Prediction method of austenite grain boundary cracks on the surface of continuous casting billet based on as-cast structure
By introducing mixed crystal index parameters, combining the area percentage of grain equivalent circle diameter and the distribution of mixed crystal structure, the austenite grain boundary crack sensitivity on the surface of continuous casting billets is solved, and the problem of insufficient prediction in the prior art is significantly Improved prediction accuracy.
Patent Information
- Application Number
- CN202110051390.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-01-15
AI Technical Summary
The prior art has insufficient in predicting the susceptibility of austenite grain boundary cracks on the surface of continuous casting billets, and the prediction based solely on the original austenite grain size is not accurate enough, and the influence of mixed crystal structure is not fully considered.
Using the mixed crystal index parameters, the surface of continuous casting blank is cleaned and metallographic microscope observed, the area percentage of the grain equivalent circle diameter is calculated, the coarse grain region and fine grain region are divided, and the mixed crystal index is calculated, so as to judge the Grain boundary crack sensitivity.
The accuracy of judging the sensitivity of austenite grain boundary cracks in the surface of continuous casting billets was improved, from 64.1% to 97.4%, achieving accurate prediction of grain boundary crack sensitivity.
Smart Images

Figure CN114764067B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to continuous casting production technology, and more specifically to a method for predicting austenite grain boundary cracks on the surface of a continuous casting small square billet based on as-cast structure. Background Art
[0002] The grain boundary cracks on the surface of the continuous casting billet have always been an important factor affecting the surface quality of the casting billet. This type of crack always occurs along the coarse austenite grain boundaries, extends along the grain boundaries under the action of external stress, and eventually forms surface macro cracks. The coarser the size of the original austenite, the easier it is for the grain boundary cracks to occur on the surface of the continuous casting billet. That is, the coarse original austenite grains are the key factor leading to the grain boundary cracks on the surface of the continuous casting billet.
[0003] At present, the sensitivity of grain boundary cracks in continuous casting billets is mainly predicted by the critical size of the original austenite grains. When the original austenite grain size is greater than 1 mm, the crack sensitivity of the grain structure is strong, and the continuous casting billet is prone to grain boundary cracks; when the original austenite grain size is less than 1 mm, the crack sensitivity of the grain structure is weak, and the continuous casting billet is not prone to grain boundary cracks. However, through the analysis of the actual billet surface, it is found that there are grains less than 1 mm in the austenite structure at the crack, and there are also austenite grains greater than 1 mm without grain boundary cracks. This shows that there are deficiencies in predicting the sensitivity of grain boundary cracks on the surface of continuous casting billets based only on the original austenite grain size. Therefore, it is very necessary to improve the existing crack sensitivity criterion to improve the prediction accuracy of the sensitivity of grain boundary cracks on the surface of continuous casting billets.
[0004] The observation of the surface austenite structure of the continuous casting billet shows that the grain sizes are mixed and randomly distributed, the grain shapes in the structure are different, and the large grain groups are mixed with small grains, or the small grain groups are mixed with large grains, that is, the mixed crystal structure. For example, the literature "Characterisation of bimodal grain structures in HSLA steels" (DebalayChakrabarti, et al. Materials Characterization, 2007, 58: 423-438.) proposed to quantitatively characterize the mixed crystal structure by the mixed crystal index, but did not study the relationship between the mixed crystal index and austenite grain boundary cracks. Summary of the invention
[0005] In view of the above-mentioned defects existing in the prior art, the purpose of the present invention is to provide a method for predicting austenite grain boundary cracks on the surface of continuous casting small square billets based on the as-cast structure. On the basis of the existing austenite grain boundary crack criterion, a mixed crystal index parameter is introduced to achieve accurate prediction of the sensitivity of austenite grain boundary cracks on the surface of the continuous casting billet.
[0006] To achieve the above object, the present invention adopts the following technical solution:
[0007] A method for predicting austenite grain boundary cracks on the surface of a continuous casting billet based on as-cast structure comprises the following steps:
[0008] 1) cleaning the surface of the continuous casting billet and obtaining a cast microstructure image of the surface layer of the continuous casting billet through a metallographic microscope;
[0009] 2) using the grain equivalent circle diameter as the grain equivalent diameter, dividing the grain equivalent circle diameters of all grains in the field of view of the as-cast microstructure image into multiple levels in ascending order, and calculating the percentage of grain area within different levels, and plotting with the grain equivalent circle diameters of different levels as the abscissa and the corresponding grain area percentage as the ordinate, a bimodal distribution image of the mixed crystal structure can be obtained;
[0010] 3) dividing the mixed crystal structure into a coarse grain region and a fine grain region according to the bimodal distribution image in step 2), wherein the maximum value of the area percentage exists in both the coarse grain region and the fine grain region, and the peak height ratio is calculated as the mixed crystal index;
[0011] 4) Determining the grain boundary crack sensitivity according to the austenite grain size and the mixed crystal index.
[0012] Preferably, in the step 1), nitric acid is used to clean the surface of the continuous casting billet.
[0013] Preferably, in the step 2), the grain equivalent circle diameter is divided into 15 levels in ascending order.
[0014] Preferably, in step 4), the grain boundary crack sensitivity is determined as follows:
[0015] When the grain equivalent circle diameter is greater than the critical diameter of 1 mm and the mixed crystal index is greater than 0.5, grain boundary cracks are easily generated on the surface of the ingot, and the grain boundary cracks are highly sensitive;
[0016] When the grain equivalent circle diameter is greater than the critical diameter of 1 mm and the mixed crystal index is less than 0.5, it is not easy to generate grain boundary cracks on the surface of the ingot, and the grain boundary crack sensitivity is weak;
[0017] When the grain equivalent circle diameter is less than the critical diameter of 1 mm and the mixed crystal index is greater than 0.7, grain boundary cracks are easily generated on the surface of the ingot, and the grain boundary cracks are highly sensitive;
[0018] When the grain equivalent circle diameter is less than the critical diameter of 1 mm and the mixed crystal index is less than 0.7, grain boundary cracks are not easily generated on the surface of the ingot and the grain boundary crack sensitivity is weak.
[0019] The present invention provides a method for predicting austenite grain boundary cracks on the surface of a continuous casting small square billet based on the as-cast structure. The method has high accuracy, simplicity and strong applicability, and increases the accuracy of judging the sensitivity of austenite grain boundary cracks on the surface of the continuous casting billet from 64.1% to 97.4%, thereby achieving accurate prediction of the sensitivity of grain boundary cracks. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a schematic diagram of the sensitivity criterion of austenite grain boundary cracks on the surface of continuous casting billet according to the method for predicting austenite grain boundary cracks on the surface of continuous casting billet of the present invention. DETAILED DESCRIPTION
[0021] In order to better understand the above technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0022] Please combine Figure 1 As shown, the present invention provides a method for predicting austenite grain boundary cracks on the surface of a continuous casting billet based on as-cast structure, comprising the following steps:
[0023] 1) The surface of the continuous casting billet is cleaned with nitric acid alcohol, and the as-cast microstructure image of the surface layer of the continuous casting billet is obtained by metallographic microscope;
[0024] 2) Use the equivalent circular diameter of the grain (see Figure 1 The grain equivalent circle diameter (ECD) of all grains in the field of view of the as-cast microstructure image is divided into 15 levels in ascending order, and the percentage of grain area in different levels (the proportion of grain area in different levels in the total grain area) is calculated. The grain equivalent circle diameter (ECD) of different levels is used as the abscissa and the corresponding grain area percentage is used as the ordinate to draw a graph, and a bimodal distribution image of the mixed crystal structure (there are two maximum points of grain area percentage) can be obtained.
[0025] 3) According to the bimodal distribution image in step 2), the mixed crystal structure is divided into a coarse grain region and a fine grain region according to the grain equivalent circle diameter (ECD) (usually the equivalent circle diameter corresponding to the minimum grain area percentage between the bimodal distribution images is taken as the breakpoint). There are maximum values of area percentage (i.e., bimodal distribution images) in both the coarse grain region and the fine grain region. The peak height ratio is calculated to be the mixed crystal index (see Figure 1 The label PHR in the figure);
[0026] 4) According to the austenite grain size and mixed crystal index, the sensitivity of grain boundary cracks is determined as follows:
[0027] When the grain equivalent circle diameter (ECD) is greater than the critical diameter of 1 mm and the mixed crystal index (PHR) is greater than 0.5, grain boundary cracks are easily generated on the surface of the ingot, and the grain boundary crack sensitivity is strong;
[0028] When the grain equivalent circle diameter (ECD) is greater than the critical diameter of 1 mm and the mixed crystal index (PHR) is less than 0.5, it is not easy to produce grain boundary cracks on the surface of the ingot, and the sensitivity of grain boundary cracks is weak;
[0029] When the grain equivalent circle diameter (ECD) is less than the critical diameter of 1 mm and the mixed crystal index (PHR) is greater than 0.7, grain boundary cracks are prone to occur on the surface of the ingot, and the grain boundary crack sensitivity is strong;
[0030] When the grain equivalent circle diameter (ECD) is less than the critical diameter of 1 mm and the mixed crystal index (PHR) is less than 0.7, it is not easy to generate grain boundary cracks on the surface of the ingot and the sensitivity of grain boundary cracks is weak.
[0031] Under ideal conditions, the grain size is in a unimodal distribution, the mixed crystal index (PHR) is zero (peak height ratio = 0), the grain size is uniform, and the surface austenite structure of the ingot has higher high-temperature plasticity; the higher the mixed crystal index (PHR), the more serious the mixed crystals, the more uneven the grain size distribution, the worse the high-temperature plasticity of the ingot, the stronger the crack sensitivity of the ingot surface, and the easier it is to produce cracks during the continuous casting process.
[0032] The following Examples 1 to 3 are based on alloy cold heading steel continuous casting billets (brand: 10B21, SCM440, SWRCH22A, cross section 160mm×160mm) actually produced by a certain factory. By observing and analyzing the surface grain boundary cracks, surface depressions, deep vibration marks and the as-cast structure of the original austenite grains in the normal position of the cold heading steel billet, the original austenite grain size was counted and the mixed crystal index was calculated.
[0033] Example 1
[0034] 10B21 continuous casting billet
[0035] In this embodiment, 10B21 alloy cold heading steel continuous casting small square billets (specifications: cross-section 160mm×160mm) were used to observe and analyze the surface grain boundary cracks, surface depressions, deep vibration marks and the cast microstructure of the surface original austenite grains in the normal position of the cold heading steel billet, and the original austenite grain size was counted and the mixed crystal index was calculated.
[0036] Table 1 Relationship between characteristic parameters of austenite grain size and grain boundary cracks in the surface layer of ingot
[0037] Sample Maximum austenite grain size (μm) Mixed crystal index Whether there are cracks 1# 1188 0.96 have 2# 1572 1.12 have 3# 1042 0.41 none 4# 1082 0.68 have 5# 1576 1.04 have 6# 936 0.94 have 7# 865 0.51 none 8# 874 1.12 have 9# 927 0.68 none 10# 742 0.61 none
[0038] In Table 1 above, when the original austenite grain size (equivalent grain circle diameter ECD) is greater than 1 mm and the mixed crystal index (PHR) is greater than 0.5, grain boundary cracks are generated on the surface of the ingot; when the mixed crystal index is less than 0.5, no grain boundary cracks are generated. When the original austenite grain size is less than 1 mm and the mixed crystal index is greater than 0.7, grain boundary cracks are easily generated on the surface of the ingot; when the mixed crystal index is less than 0.7, no grain boundary cracks are generated on the surface of the ingot. This meets the austenite grain boundary crack sensitivity criterion proposed in the present invention.
[0039] Example 2
[0040] SCM440 continuous casting billet
[0041] In this embodiment, SCM440 alloy cold heading steel continuous casting small square billets (specifications: cross-section 160mm×160mm) are observed and analyzed for the surface grain boundary cracks, surface depressions, deep vibration marks and the cast microstructure of the surface original austenite grains in the normal position of the cold heading steel billet, and the original austenite grain size is counted and the mixed crystal index is calculated.
[0042] Table 2 Relationship between characteristic parameters of austenite grain size and grain boundary cracks in the surface layer of ingot
[0043] Sample Maximum austenite grain size (μm) Mixed crystal index Whether there are cracks 1# 1129 0.43 none 2# 1239 0.51 have 3# 1104 0.35 none 4# 1135 0.82 have 5# 668 0.32 none 6# 623 0.26 none 7# 558 0.06 none 8# 686 0.47 none 9# 794 1.33 have
[0044] In Table 2 above, when the original austenite grain size (equivalent grain circle diameter ECD) is greater than 1 mm and the mixed crystal index (PHR) is greater than 0.5, grain boundary cracks are generated on the surface of the ingot; when the mixed crystal index is less than 0.5, no grain boundary cracks are generated. When the original austenite grain size is less than 1 mm and the mixed crystal index is greater than 0.7, grain boundary cracks are easily generated on the surface of the ingot; when the mixed crystal index is less than 0.7, no grain boundary cracks are generated on the surface of the ingot. This meets the austenite grain boundary crack sensitivity criterion proposed in the present invention.
[0045] Example 3
[0046] SWRCH22A continuous casting billet
[0047] In this embodiment, SWRCH22A alloy cold heading steel continuous casting small square billet (specification: cross-section 160mm×160mm) is used to observe and analyze the surface grain boundary cracks, surface depressions, deep vibration marks and the as-cast structure of the surface original austenite grains in the normal position of the cold heading steel billet, and the original austenite grain size is counted and the mixed crystal index is calculated.
[0048] Table 3 Relationship between characteristic parameters of austenite grain size and grain boundary cracks in the surface layer of ingot
[0049] Sample Maximum austenite grain size (μm) Mixed crystal index Whether there are cracks 1# 1867 0.56 have 2# 1267 0.45 have 3# 667 1.01 have 4# 798 0.86 have 5# 886 0.47 none 6# 894 1.31 have
[0050] In Table 3 above, when the original austenite grain size (equivalent grain circle diameter ECD) is greater than 1 mm and the mixed crystal index (PHR) is greater than 0.5, grain boundary cracks are generated on the surface of the ingot; when the mixed crystal index is less than 0.5, grain boundary cracks are also generated. When the original austenite grain size is less than 1 mm and the mixed crystal index is greater than 0.7, grain boundary cracks are easily generated on the surface of the ingot; when the mixed crystal index is less than 0.7, grain boundary cracks are not generated on the surface of the ingot. This meets the austenite grain boundary crack sensitivity criterion proposed in the present invention.
[0051] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present invention, and are not intended to limit the present invention. As long as they are within the spirit of the present invention, any changes or modifications to the above embodiments will fall within the scope of the claims of the present invention.
Claims
1. A method for predicting austenite grain boundary cracks on the surface of continuous casting billet based on as-cast structure, characterized in that: The following steps are involved: 1) cleaning the surface of the continuous casting billet and obtaining a cast microstructure image of the surface layer of the continuous casting billet through a metallographic microscope; 2) using the grain equivalent circle diameter as the grain equivalent diameter, dividing the grain equivalent circle diameters of all grains in the field of view of the as-cast microstructure image into multiple levels in ascending order, and calculating the percentage of grain area within different levels, and plotting with the grain equivalent circle diameters of different levels as the abscissa and the corresponding grain area percentage as the ordinate, a bimodal distribution image of the mixed crystal structure can be obtained; 3) dividing the mixed crystal structure into a coarse grain region and a fine grain region according to the bimodal distribution image in step 2), and calculating the peak height ratio as the mixed crystal index according to the ratio of the maximum area percentage in the coarse grain region to the maximum area percentage in the fine grain region; 4) judging the grain boundary crack sensitivity according to the austenite grain size and the mixed crystal index, In the step 4), the grain boundary crack sensitivity is determined as follows: When the grain equivalent circle diameter is greater than the critical diameter of 1 mm and the mixed crystal index is greater than 0.5, grain boundary cracks are easily generated on the surface of the ingot, and the grain boundary cracks are highly sensitive; When the grain equivalent circle diameter is greater than the critical diameter of 1 mm and the mixed crystal index is less than 0.5, it is not easy to generate grain boundary cracks on the surface of the ingot, and the grain boundary crack sensitivity is weak; When the grain equivalent circle diameter is less than the critical diameter of 1 mm and the mixed crystal index is greater than 0.7, grain boundary cracks are easily generated on the surface of the ingot, and the grain boundary cracks are highly sensitive; When the grain equivalent circle diameter is less than the critical diameter of 1 mm and the mixed crystal index is less than 0.7, grain boundary cracks are not easily generated on the surface of the ingot and the grain boundary crack sensitivity is weak.
2. The method for predicting austenite grain boundary cracks on the surface of continuous casting billet based on as-cast structure according to claim 1, characterized in that: In the step 1), nitric acid is used to clean the surface of the continuous casting billet.
3. The method for predicting austenite grain boundary cracks on the surface of continuous casting billet based on as-cast structure according to claim 1, characterized in that: In the step 2), the grain equivalent circle diameter is divided into 15 levels in ascending order.
Citation Information
Patent Citations
Galvanized full-hard board cold-rolling edge crack control method in consideration of board shape
CN103801580A
Detection method of solidification dendritic structure of steel continuous casting billet
CN107014813A
Methods and systems for the quantitative measurement of internal defects in as-cast steel products
CN109983324A
WC-based cemented carbide cutting tool having excellent defect resistance and chipping resistance, and surface-coated WC-based cemented carbide cutting tool
WO2020196590A1