Curable composition
By introducing (meth)acryloyl oligomers with branched polyolefins, saturated cyclic hydrocarbons and saturated chain hydrocarbon structures into the curable composition, and utilizing the reaction of light and moisture, the curing problems in the prior art are solved. The problem of insufficient elongation properties of materials has been solved, and the electrical insulation and elongation properties have been improved.
Patent Information
- Application Number
- CN202080084775.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-12-10
AI Technical Summary
It is difficult for existing curable compositions to obtain good elongation properties under repeated high and low temperature environments, which may lead to cracks in the cured product.
A (meth)acryloyl curable oligomer containing a branched polyolefin structure, a saturated cyclic hydrocarbon structure, and a saturated chain hydrocarbon structure is used to achieve full curing through light irradiation and moisture reaction, combined with the bonding of isocyanate groups. , optimize the electrical insulation and elongation properties of the cured product.
A cured product with good electrical insulation properties and elongation properties is realized, the moisture resistance and mechanical properties of the cured product are improved, and the occurrence of cracks is avoided.
Smart Images

Figure BDA0003680487220000041 
Figure BDA0003680487220000042 
Figure BDA0003680487220000051
Abstract
Description
[0001] Cross-references to related applications
[0002] This application claims the priority of Japanese Patent Application No. 2019-225772, which is incorporated herein by reference in the description of the present application. Technical Field
[0003] The present invention relates to a curable composition that is cured by a curing treatment such as light irradiation. Background Art
[0004] Conventionally, for example, there is known a curable composition comprising a urethane resin having a hydrogenated butadiene skeleton and / or a hydrogenated isoprene skeleton, a monofunctional (meth)acrylate monomer having no ring structure and an alkyl group having 10 or less carbon atoms, and a photopolymerization initiator.
[0005] Such a curable composition is applied on an electronic circuit, for example, and cured by irradiation with light such as ultraviolet rays, and is used for covering the electronic circuit.
[0006] As such a curable composition, a curable composition in which the above-mentioned urethane resin is a specific polymer is known (for example, Patent Document 1).
[0007] In the curable composition described in Patent Document 1, the urethane resin is a polymer of an alcohol (a1) and a polyisocyanate (a2), wherein the alcohol (a1) comprises a polyol (a1-1) comprising a hydrogenated polybutadiene polyol and / or a hydrogenated polyisoprene polyol. In addition, the equivalent ratio (isocyanate group / hydroxyl group) of the isocyanate group in the polyisocyanate (a2) relative to the hydroxyl group in the alcohol (a1) is greater than 1 and is less than 8. In addition, the polyisocyanate (a2) comprises a polyisocyanate having an alicyclic structure of 2 to 6 monocyclic rings or an aromatic ring of 3 to 7 monocyclic rings in one molecule.
[0008] Regarding the curable composition described in Patent Document 1, the monofunctional (meth)acrylate monomers react with each other and polymerize with the irradiation of light such as ultraviolet rays, thereby forming a cured film. In addition, regarding the curable composition described in Patent Document 1, the isocyanate groups of the urethane resin react with each other due to moisture in the air and polymerize. Therefore, a cured film cured by both light irradiation and moisture can be obtained.
[0009] The curable composition described in Patent Document 1 can provide a cured film having a certain degree of electrical insulation.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application Publication No. 2017-179171 Summary of the invention
[0013] Problem that the invention aims to solve
[0014] However, it is difficult to obtain a cured film (cured product) having good elongation performance from the curable composition described in Patent Document 1. If the elongation performance of the cured product is insufficient, the cured product may crack under repeated high and low temperature conditions.
[0015] In view of the above problems and the like, an object of the present invention is to provide a curable composition capable of obtaining a cured product having both good electrical insulation performance and good elongation performance.
[0016] Solutions for solving problems
[0017] In order to solve the above-mentioned problems, the curable composition of the present invention is characterized in that it contains:
[0018] A curable oligomer having a branched polyolefin structure and a (meth)acryloyl group in the molecule;
[0019] A saturated cycloalkyl (meth)acrylate monomer having a saturated cyclic hydrocarbon structure and a (meth)acryloyl group in the molecule; and
[0020] A saturated chain alkyl (meth)acrylate monomer having a saturated chain hydrocarbon structure and a (meth)acryloyl group in the molecule.
[0021] In the curable composition of the present invention, the saturated chain alkyl (meth)acrylate monomer is preferably a saturated branched alkyl (meth)acrylate monomer having a saturated branched hydrocarbon structure and a (meth)acryloyl group in the molecule.
[0022] In the curable composition of the present invention, the saturated chain alkyl (meth)acrylate monomer is preferably a (meth)acrylate monomer having a saturated chain hydrocarbon having 9 to 12 carbon atoms.
[0023] The curable composition of the present invention preferably further contains an isocyanate monomer having one or more isocyanate groups in the molecule.
[0024] In the curable composition of the present invention, the ratio of the saturated cycloalkyl (meth)acrylate monomer to 100 parts by mass of the total mass of the saturated cycloalkyl (meth)acrylate monomer and the saturated linear alkyl (meth)acrylate monomer is preferably 70 parts by mass or more and 95 parts by mass or less. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a figure which shows the IR spectrum analyzed by FT-IR. DETAILED DESCRIPTION
[0026] Hereinafter, one embodiment of the curable composition of the present invention will be described.
[0027] The curable composition of this embodiment includes:
[0028] A curable oligomer having a branched polyolefin structure and a (meth)acryloyl group in the molecule;
[0029] A saturated cycloalkyl (meth)acrylate monomer having a saturated cyclic hydrocarbon structure and a (meth)acryloyl group in the molecule; and
[0030] A saturated chain alkyl (meth)acrylate monomer having a saturated chain hydrocarbon structure and a (meth)acryloyl group in the molecule.
[0031] According to the curable composition, a cured product having both good electrical insulation performance and good elongation performance can be obtained.
[0032] The curable oligomer is not particularly limited as long as it is a compound having a branched polyolefin structure and at least one (meth) acryloyl group in the molecule. In the present embodiment, the curable oligomer has a branched polyolefin structure, a (meth) acryloyl group and an isocyanate group in the molecule. Hereinafter, the curable oligomer is described in detail.
[0033] The curable oligomer contained in the curable composition has a (meth)acryloyl group in the molecule. In addition, the (meth)acrylic acid saturated cycloalkyl ester monomer and the (meth)acrylic acid saturated chain alkyl ester monomer contained in the curable composition both have a (meth)acryloyl group in the molecule. Therefore, if irradiated with light such as ultraviolet rays, the curable composition is polymerized (curing reaction) by polymerization reactions such as free radical polymerization, and thus a fully cured cured product can be obtained.
[0034] In addition, the curable oligomer further includes a substance having at least one isocyanate group (-NCO) in the molecule. Thus, the -NCO groups of the curable oligomers react with each other through moisture in the air, and the curable oligomers bond with each other. The curing of the curable composition is also carried out through this bonding, so a fully cured cured product can be obtained.
[0035] As described above, the curable composition of the present embodiment can be cured by light, and when the curable oligomer has a -NCO group in the molecule, it can be sufficiently cured by moisture.
[0036] Furthermore, since the curable composition of the present embodiment contains a saturated cycloalkyl (meth)acrylate monomer having a saturated cyclic hydrocarbon structure in the molecule, the curable composition can have sufficient moisture resistance after curing.
[0037] Furthermore, since the curable composition of the present embodiment contains a saturated chain alkyl (meth)acrylate monomer having a saturated chain hydrocarbon structure in the molecule, the cured product can have sufficient elongation performance.
[0038] It should be noted that the curable oligomer preferably does not have both a benzene ring structure (aromatic hydrocarbon composed of 6 cyclic carbon atoms) and a saturated cyclic hydrocarbon structure in the molecule.
[0039] Examples of the curable oligomer include compounds represented by the following general formula (1).
[0040]
[0041] [In the general formula (1), X represents a branched polyolefin structure, and Y' and Y" each represent any one of the following general formulas (a) to (d).
[0042] In each of the general formulas (a) to (d), Z 1 , Z 2 Each independently represents a molecular structure represented by the following general formula (α) or -NCO, and two Zs among Y' and Y" 1 and 2 Z 2 At least one of them is a molecular structure represented by the following general formula (α).]
[0043]
[0044] [In the general formula (a), R a1 , R a2 , R a3 Each independently represents an organic group, Z 1 , Z 2 As above.]
[0045]
[0046] [In the general formula (b), R b1 , R b2 , R b3 , R c Each independently represents an organic group, Z 1 , Z 2 As above.]
[0047]
[0048] [In general formula (c), R d1 , Rd2 , R d3 Each independently represents an organic group, Z 1 , Z 2 As above.]
[0049]
[0050] [In the general formula (d), R e1 , R e2 , R e3 Each independently represents an organic group, Z 1 , Z 2 As above.]
[0051]
[0052] [In the general formula (α), Q represents a saturated hydrocarbon group having 2 to 4 carbon atoms, and M represents H or CH3.]
[0053] In the general formula (1), X is a branched polyolefin structure. The polyolefin in this part is preferably a saturated polyolefin. That is, the polyolefin in X is preferably a branched saturated polyolefin. Examples of the branched saturated polyolefin include hydrogenated polybutadiene.
[0054] The molecular weight of the polyolefin structure in the general formula (1) is preferably 1000 or more and 6000 or less. By making the molecular weight 1000 or more, the mechanical properties of the cured product can be further suppressed from being reduced. In addition, by making the molecular weight 6000 or less, the cured product can be further suppressed from being phase-separated and becoming non-uniform.
[0055] The molecular weight of the polyolefin structure can be determined from a standard polystyrene conversion value measured by GPC (gel permeation chromatography) before synthesizing the curable oligomer of the general formula (1).
[0056] In the general formula (1), Y' and Y" each include an isocyanurate, adduct or biuret structure of an aliphatic diisocyanate having 6 to 10 carbon atoms in total. For example, in other words, Z is removed from the structure represented by the general formula (a). 1 and Z 2 The part after is the above isocyanurate structure, which is obtained by removing Z from the structure shown in general formula (b). 1 and Z 2 The part after is the above-mentioned adduct structure, and Z is removed from the structure shown in general formula (c) or (d). 1 and Z 2 The latter part is a biuret structure.
[0057] The aliphatic diisocyanate having a total carbon number of 6 to 10 before forming the above-mentioned isocyanurate body, adduct body or biuret body structure has an isocyanate group at both ends of a linear alkylene group having 4 to 8 carbon atoms. Y' and Y" are composed of, for example, an isocyanurate body, an adduct body or a biuret body structure of an aliphatic diisocyanate, and therefore, do not include both a benzene ring structure and a saturated cyclic hydrocarbon structure (a saturated structure in which the ring consists only of carbon atoms).
[0058] By making Y' and Y" consist of an isocyanurate, adduct or biuret structure of an aliphatic diisocyanate, Y' and Y" do not have both a benzene ring structure and a cycloalkyl structure, and the above-mentioned curable oligomer does not have both a benzene ring structure and a cycloalkyl structure in the molecule. Corresponding to the fact that Y' and Y" do not have both a benzene ring structure and a cycloalkyl structure, the moisture resistance or weather resistance of the cured product after curing becomes good.
[0059] Examples of the aliphatic diisocyanate having 6 to 10 total carbon atoms include hexamethylene diisocyanate (HMDI) and the like.
[0060] The above-mentioned isocyanurate is a trimer of the above-mentioned aliphatic diisocyanate. For example, the structure after removing the terminal -NCO of the trimer is equivalent to removing Z from the general formula (a). 1 and Z 2 The structure after.
[0061] The adduct is a reaction product of the aliphatic diisocyanate and a triol having 3 to 6 carbon atoms. For example, the structure after the terminal -NCO of the reaction product is removed is equivalent to removing Z from the general formula (b). 1 and Z 2 The structure after.
[0062] The triol having 3 to 6 carbon atoms contains only carbon (C), oxygen (O) and hydrogen (H) as elements. Examples of the triol having 3 to 6 carbon atoms include trimethylolpropane (CH3-CH2-C(CH2-OH)3) and glycerol.
[0063] The biuret is a reaction product of the aliphatic diisocyanate and water or a tertiary alcohol. For example, the structure of the inner portion of the terminal -NCO of the reaction product is equivalent to removing Z from the general formula (c) or the general formula (d). 1 and Z 2 The structure after.
[0064] It should be noted that in the general formula (1), Y' and Y" may have the same molecular structure or different molecular structures.
[0065] In the general formulas (a) to (d), R a1 ~R a3, R b1 ~R b3 , R c , R d1 ~R d3 , R e1 ~R e3 is an organic group containing at least carbon atoms. a1 ~R a3 , R b1 ~R b3 , R c , R d1 ~R d3 , R e1 ~R e3 It may contain a urea bond, a biuret bond or an allophanate bond. a1 ~R a3 , R b1 ~R b3 , R d1 ~R d3 , R e1 ~R e3 It is preferably a saturated hydrocarbon having 4 to 8 carbon atoms, more preferably a linear saturated hydrocarbon having 6 carbon atoms, and may contain heteroatoms (N, O, S, P, etc.) and may have a branched structure. c It is preferably a saturated hydrocarbon having 4 to 8 carbon atoms, and preferably a branched saturated hydrocarbon having 6 carbon atoms. It may contain a heteroatom (N, O, S, P, etc.) and may have a linear structure.
[0066] In the general formulas (a) to (d), Z 1 , Z 2 Each independently represents the molecular structure represented by the above general formula (α) or -NCO. 1 and 2 Z 2 At least one of them is a molecular structure represented by the above general formula (α). In other words, the curable oligomer represented by the general formula (1) has at least one molecular structure represented by the general formula (α) in the molecule.
[0067] Preferred is: 2 Z 1 and 2 Z 2 At least one (a part) of them is the molecular structure represented by the above general formula (α), and at least one (all the remaining) is -NCO. In other words, the curable oligomer represented by general formula (1) preferably has at least one molecular structure represented by general formula (α) and at least one -NCO in the molecule.
[0068] It should be noted that the two Z 1 and 2 Z 2All of them may be molecular structures represented by the above general formula (α). In other words, the curable oligomer represented by the general formula (1) may have four molecular structures represented by the general formula (α) in the molecule and may not have -NCO.
[0069] In the general formula (1), Z 1 , Z 2 They may be the same or different from each other. In the general formula (1), Y' and Y" each include Z 1 and Z 2 Therefore, there are two Z in the general formula (1) 1 , and there are 2 Z 2 . 2 Z 1 They can be the same or different. 2 In other words, 2 Z 1 and 2 Z 2 Each is individually and independently defined.
[0070] In the general formula (α), the saturated hydrocarbon group having 2 to 4 carbon atoms in Q is preferably a linear saturated hydrocarbon group. In other words, Q is preferably a linear saturated hydrocarbon group having 2 to 4 carbon atoms. The saturated hydrocarbon group in Q preferably has 2 carbon atoms.
[0071] Examples of the curable oligomer represented by the general formula (1) include compounds represented by the following general formulae (1a) to (1f).
[0072]
[0073] [Among them, R a1 , R a2 , R a3 Each independently represents an organic group, preferably a linear saturated hydrocarbon having 4 to 8 carbon atoms, p is 20 to 300, and M is each independently H or CH3.]
[0074]
[0075] [Among them, R a1 , R a2 , R a3 Each independently represents an organic group, preferably a linear saturated hydrocarbon having 4 to 8 carbon atoms, p is 20 to 300, and M is each independently H or CH3.]
[0076]
[0077] [Among them, R a1 , R a2 , R a3Each independently represents an organic group, preferably a linear saturated hydrocarbon having 4 to 8 carbon atoms, p is 20 to 300, and M is each independently H or CH3.]
[0078]
[0079] [Among them, R b1 , R b2 , R b3 Each independently represents an organic group, preferably a linear saturated hydrocarbon having 4 to 8 carbon atoms, p is 20 to 300, and M is each independently H or CH3.]
[0080]
[0081] [Among them, R b1 , R b2 , R b3 Each independently represents an organic group, preferably a linear saturated hydrocarbon having 4 to 8 carbon atoms, p is 20 to 300, and M is each independently H or CH3.]
[0082]
[0083] [Among them, R b1 , R b2 , R b3 Each independently represents an organic group, preferably a linear saturated hydrocarbon having 4 to 8 carbon atoms, p is 20 to 300, and M is each independently H or CH3.]
[0084] As the molecular structure represented by the general formula (α), the molecular structure represented by the following formula (α-1) is preferred. By using the molecular structure represented by the following formula (α-1), the ethylene group has a small steric hindrance, and there is an advantage of increasing the polymerization rate based on irradiation with ultraviolet rays, etc. It should be noted that if the number of carbon atoms of Q in the general formula (α) is 1 (i.e., methylene), it is easy to decompose during curing.
[0085]
[0086] The curable composition of the present embodiment contains, for example, a branched polyolefin diol (hereinafter also simply referred to as <Component A>), at least one selected from isocyanurate bodies, adducts, and biuret bodies of aliphatic diisocyanates having a total carbon atom number of 6 to 10 (hereinafter also simply referred to as <Component B>), and a urethanization reaction product of a (meth)acrylic acid hydroxy-saturated C1-C4 alkyl ester (hereinafter also simply referred to as <Component C>). In other words, the curable composition of the present embodiment contains, for example, a curable oligomer obtained by at least subjecting <Component A>, <Component B>, and <Component C> to a urethanization reaction, the above-mentioned (meth)acrylic acid saturated cycloalkyl ester monomer, and the above-mentioned (meth)acrylic acid saturated linear alkyl ester monomer.
[0087] The above-mentioned curable oligomer is a part of the urethanization reaction product of at least <Component A>, <Component B>, and <Component C>. In other words, the above-mentioned curable oligomer can be obtained by at least subjecting <Component A>, <Component B>, and <Component C> to a urethanization reaction.
[0088] For example, in the curable composition of the present embodiment, as the above-mentioned urethanization reaction product, at least the curable oligomer represented by the above general formula (1) is contained. In addition, in the curable composition of the present embodiment, in addition to the curable oligomer represented by the above general formula (1), by-products generated by the urethanization reaction are also contained.
[0089] In addition, the curable composition of the present embodiment further contains a trace amount of a urethanization reaction catalyst compounded for the urethanization reaction. It should be noted that details of the urethanization reaction product will be described later.
[0090] Since the curable composition of the present embodiment contains at least the curable oligomer represented by the above general formula (1), it can be cured by light as described above.
[0091] When the curable oligomer still has an -NCO group, the curable composition of the present embodiment can be sufficiently cured not only by light but also by moisture.
[0092] In addition, the curable composition of the present embodiment further contains by-products generated by the above-mentioned urethanization reaction, and these by-products can also undergo a curing reaction by light irradiation or moisture. Therefore, it can be sufficiently cured not only by light but also by moisture.
[0093] <Component A>
[0094] Component A is a branched polyolefin diol. The polyolefin diol has hydroxyl groups at both molecular ends. The olefin part does not contain polar groups such as ether groups and ester groups and is composed only of saturated hydrocarbons.
[0095] Examples of Component A include polypropylene glycol, polybutylene glycol (hydrogenated 1,2-polybutadiene glycol), hydrogenated polyisoprene glycol, etc. From the viewpoint of being able to impart sufficient mechanical flexibility to the cured product (coating film), polybutylene glycol (hydrogenated 1,2-polybutadiene glycol) is preferred as Component A.
[0096] The molecular weight of Component A is preferably 1000 or more and 6000 or less.
[0097] <Component B>
[0098] Component B is a polyisocyanate and is at least one selected from among isocyanurate bodies, adducts, and biuret bodies of aliphatic diisocyanates having 6 to 10 total carbon atoms. Component B has 3 or 4 isocyanate groups in the molecule. Component B preferably does not have both a benzene ring structure (aromatic ring structure) and a saturated cyclic hydrocarbon structure (saturated ring structure in which the ring is composed only of carbon atoms) in the molecule.
[0099] The isocyanurate body of Component B is, for example, a trimer of the above-mentioned hexamethylene diisocyanate (HMDI) and has 3 isocyanate groups in the molecule.
[0100] The adduct of Component B is, for example, a reaction product of trimethylolpropane and an aliphatic diisocyanate having 6 to 10 total carbon atoms (such as the above-mentioned HMDI). This adduct has 3 isocyanate groups in the molecule.
[0101] As Component B, from the viewpoints of good weather resistance after curing due to the absence of a benzene ring and good solubility in a diluent when a diluent coexists in the urethanization reaction, an adduct obtained by reacting hexamethylene diisocyanate (HMDI) with trimethylolpropane or an isocyanurate body (trimer) of hexamethylene diisocyanate (HMDI) is preferred.
[0102] <Component C>
[0103] Component C is a C1 - C4 saturated alkyl ester of (meth)acrylic acid and has 1 hydroxyl group bonded to any carbon in the alkyl part. Component C is preferably a C2 - C3 saturated alkyl ester of (meth)acrylic acid having a hydroxyl group.
[0104] Examples of Component C include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, etc. From the viewpoint of better polymerizability based on light irradiation, Component C is preferably 2-hydroxyethyl (meth)acrylate, and more preferably 2-hydroxyethyl acrylate.
[0105] The molar ratio of the component B to the component A in the urethanization reaction is preferably 2.0 or more and 2.5 or less, and more preferably 2.0 or more and 2.2 or less.
[0106] The molar ratio of the component C to the component B in the urethanization reaction is preferably 0.5 or more and 2.0 or less, and more preferably 0.5 or more and 1.5 or less.
[0107] The molar ratio of the component C to the component A in the urethanization reaction is preferably 1.0 or more and 4.0 or less, and more preferably 1.0 or more and 3.0 or less.
[0108] <Urethane Reaction Catalyst>
[0109] As the urethanization reaction catalyst, an organic tin catalyst such as dibutyltin dilaurate or stannous octoate, or a metal catalyst such as an acetylacetone complex catalyst can be used. In addition, a tertiary amine catalyst can be used as the urethanization reaction catalyst.
[0110] The curable composition (curing composition) of the present embodiment includes a urethanization reaction product generated by a urethanization reaction in the presence of the A component, the B component, and the C component.
[0111] Examples of the urethanization reaction product include compounds represented by the general formula (1) such as the general formulas (1a) to (1f).
[0112] Furthermore, examples of the urethanization reaction product include a compound having only an isocyanate group as a reactive group and a compound having only a hydroxyl group as a reactive group.
[0113] From another viewpoint, examples of the above-mentioned carbamate reaction product include: a compound which is a carbamate reaction product of component A and component B and in which component C is not introduced into the molecule; a compound which is a carbamate reaction product of component B and component C and in which component A is not introduced into the molecule; and the like.
[0114] The curable composition of the present embodiment further includes a photopolymerizable monomer that does not undergo a urethanization reaction. The photopolymerizable monomer that does not undergo a urethanization reaction, for example, does not have active hydrogen in the molecule. Such a photopolymerizable monomer may be blended as a diluent before the urethanization reaction in order to reduce the viscosity in the urethanization reaction system, or may be blended after the urethanization reaction.
[0115] Specifically, the curable composition of the present embodiment contains at least the following two monomers as photopolymerizable monomers that do not undergo urethanization reaction. These monomers are compounds that generate polymerization reaction products upon light irradiation.
[0116] Examples of the two monomers include a saturated cycloalkyl (meth)acrylate monomer having a saturated cyclic hydrocarbon structure and a (meth)acryloyl group in the molecule, and a saturated chain alkyl (meth)acrylate monomer having a saturated chain hydrocarbon structure and a (meth)acryloyl group in the molecule.
[0117] The saturated cycloalkyl (meth)acrylate monomer is preferably an esterified compound of a monohydric alcohol containing a saturated cyclic hydrocarbon structure (a structure of a cyclic portion formed only by carbon atoms) and (meth)acrylic acid. The number of carbon atoms of the monohydric alcohol containing a saturated cyclic hydrocarbon structure is preferably 8 or more and 15 or less. The saturated cycloalkyl (meth)acrylate monomer preferably does not contain a benzene ring, an ether bond (-CH2-O-CH2-), a polar group such as an -OH group and a -COOH group in the molecule. The saturated cycloalkyl (meth)acrylate monomer is preferably a monofunctional monomer having one (meth)acrylate group in the molecule. In the saturated cycloalkyl (meth)acrylate monomer, the saturated cyclic hydrocarbon structure may be a structure that does not contain heteroatoms and forms a carbon ring with 4 to 8 carbon atoms. The saturated cycloalkyl (meth)acrylate monomer may be monocyclic, bicyclic, or polycyclic. The bicyclic or polycyclic saturated cyclic hydrocarbon structure may share more than 2 carbon atoms. In the saturated cycloalkyl (meth)acrylate monomer, the carbon of the saturated cyclic hydrocarbon structure may be further bonded with a methyl group or an ethyl group.
[0118] As the saturated cycloalkyl (meth)acrylate monomer, one containing a norbornane structure is preferred.
[0119] Specifically, examples of the saturated cycloalkyl (meth)acrylate monomer include isobornyl (meth)acrylate (containing a norbornane structure), dicyclopentanyl (meth)acrylate, adamantyl (meth)acrylate, tricyclodecane (meth)acrylate, dicyclopentadienyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, morpholine (meth)acrylate, and dicyclopentanyl di(meth)acrylate.
[0120] When the curable composition contains a saturated cycloalkyl (meth)acrylate monomer, the saturated cycloalkyl (meth)acrylate monomer can dissolve the curable oligomer more fully in the curable composition.
[0121] The saturated chain alkyl (meth)acrylate monomer is preferably a (meth)acrylate monomer having 11 or more and 19 or less carbon atoms (a saturated chain hydrocarbon having 8 or more and 15 or less carbon atoms) in the molecule, and more preferably a (meth)acrylate monomer having 12 or more and 16 or less carbon atoms (a saturated chain hydrocarbon having 9 or more and 12 or less carbon atoms) in the molecule. Such a monomer has a high and stable flash point and good handling properties. The saturated chain alkyl (meth)acrylate monomer preferably does not contain a benzene ring, an ether bond (-CH2-O-CH2-), a polar group such as an -OH group and a -COOH group in the molecule. The saturated chain alkyl (meth)acrylate monomer is preferably a monofunctional monomer having one (meth)acrylate group in the molecule. In the saturated chain alkyl (meth)acrylate monomer, the saturated chain hydrocarbon structure may be a saturated chain hydrocarbon structure that does not contain atoms other than C and H and is composed of 7 to 11 carbon atoms.
[0122] By including a saturated linear alkyl (meth)acrylate monomer in the curable composition, the flexibility of a cured product obtained by curing the curable composition can be further improved.
[0123] In the saturated chain alkyl (meth)acrylate monomer, the saturated chain hydrocarbon structure may be linear or branched. In other words, the saturated chain hydrocarbon structure may be a saturated linear hydrocarbon structure or a saturated branched hydrocarbon structure. In further other words, the saturated chain alkyl (meth)acrylate monomer may be a saturated linear alkyl (meth)acrylate monomer or a saturated branched alkyl (meth)acrylate monomer.
[0124] As a (meth) acrylic acid saturated chain alkyl ester monomer, from the viewpoint of being able to more fully dissolve the above-mentioned curable oligomer in the curable composition, it is preferably a (meth) acrylic acid saturated branched alkyl ester monomer. Thus, the (meth) acrylic acid saturated chain alkyl ester monomer has a saturated branched alkyl group, and therefore, in the curable composition, the compatibility with the curable oligomer having a branched polyolefin structure is improved. Therefore, the uniformity of the curable composition is further improved, and therefore, a more uniform cured film can be obtained without being affected by the substrate supporting the cured product, the thickness of the cured product, or the curing reaction conditions.
[0125] In the curable composition of the present embodiment, the ratio of the saturated cycloalkyl (meth)acrylate monomer to 100 parts by mass of the total mass of the saturated cycloalkyl (meth)acrylate monomer and the saturated linear alkyl (meth)acrylate monomer is preferably 70 parts by mass or more and 95 parts by mass or less.
[0126] This makes it possible to obtain a cured product having both electrical insulation performance and elongation performance in a better balance.
[0127] The hydrocarbon structure of the saturated linear alkyl (meth)acrylate monomer may be a saturated linear alkyl structure.
[0128] Specifically, examples of the saturated linear alkyl (meth)acrylate monomer include n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, and n-decyl (meth)acrylate.
[0129] The hydrocarbon structure of the saturated branched alkyl (meth)acrylate monomer may be any saturated branched alkyl structure, and may be an iso-structure, a secondary structure, a neo-structure, or a tertiary structure.
[0130] Specifically, examples of the saturated branched alkyl (meth)acrylate monomer include isoheptyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.
[0131] The saturated branched alkyl (meth)acrylate monomer is preferably at least one of isononyl (meth)acrylate and isodecyl (meth)acrylate from the viewpoint of better solubility in the curable oligomer and the viewpoint of easily obtaining a more uniform cured film.
[0132] The curable composition of the present embodiment may contain unreacted components A, B, and C that have not undergone urethanization reaction. The curable composition of the present embodiment may contain a urethanization reaction catalyst blended to promote urethanization reaction.
[0133] As such, the curable composition of the present embodiment contains various reaction products and unreacted products. However, the molecular structure of the compound before the urethanization reaction is determined, and the product brought about by the urethanization reaction can be fully predicted. Therefore, the molecular structure of the reaction product (main reactant, side reactant) can be fully predicted. However, it can be said that it is basically impractical to determine the molecular structure of the compound other than the main reaction product. In other words, it can be said that the compounds contained in the curable composition of the present embodiment involve multiple types, and therefore, it is basically impractical to directly determine all the structures or characteristics of these compounds separately.
[0134] The curable composition of the present embodiment may contain a photopolymerizable monomer further added after the urethanization reaction, an isocyanate monomer having one or more isocyanate groups in the molecule, a photopolymerization initiator, etc. Examples of the photopolymerizable monomer include the above-mentioned saturated cycloalkyl (meth)acrylate monomer and saturated linear alkyl (meth)acrylate monomer, and other photopolymerizable monomers other than these (which do not undergo urethanization reaction).
[0135] As other photopolymerizable monomers that do not undergo urethanization reaction, for example, monofunctional (meth)acrylate monomers and polyfunctional (meth)acrylate monomers described below may be mentioned.
[0136] Examples of the monofunctional (meth)acrylate monomer include phenoxyethyl (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, benzyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, tridecyl (meth)acrylate, and ethoxydiethylene glycol (meth)acrylate.
[0137] Examples of the polyfunctional (meth)acrylate monomer include neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, polypropylene glycol di(meth)acrylate, ethylene oxide-modified bisphenol A di(meth)acrylate, ethylene oxide-modified trimethylolpropane tri(meth)acrylate, ethylene oxide-modified pentaerythritol tetra(meth)acrylate, tris[(meth)acryloyloxyethyl]isocyanurate, ethylene oxide-modified dipentaerythritol hexa(meth)acrylate, and epoxy (meth)acrylate.
[0138] These monomers may be used alone or in combination of two or more.
[0139] From the viewpoint of improving the weather resistance of the cured product after curing, the photopolymerizable monomer is preferably a monomer not containing a benzene ring, an ether bond (-CH2-O-CH2-), a polar group such as an -OH group and a -COOH group.
[0140] By adding the above-mentioned isocyanate monomer to the curable composition of the present embodiment, the elongation performance of the cured product can be further improved.
[0141] Examples of the isocyanate monomer added after the urethanization reaction include aromatic diisocyanate monomers, alicyclic diisocyanate monomers, aliphatic diisocyanate monomers, etc. These monomers may have one isocyanate group in the molecule or may have a plurality of (eg, 2 to 4) isocyanate groups in the molecule.
[0142] Examples of the aromatic diisocyanate monomer include various monomers such as tolylene diisocyanate, diphenylmethane diisocyanate, diphenylpropane diisocyanate, triphenylmethane diisocyanate, phenylene diisocyanate, xylylene diisocyanate, naphthalene diisocyanate, and tolidine diisocyanate.
[0143] Examples of the alicyclic diisocyanate monomers include hydrogenated toluene diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, cyclohexylene diisocyanate, 3-isocyanate methyl-3,5,5-trimethylcyclohexyl isocyanate (isophorone diisocyanate), 3-isocyanate ethyl-3,5,5-trimethylcyclohexyl isocyanate, and various other monomers.
[0144] As an aliphatic diisocyanate monomer, a hexamethylene diisocyanate monomer etc. are mentioned, for example.
[0145] It should be noted that the isocyanate monomer may be an adduct, a biuret form, an isocyanurate form, or a polymer of at least any one of the above-mentioned monomers.
[0146] These monomers may be used alone or in combination of two or more.
[0147] As the isocyanate monomer, a monomer containing no benzene ring and no unsaturated bond is preferred from the viewpoint of further improving the weather resistance of the cured product after curing.
[0148] In addition, the curable composition of the present embodiment preferably does not contain a compound having a benzene ring (aromatic hydrocarbon composed of 6 cyclic carbon atoms) in the molecule as a urethanization reaction product (curable oligomer), a photopolymerizable monomer, or an isocyanate monomer.
[0149] The photopolymerization initiator is not particularly limited as long as it is a compound that generates free radicals by irradiated light (ultraviolet rays, etc.). Examples of the photopolymerization initiator include acetophenone-based photoinitiators, benzoin-based photoinitiators, benzophenone-based photoinitiators, thioxanthone-based photoinitiators, and acylphosphine oxide-based photoinitiators.
[0150] As the photopolymerization initiator, a commercially available product can be used.
[0151] In addition, the curable composition of this embodiment may contain a photosensitizer, a polymerization inhibitor, an antioxidant, a dye, a pigment, a fluorescent substance, etc. as needed.
[0152] The curable composition of the present embodiment preferably contains 10% by mass or more of the compound represented by the general formula (1). This allows the composition to be cured more fully by both light and moisture.
[0153] In addition, the curable composition of this embodiment may contain 90 mass % or less of the curable oligomer represented by general formula (1).
[0154] The curable composition of the present embodiment may contain 10% by mass or more of a photopolymerizable monomer (which does not undergo urethanization reaction) such as a saturated cycloalkyl (meth)acrylate monomer or a saturated linear alkyl (meth)acrylate monomer, or may contain 85% by mass or less.
[0155] The curable composition of the present embodiment may contain 2% by mass or more of an isocyanate monomer other than the curable oligomer, or may contain 20% by mass or less.
[0156] Next, one embodiment of the method for producing the curable composition of the present invention will be described.
[0157] In the method for producing a curable composition of the present embodiment, a curable composition including a reaction product of the urethanization reaction is produced by, for example, carrying out a urethanization reaction between a branched polyolefin diol (the above-mentioned component A) and at least one selected from isocyanurate forms, adduct forms and biuret forms of aliphatic diisocyanates having a total carbon number of 6 to 10 (the above-mentioned component B) and a (meth)acrylic acid hydroxy saturated C1 to C4 alkyl ester (the above-mentioned component C).
[0158] Specifically, the method for producing a curable composition according to the present embodiment comprises a reaction step of synthesizing a urethanization reaction product including the curable oligomer by a urethanization reaction in the presence of the components A, B and C and a urethanization reaction catalyst.
[0159] The method for producing a curable composition according to the present embodiment further includes an adding step of adding a photopolymerizable monomer, an isocyanate monomer, and a photopolymerization initiator after the reaction step.
[0160] The component A, component B, component C and the urethanization reaction catalyst used in the reaction step are as described above.
[0161] In the above-mentioned production method, in order to prevent reaction with moisture, the reaction step is usually carried out after replacing the air in the reaction container with nitrogen.
[0162] In the reaction step, general reaction conditions suitable for the urethanization reaction can be adopted. Preferably, in the reaction step, the urethanization reaction is carried out by maintaining the temperature at 50 to 70° C. for 0.5 to 3 hours.
[0163] In the reaction step, a preferred ratio (molar ratio) of the amounts of component A, component B, and component C is as described above.
[0164] In the reaction step, a compound that does not participate in the urethanization reaction may coexist, and the compound generates a polymerization reaction product by light irradiation. As described above, the compound may include photopolymerizable monomers such as a saturated cycloalkyl (meth)acrylate monomer or a saturated linear alkyl (meth)acrylate monomer.
[0165] In the adding step, the above-mentioned photopolymerizable monomer, isocyanate monomer, and photopolymerization initiator may be further added after the urethanization reaction. The further added photopolymerizable monomer and isocyanate monomer have low viscosity, and therefore play a role like a solvent that dilutes the above-mentioned curable oligomer. On the other hand, they themselves are cured by light or moisture, and therefore also play a role in making the cured product more fully cured. The viscosity of the curable composition used for curing becomes lower according to the further addition of the photopolymerizable monomer and isocyanate monomer, and the process of applying the curable composition can be simplified.
[0166] In the adding step, a photosensitizer, a polymerization inhibitor, an antioxidant, a dye, a pigment, a fluorescent substance, etc. may be further blended as necessary.
[0167] The curable composition of this embodiment is used as a cured product that is cured by irradiation with ultraviolet light or the like. For example, after applying the curable composition on an electronic circuit to be covered, the composition is cured by irradiation with ultraviolet light or the like to form a covering film of the cured product. Furthermore, by leaving it in the air for several hours to several days, a curing reaction based on moisture in the air can be performed.
[0168] As the light irradiated for the curing reaction, ultraviolet rays can be used. As the light source, a high pressure mercury lamp, a metal halide lamp, a xenon lamp, a chemical lamp, an LED lamp, etc. can be used. As the irradiation intensity, for example, 10 to 10,000 mW / cm 2 .
[0169] In order to further promote the curing reaction based on moisture, the temperature of the air is preferably 20 to 40° C., and the humidity of the air is preferably 40 to 90 RH%.
[0170] As objects to be covered by applying the above-mentioned curable composition, there can be listed, for example, electronic circuits and terminals on mounting substrates used in precision instruments; electronic circuits and terminals on mounting substrates carried in automobiles, bicycles, trains, airplanes, ships, etc.; electronic circuits and terminals on mounting substrates used in mobile devices (cellular phones, digital cameras, digital video cameras, etc.); electronic circuits and terminals on substrates used in outdoor equipment (water heaters, air conditioner outdoor units, etc.); electronic circuits and terminals on mounting substrates used in water-related equipment such as washing machines, warm water flushing toilets, dishwashers and dryers, etc.
[0171] The curable composition of the present embodiment and the method for producing the composition are as exemplified above, but the present invention is not limited to the curable composition and the method for producing the composition exemplified above.
[0172] That is, various forms used in general curable compositions and methods for producing the compositions can be adopted within a range that does not impair the effects of the present invention.
[0173] Example
[0174] Next, the present invention will be described in more detail using experimental examples, but the present invention is not limited to these.
[0175] (A) to (C) are mixed to carry out urethanization reaction as follows to produce a curable composition containing a curable oligomer represented by the general formula (1).
[0176] <Raw Materials in Reaction Process>
[0177] (A) Branched polyolefin diol
[0178] (A-1) Hydrogenated polybutadiene glycol (average molecular weight 1,500)
[0179] Product name: NISSO-PB GI-1000
[0180] :Hydroxy value (KOHmg / g=67mg) Made by Nippon Soda Co., Ltd.
[0181] (A-2) Hydrogenated polybutadiene diol (average molecular weight: 2,000)
[0182] Product name: NISSO-PB GI-2000
[0183] :Hydroxy value (KOHmg / g=50mg) Made by Nippon Soda Co., Ltd.
[0184] (A-3) Hydrogenated polybutadiene diol (average molecular weight 3,100)
[0185] Product name: NISSO-PB GI-3000
[0186] :Hydroxy value (KOHmg / g=30mg) Made by Nippon Soda Co., Ltd.
[0187] (B) Derivatives of aliphatic diisocyanates having 6 to 10 total carbon atoms
[0188] (B-1) Isocyanurate derivatives of hexamethylene diisocyanate (HMDI)
[0189] Product name: DURANATE TSR-100: Isocyanate group content 20.4%, manufactured by Asahi Kasei Corporation
[0190] (B-2) Isocyanurate derivatives of hexamethylene diisocyanate (HMDI)
[0191] Product name: DURANATE TPA-100: Isocyanate group content 23.0%, manufactured by Asahi Kasei Corporation
[0192] (C) (Meth) Acrylic Acid Hydroxy Saturated C1-C4 Alkyl Ester
[0193] ·2-Hydroxyethyl acrylate (abbreviated as: HEA, commercial product)
[0194] (other)
[0195] · Photopolymerizable monomer (reaction solvent / diluent) (Isobornyl acrylate abbreviation: IBXA commercial product)
[0196] Carbamate reaction catalyst (commercially available dibutyltin dilaurate)
[0197] <Raw materials in the addition process>
[0198] Photopolymerizable monomer: (meth) acrylate saturated cycloalkyl ester monomer
[0199] (Isobornyl acrylate abbreviation: IBXA commercial product)
[0200] Photopolymerizable monomer: (meth)acrylic acid saturated chain (saturated branched) alkyl ester monomer
[0201] (Abbreviation of isononyl acrylate: INAA commercial product)
[0202] ·Multifunctional isocyanate
[0203] Isocyanurate derivatives of hexamethylene diisocyanate (HMDI)
[0204] The product name of (B-1) is "DURANATE TSR-100", manufactured by Asahi Kasei Corporation
[0205] The product name of (B-2) is "DURANATE TPA-100", manufactured by Asahi Kasei Corporation
[0206] · Fluorescent dye product name "Tinopal OB", manufactured by BASF JAPAN
[0207] · Photopolymerization initiator Product name: IRGACURE 907, manufactured by IGM Resins
[0208] Photosensitizer (2,4-diethylthioxanthone)
[0209] Product name: KAYACURE DETX-S, manufactured by Nippon Kayaku Co., Ltd.
[0210] (Example 1)
[0211] The reaction step was carried out by performing a urethanization reaction at 60° C. for 1 hour in the presence of the above (A), (B), (C), a reaction solvent and a catalyst in the amounts shown in Table 1.
[0212] Next, the above raw materials were added to the composition after the reaction step in the amounts shown in Table 1 and mixed to perform an adding step.
[0213] In this manner, a curable composition is produced.
[0214] (Examples 2 to 8)
[0215] A curable composition was produced in the same manner as in Example 1 except that the addition step was changed to the compounding composition shown in Table 1.
[0216] In Examples 2 to 7, the reaction step was carried out at an excess ratio of -NCO groups in the urethanization reaction, while in Example 8, the reaction step was carried out at an excess ratio such that all -NCO groups could form urethane bonds in the urethanization reaction.
[0217] It should be noted that the compositions before and after the reaction step of Example 1 were analyzed by FT-IR. Figure 1 .exist Figure 1 In the above, the upper spectrum is the composition before the reaction step, and the lower spectrum is the spectrum of the composition after the reaction step. From the IR spectrum of the reaction product generated by the reaction step, it can be confirmed that the compound represented by the general formula (1) has been synthesized.
[0218] (Comparative Examples 1 and 2)
[0219] Each curable composition was obtained in the same manner as in Example 1 using the blending compositions shown in Table 1 except that isobornyl acrylate was used as the photopolymerizable monomer instead of using isobornyl acrylate and isononyl acrylate in combination.
[0220] Table 1 shows the compounding compositions used for producing the curable compositions of Examples 1 to 8 and Comparative Examples 1 and 2.
[0221] [Table 1]
[0222]
[0223] The curable compositions produced in Examples and Comparative Examples were evaluated as shown below. Specifically, the volume resistivity and tensile elongation of the cured products of the produced curable compositions were examined.
[0224] It should be noted that, generally speaking, the higher the tensile elongation, the more the strain during cooling (caused by the difference in thermal expansion coefficient between the cured product and the substrate) can be relaxed, and the occurrence of cracks associated therewith can be suppressed, thus providing high thermal reliability.
[0225] <Curing>
[0226] Each composition was applied onto a tinplate of 0.3×130×180 mm so that the thickness of the cured product after curing was 100 μm. Furthermore, a 500 W UV lamp was used to provide a cumulative light intensity of 3000 mJ / cm 2 The obtained sample was further left to stand in a constant temperature and humidity chamber at 25°C / 60%RH for 3 days.
[0227] <Volume Resistivity>
[0228] On each cured product cured as above, a paste-like silver conductive coating is applied in a circular shape (30 mm in diameter). Dry at 60°C for 30 minutes to form an upper electrode. On the other hand, a tinplate disposed on the opposite side of each cured product is used as a lower electrode. A voltage of DC100V is applied to determine the resistance value after 60 seconds. In addition, the electrode area is multiplied by the resistance value and divided by the thickness of the cured product (cured film) to determine the volume resistivity.
[0229] <Tensile elongation>
[0230] Each composition was applied onto a release-treated PET film so that the thickness of the cured product after curing was 100 μm. Furthermore, a 500 W UV lamp was used to provide a cumulative light intensity of 3,000 mJ / cm 2 The film was irradiated with ultraviolet light at a light intensity of 200 nm, and then left in a constant temperature and humidity chamber at 25°C / 60%RH for 3 days. Then, the cured film was peeled off from the PET film, cut into a dumbbell No. 2 shape, and the tensile elongation was measured. The measurement conditions were: chuck distance: 20 mm, tensile speed: 300 mm / min.
[0231] The evaluation results of the volume resistivity and tensile elongation of the cured product after curing are shown in Table 2. The oligomer ratio in Table 2 is the ratio of the curable oligomer in the curable composition and is a value calculated from the blending ratio after confirming that the yield of the urethanization reaction in the above reaction step is 100%.
[0232] [Table 2]
[0233]
[0234] From the evaluation results shown in Table 2, it can be confirmed that the curable composition of each example can obtain a cured product having both good electrical insulation performance and good elongation performance.
[0235] On the other hand, the cured products obtained from the curable compositions of the comparative examples could not have both good electrical insulation performance and good elongation performance.
[0236] If the above results are explained in addition, when the ratio of the saturated linear alkyl (meth)acrylate monomer to the saturated cycloalkyl (meth)acrylate monomer in the photopolymerizable monomer increases, there is a tendency for the tensile elongation of the cured product to increase.
[0237] In addition, when the above-mentioned raw material "DURANATE TSR-100" is used as the polyfunctional isocyanate, the tensile elongation of the cured product tends to be higher than when "DURANATE TPA-100" is used. On the other hand, when the above-mentioned raw material "DURANATE TPA-100" is used, the volume resistivity of the cured product tends to be higher than when "DURANATE TSR-100" is used.
[0238] Industrial Applicability
[0239] The curable composition of the present invention is applied to an electronic circuit, for example, to cover the electronic circuit with a cured product, and then cured by light irradiation to form a cured product, which is suitably used. The curable composition of the present invention can be suitably used, for example, as a curable composition for an insulating film.
Claims
1. A curable composition for an insulating film, comprising: A curable oligomer having a branched polyolefin structure and a (meth)acryloyl group in the molecule; Isobornyl (meth)acrylate; Isononyl (meth)acrylate, and Isocyanurate derivatives of hexamethylene diisocyanate, The ratio of the isobornyl (meth)acrylate to 100 parts by mass of the total mass of the isobornyl (meth)acrylate and the isononyl (meth)acrylate is 70 parts by mass or more and 80 parts by mass or less, The curable oligomer is a compound represented by the following general formula (1): In the general formula (1), X represents a branched hydrogenated polybutadiene structure, and Y' and Y" respectively represent the following general formula (a), In the general formula (a), Z 1 , Z 2 Each independently represents a molecular structure represented by the following general formula (α) or -NCO, and two Zs among Y' and Y" 1 and 2 Z 2 At least one of them is a molecular structure represented by the following general formula (α), In the general formula (a), R a1 , R a2 , R a3 Each independently represents a saturated hydrocarbon having 4 to 8 carbon atoms, and Z 1 , Z 2 As mentioned above, In the general formula (α), Q represents a saturated hydrocarbon group having 2 to 4 carbon atoms, and M represents H or CH 3 .
Citation Information
Patent Citations
Moisture curing combination curable composition, conformal coating agent and cured article
JP2017179171A
Curable resin composition
CN102985446A
Photocurable adhesive composition suitable for adhesion of engineering plastic, optical part assembled by using the same and assembling method of optical part using the same
JP2012001648A
Moisture- / light-curable composition, and electronic circuit device including cured film formed from the composition
JP2014201593A
Photocurable resin composition, protective coating agent, hard coating film, liquid crystal display module, and method for manufacturing same
WO2012090298A1