoms in the alkyl portion; R 6 represents an arylene group having 6 to 20 carbon atoms, an alkylene group having 1 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl moiety, and optionally contains -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -; R 111 represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms; R 40 represents a divalent aliphatic hydrocarbon group having 3 to 400 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 400 carbon atoms, or a divalent aromatic hydrocarbon group having 8 to 400 carbon atoms, which is optionally substituted by a substituent; the divalent aliphatic hydrocarbon group, the divalent alicyclic hydrocarbon group, or the divalent aromatic hydrocarbon group optionally contains at least one heteroatom selected from oxygen atoms, nitrogen atoms, and sulfur atoms, and at least one halogen atom selected from fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms; a represents an integer of 2 to 500, and u represents 0 or 1; R 10 represents a divalent aliphatic hydrocarbon group having 2 to 40 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 40 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, which is optionally substituted by a substituent; the divalent aliphatic hydrocarbon group, the divalent alicyclic hydrocarbon group, or the divalent aromatic hydrocarbon group optionally contains at least one heteroatom selected from oxygen atoms, nitrogen atoms, and sulfur atoms, and at least one halogen atom selected from fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms; y represents an integer of 10 to 500, In the formula, R 1 ~R 4 , R 6 and a are the same as defined above; R 5 represents an arylene group having 6 to 20 carbon atoms, an alkylene group having 1 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl moiety, and optionally contains -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -; R 7 represents an arylene group having 6 to 20 carbon atoms, an alkylene group having 2 to 10 carbon atoms, a branched alkylene group having 3 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl portion, and optionally contains -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -; Multiple R 8 The same or different groups are each independently an arylene group having 6 to 20 carbon atoms, an alkylene group having 2 to 10 carbon atoms, a branched alkylene group having 3 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl moiety, and as a functional group, -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -; R 111 represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms; z represents 0 or 1; z1 represents 0 or 1; b represents an integer from 2 to 200; b1 represents an integer from 2 to 200; β represents a divalent group derived from a diisocyanate compound, or a divalent group derived from a dicarboxylic acid or a halide of a dicarboxylic acid.

2. The polycarbonate-polyorganosiloxane copolymer according to claim 1, wherein The polycarbonate block (A-2) has a structure represented by the following general formula (111) and a structure represented by the following general formula (112), In the formula, R 55 and R 56 Each independently represents a halogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms; X represents a single bond, an alkylene group having 1 to 8 carbon atoms, an alkylidene group having 2 to 8 carbon atoms, a cycloalkylene group having 5 to 15 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, a fluorenediyl group, an arylalkylene group having 7 to 15 carbon atoms, an arylalkylidene group having 7 to 15 carbon atoms, -S-, -SO-, -SO2-, -O-, or -CO-; R 100 represents a divalent aliphatic hydrocarbon group having 2 to 40 carbon atoms, which may contain a branched structure or a cyclic structure; R 100 It optionally contains at least one hetero atom selected from oxygen, nitrogen and sulfur atoms, and at least one halogen atom selected from fluorine, chlorine, bromine and iodine atoms; y represents an integer of 10 to 500; s and t each independently represent an integer of 0 to 4.

3. The polycarbonate-polyorganosiloxane copolymer according to claim 1 or 2, wherein The polycarbonate block (A-2) comprising a repeating unit represented by the general formula (2) comprises a structural unit derived from an aromatic bisphenol selected from the group consisting of 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3-methylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane and 1,1-bis(4-hydroxyphenyl)cyclododecene, or a structural unit derived from an aliphatic diol selected from the group consisting of isosorbide, cyclohexane-1,4-dimethanol, tricyclodecane dimethanol, 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 1,3-propylene glycol and 1,4-butanediol.

4. The polycarbonate-polyorganosiloxane copolymer according to claim 1 or 2, wherein The polycarbonate block (A-2) has one or more selected from the group consisting of repeating units represented by the following general formulae (ai) to (av), 5. The polycarbonate-polyorganosiloxane copolymer according to claim 4, wherein The polycarbonate block (A-2) has one or more selected from the group consisting of repeating units represented by (ai), (a-ii) and (av).

6. The polycarbonate-polyorganosiloxane copolymer according to claim 1 or 2, wherein In the general formula (1), a is an integer of 2 to 300.

7. The polycarbonate-polyorganosiloxane copolymer according to claim 1 or 2, wherein: In the general formula (1), R 1 ~R 4 All represent methyl.

8. The polycarbonate-polyorganosiloxane copolymer according to claim 1 or 2, wherein In the general formula (1), R 6 It is trimethylene (-(CH2)3-).

9. The polycarbonate-polyorganosiloxane copolymer according to claim 1 or 2, wherein: In the general formulas (1-1) to (1-3), R 8 It is any structure selected from the group consisting of dimethylene (-(CH2)2-), methyl-substituted dimethylene (-CH2CHMe-), trimethylene (-(CH2)3-), and tetramethylene (-(CH2)4-).

10. The polycarbonate-polyorganosiloxane copolymer according to claim 1 or 2, wherein The content of the polyorganosiloxane block represented by the general formula (1) in the polycarbonate-polyorganosiloxane copolymer is 0.1% by mass or more and 60% by mass or less.

11. The polycarbonate-polyorganosiloxane copolymer according to claim 10, wherein The content of the polyorganosiloxane block represented by the general formula (1) in the polycarbonate-polyorganosiloxane copolymer is 3% by mass or more and 20% by mass or less. 12 . The polycarbonate-polyorganosiloxane copolymer according to claim 1 , which satisfies both the condition (A) and the condition (B). 13 . The polycarbonate-polyorganosiloxane copolymer according to claim 1 , wherein the hexane extract amount of the polycarbonate-polyorganosiloxane copolymer in the condition (A) is 10 ppm by mass or more and 100 ppm by mass or less. The polycarbonate-polyorganosiloxane copolymer according to claim 13, wherein the hexane extraction amount of the polycarbonate-polyorganosiloxane copolymer in the condition (A) is 20 mass ppm or more and 60 mass ppm or less.

15. The polycarbonate-polyorganosiloxane copolymer according to claim 1 or 2, In the condition (B), the lower limit of [POS-Mh] / [POS-Ml] is 0.35 or more, and the upper limit is 2 or less.

16. The polycarbonate-polyorganosiloxane copolymer according to claim 15, In the condition (B), the lower limit of [POS-Mh] / [POS-Ml] is 0.8 or more, and the upper limit is 1.2 or less. 17 . The polycarbonate-polyorganosiloxane copolymer according to claim 1 , which has a viscosity average molecular weight Mv of 5,000 to 50,000. 18 . The polycarbonate-polyorganosiloxane copolymer according to claim 17 , which has a viscosity average molecular weight Mv of 16,000 to 21,000.

19. The polycarbonate-polyorganosiloxane copolymer according to claim 1 or 2, The haze value of a 1 mm thick plate obtained by molding the polycarbonate-polyorganosiloxane copolymer is 40 or less as measured in accordance with ISO 14782:1999.

20. The polycarbonate-polyorganosiloxane copolymer according to claim 1, which is obtained by a melt polymerization method.

21. The polycarbonate-polyorganosiloxane copolymer according to claim 1, which is obtained using a diol monomer (a1). 22 . The polycarbonate-polyorganosiloxane copolymer according to claim 20 , which is obtained by reacting a diol monomer (a1), a polyorganosiloxane (a2) and a carbonic acid diester compound by a melt polymerization method in the presence of a basic catalyst.

23. The polycarbonate-polyorganosiloxane copolymer according to claim 22, wherein The polyorganosiloxane (a2) has a structure represented by the following general formula (a2-0): In the formula, R 1 ~R 4 are optionally the same or different, and each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkylaryl group having 1 to 10 carbon atoms in the alkyl moiety, 5 and R 6 may be the same or different, each independently represents an arylene group having 6 to 20 carbon atoms, an alkylene group having 1 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl moiety, and as a functional group, may include -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -, R 111 represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms, and a represents an integer of 2 to 500, R 40’ represents a divalent aliphatic hydrocarbon group having 2 to 380 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 380 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 380 carbon atoms, which is optionally substituted with a substituent, wherein the divalent aliphatic hydrocarbon group, the divalent alicyclic hydrocarbon group, or the divalent aromatic hydrocarbon group optionally contains at least one hetero atom selected from an oxygen atom, a nitrogen atom, and a sulfur atom, and at least one halogen atom selected from a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and R 40” It represents a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, which may be substituted with a substituent; and e and u represent 0 or 1.

24. The polycarbonate-polyorganosiloxane copolymer according to claim 22, wherein The polyorganosiloxane (a2) has any one of the structures represented by the following general formulas (a2-1) to (a2-3), In the formula, R 1 ~R 4 are optionally the same or different, and each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkylaryl group having 1 to 10 carbon atoms in the alkyl portion; R 5 and R 6 are optionally the same or different, and each independently represents an arylene group having 6 to 20 carbon atoms, an alkylene group having 1 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl moiety, and as a functional group, may include -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -; R 7 and R 8 are optionally the same or different, and each independently represents an arylene group having 6 to 20 carbon atoms, an alkylene group having 2 to 10 carbon atoms, a branched alkylene group having 3 to 10 carbon atoms, or an alkylarylene group having 1 to 10 carbon atoms in the alkyl portion, and as a functional group, may include -O-, -COO-, -CO-, -S-, -NH-, -NR 111 -; R 111 represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms; β represents a divalent group derived from a diisocyanate compound, or a divalent group derived from a dicarboxylic acid or a halide of a dicarboxylic acid; z and z1 each independently represent 0 or 1; a represents an integer of 2 to 500; b and b1 each independently represent an integer of 0 to 200.

25. The polycarbonate-polyorganosiloxane copolymer according to claim 22, wherein The carbonic acid diester is at least one compound selected from the group consisting of a diaryl carbonate compound, a dialkyl carbonate compound, and an alkyl aryl carbonate compound.

26. The polycarbonate-polyorganosiloxane copolymer according to claim 25, wherein The diaryl carbonate compound is a compound represented by the following general formula (11) or a compound represented by the following general formula (12), In formula (11), Ar 1 and Ar 2 Each represents an aromatic group, and they may be the same or different from each other. In formula (12), Ar 3 and Ar 4 Each represents an aryl group, which may be the same or different from each other, D 1 represents a residue obtained by removing two hydroxyl groups from an aromatic dihydroxy compound or an aliphatic dihydroxy compound having a structure represented by the following general formula (a1), HO—R 10 -OH (a1) In the general formula (a1), R 10 represents a divalent aliphatic hydrocarbon group having 2 to 40 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 40 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, which is optionally substituted by a substituent; the divalent aliphatic hydrocarbon group, the divalent alicyclic hydrocarbon group or the divalent aromatic hydrocarbon group optionally contains at least one heteroatom selected from an oxygen atom, a nitrogen atom and a sulfur atom, and at least one halogen atom selected from a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

27. The polycarbonate-polyorganosiloxane copolymer according to claim 25, wherein The diaryl carbonate compound is at least one selected from diphenyl carbonate, ditolyl carbonate, dichlorophenyl carbonate, di(m-tolyl) carbonate, dinaphthyl carbonate, bis(biphenyl) carbonate, and bisphenol A bisphenyl carbonate.

28. The polycarbonate-polyorganosiloxane copolymer according to claim 25, wherein The dialkyl carbonate compound is a compound represented by the following general formula (13) or a compound represented by the following general formula (14), In formula (13), R 21 and R 22 Each represents an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 4 to 20 carbon atoms, and they may be the same or different from each other. In formula (14), R 23 and R 24 Each represents an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 4 to 20 carbon atoms, and they may be the same or different from each other, and D 2 represents a residue obtained by removing two hydroxyl groups from an aromatic dihydroxy compound or an aliphatic dihydroxy compound having a structure represented by the following general formula (a1), HO-R 10 -OH (a1) In the general formula (a1), R 10 represents a divalent aliphatic hydrocarbon group having 2 to 40 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 40 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, which is optionally substituted by a substituent; the divalent aliphatic hydrocarbon group, the divalent alicyclic hydrocarbon group or the divalent aromatic hydrocarbon group optionally contains at least one heteroatom selected from an oxygen atom, a nitrogen atom and a sulfur atom, and at least one halogen atom selected from a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

29. The polycarbonate-polyorganosiloxane copolymer according to claim 25, wherein The dialkyl carbonate compound is diethyl carbonate, dimethyl carbonate, dibutyl carbonate, dicyclohexyl carbonate, or bisphenol A dimethyl carbonate.

30. The polycarbonate-polyorganosiloxane copolymer according to claim 25, wherein The alkyl aryl carbonate compound is a compound represented by the following general formula (15) or a compound represented by the following general formula (16), In formula (15), Ar 5 Represents an aryl group, R 25 represents an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 4 to 20 carbon atoms. In the formula (16), Ar 6 Represents an aryl group, R 26 represents an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 4 to 20 carbon atoms, D 1 represents a residue obtained by removing two hydroxyl groups from an aromatic dihydroxy compound or an aliphatic dihydroxy compound having a structure represented by the following general formula (a1), HO-R 10 -OH (a1) In the general formula (a1), R 10 represents a divalent aliphatic hydrocarbon group having 2 to 40 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 40 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, which is optionally substituted by a substituent; the divalent aliphatic hydrocarbon group, the divalent alicyclic hydrocarbon group or the divalent aromatic hydrocarbon group optionally contains at least one heteroatom selected from an oxygen atom, a nitrogen atom and a sulfur atom, and at least one halogen atom selected from a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

31. The polycarbonate-polyorganosiloxane copolymer according to claim 25, wherein The alkyl aryl carbonate compound is methyl phenyl carbonate, ethyl phenyl carbonate, butyl phenyl carbonate, cyclohexyl phenyl carbonate, or bisphenol A methyl phenyl carbonate. 32 . A polycarbonate-based resin composition comprising the polycarbonate-polyorganosiloxane copolymer according to claim 1 . The polycarbonate-based resin composition according to claim 32 , further comprising an inorganic filler.

34. The polycarbonate resin composition according to claim 33, wherein The inorganic filler is contained in an amount of 1 to 150 parts by mass based on 100 parts by mass of the polycarbonate-polyorganosiloxane copolymer.

35. The polycarbonate resin composition according to claim 34, wherein The inorganic filler is contained in an amount of 15 to 40 parts by mass based on 100 parts by mass of the polycarbonate-polyorganosiloxane copolymer.

36. The polycarbonate resin composition according to any one of claims 33 to 35, wherein The inorganic filler is glass fiber or carbon fiber. 37 . A molded article formed from the polycarbonate resin composition according to claim 32 .

38. The formed body according to claim 37, wherein the thickness of the formed body is 0.2 mm to 4.0 mm.

39. According to the molded body described in claim 38, when it is formed into a flat plate, when the content of the polyorganosiloxane block represented by formula (1) in the polycarbonate-polyorganosiloxane copolymer is less than 5 mass% and the average chain length a of the polyorganosiloxane block (A-2) in the polycarbonate-polyorganosiloxane copolymer is less than 70, the total transmittance to visible light is greater than 60%. The molded body according to claim 39 , wherein the total light transmittance is 90% or more.

41. A molded body according to any one of claims 37 to 40, which, when formed into a flat plate, has a haze of 40 or less when the content of the polyorganosiloxane block represented by formula (1) in the polycarbonate-polyorganosiloxane copolymer is less than 5% by mass and the average chain length a of the polyorganosiloxane block (A-2) in the polycarbonate-polyorganosiloxane copolymer is less than 70. The molded article according to claim 41 , wherein the haze is 5 or less.

43. The molded article according to claim 41, which, when molded into a flat plate, has a total transmittance to visible light of 25% or more when the content of the polyorganosiloxane block represented by formula (1) in the polycarbonate-polyorganosiloxane copolymer is 5% by mass or more.

Citation Information

Patent Citations

  • Preparation of polysiloxane / Polycarbonate block cocondensation product

    JP1998251408A

  • Process for producing poly(diorganosiloxane) / polycarbonate block copolymer

    JP2008248262A

  • Method for producing modified polycarbonate using a spray crystallization method

    JP2008513594A

  • Method for producing polycarbonate-polyorganosiloxane copolymer

    JP2015189953A

  • Polysiloxane-polycarbonate block cocondensates with improved rheological properties

    JP2017505841A