Acrylic resin masterbatch

By dispersing non-volatile liquids with boiling points higher than 200°C in the acrylic resin and combining nucleating agents to generate fine spherical crystals, the problem of liquid seepage of masterbatch is solved, and the stability of liquid concentration and production efficiency are improved. .

CN114746481BActive Publication Date: 2024-11-08TOYO SEIKAN GRP HLDG LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080083263.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-02
Filing Date
2020-09-03
Publication Date
2024-11-08
Estimated Expiration
2040-09-03

AI Technical Summary

Technical Problem

In the prior art, liquid-containing masterbatches are difficult to suppress liquid leakage at high concentrations, resulting in insufficient liquid concentration of the resin composition for molding, affecting molding quality and production efficiency.

Method used

A non-volatile liquid with a boiling point higher than 200°C is dispersed in the acrylic resin, and fine spherical crystals are generated to seal the liquid and inhibit its ooze.

Benefits of technology

It effectively inhibits the leakage of liquid, prevents the particles from becoming sticky, ensures the stable liquid volume in the molding resin, meets the design requirements, and maintains low exudation during long-term storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114746481B_ABST
    Figure CN114746481B_ABST
Patent Text Reader

Abstract

The present invention provides a masterbatch, characterized in that the masterbatch is a masterbatch in which a non-volatile liquid with a boiling point higher than 200°C is dispersed in a matrix resin containing a propylene resin, and in a DSC measurement, after being heat-treated at 200°C for 5 minutes, the crystallization temperature Tc represented as the peak top temperature of the exothermic peak observed on the highest temperature side when cooled to -50°C at a cooling rate of 10°C / min; and the melting point Tm represented as the peak top temperature of the melting peak observed on the highest temperature side when subsequently heated from -50°C to 200°C at a heating rate of 10°C / min satisfies the temperature conditions represented by the following formulas: Tm<159°C, Tc≥97°C, Tm-Tc<49°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a masterbatch of a propylene resin, and more particularly to a masterbatch of a propylene resin containing a non-volatile liquid having a boiling point higher than 200°C. Background Art

[0002] Plastic containers are widely used in various applications because they are easy to mold and can be manufactured at low cost. For example, olefin resins such as polyethylene and polypropylene are preferably used in the molding of bottles for containing viscous slurry or paste contents such as ketchup.

[0003] Furthermore, in containers such as bottles that hold viscous contents, in order to quickly discharge the contents or to use them cleanly to the end without any residue in the container, the containers are often stored in an inverted state. Therefore, when the container is inverted, it is desired that the viscous contents do not adhere to the inner surface of the container but fall quickly.

[0004] In order to meet such requirements, as described in Patent Document 1, a method has been adopted in which a solid lubricant such as aliphatic amide is mixed in advance on the inner surface of a resin forming the inner surface of a container, and the lubricant bleeds onto the inner surface of the container, thereby improving the sliding properties of the container contents.

[0005] However, recently, as described in Patent Document 2, the following method has attracted attention: a layer of a liquid different from the contents is formed on the inner surface in contact with the contents. In this method, by forming a liquid layer made of a liquid that is immiscible with the contents on the inner surface of the container in advance, the sliding property with respect to the contents can be significantly improved compared to the conventionally known methods, and by inverting or tilting the container, the contents can be discharged quickly to the outside of the container without being attached to or remaining on the inner wall of the container.

[0006] The method of modifying surface properties such as slipperiness by forming a liquid layer on the surface is not limited to the shape of the container, but can also be applied to a molded body having a film or the like. By appropriately selecting the type of liquid, the surface properties can be significantly modified.

[0007] However, in the method of modifying the surface properties by forming a layer of liquid on the surface of a molded body such as a container as described above, after the container is molded, a liquid that is not the content is applied to the inner surface of the container by dipping, spraying, etc. to form a liquid layer, but in this case, a special treatment process for forming the liquid layer is required, which has problems in terms of productivity. Therefore, the following method is studied: a liquid that forms a liquid layer is mixed with a resin that forms the inner surface of the container, and a resin composition mixed with such a liquid is used for molding, and a liquid layer is formed on the surface of the molded body by the seepage of the liquid after molding. That is, the reason is that even if no special treatment is performed after molding, the liquid contained in the resin composition segregates on the inner surface of the container, and thus a liquid layer is spontaneously formed on the surface.

[0008] Furthermore, when a container is molded using a resin composition containing a liquid (hereinafter, sometimes referred to as a lubricating liquid) as described above, a master batch in the form of particles in which the lubricating liquid is mixed with the molding resin should be used industrially. That is, during molding, it is inefficient to prepare the resin composition by mixing the lubricating liquid with the molding resin each time, and a large number of tanks for storing the lubricating liquid are required. Therefore, a master batch in the form of particles containing the lubricating liquid at a high concentration is prepared in advance, and the lubricating liquid is handled in the form of the master batch during storage, transportation, and other operations. During molding, the master batch is diluted with the molding resin to prepare a surface-forming resin composition, and molding is performed into a container or the like.

[0009] Therefore, the problem is the bleed of the lubricating liquid from the masterbatch. That is, when the concentration of the liquid contained in the masterbatch is low (for example, 20% by mass or less), there is no problem, but when the concentration of the liquid in the masterbatch is high, there are the following problems: the liquid bleeds from the masterbatch, the pellets become sticky and difficult to handle; due to the bleed of the liquid, when the resin composition for molding is prepared by diluting it, the liquid concentration becomes less than the target value. This tendency is significant when the molding resin mixed with the liquid is an olefin resin such as polyethylene and polypropylene used in molding of extrusion containers, etc.

[0010] In addition, regarding the masterbatch containing a liquid component, the examples of Patent Document 3 describe that 5% of a fatty acid ester of polyglycerol (liquid component) is added to polyethylene or polypropylene, a masterbatch pellet is prepared by an extruder, and the masterbatch pellet is mixed with resin pellets of polyethylene or polypropylene and extruded to form a film. However, in Patent Document 3, the concentration of polyglycerol as a liquid component is as low as 5%, so the molding resin composition formed from the masterbatch is limited to a composition having a very low concentration of the liquid component (in the examples of Patent Document 4, all are 1.5% or less), and it is impossible to prepare a molding resin composition containing a liquid component at a high concentration.

[0011] In addition, Patent Document 4 discloses a masterbatch in which 1 to 30 parts by weight of an antistatic agent and 0.1 to 1 parts by weight of a nucleating agent are mixed with 100 parts by weight of a crystalline thermoplastic resin such as polypropylene. Examples of the antistatic agent include nonionic surfactants such as fatty acid esters of glycerol. That is, the technology of Patent Document 4 is a technology that suppresses the amount of antistatic agent seepage by crystallizing the crystalline thermoplastic resin in advance, thereby preventing stickiness caused by the seepage of the antistatic agent. However, in this technology, the content of the antistatic agent per masterbatch is about 20% by mass, and the amount of seepage is only suppressed to about 7 to 9% by mass. Moreover, the antistatic agent mixed here is a substance used to prevent the adhesion of dust, etc., and is not a substance used to improve the sliding property of a fluid substance, so a liquid layer will not be formed on the surface. That is, in order to prevent the stickiness of the masterbatch that is mixed with a large amount of liquid (lubricating liquid) instead of a large amount of antistatic agent to form a liquid layer (lubricating layer), further research is needed.

[0012] Moreover, in Patent Document 5, the applicant proposed a masterbatch characterized in that a liquid (B) having a viscosity (23°C) of 1000 mPa·s or less is dispersed in a matrix resin (A) having a glass transition temperature of 35°C or more. The masterbatch contains a lubricating liquid (liquid (B)) for improving the sliding property relative to a fluid substance, and the exudation of the liquid (B) is suppressed by using a matrix resin (A) having a high glass transition temperature, and the exudation suppression effect is extremely high. However, the matrix resin having a high glass transition temperature used in Patent Document 5 is a cyclic olefin resin, which is extremely expensive and has the disadvantage of not being applicable to cheap propylene resins such as ordinary polypropylene or copolymers of propylene and α-olefin.

[0013] Prior art literature

[0014] Patent Literature

[0015] Patent Document 1: Japanese Patent Application Publication No. 2008-222291

[0016] Patent Document 2: WO2014 / 010534

[0017] Patent Document 3: Japanese Patent Publication No. 43-8605

[0018] Patent Document 4: Japanese Patent Application Publication No. 2012-72335

[0019] Patent Document 5: Japanese Patent Application Publication No. 2015-105308 Summary of the invention

[0020] Problem that the invention aims to solve

[0021] Therefore, an object of the present invention is to provide a liquid-containing masterbatch which effectively suppresses the bleeding of the liquid for a long period of time even when the liquid contained therein is contained at a high concentration.

[0022] Another object of the present invention is to provide a liquid-containing masterbatch in which a liquid is dispersed in an inexpensive propylene-based resin.

[0023] Technical Solution

[0024] The inventors of the present invention conducted a large number of experiments on masterbatches containing liquid and studied their exudation properties. As a result, they found that when liquid is added to propylene resin, fine spherulites are uniformly generated in large quantities, thereby significantly suppressing the exudation of the liquid, thereby completing the present invention.

[0025] According to the present invention, there is provided a masterbatch, characterized in that the masterbatch is a masterbatch in which a non-volatile liquid having a boiling point higher than 200° C. is dispersed in a matrix resin including a propylene resin.

[0026] In DSC measurement, after heat treatment at 200°C for 5 minutes, the crystallization temperature Tc represented as the peak top temperature of the exothermic peak observed on the highest temperature side when cooled to -50°C at a temperature drop rate of 10°C / min; and the melting point Tm represented as the peak top temperature of the melting peak observed on the highest temperature side when subsequently heated from -50°C to 200°C at a temperature rise rate of 10°C / min satisfy the temperature conditions represented by the following formula:

[0027] Tm<159℃,

[0028] Tc≥97℃,

[0029] Tm-Tc<49℃.

[0030] In the masterbatch of the present invention, the following aspects are preferably adopted.

[0031] (1) The temperature condition satisfies the following formula:

[0032] Tm-Tc<42℃.

[0033] (2) A nucleating agent is compounded in the matrix resin.

[0034] (3) Propylene resin is a copolymer of propylene and α-olefin.

[0035] (4) The non-volatile liquid is glycerol fatty acid ester or vegetable oil.

[0036] (5) The nonvolatile liquid is contained in an amount of 10 parts by mass or more per 100 parts by mass of the matrix resin comprising the propylene resin.

[0037] (6) After storage for 60 days under an environment of 22° C. and 60% RH, the amount of the nonvolatile liquid exuded from the surface per 1 g of the masterbatch is 20 mg or less.

[0038] According to the present invention, there is also provided a plastic container, characterized in that the inner surface is formed by a blend of the masterbatch according to claim 1 and a container molding resin.

[0039] Beneficial Effects

[0040] The masterbatch of the present invention has the following important features, whereby the bleeding of the masterbatch can be effectively suppressed for a long period of time, wherein a non-volatile liquid having a boiling point higher than 200° C. is contained in a matrix resin having a propylene resin as a main component, and a melting point Tm and a crystallization temperature Tc calculated in a DSC measurement satisfy the temperature conditions represented by the following formula:

[0041] Tm<159℃,

[0042] Tc≥97℃,

[0043] Tm-Tc<49°C (preferably Tm-Tc<42°C). In particular, as shown in the examples described later, when a master batch containing a large amount of non-volatile liquid of 20% by mass is stored for 60 days, the amount of seepage per 1g of the master batch is suppressed to 20 mg or less, so that stickiness caused by the seepage of the liquid can be effectively prevented. In addition, when a predetermined resin is added to the master batch to form a molding resin, the amount of liquid in the molding resin can be stably maintained, and modification using the liquid can be performed as designed.

[0044] That is, in the present invention, the masterbatch satisfies the above-mentioned temperature condition and further satisfies Tm-Tc<42°C, which means that a nucleating agent is compounded in the propylene resin, and when the matrix resin containing the propylene resin and the non-volatile liquid are melt-kneaded and cooled, fine spherulites are uniformly generated in large quantities. Through such a large number of fine spherulites, the dissolved non-volatile liquid is sealed in the amorphous part between the spherulites, and its seepage is effectively suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is a polarizing microscope photograph taken under a cross nicol lens, showing the crystal state of the central cross section of the mother particle of Example 1 that satisfies the temperature conditions of the present invention by DSC.

[0046] Figure 2 This is a polarizing microscope photograph taken under crossed Nicol prisms, showing the crystal state of the central cross section of the mother particle of Comparative Example 1 that does not satisfy the temperature conditions by DSC in the present invention. DETAILED DESCRIPTION

[0047] The masterbatch of the present invention contains a matrix resin and a high boiling point liquid dispersed in the matrix resin as essential components.

[0048] <High boiling point liquid>

[0049] The high boiling point liquid dispersed in the matrix resin is a liquid that forms a liquid layer on the surface of the molded body when the masterbatch is mixed with the molding resin to produce a molded body. The surface properties corresponding to the type of liquid are reflected on the surface of the molded body according to the liquid layer. Therefore, the liquid should have a boiling point that is not volatile under atmospheric pressure, for example, a boiling point higher than 200°C, and is selected according to the surface properties that are desired to be imparted to the surface of the molded body.

[0050] For example, when it is desired to impart hydrophobicity, it can be selected from silicone oil, glycerol fatty acid ester, vegetable oil (or edible oil) and the like.

[0051] Furthermore, when it is desired to impart oleophobicity, a highly hydrophilic ionic liquid or the like may be used, and an appropriate liquid may be selected in consideration of the intended use of the molded article.

[0052] Furthermore, when the molded article is a container and the sliding property with respect to the viscous contents is to be improved, the liquid used is selected to be immiscible with the contents and not mixed with the contents. The reason is that if the liquid is miscible with the contents, the liquid exposed on the inner surface of the container will mix with the contents and fall off from the inner surface of the container, making it difficult to impart the target surface properties.

[0053] In particular, as the content, when it is a substance containing water, such as ketchup, as a liquid, silicone oil, glycerol fatty acid ester, liquid paraffin, vegetable oil, etc. are preferably used. Among them, glycerol fatty acid esters represented by medium-chain fatty acid triglycerides (commercially available substances with C numbers 6 to 12), glycerol trioleate and glycerol diacetyl monooleate, and vegetable oils are difficult to volatilize and are recognized as food additives, and are tasteless and have the advantage of not damaging the flavor of the content. In particular, medium-chain fatty acid esters (MCT) are the best in terms of easily satisfying the temperature conditions.

[0054] In addition, for emulsified contents such as mayonnaise, silicone oil, glycerol fatty acid esters, vegetable oils, etc. are preferred as high-boiling-point liquids, and liquids that exhibit the property of emulsification over time are the best. Liquids that have such properties are substances with higher molecular weights among these.

[0055] In the present invention, the high boiling point liquid exudes in the form of a liquid layer on the surface of the molded body when the masterbatch is diluted with a predetermined molding resin for molding, so it is preferably blended in a large amount. However, if the blended amount is too large, the effect of the nucleating agent during masterbatch molding becomes small, and the high boiling point liquid may not be effectively suppressed from exuding from the masterbatch. Therefore, the blended amount of the high boiling point liquid is preferably in the range of 10 parts by mass or more and less than 100 parts by mass, particularly preferably in the range of 20 parts by mass or more and less than 70 parts by mass, and further preferably in the range of 25 parts by mass or more and less than 40 parts by mass per 100 parts by mass of the masterbatch described later.

[0056] <Matrix resin>

[0057] In the present invention, a propylene resin is used as a matrix resin for dispersing the high boiling point liquid. By using a propylene resin as a matrix resin, the crystallinity can be adjusted so as to satisfy a predetermined temperature condition.

[0058] As such a propylene resin, not only a propylene homopolymer but also a random copolymer or block copolymer of propylene and a linear α-olefin such as ethylene, butene-1, hexene-1, 4-methyl-1-pentene can be used according to its application, but from the viewpoint of crystallinity, the propylene content in the copolymer is preferably 90 mol% or more, particularly preferably 95 mol% or more. In addition, from the viewpoint of moldability, it is preferred that the MFR (230°C) is in the range of 0.1 g / 10min or more and less than 26 g / 10min, more preferably in the range of 0.3 to 10 g / 10min.

[0059] As long as the prescribed temperature conditions based on DSC measurement can be ensured, a resin mixed with other thermoplastic resins other than the above-mentioned propylene resin can also be used as the matrix resin. Such other thermoplastic resins are not particularly limited, but generally, from the viewpoint of moldability, olefin resins can be cited, such as polyethylene, copolymers of ethylene and other α-olefins, and the mixing amount thereof in the matrix resin is preferably 30% by mass or less.

[0060] In addition, in order to satisfy the prescribed temperature conditions, such a matrix resin must be formulated with a nucleating agent. Representative examples of such nucleating agents include substances known as crystallization nucleating agents for polypropylene, such as carboxylic acid metal salts such as sodium benzoate, aluminum dibenzoate, potassium benzoate, lithium benzoate, sodium β (sodium naphthalene dicarboxylate cyclohexane carboxylate); sorbitols such as benzylidene sorbitol and its derivatives; and polymers such as poly-3-methylbutene-1, polyvinyl cycloalkane, and polyvinyl trialkylsilane.

[0061] It should be noted that the above nucleating agent is usually mixed with propylene resin and sold commercially. For example, such propylene resin with nucleating agent is sold commercially under the following trade names: random polypropylene PM931M made by SunAllomer, random polypropylene EG7FTB made by Japan POLYPRO, random polypropylene PM731M made by SunAllomer, random polypropylene PS320M made by SunAllomer, etc.

[0062] In the present invention, the masterbatch comprising the matrix resin, high boiling point liquid and nucleating agent as described above is subjected to heat treatment at 200°C for 5 minutes and then cooled to -50°C at a cooling rate of 10°C / min in DSC measurement. The crystallization temperature Tc represented by the peak top temperature of the exothermic peak observed on the highest temperature side; and the melting point Tm represented by the peak top temperature of the melting peak observed on the highest temperature side when subsequently heated from -50°C to 200°C at a heating rate of 10°C / min need to satisfy the following temperature conditions.

[0063] Temperature conditions:

[0064] Tm<159℃,

[0065] Tc≥97℃,

[0066] Tm-Tc<49°C (preferably Tm-Tc<42°C).

[0067] According to the above temperature conditions, the masterbatch can be molded at low temperature (Tm is less than 159°C, especially less than 155°C, and further less than 150°C), and the crystallization temperature Tc is high (Tc is above 97°C, especially above 100°C, and further above 102°C) and the supercooling degree (Tm-Tc) is low (less than 49°C, especially less than 42°C, and further less than 40°C). Therefore, during the cooling process after extrusion, the matrix resin can be crystallized from a higher temperature state in which the non-volatile liquid is uniformly microdispersed in the matrix resin. For example, in Figure 1 The polarizing microscope photograph of the central cross section of the masterbatch (Example 1) satisfying the temperature condition is shown in Figure 2The polarizing microscope photographs under the orthogonal Nicol prism of the masterbatch (Comparative Example 1) that does not meet the temperature condition are shown in . By comparing these figures, it can be understood that in the masterbatch that meets the above-mentioned temperature condition, fine spherulites are uniformly generated in large quantities, and the high-boiling point liquid is sealed in the amorphous part between the spherulites or inside the spherulites. Therefore, the amount of the high-boiling point liquid that seeps out is as little as 13.2 mg per 1g of the masterbatch (refer to Example 1). On the other hand, it is speculated that in the masterbatch that does not meet the temperature condition, coarse spherulites are unevenly generated, and amorphous parts like cracks are generated between the spherulites, thereby making it easy for the high-boiling point liquid present in the amorphous part to transfer to the surface of the masterbatch along the amorphous part. As a result, the amount of the high-boiling point liquid that seeps out is a considerable amount of 23.7 mg (refer to Comparative Example 1).

[0068] In the present invention, from the viewpoint of suppressing the seepage of the liquid, the crystallinity of the matrix resin of the masterbatch containing the high-boiling point liquid and the nucleating agent is preferably greater, but if it is too large, the proportion of the amorphous part decreases, and the saturated solubility of the liquid relative to the matrix resin may decrease. Therefore, the crystallinity of the matrix resin is preferably in the range of 5% to 60%, particularly preferably in the range of 10% to 50%, 15% to 40%, 15% to 35%, 20% to 40%, and more preferably in the range of 20% to 35%. In this specification, the crystallinity refers to the value obtained by the ratio of the melting enthalpy of the matrix resin to the melting enthalpy of the complete crystallization of the matrix resin according to the differential scanning calorimeter (DSC).

[0069] In the present invention, from the viewpoint of suppressing the seepage of the liquid, the size of the spherulites in the matrix resin of the masterbatch containing the high boiling point liquid and the nucleating agent is preferably smaller, for example, preferably 50 μm or less, particularly preferably 30 μm or less, 10 μm or less, and further preferably 5 μm or less. The lower limit is not particularly limited, but is preferably 0.1 μm or more. In this specification, the size of the spherulites refers to the average particle size of the spherulites existing in the central cross section of the masterbatch, which can be measured using a polarizing microscope or SEM.

[0070] In the present invention, in order to meet the above-mentioned temperature conditions, it is necessary to set the type and amount of the nucleating agent according to the propylene resin; and the type and amount of the high boiling point liquid to a specified range. For example, the high boiling point liquid is mixed in a considerable amount, but if the amount is too much, the melting point Tm becomes lower. Although the conditions for the melting point Tm can be met, the crystallization temperature Tc also becomes lower, and as a result, the supercooling (Tm-Tc) becomes larger, and there is a tendency to be difficult to meet these conditions. In addition, depending on the type of nucleating agent, in order to ensure the specified crystallization temperature Tc, a large amount of nucleating agent needs to be mixed, and as a result, the melting point Tm becomes higher, which may affect the moldability and processability. Therefore, in order to obtain a masterbatch that meets the above-mentioned temperature conditions, it is better to adopt the following method: a high boiling point liquid is mixed with a commercially available propylene resin to produce a masterbatch, and the masterbatch is subjected to DSC measurement to calculate each temperature Tm and Tc. According to the result, the amount of the high boiling point liquid, the type and amount of the nucleating agent, etc. are adjusted in a manner to meet the specified temperature conditions. Generally, there are resins whose types and amounts of nucleating agents to be blended are not disclosed depending on the resin manufacturer, and therefore it is better to adopt such a method.

[0071] <Preparation and use of masterbatch>

[0072] In the masterbatch of the present invention, the matrix resin containing the nucleating agent and a predetermined amount of the high-boiling-point liquid are supplied to, for example, a kneading section of an extruder, kneaded, melt-extruded, and the molten extrudate is cut by a granulator, and the molten extrudate is stored, transported, or sold in the form of pellets of a predetermined size for use. That is, from the time immediately after production to the time of use, it is possible to effectively prevent the high-boiling-point liquid from seeping out and causing the pellets to become sticky, and other undesirable conditions.

[0073] The masterbatch pellets may be used in the form of two-layer pellets having a core layer made of a matrix resin containing a nucleating agent in which the high boiling point liquid is dispersed, as long as the predetermined temperature conditions based on DSC measurement are ensured.

[0074] The masterbatch particles are particularly used for molding a molded body in which a liquid layer obtained from a high-boiling-point liquid (B) is formed on the surface. That is, the masterbatch particles are kneaded with a molding resin (diluent resin) to prepare a kneaded product containing a high-boiling-point liquid at a specified concentration, and the kneaded product is molded into a specified shape to obtain a target molded body. In addition, in the case where the molded body is composed of a multilayer structure, not only a liquid layer is formed on the surface, but also the masterbatch particles can be mixed with a molding resin (diluent resin) for use, for example, in order to adjust the concentration of the liquid component in any layer in the multilayer structure.

[0075] The molding resin mixed with the masterbatch particles is not particularly limited as long as it can be uniformly mixed with the matrix resin, but it is usually preferred to use a material of the same type as the olefin resin in the matrix resin, such as propylene resin or polyethylene. This is because it is easy to set the molding conditions and a molded body that maximizes the properties of the resin can be obtained.

[0076] Moreover, the kneading method and the molding method can adopt appropriate methods according to the physical properties of the resin (such as melt flow rate), but from the viewpoint of kneading the liquid with the solid matrix resin, the kneading of the two is preferably carried out by melt kneading in the kneading section of a molding machine such as an extruder, and the molding method is preferably extrusion molding, extrusion blow molding (direct blow molding). The reason is that such a method can effectively avoid the escape of high-boiling point liquid during kneading and molding, and can ignore the influence of the presence of high-boiling point liquid on molding (such as the adhesion of liquid to molding, etc.).

[0077] Such a masterbatch mainly composed of propylene resin and containing a high-boiling-point liquid is preferably used in the molding of flexible containers such as squeeze containers (direct blow molding bottles) for extruding viscous contents. When the masterbatch of the present invention is used in the molding of such flexible containers, the surface characteristics brought by the liquid layer of the high-boiling-point liquid can be used to the maximum extent. Of course, it can also be used in the molding of containers with various shapes such as cups or glasses, bottles, bags (pouches), syringes, cans, trays, etc., and can also be applied to stretch-molded containers.

[0078] Example

[0079] The excellent properties of the masterbatch of the present invention are described by the following examples. It should be noted that the methods for measuring various physical properties and characteristics and the preparation of the masterbatch in the following examples are as follows.

[0080] 1. Determination of melting point and crystallization temperature

[0081] The crystallization temperature Tc and melting point Tm of the produced master pellets were measured using a differential scanning calorimeter (Diamond DSC manufactured by PERKIN ELMER).

[0082] Fill 5 mg of the sample into a B0143003 / B0143017 sample pan (trade name, manufactured by PERKIN ELMER). After heat treating the sample at 200°C for 5 minutes in a nitrogen atmosphere, cool it to -50°C at a cooling rate of 10°C / min. The peak top temperature of the exothermic peak observed on the highest temperature side during the cooling process is set as Tc(°C). Then, after keeping at -50°C for 3 minutes, heat the sample from -50°C to 200°C at a heating rate of 10°C / min. The peak top temperature of the melting peak observed on the highest temperature side during the heating process is set as Tm(°C).

[0083] 2. Crystallinity Determination

[0084] The crystallinity of the matrix resin was measured using a differential scanning calorimeter (Diamond DSC manufactured by PERKIN ELMER).

[0085] 5 mg of the sample was filled into a B0143003 / B0143017 sample pan (trade name, manufactured by PERKIN ELMER). The sample was kept at 25°C for 3 minutes under a nitrogen atmosphere, and then cooled to -50°C at a cooling rate of 10°C / min. Then, after being kept at -50°C for 3 minutes, the sample was heated from -50°C to 200°C at a heating rate of 10°C / min. The melting enthalpy ΔH (J / g) of the matrix resin was determined based on the peak area of ​​the melting peak observed on the highest temperature side during the heating process and the weight of the matrix resin contained in the filled sample, and the crystallinity was calculated according to the following formula.

[0086] Crystallinity (%) = (ΔH / ΔH0) × 100

[0087] ΔH0 is the melting enthalpy of complete crystallization of the matrix resin, but in Examples 1 to 4 and Comparative Examples 1 to 4, ΔH0 is set to the melting enthalpy of complete crystallization of the propylene resin, and in Examples 5 to 8, ΔH0 is set to the sum of the values ​​obtained by multiplying the melting enthalpy of complete crystallization of the propylene resin and the ethylene resin by their respective weight fractions. Here, the melting enthalpy of complete crystallization of the propylene resin is set to 207 J / g, and the melting enthalpy of complete crystallization of the ethylene resin is set to 293 J / g.

[0088] 3. Evaluation of the surface exudation of masterbatch

[0089] 8 g of the masterbatch prepared by the method described below was placed in a glass bottle and stored for 60 days at 22°C and 60% RH. 8 g of heptane was added to the glass bottle containing the masterbatch after storage for 10 seconds to extract the non-volatile liquid on the surface of the masterbatch. After the extract was dried at 120°C, the weight of the remaining non-volatile liquid was measured and divided by the weight of the masterbatch put in, thereby calculating the surface exudation amount of the non-volatile liquid relative to 1 g of the masterbatch.

[0090] <Matrix resin for masterbatch production>

[0091] Propylene resin A: random polypropylene, PM931M manufactured by SunAllomer.

[0092] Propylene resin B: random polypropylene, EG7FTB manufactured by Japan POLYPRO Co., Ltd.

[0093] Propylene resin C: random polypropylene, PM731M manufactured by SunAllomer.

[0094] Propylene resin D: random polypropylene, PS320M manufactured by SunAllomer.

[0095] Propylene resin E: random polypropylene, PC630A manufactured by SunAllomer.

[0096] Propylene resin F: block polypropylene, CM688A manufactured by SunAllomer.

[0097] Propylene resin G: homopolypropylene, PM600A manufactured by SunAllomer.

[0098] Ethylene resin: Metallocene C6-LLDPE, FV103 manufactured by Sumitomo Chemical Co., Ltd.

[0099] In addition, the propylene-based resins A to D contain a nucleating agent.

[0100] <Non-volatile liquids with a boiling point higher than 200°C>

[0101] Medium chain triglycerides (MCT).

[0102] Surface tension: 28.8 mN / m (23°C).

[0103] Viscosity: 33.8 mPa·s (23°C).

[0104] Boiling point: above 210℃.

[0105] Flash point: 242℃ (reference value)

[0106] The surface tension of the liquid was measured at 23° C. using a solid-liquid interface analysis system DropMaster 700 (manufactured by Kyowa Interface Science Co., Ltd.). The density of the liquid required for the surface tension measurement of the liquid was measured at 23° C. using a density specific gravity meter DA-130 (manufactured by Kyoto Electronics Co., Ltd.). The viscosity of the lubricating fluid was measured at 23° C. using a tuning fork vibration viscometer SV-10 (manufactured by A&D Co., Ltd.).

[0107] (Example 1)

[0108] Propylene resin A was used as a matrix resin for preparing masterbatches, and medium-chain fatty acid triglyceride (MCT) was used as a non-volatile liquid having a boiling point higher than 200°C, so that the ratio of propylene resin A:MCT=100:25 (parts by mass) was obtained. The mixture was melt-kneaded using a twin-screw compounding extruder (KZW20TW manufactured by Technovel Co., Ltd.) at a barrel temperature of 220°C to prepare masterbatches.

[0109] <Example 2>

[0110] Master pellets were prepared using a twin-screw kneading extruder under the same conditions as in Example 1 except that the ratio of propylene resin B:MCT was 100:25 (parts by mass).

[0111] <Example 3>

[0112] Master pellets were prepared using a twin-screw kneading extruder under the same conditions as in Example 1 except that the ratio of propylene resin C:MCT was 100:25 (parts by mass).

[0113] <Example 4>

[0114] Master pellets were prepared using a twin-screw kneading extruder under the same conditions as in Example 1 except that the propylene resin D:MCT=100:25 (parts by mass).

[0115] <Example 5>

[0116] Master pellets were prepared using a twin-screw kneading extruder under the same conditions as in Example 1 except that the ratio of propylene resin A:ethylene resin:MCT was 85:15:25 (parts by mass).

[0117] <Example 6>

[0118] Master pellets were prepared using a twin-screw kneading extruder under the same conditions as in Example 1 except that the ratio of propylene resin B:ethylene resin:MCT was 85:15:25 (parts by mass).

[0119] <Example 7>

[0120] Master pellets were prepared using a twin-screw kneading extruder under the same conditions as in Example 1 except that the ratio of propylene resin C:ethylene resin:MCT was 85:15:25 (parts by mass).

[0121] <Example 8>

[0122] Master pellets were prepared using a twin-screw kneading extruder under the same conditions as in Example 1 except that the ratio of propylene resin D:ethylene resin:MCT was 85:15:25 (parts by mass).

[0123] <Comparative Example 1>

[0124] Master pellets were prepared using a twin-screw kneading extruder under the same conditions as in Example 1 except that the propylene resin E:MCT=100:25 (parts by mass).

[0125] <Comparative Example 2>

[0126] Master pellets were prepared using a twin-screw kneading extruder under the same conditions as in Example 1 except that the propylene resin F:MCT=100:25 (parts by mass).

[0127] <Comparative Example 3>

[0128] Master pellets were prepared using a twin-screw kneading extruder under the same conditions as in Example 1 except that the propylene resin G:MCT=100:25 (parts by mass).

[0129] <Comparative Example 4>

[0130] Master pellets were prepared using a twin-screw kneading extruder under the same conditions as in Example 1 except that the ratio of propylene resin C:MCT was 100:43 (parts by mass).

[0131] For the master pellets prepared in Examples 1 to 8 and Comparative Examples 1 to 4, the melting point Tm and the crystallization temperature Tc were measured by DSC, and the degree of supercooling (Tm-Tc) was calculated. In addition, the oozing amount was measured, and the results are shown in Table 1. In Examples 1 to 8, the results of the evaluation of the surface oozing amount of the master pellets show that the surface oozing of the blended non-volatile liquid can be suppressed compared to Comparative Examples 1 to 4.

[0132] In addition, polarizing microscope photographs of the masterbatch of Example 1 and Comparative Example 1 under crossed Nikkor prisms are shown in Figure 1 and Figure 2 .

[0133] [Table 1]

[0134]

[0135]

Claims

1. A masterbatch, It is characterized in that The masterbatch is a masterbatch in which a non-volatile liquid having a boiling point higher than 200° C. is dispersed in a matrix resin including a propylene resin. The masterbatch contains a nucleating agent, and in DSC measurement, after heat treatment at 200°C for 5 minutes, when cooled to -50°C at a temperature drop rate of 10°C / min, the crystallization temperature Tc represented as the peak top temperature of the exothermic peak observed on the highest temperature side; and the melting point Tm represented as the peak top temperature of the melting peak observed on the highest temperature side when heated from -50°C to 200°C at a temperature increase rate of 10°C / min, satisfy the temperature conditions represented by the following formula: Tm<159℃, Tc≥97℃, Tm-Tc<49℃, The propylene resin is a random polypropylene having an MFR at 230° C. of 0.1 g / 10 min or more and less than 26 g / 10 min.

2. The masterbatch according to claim 1, in, The temperature condition satisfies the following formula: Tm-Tc<42℃.

3. The masterbatch according to claim 1, in, After storage for 60 days in an environment of 22° C. and 60% RH, the amount of the nonvolatile liquid exuded from the surface per 1 g of the masterbatch was 20 mg or less.

4. The masterbatch according to claim 1, in, The non-volatile liquid is silicone oil, glycerol fatty acid ester or vegetable oil.