Prepregs, laminates and integrated moldings

By using prepregs of thermoplastic resin and thermosetting resin with aromatic rings in fiber-reinforced composite materials, combined with reinforcing fibers, the problem of insufficient joint strength is solved, and efficient jointing and molding of fiber-reinforced composite materials is achieved, which is suitable for Highly demanding structural components.

CN114787252BActive Publication Date: 2024-10-15TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080084864.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-11
Filing Date
2020-11-20
Publication Date
2024-10-15
Estimated Expiration
2040-11-20

AI Technical Summary

Technical Problem

In the existing technology, the joint strength of fiber-reinforced composite materials is insufficient, especially in high-temperature environments, and the manufacturing process takes a long time, leading to problems such as increased manufacturing costs and reduced material strength.

Method used

Prepreg is used, which contains more than 10% of thermoplastic resin and thermosetting resin with aromatic rings. It is joined with reinforcing fibers through the boundary surface spanning the two resin areas to form a laminate or integrated molded product, using thermosetting resin and thermoplastic The combination of resins increases joint strength and interlaminar fracture toughness.

Benefits of technology

It achieves efficient welding of fiber-reinforced composite materials, shortens the manufacturing process time, improves the joint strength and interlayer damage toughness, is suitable for high-demand structural components such as aircraft, and reduces molding time and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114787252B_ABST
    Figure CN114787252B_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide a prepreg and a laminate for manufacturing a laminate suitable as a structural material, which is high quality as a prepreg, has an excellent interlaminar fracture toughness value, and can be firmly integrated with other structural parts by welding. The present invention is a prepreg comprising the following components [A], [B] and [C], [B] comprising 10% by mass or more of a thermoplastic resin having an aromatic ring, a resin region comprising [B] existing on one surface of the prepreg, and a resin region comprising [C] existing on the other surface of the prepreg, and in the prepreg, there is [A] that crosses the boundary surface between the resin region comprising [B] and the resin region comprising [C] and is in contact with the two resin regions. [A] Reinforcing fiber; [B] Thermosetting resin; [C] Thermoplastic resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a prepreg in which reinforcing fibers are impregnated with a thermosetting resin and a thermoplastic resin, and a laminate or an integrated molded product comprising a thermosetting resin, a thermoplastic resin and reinforcing fibers. Background Art

[0002] For the fiber-reinforced composite material using thermosetting resin or thermoplastic resin as a matrix and combined with reinforcing fibers such as carbon fiber and glass fiber, it is lightweight, and has excellent mechanical properties such as strength and rigidity, heat resistance, and corrosion resistance, so it is used in many fields such as aerospace, automobiles, railway vehicles, ships, civil engineering and sports goods. However, these fiber-reinforced composite materials are not suitable for manufacturing parts and structures with complex shapes with a single molding process. In the above-mentioned uses, it is necessary to prepare parts formed by fiber-reinforced composite materials, and then integrate with the same or different parts. As a method for integrating fiber-reinforced composite materials containing reinforcing fibers and thermosetting resins with the same or different types, mechanical joining methods such as bolts, rivets, screws, and joining methods using adhesives can be used. In the mechanical joining method, since it is necessary to pre-process the process of the joining part such as the opening, the manufacturing process time becomes longer and the manufacturing cost increases. In addition, there is a problem that the material strength is reduced due to the opening. The bonding method using an adhesive requires a bonding step including preparation of the adhesive, application of the adhesive, and a curing step, which results in a long manufacturing process and a problem that reliability in terms of bonding strength cannot be fully satisfied.

[0003] For fiber-reinforced composite materials using thermoplastic resins in the matrix, in addition to the above-mentioned mechanical joining methods and joining using adhesives, a method of joining the parts by welding can also be applied, so there is a possibility that the time required for joining the parts can be shortened. On the other hand, in the case of mechanical properties at high temperatures and excellent resistance to chemicals such as aircraft structural parts, there is a problem that the heat resistance and chemical resistance are insufficient compared to fiber-reinforced composite materials formed of thermosetting resins and reinforcing fibers.

[0004] Here, Patent Document 1 discloses a method of joining a fiber-reinforced composite material composed of a thermosetting resin and reinforcing fibers with an adhesive.

[0005] Patent Document 2 discloses a method for integrating a component formed of a thermoplastic resin and a component formed of a fiber-reinforced composite material formed of a thermosetting resin. That is, a thermoplastic resin film is laminated on the surface of a prepreg sheet formed of reinforcing fibers and a thermosetting resin, and the prepreg is heated and pressurized to obtain a fiber-reinforced composite material. Thereafter, the obtained fiber-reinforced composite material is placed in a mold, and a thermoplastic resin is injection molded, and the formed thermoplastic resin component and the fiber-reinforced composite material are joined by injection molding.

[0006] Patent Document 3 describes a method for producing a laminate having a thermoplastic resin adhesive layer formed on the surface of a composite material composed of a thermosetting resin and reinforcing fibers, and describes that the laminate exhibits an adhesive effect with other members via the thermoplastic resin.

[0007] Patent Document 4 describes a prepreg and a fiber-reinforced composite material thereof, wherein particles, fibers, or films made of a thermoplastic resin are arranged on the surface layer of a prepreg made of reinforcing fibers and a thermosetting resin.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2018-161801

[0011] Patent Document 2: Japanese Patent Application Laid-Open No. 10-138354

[0012] Patent Document 3: Japanese Patent No. 3906319

[0013] Patent Document 4: Japanese Patent Application Laid-Open No. 8-259713 Summary of the invention

[0014] Problems to be solved by the invention

[0015] However, since the method disclosed in Patent Document 1 is a method of bonding fiber-reinforced composite materials formed of reinforcing fibers and thermosetting resins to each other using an adhesive, and since the thermosetting resin is a matrix resin, welding cannot be directly applied as a method of bonding fiber-reinforced composite materials. Since the curing of the adhesive takes time, there is a problem that time is required in the bonding process, and the bonding strength exhibited is insufficient.

[0016] In the method described in Patent Document 2, the bonding strength at the bonding portion between the thermosetting resin and the thermoplastic resin film in the fiber-reinforced composite material is insufficient.

[0017] The fiber-reinforced composite material disclosed in Patent Document 3 can be integrated by welding with a thermoplastic resin and exhibits excellent bonding strength at room temperature, but has insufficient bonding strength at high temperatures.

[0018] Patent Document 4 shows that the interlaminar fracture toughness value is improved by using particles, fibers or films formed of a thermoplastic resin. However, in this method, the bonding strength at the boundary between the thermosetting resin and the thermoplastic resin in the fiber-reinforced composite material is insufficient.

[0019] Therefore, an object of the present invention is to provide a prepreg which has excellent quality as a prepreg, can be joined to parts of the same or different types by welding, and exhibits excellent joining strength. In addition, it also has excellent interlaminar fracture toughness value and can provide a laminate suitable as a structural material. Another object of the present invention is to provide a laminate and an integrated molded product.

[0020] Means for solving problems

[0021] In order to solve the above-mentioned problems, the prepreg of the present invention has the following constitution. That is, the prepreg comprises the following constituent elements [A], [B] and [C], [B] comprises 10% by mass or more of a thermoplastic resin having an aromatic ring, a resin region comprising [B] is present on one surface of the prepreg, and a resin region comprising [C] is present on the other surface of the prepreg, and in the prepreg, [A] exists across the boundary surface between the resin region comprising [B] and the resin region comprising [C] and is in contact with the two resin regions.

[0022] [A] Reinforcement Fiber

[0023] [B] Thermosetting resin

[0024] [C] Thermoplastic resin

[0025] In addition, a laminated body as another aspect of the present invention has any of the following structures: That is, a laminated body in which at least a part of the layers is formed by a cured product of the above-mentioned prepreg, or a laminated body having the following structure.

[0026] That is, a laminate comprising a layer comprising the following constituent elements [A], [C] and [D], wherein [D] comprises 10% by mass or more of a thermoplastic resin having an aromatic ring, and in the laminate, there is [A] which straddles the boundary surface between a resin region comprising [C] and a resin region comprising [D] and is in contact with the two resin regions.

[0027] [A] Reinforcement Fiber

[0028] [C] Thermoplastic resin

[0029] [D] Thermosetting resin cured product

[0030] It should be noted that, in this specification, when referred to as a "laminated body", it refers to any of these laminates according to the context, unless otherwise specified. In addition, as can be seen from this specification, the laminate of the present invention is typically a fiber-reinforced resin that can be produced by using a preform containing the prepreg of the present invention, but is not particularly limited.

[0031] Effects of the Invention

[0032] The prepreg and laminate of the present invention use thermosetting resin and thermoplastic resin, which are firmly joined and can be well welded with the same or different parts, so relative to the fiber-reinforced composite material formed by thermosetting resin and reinforcing fiber in the past, the time required in the joining process can be shortened, and the molding of structural parts can be accelerated. In addition, the thermosetting resin becomes suitable resin properties in the prepreg manufacturing process by containing a thermoplastic resin with an aromatic ring more than a specified amount, and a high-quality prepreg is obtained. In addition, excellent bonding strength is presented, and a laminate excellent as a structural material can be obtained, and because it is suitable for computer uses such as aircraft structural parts, windmill blades, automobile structural parts and IC trays, and notebook computer shells, etc., it shows excellent performance as a structure, and the molding time and molding cost of the products involved in the above-mentioned uses can be greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] [ Figure 1 ] is a schematic diagram of a prepreg or laminate according to the present invention, and is a schematic diagram showing Figure 2 The diagram relates to a cross section perpendicular to the plane of the prepreg or the plane of the laminate.

[0034] [ Figure 2 ] is a schematic diagram of a cross section perpendicular to the plane of the prepreg blank or the plane of the laminate in the present invention, and is a diagram that helps to illustrate the method of measuring the average length RSm of roughness and the average height Rc of roughness. DETAILED DESCRIPTION

[0035] <Component [A]>

[0036] As the component [A] reinforcing fiber used in the present invention, there are glass fiber, carbon fiber, metal fiber, aromatic polyamide fiber, polyaramid fiber, aluminum oxide fiber, silicon carbide fiber, boron fiber, basalt fiber, etc. The above substances can be used alone or in combination of two or more. The above reinforcing fibers can be subjected to surface treatment. As surface treatment, there are metal deposition treatment, treatment using a coupling agent, treatment using a sizing agent, and additive adhesion treatment. It should be noted that in this specification, when such a surface treatment is applied to the reinforcing fibers, the reinforcing fibers in the state after the surface treatment are included and referred to as reinforcing fibers. The above reinforcing fibers also include reinforcing fibers with conductivity. As reinforcing fibers, carbon fibers are preferably used because they have a small specific gravity and are high in strength and elastic modulus.

[0037] Commercially available products of carbon fibers include "Torayca (registered trademark)" T800G-24K, "Torayca (registered trademark)" T800S-24K, "Torayca (registered trademark)" T700G-24K, "Torayca (registered trademark)" T700S-24K, "Torayca (registered trademark)" T300-3K, and "Torayca (registered trademark)" T1100G-24K (all manufactured by Toray Co., Ltd.).

[0038] The form and arrangement of the reinforcing fibers can be appropriately selected from the form and arrangement of reinforcing fibers arranged in one direction; a laminate of objects in which reinforcing fibers are arranged in one direction; or a woven form. However, in order to obtain a lightweight laminate with a higher level of durability, in each prepreg, it is preferred that the reinforcing fibers be arranged in one direction in the form of long fibers (fiber bundles) or continuous fibers such as woven fabrics.

[0039] The reinforcing fiber bundle may be composed of multiple fibers of the same form, or may be composed of multiple fibers of different forms. The number of reinforcing fibers constituting one reinforcing fiber bundle is usually 300 to 60,000, and if the manufacture of the substrate is considered, it is preferably 300 to 48,000, and more preferably 1,000 to 24,000. It may also be a range formed by a combination of any of the upper limits and any of the lower limits.

[0040] As the reinforcing fiber, it is preferable to use a fiber having a surface free energy of 10 to 50 mJ / m 2By controlling the surface free energy within this range, the reinforcing fibers show high affinity with [B] thermosetting resin or [D] thermosetting resin cured product and [C] thermoplastic resin, and show high bonding strength in the boundary surface between the resin region containing [B] or [D] and the resin region containing [C] where the reinforcing fibers exist across. In addition, the aggregation of the reinforcing fibers is suppressed, the reinforcing fibers are well dispersed in the molded product, and the deviation (coefficient of variation) of the bonding strength is reduced. The surface free energy of the reinforcing fibers is preferably 15 to 40 mJ / m 2 , more preferably 18 to 35 mJ / m 2 .

[0041] As a method for controlling the surface free energy of the above-mentioned reinforcing fibers, there are: a method of controlling the surface by oxidizing the surface and adjusting the amount of oxygen-containing functional groups such as carboxyl and hydroxyl groups; a method of controlling the surface by attaching a single or multiple compounds to the surface. In the case of attaching multiple compounds to the surface, compounds with high surface free energy and compounds with low surface free energy can be attached in a mixed manner. The following is an explanation of the method for calculating the surface free energy of the reinforcing fibers. The surface free energy can be calculated by the following method: After measuring the contact angles of the reinforcing fibers relative to three solvents (purified water, ethylene glycol, and tricresyl phosphate), the surface free energy is calculated using the Owens approximation. The steps are shown below, but the measuring equipment and detailed methods are not necessarily limited to this.

[0042] Using DCAT11 manufactured by DataPhysics, first, take out a single fiber from the reinforcing fiber bundle, cut it into 8 pieces with a length of 12±2mm, and then paste them in parallel on a special holder FH12 (a flat plate coated with an adhesive material) with a distance of 2 to 3mm between the single fibers. Then, cut the front end of the single fiber and set it in the holder DCAT11. During the measurement, bring a cell containing each solvent close to the lower end of the 8 single fibers at a speed of 0.2mm / s and immerse until it reaches 5mm from the front end of the single fiber. Then, lift the single fiber at a speed of 0.2mm / s. Repeat this operation more than 4 times. Use an electronic balance to measure the force F exerted on the single fiber when immersed in the liquid. Use this value and the following formula to calculate the contact angle θ.

[0043] COSθ = (force F (mN) on 8 single fibers) / ((8 (number of single fibers) × circumference of single fiber (m) × surface tension of solvent (mJ / m 2 ))

[0044] The measurement was performed on single fibers extracted from three different locations of the reinforcing fiber bundle. That is, the average value of the contact angles of a total of 24 single fibers was calculated for one reinforcing fiber bundle.

[0045] Surface free energy of reinforcing fibersγ f As the polar component of surface free energy γ p f , and the nonpolar component of the surface free energy γ d f Calculate the sum.

[0046] The polar component of surface free energy γ p f For example, the surface tension components and contact angles of each liquid are substituted into the Owens approximation shown below (a formula consisting of the polar and non-polar components of the surface tension inherent in each solvent and the contact angle θ), and then plotted on X and Y. The square of the slope a when the linear approximation is performed using the least squares method is used to obtain the non-polar component γ of the surface free energy. d f Calculated from the square of the intercept b. Surface free energy γ of the reinforcing fiber f It is the sum of the square of the slope a and the square of the intercept b.

[0047] Y=a·X+b

[0048] X=√(Polar component of the solvent surface tension (mJ / m 2 )) / √(Non-polar component of the solvent surface tension (mJ / m 2 )

[0049] Y = (1 + COSθ) (polar component of the surface tension of the solvent (mJ / m 2 )) / 2√(non-polar component of the solvent surface tension (mJ / m 2 )

[0050] Polar component of the surface free energy of the reinforcing fiberγ p f =a 2

[0051] Nonpolar component of the surface free energy of reinforcing fibersγ d f =b 2

[0052] Total surface free energy γ f =a 2 +b 2

[0053] The polar component and nonpolar component of the surface tension of each solvent are shown below.

[0054] Purified water

[0055] Surface tension 72.8mJ / m 2, polar component 51.0 mJ / m 2 , non-polar component 21.8 (mJ / m 2 )

[0056] · Ethylene glycol

[0057] Surface tension 48.0 mJ / m 2 , polar component 19.0 mJ / m 2 , non-polar component 29.0 (mJ / m 2 )

[0058] · Tricresyl phosphate

[0059] Surface tension 40.9 mJ / m 2 , polar component 1.7 mJ / m 2 , non-polar component 39.2 (mJ / m 2 )

[0060] <Component [B]>

[0061] The thermosetting resin of Component [B] used in the present invention contains 10% by mass or more of a thermoplastic resin having an aromatic ring. (The "thermosetting resin" as Component [B] in this specification refers to a resin composition containing more than 50% by mass of a thermosetting resin and showing the behavior of a thermosetting resin as a whole.) If the content of the thermoplastic resin having an aromatic ring is less than 10% by mass, resin peeling (Japanese: 樹脂取られ) from the release paper and the covering film occurs during the resin film manufacturing process and the resin impregnation process into carbon fiber when manufacturing prepregs, the unevenness of the unit area weight of the thermosetting resin becomes larger, and high-quality prepregs cannot be obtained. If the unevenness of the unit area weight of the resin becomes larger, the amount of the thermosetting resin in the laminate deviates, and deviations in the proportion of the reinforcing fiber and disorder in the arrangement also occur. Therefore, the deviation (coefficient of variation) of the bonding strength of the integrally molded product becomes larger. More preferably, the content of the thermoplastic resin having an aromatic ring is 13% by mass or more.

[0062] The thermoplastic resin component having an aromatic ring is another thermoplastic resin component different from the constituent element [C], and is preferably soluble in the thermosetting resin [B]. Here, the term "soluble in a thermosetting resin" means that there is a temperature region in which a uniform phase is formed by heating or heating and stirring the resin obtained by mixing the thermoplastic resin component with the thermosetting resin. Here, "forming a uniform phase" means that a state in which no separation can be observed visually can be obtained. Here, "dissolved state" means that the thermosetting resin containing the thermoplastic resin component is placed in a certain temperature region and becomes a uniform phase. Once a uniform phase is formed in a certain temperature region, it does not matter if separation occurs outside the temperature region, for example, at room temperature. By including the thermoplastic resin having an aromatic ring, the affinity with the thermoplastic resin [C] is increased, and the interface strength between the resin region containing [B] or [D] and the resin region containing [C] is improved, and as an integrated molded product, excellent bonding strength is exhibited.

[0063] As the thermoplastic resin having an aromatic ring, in general, a thermoplastic resin having a bond selected from the group consisting of a carbon-carbon bond, an amide bond, an imide bond, an ester bond, an ether bond, a carbonate bond, a carbamate bond, a thioether bond, a sulfone bond and a carbonyl bond in the main chain is preferred. In addition, for the thermoplastic resin component, it is also possible to partially have a cross-linked structure, and it may be crystalline or amorphous. In particular, at least one resin selected from the group consisting of polycarbonate, polyphenylene ether, polyphenylene sulfide, polyarylate, polyester, polyamide-imide, polyimide, polyetherimide polysulfone, polyethersulfone, polyetherketone, polyetheretherketone, phenoxy resin and polybenzimidazole is preferred.

[0064] Among them, the thermoplastic resin having an aromatic ring is preferably polyethersulfone or polyetherimide. Polyetherimide and polyethersulfone have strong interaction with the constituent element [C] due to their hydrogen bonding properties, and the interface strength between the resin region containing [B] or [D] and the resin region containing [C] is improved, so that as an integrated molded product, excellent bonding strength is exhibited. In addition, polyetherimide and polyethersulfone are also excellent in heat resistance, and therefore, excellent bonding strength is exhibited even in a high temperature environment, and can be cited as suitable examples.

[0065] In addition, the weight average molecular weight of the thermoplastic resin having an aromatic ring is preferably 10,000 g / mol or more and 40,000 g / mol or less. When the weight average molecular weight is 10,000 g / mol or more, the thermoplastic resin has excellent heat resistance and mechanical properties, and therefore exhibits excellent bonding strength at room temperature and high temperature environments. When the weight average molecular weight is 40,000 g / mol or less, the compatibility with the component [C] increases, and the interface strength between the resin region containing [B] or [D] and the resin region containing [C] is improved, thereby exhibiting excellent bonding strength.

[0066] For component [B], the storage modulus at 90°C during the heating process at 1.5°C / min using a rheometer is preferably 1.0 to 100 Pa. If the storage modulus at 90°C of [B] is 1.0 Pa or more, in the thermosetting resin film manufacturing process and the resin impregnation process into carbon fibers when manufacturing the prepreg, the resin will not fall off to the release paper and the cover film, and a high-quality prepreg with small resin unit weight variation can be obtained. In addition, if the storage modulus at 90°C of component [B] is 100 Pa or less, in the thermosetting resin film manufacturing process when manufacturing the prepreg, a resin film with no resin scratches and uniform thickness can be obtained, and a high-quality prepreg with small resin unit weight variation can be obtained. By reducing the resin unit weight variation, the deviation of the amount of thermosetting resin in the laminate is small, and the formation of defects such as voids can be suppressed, so the deviation (coefficient of variation) of the bonding strength of the integrated molded product can be suppressed to a low level. The storage elastic modulus at 90°C is more preferably 1.0 to 50 Pa, and even more preferably 1.0 to 30 Pa.

[0067] In addition, the temperature for reaching the minimum viscosity of the component [B] during the heating process at 1.5°C / min is preferably in the range of 120°C or above. As a result, in the prepreg manufacturing process, the viscosity of the resin is not easily increased, a resin film with uniform thickness can be obtained, and a high-quality prepreg with less uneven weight per unit area of ​​the resin can be obtained. Here, in the process of heating at 1.5°C / min using the rheometer, although the viscosity of the component [B] gradually decreases, the higher the temperature, the more the curing reaction proceeds, and it becomes difficult to flow, so when a certain temperature is exceeded, the viscosity begins to increase. This temperature is taken as the temperature for reaching the minimum viscosity, and the viscosity just before the viscosity begins to increase is taken as the minimum viscosity. From the viewpoint of manufacturing efficiency, the temperature for reaching the minimum viscosity is preferably 180°C or less. In addition, if the above-mentioned minimum viscosity is 0.5Pa·s or more, the arrangement of the carbon fibers is not easily disturbed during the molding of the laminate, and the integrated molded product exhibits a high bonding strength, which can suppress the deviation of the bonding strength to a low level. The minimum viscosity when heated at 1.5°C / min using a rheometer is more preferably 1.0 Pa·s or more, and further preferably 2.0 Pa·s or more. From the viewpoint of the quality of the laminate obtained after molding, the minimum viscosity is 100 Pa·s or less, and more preferably 10 Pa·s or less.

[0068] Examples of the thermosetting resin used in component [B] include unsaturated polyester resins, vinyl ester resins, epoxy resins, phenolic resins, urea resins, melamine resins, polyimide resins, cyanate resins, bismaleimide resins, benzoxazine resins, copolymers thereof, modified products thereof, and resins obtained by blending at least two of them. In order to improve impact resistance, an elastomer or rubber component may be added to the thermosetting resin. Among them, epoxy resin is preferred because of its excellent mechanical properties, heat resistance, and adhesion to reinforcing fibers. Examples of the epoxy resin main agent include bisphenol-type epoxy resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol AD ​​epoxy resin, and bisphenol S epoxy resin, brominated epoxy resins such as tetrabromobisphenol A diglycidyl ether, epoxy resins having a biphenyl skeleton, epoxy resins having a naphthalene skeleton, epoxy resins having a dicyclopentadiene skeleton, phenol Novolac epoxy resins, cresol Novolac epoxy resins, and other Novolac epoxy resins, N,N,O-triglycidyl meta-aminophenol, N,N,O-tris(2-hydroxy-2-nitrophenol)-1-yl-4-nitrophenol, and N,N,O-tris(2-hydroxy-2-nitrophenol)-1-yl-4-nitrophenol. Glycidylamine type epoxy resins such as hydroglyceryl p-aminophenol, N,N,O-triglycidyl-4-amino-3-methylphenol, N,N,N',N'-tetraglycidyl-4,4'-methylenedianiline, N,N,N',N'-tetraglycidyl-2,2'-diethyl-4,4'-methylenedianiline, N,N,N',N'-tetraglycidyl-m-phenylenediamine, N,N-diglycidyl aniline, N,N-diglycidyl o-toluidine, resorcinol diglycidyl ether, triglycidyl isocyanurate, etc.

[0069] The thermosetting resin used in the component [B] of the present invention preferably includes an epoxy resin. It is a more preferred embodiment that the thermosetting resin includes 40 to 100 parts by mass of a glycidylamine epoxy resin having three or more glycidyl groups relative to 100 parts by mass of all epoxy resins included in the thermosetting resin, because a cured product having high heat resistance can be obtained. Examples of the glycidylamine epoxy resin having three or more glycidyl groups include N,N,O-triglycidyl-m-aminophenol, N,N,O-triglycidyl-p-aminophenol, N,N,O-triglycidyl-4-amino-3-methylphenol, N,N,N',N'-tetraglycidyl-4,4'-methylenedianiline, N,N,N',N'-tetraglycidyl-2,2'-diethyl-4,4'-methylenedianiline, and N,N,N',N'-tetraglycidyl-m-xylylenediamine.

[0070] Examples of the epoxy resin curing agent included in component [B] include dicyandiamide, aromatic amine compounds, phenol Novolac resins, cresol Novolac resins, polyphenol compounds, imidazole derivatives, tetramethylguanidine, thiourea-added amines, formic hydrazide, formamide, and polythiol.

[0071] Among them, by using an aromatic amine curing agent as a curing agent for an epoxy resin, an epoxy resin with good heat resistance can be obtained. Examples of the aromatic amine compound include 3,3'-diisopropyl-4,4'-diaminodiphenyl sulfone, 3,3'-di-tert-butyl-4,4'-diaminodiphenyl sulfone, 3,3'-diethyl-5,5'-dimethyl-4,4'-diaminodiphenyl sulfone, 3,3'-diisopropyl-5,5'-dimethyl-4,4'-diaminodiphenyl sulfone, 3,3'-di-tert-butyl-5,5'-dimethyl-4,4'-diaminodiphenyl sulfone, 3,3',5,5'-tetraethyl-4,4'-diaminodiphenyl sulfone, 3,3'-diisopropyl-5,5'-diethyl-4,4'-diaminodiphenyl sulfone, 3,3'-di-tert-butyl-5,5'-diethyl-4,4'-diaminodiphenyl sulfone, 3,3',5,5'-tetraisopropyl-4,4'-diaminodiphenyl sulfone, 3,3'-di-tert-butyl-5,5'-diisopropyl-4,4'-diaminodiphenyl sulfone, 3,3',5,5'-tetra-tert-butyl-4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, etc.

[0072] The component [D] of the laminate of the present invention is typically a material obtained by heating and curing the component [B] of the prepreg of the present invention. The temperature conditions for heat curing can be appropriately set according to the type and amount of the thermosetting resin and the curing agent and accelerator. For example, when epoxy resin is used as the thermosetting resin and diaminodiphenyl sulfone is used as the amine compound, a temperature condition of 180°C for 2 hours can be preferably used.

[0073] <Component [C]>

[0074] The thermoplastic resin constituting component [C] (the "thermoplastic resin" as component [C] in this specification refers to a resin composition containing more than 50% by mass of a thermoplastic resin and exhibiting the behavior of a thermoplastic resin as a whole) is not particularly limited, and examples thereof include polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, polyethylene naphthalate, and liquid crystal polyesters, polyethylene, Polyolefins such as polypropylene and polybutene, styrene resins, polyurethane resins, and polyamides such as polyoxymethylene, polyamide 6, and polyamide 66, polycarbonate, polymethyl methacrylate, polyvinyl chloride, polyphenylene sulfide, polyphenylene ether, modified polyphenylene ether, polyimide, polyamide-imide, polyetherimide, polysulfone, modified polysulfone, polyethersulfone, polyketone, polyetherketone, polyetheretherketone, polyetherketoneketone, and polyaryletherketone, polyarylate, polyethernitrile, phenolic resin, phenoxy resin, etc. In addition, the above-mentioned thermoplastic resin can be a copolymer, a modified product, and / or a resin obtained by blending two or more of the above-mentioned resins. Among these, when [C] is one or more selected from polyamide, polyarylene etherketone, polyphenylene sulfide, polyethersulfone or polyetherimide, it has excellent heat resistance and exhibits high bonding strength as an integrated molded product even under high temperature conditions, so it is preferred.

[0075] In addition, if the thermoplastic resin constituting [C] is a crystalline thermoplastic resin, the viscosity at a temperature 40°C higher than the melting point is 1,000 Pa·s or more and 100,000 Pa·s or less, or if it is an amorphous thermoplastic resin, the viscosity at a temperature 40°C higher than the glass transition temperature is 1,000 Pa·s or more and 100,000 Pa·s or less, then when joining by welding the surface where the component [C] is present, the flow of the resin [C] can be suppressed, and excellent joining strength can be exhibited, which is preferred. The viscosity is more preferably 1,000 Pa·s or more and 10,000 Pa·s or less.

[0076] In order to improve the impact resistance, an elastomer or a rubber component may be added to the component [C]. In addition, other fillers and additives may be appropriately contained according to the application, etc., within the range that does not impair the purpose of the present invention. For example, inorganic fillers, flame retardants, conductivity imparting agents, crystal nucleating agents, ultraviolet absorbers, antioxidants, vibration damping agents, antibacterial agents, insect repellents, deodorants, anti-coloring agents, heat stabilizers, mold release agents, antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, foaming agents, coupling agents, etc. may be mentioned.

[0077] <Prepreg>

[0078] In the prepreg of the present invention, the resin region containing [B] is present on one surface thereof, and the resin region containing [C] is present on the other surface thereof. In addition, in the prepreg of the present invention, there is a reinforcing fiber [A] that crosses the boundary surface between the resin region containing [B] and the resin region containing [C] and is connected to the two resin regions. By having a reinforcing fiber [A] that crosses the boundary surface between the resin region containing the component [B] and the resin region containing the component [C] and is connected to the two resin regions, [A] is chemically or / and physically combined with [B] and [C], and the resin region containing [B] and the resin region containing [C] are not easy to peel off, so the bonding strength is improved. In addition, the component [A] that crosses the boundary surface and is connected to the above-mentioned two resin regions is chemically or / and physically combined with the component [B] and the component [C], so that the adhesion between the resin region containing the component [B] and the resin region containing the component [C] is improved.

[0079] In the prepreg of the present invention, it is preferred that the resin region containing [B] and the resin region containing [C] are each formed in a layered manner and are adjacent to each other. Figure 1 is a schematic diagram of a prepreg or laminate according to the present invention, Figure 2 yes Figure 1 Schematic diagram of a cross section perpendicular to the prepreg plane or the laminate plane, shown as a cross-sectional observation plane 5 in FIG.

[0080] In the prepreg of the present invention, the term "formed in layers and adjacent to each other" means, for example, Figure 2 As shown, in a cross section cut perpendicularly to the plane direction of the prepreg, the resin region 7 containing [C] and the resin region 8 containing [B] which are continuous in the plane direction are in a state of being closely present while forming a boundary surface 10. In the case where the resin region 7 containing [C] is not in a continuous layered state but exists in a particle form, a fiber form, a nonwoven fabric form, etc., the ratio of the area where the [B] thermosetting resin is exposed on the surface increases, and the coverage of the [C] on the outermost surface decreases, so there is a tendency for the weldability to decrease.

[0081] Furthermore, from the perspective of improving the bonding strength, it is preferred that, when the prepreg is viewed from above, in a cross section perpendicular to the plane of the prepreg including the fibers of [A] existing across the above-mentioned two resin regions, obtained from a direction that differs by 45 degrees (whether clockwise or counterclockwise) with respect to the fiber direction of any [A] that is in contact with the above-mentioned two resin regions, that is, in a cross section obtained by cutting perpendicularly with respect to the plane direction of the prepreg, the cross-sectional curve formed by the boundary surfaces of the two resins has a roughness average length RSm of less than 100 μm and a roughness average height Rc of more than 3.5 μm as defined in JIS B0601 (2001).

[0082] If the roughness average length RSm is less than 100 μm, not only chemical and / or physical bonding forces exist, but also mechanical bonding forces such as interweaving are superimposed, and the resin region containing component [B] and the resin region containing component [C] become difficult to peel off. The lower limit is not particularly limited, but from the perspective of avoiding the reduction of mechanical bonding forces caused by stress concentration, it is preferably 15 μm or more. In addition, by making the roughness average height Rc of the cross-sectional curve greater than 3.5 μm, not only the mechanical bonding forces caused by interweaving will appear, but also the component [A] that crosses the boundary surface and contacts the two resin regions is chemically or / and physically combined with the component [B] and the component [C], and the adhesion between the resin region containing component [B] and the resin region containing component [C] is improved. The preferred range of the roughness average height Rc of the cross-sectional curve is 10 μm or more (component [A] becomes easy to contact the two resin regions, and the adhesion is further improved), and particularly preferably 20 μm or more. The upper limit is not particularly limited, but is preferably 100 μm or less from the viewpoint of avoiding a decrease in mechanical bonding strength due to stress concentration.

[0083] Here, as a method for measuring the roughness average height Rc and the roughness average length RSm of the cross-sectional curve, a known method can be used. For example, after the component [B] is solidified, a method for measuring the cross-sectional image obtained using X-ray CT, a method for measuring the element analysis distribution image using an energy dispersive X-ray spectrometer (EDS), or a method for measuring the cross-sectional observation image using an optical microscope or a scanning electron microscope (SEM) or a transmission electron microscope (TEM). During the observation, in order to adjust the contrast, the component [B] and / or the component [C] can also be stained. In the image obtained by any of the above methods, the roughness average height Rc and the roughness average length RSm of the cross-sectional curve are measured within a range of 500 μm square.

[0084] use Figure 2 An example of a method for measuring the roughness average height Rc and the roughness average length RSm of a cross-sectional curve is shown below. Figure 2 In the observed image 9 shown in FIG. 1 , the resin region 7 including the component [C] and the resin region 8 including the component [B] are closely attached to each other and are shown as a boundary surface 10 in the observed image 9 . In addition, a plurality of components [A] 6 are present on the boundary surface 10 .

[0085] An example of a method for measuring the roughness average height Rc and the roughness average length RSm of a cross-sectional curve 13 is shown (a method for measuring cross-sectional curve elements 1). The end of the rectangular observation image 9 on the side of the resin region 8 containing the component [B] is used as a reference line 11, and a vertical baseline 12 is drawn at intervals of 5 μm from the resin region 8 containing the component [B] toward the resin region 7 containing the component [C]. The point where the vertical baseline 12 drawn from the reference line 11 first intersects with the component [C] is plotted, and the line connecting the plotted points is set as the cross-sectional curve 13. The obtained cross-sectional curve 13 is screened based on JIS B0601 (2001), and the roughness average height Rc and the roughness average length RSm of the cross-sectional curve 13 are calculated.

[0086] The thermoplastic resin component [C] in the prepreg of the present invention preferably has a weight per unit area of ​​10 g / m 2 If 10g / m 2 More preferably, it is 20 g / m 2 The upper limit is not particularly limited, but is preferably 500 g / m 2 This is because the amount of the thermoplastic resin does not become too much compared to the reinforcing fiber, and a laminate having excellent specific strength and specific elastic modulus can be obtained. 2 The mass (g) of the component [C] contained in the prepreg.

[0087] The prepreg of the present invention preferably has a reinforcing fiber content of 30 to 2,000 g / m2 per unit area. 2 If the amount of reinforcing fiber is 30g / m 2 If the amount of reinforcing fiber is 2,000 g / m 2 Below, the drapability of the prepreg becomes easy to improve.

[0088] The reinforcing fiber mass content of the prepreg of the present invention is preferably 30 to 90% by mass, more preferably 35 to 85% by mass, and further preferably 40 to 80% by mass. It can be a range formed by a combination of any one of the above upper limits and any one of the lower limits. When the reinforcing fiber mass content is 30% by mass or more, the amount of resin does not become too much compared to the fiber, and it is easy to obtain the advantages of a laminate with excellent specific strength and specific elastic modulus. In addition, when the laminate is formed, the heat generation during curing is not easy to become excessively high. In addition, when the reinforcing fiber mass content is 90% by mass or less, poor impregnation of the resin is not likely to occur, and the voids of the obtained laminate are easy to become less.

[0089] <Laminated body>

[0090] Another aspect of the present invention is a laminated body produced by a method of curing a preform of which at least a part of the layer is composed of the prepreg of the present invention, i.e., a laminated body of which at least a part of the layer is composed of the cured product of the prepreg of the present invention, the preformed body being produced by laminating a plurality of the prepregs of the present invention, or laminating the prepreg of the present invention together with other prepregs other than the prepreg of the present invention. Here, as a method of applying heat and pressure, for example, a press molding method, an autoclave molding method, a bag molding method, a tape wrapping method, an internal pressure molding method, etc. can be used.

[0091] Alternatively, another aspect of the present invention is a laminate comprising a layer comprising components [A], [C] and [D], wherein [D] comprises 10% by mass or more of a thermoplastic resin having an aromatic ring, and in the laminate, there is a reinforcing fiber [A] that straddles a boundary surface between a resin region comprising [C] and a resin region comprising [D] and is in contact with both resin regions.

[0092] When looking down at the laminate, the cross section perpendicular to the plane of the laminate containing [A] existing across the above two resin regions is obtained from the direction of the fiber direction of any [A] connected to the above two resin regions at an angle of 45 degrees (whether clockwise or counterclockwise), that is, the cross section obtained by cutting perpendicularly to the plane direction of the laminate, the cross-sectional curve formed by the close boundary surface of the two resin regions is defined by JIS B0601 (2001) as being less than 100 μm, and the roughness average height Rc is preferably 3.5 μm or more. The roughness average height Rc is further preferably 10 μm or more. The lower limit of RSm and the upper limit of Rc are not particularly limited. From the perspective of the possibility of reduced mechanical bonding force caused by stress concentration, RSm is preferably 15 μm or more, and Rc is preferably 100 μm or less.

[0093] The roughness average height Rc and the roughness average length RSm of the cross-sectional curve can be determined by the above-mentioned method in the same manner as the measurement method for the prepreg of the present invention.

[0094] As a method for molding the laminate of the present invention, it can be prepared by molding methods such as press molding, autoclave molding, bag mold molding, tape winding, internal pressure molding, hand lay-up molding, filament winding, pultrusion, resin injection molding, and resin transfer molding.

[0095] In the laminate of the present invention, it is preferred that the component [C] thermoplastic resin is present on the surface, that is, the laminate has a layer containing [A], [C] and [D] as the outermost layer, and [C] is exposed. It is further preferred that the component [C] is present on both the surface and the inside of the laminate of the present invention, that is, the laminate also has a layer containing [A], [C] and [D] as the inner layer. By having the component [C] thermoplastic resin on the surface of the laminate, the laminate of the present invention can be joined to the same or different parts by welding via the component [C]. On the other hand, when the component [C] thermoplastic resin is also present inside the laminate, an excellent interlaminar fracture toughness value (G IIC ).

[0096] <Integrated molded products>

[0097] For the laminate of the present invention, some heating means can be utilized to make other parts, i.e., parts of the same kind and / or different kinds as the parts constituting the laminate (adherends) be joined to the surface where [C] exists, especially the constituent element [C] existing on the surface of the laminate, so as to make an integrated molded product integrated (welded) with the laminate via the constituent element [C]. As different kinds of parts (adherends), parts formed by thermoplastic resins and parts formed by metal materials can be cited. In the parts formed by thermoplastic resins, reinforcing fibers, fillers, etc. can be included. The integration method is not particularly limited, and for example, heat welding, vibration welding, ultrasonic welding, laser welding, resistance welding, induction welding, insert injection molding, injection molding on substrate, etc. can be cited.

[0098] The strength of the joint of the integrated molded product can be evaluated based on ISO4587:1995 (JIS K6850 (1994)). The tensile shear bonding strength measured based on ISO4587:1995 is preferably 25 MPa or more, and more preferably 28 MPa or more when the test environment temperature is 23°C. Generally speaking, if it is 20 MPa or more, the laminate can be used as a bonding material for structural materials, and it is also high strength compared with the tensile shear bonding strength (about 10 MPa) of a conventional adhesive at a test environment temperature of 23°C. In applications requiring mechanical properties under high temperature environments, when the test environment temperature is 80°C, it is preferred to show a bonding strength of 13 MPa or more, and more preferably 16 MPa or more, in the evaluation based on ISO4587:1995. The higher the tensile shear bonding strength, the more preferred it is. There is no particular upper limit. In the integrated molded product of a conventional laminate, the tensile shear bonding strength at a test environment temperature of 23°C or 80°C is 200 MPa as the upper limit.

[0099] The laminate of the present invention is preferably used for aircraft structural parts, wind turbine blades, automobile outer panels and IC trays, computer applications such as notebook computer housings, and sports applications such as golf clubs and tennis rackets.

[0100] Example

[0101] Hereinafter, the present invention will be described in detail using examples. However, the scope of the present invention is not limited to these examples. It should be noted that, for the unit "part" of the composition ratio, it refers to mass parts unless otherwise noted. In addition, for the measurement of various properties, unless otherwise specified, it is carried out under an environment of a temperature of 23° C. and a relative humidity of 50%.

[0102] <Materials used as component [A] reinforcing fibers>

[0103] After obtaining a common carbon fiber bundle as a raw material by the following method, various sizing agent compounds were applied to obtain it. First, an acrylonitrile copolymer copolymerized with itaconic acid was spun and calcined to obtain a total of 24,000 filaments with a specific gravity of 1.8 g / cm 3 , a carbon fiber bundle with a bundle tensile strength of 4.9 GPa and a bundle tensile elastic modulus of 230 GPa. Then, various sizing agent compounds are mixed with acetone to obtain a solution of about 1% by mass in which the compound is uniformly dissolved. Each compound is applied to the above-mentioned carbon fiber bundle by an immersion method, and then heat-treated at 210°C for 90 seconds. The attachment amount of each compound is adjusted to 0.5 parts by mass relative to 100 parts by mass of carbon fiber to which each compound is attached. The sizing agent compounds used in each carbon fiber and the surface free energy after sizing agent coating are as follows.

[0104] CF1: polyethylene glycol diglycidyl ether ("Denacol" (registered trademark) EX-841, manufactured by Nagase ChemteX Co., Ltd.), surface free energy: 20 mJ / m 2

[0105] CF2: bisphenol A diglycidyl ether ("jER" (registered trademark) 828, manufactured by Mitsubishi Chemical Corporation), surface free energy: 9 mJ / m 2

[0106] CF3: sorbitol polyglycidyl ether ("Denacol" (registered trademark) EX-614B, manufactured by Nagase ChemteX Co., Ltd.), surface free energy: 32 mJ / m 2

[0107] <Component [B] Preparation method and evaluation method of thermosetting resin>

[0108] Thermosetting resins of the specific examples described in Table 1 were prepared using the following compounds (1) to (4) by the method described in (5), and were evaluated by the method (6).

[0109] (1) Epoxy resin

[0110] Tetraglycidyl diaminodiphenylmethane ("Araldite" (registered trademark) MY721, manufactured by Huntsman Advanced Materials Co., Ltd.) Epoxy equivalent: 113 (g / eq.), tetrafunctional glycidylamine type epoxy resin)

[0111] Bisphenol F type epoxy resin ("Epc" (registered trademark) 830, manufactured by DIC Corporation) epoxy equivalent: 170 (g / eq.)

[0112] (2) Amine compounds

[0113] ·4,4'-Diaminodiphenyl sulfone (Seikacure S, manufactured by Wakayama Seika Industries, Ltd.)

[0114] ·Dicyandiamide (DICY7, manufactured by Mitsubishi Chemical Co., Ltd.)

[0115] (3) Curing catalyst

[0116] 3-(3,4-Dichlorophenyl) 1,1-dimethylurea (DCMU99, manufactured by Hodogaya Chemical Industry Co., Ltd.)

[0117] (4) Thermoplastic resins with aromatic rings

[0118] Polyethersulfone ("Sumikaexcel" (registered trademark) PES5003P, manufactured by Sumitomo Chemical Co., Ltd., weight average molecular weight 47,300 g / mol)

[0119] Polyethersulfone (Virantage 10700RFP, manufactured by Solvay, weight average molecular weight 21,000 g / mol)

[0120] (5) Preparation method of thermosetting resin

[0121] The epoxy resin and viscosity modifier listed in Table 1 were placed in a kneading device, and heated and kneaded to dissolve the viscosity modifier (in some cases, the viscosity modifier was not added). Then, while the kneading was continued, the temperature was lowered to 100° C. or lower, and an amine compound and a curing catalyst appropriately selected from the amine compound and curing catalyst listed in Table 1 were added (in some cases, the curing catalyst was not added) and stirred to obtain thermosetting resins B-1 to B-7.

[0122] (6) Viscoelasticity measurement method of thermosetting resin

[0123] The viscoelasticity of thermosetting resin is measured using a dynamic viscoelasticity device ARES-G2 (manufactured by TA Instruments). The upper and lower measuring fixtures use parallel plates with a flat plate diameter of 40 mm. After the resin is set in a way that the distance between the upper and lower fixtures is 1 mm, it is measured at an angular velocity of 3.14 rad / s. The temperature is raised from 20°C to 170°C at a rate of 1.5°C / min, and the storage modulus at 90°C, as well as the minimum viscosity and the temperature at this time, are read. In addition, as for the viscosity increase ratio at 90°C, after setting the fixture and resin in the same way as above, it is measured at a temperature of 90°C and an angular velocity of 3.14 rad / s, and calculated using the following calculation formula.

[0124] 90°C viscosity increase ratio (times) = (viscosity after 3 hours) / (viscosity at the start of measurement)

[0125] <Materials used as component [C] thermoplastic resin and evaluation method>

[0126] Among the thermoplastic resins described in Tables 2 and 3, the following were used.

[0127] PA6: Polyamide 6 ("Amilan" (registered trademark) CM1007 (manufactured by Toray Industries, Ltd., melting point 225°C)), unit weight 120 g / m 2 membrane

[0128] PPS-1: polyphenylene sulfide ("Torelina" (registered trademark) A900 (manufactured by Toray Industries, Ltd., melting point 278°C)), weight per unit area 120 g / m 2 membrane

[0129] PPS-2: polyphenylene sulfide ("Torelina" (registered trademark) A670T05 (manufactured by Toray Industries, Ltd., melting point 278°C)), weight per unit area 120 g / m 2 membrane

[0130] PEKK1: Polyetherketoneketone ("KEPSTAN" (registered trademark) 6002 (produced by Arkema, melting point 300°C)) with a unit weight of 120 g / m 2 membrane

[0131] PEKK2: Polyetherketoneketone ("KEPSTAN" (registered trademark) 7002 (produced by Arkema, melting point 331°C)) with a unit weight of 120 g / m 2 membrane

[0132] ·PEEK: Polyetheretherketone (PEEK 450G (manufactured by Victrex, melting point 343°C)) with a unit weight of 120 g / m 2 membrane

[0133] ·Semi-aromatic PA: Made of polyamide 6T (glass transition temperature 125°C), unit weight 120 g / m 2 membrane

[0134] PEI: Polyetherimide ("ULTEM" (registered trademark) 1010 (manufactured by SABIC, glass transition temperature 217°C)) with a unit weight of 120 g / m 2 membrane

[0135] (1) Method for determining the melting point and glass transition point of thermoplastic resins

[0136] The melting point of the thermoplastic resin is measured using a differential scanning calorimeter (DSC) based on JIS K7121 (2012). When a plurality of melting points or glass transition points are observed in a mixture, the highest melting point or glass transition point is adopted as the melting point or glass transition point of the thermoplastic resin.

[0137] (2) Viscoelasticity measurement method of thermoplastic resin

[0138] The viscoelasticity of thermosetting resins is measured using a dynamic viscoelasticity device ARES-G2 (manufactured by TA Instruments). The upper and lower measuring fixtures use parallel plates with a flat plate diameter of 40 mm. After the resin is set in a way that the distance between the upper and lower fixtures is 1 mm, it is measured at an angular velocity of 3.14 rad / s. In the case of crystalline thermoplastic resins, the temperature is raised from its melting point to a temperature 60°C higher than the melting point at a rate of 1.5°C / min, and the viscosity is read at a temperature 40°C higher than the melting point. In the case of amorphous thermoplastic resins, the temperature is raised from its glass transition temperature to a temperature 60°C higher than the glass transition temperature at a rate of 1.5°C / min, and the viscosity is read at a temperature 40°C higher than the glass transition temperature.

[0139] <Prepreg production method and evaluation method>

[0140] The prepregs were produced by the following two methods. The components used in each example are shown in Tables 2 and 3.

[0141] [I] Pull out the component [A] reinforcing fiber (weight per unit area 193g / m 2 ) a reinforcing fiber sheet arranged in a continuous state in one direction, which is made to run in one direction, and the unit area weight of the component [C] is 120 g / m 2The resin sheet is arranged on the continuous reinforcing fiber sheet, heated by an IR heater to melt the component [C] and adhere to the entire surface of one side of the continuous reinforcing fiber sheet, and pressed by a nip roll whose surface temperature is maintained below the melting point of the component [C], and the substance impregnated in the reinforcing fiber sheet is cooled to obtain an intermediate. The thermosetting resin related to the component [B] selected as shown in Tables 2 and 3 is coated with 100 g / m 2 The resin unit weight of the thermosetting resin film was coated on the release paper to produce a thermosetting resin film. At this time, the situation where the thermosetting resin film on the release paper was coated without scratching under visual observation was recorded as "no resin film scratching" in Tables 2 and 3. In addition, when the release paper covering the surface opposite to the release paper coated with the thermosetting resin was rolled up, the situation where the thermosetting resin remained on the release paper was recorded as "resin falling off" in Tables 2 and 3. Regarding the resin unit weight of the produced thermosetting resin film, 5 points were measured every 1m, and the standard deviation was recorded as "film unit weight unevenness" in Tables 2 and 3. Next, the above-mentioned thermosetting resin film was overlapped on the surface opposite to the surface impregnated with the component [C] in the above-mentioned intermediate, and the thermosetting resin was impregnated into the intermediate while heating and pressing with a hot roller, thereby obtaining a prepreg [I].

[0142] [II] Using a knife coater, the thermosetting resin related to the component [B] selected as described in Table 2 was coated at a rate of 50 g / m 2 The resin film was coated on release paper with a unit weight of 193 g / m2. The resin film was overlapped on the reinforcing fibers (unit weight 193 g / m2) of the component [A] which were paralleled in one direction. 2 ) on both sides, heat and pressurize using hot rollers and impregnate the carbon fibers with a thermosetting resin to obtain a prepreg [II].

[0143] <Production method of laminate and evaluation of mechanical properties>

[0144] (1) Determination method of tensile shear bond strength

[0145] The prepregs [I] and [II] prepared above are cut into a specified size to obtain 2 prepregs [I] and 6 prepregs [II]. The axial direction of the reinforcing fiber is set to 0°, the axis-orthogonal direction is defined as 90°, and [0° / 90°]2s (symbol s represents mirror symmetry) is stacked to prepare a preform. At this time, the two outermost layers of each side are stacked in a manner to become prepregs [I], and the two surface layers of the preform are configured in a manner to become thermoplastic resin layers containing constituent element [C]. The preform is set in a press molding die, and a clamp and a spacer are used as needed. A pressure of 0.6MPa is applied by a press while maintaining the shape, and heated at 180°C for 120 minutes to obtain a laminate.

[0146] The obtained laminate was cut into two pieces with a width of 250 mm and a length of 92.5 mm with the 0° direction as the length direction of the test piece, and dried in a vacuum oven for 24 hours. Then, the two sheets were overlapped with a width of 25 mm × a length of 12.5 mm with the 0° direction as the length direction, and a pressure of 3 MPa was applied at a temperature 20°C higher than the melting point of the thermoplastic resin used as the component [C], and maintained for 1 minute, thereby welding the overlapped surfaces to obtain an integrated molded product. According to ISO4587:1995 (JIS K6850 (1994)), the wing sheet was bonded to the obtained integrated molded product and cut with a width of 25 mm to obtain the target test piece.

[0147] The obtained test piece was dried in a vacuum oven for 24 hours, and the tensile shear bonding strength at the ambient temperature of 23°C and 80°C was measured according to ISO4587:1995 (JIS K6850 (1994)). The evaluation was performed as follows based on the measurement results. The coefficient of variation was calculated by finding the standard deviation and the average value from the five measurement results of the tensile shear bonding strength and dividing the standard deviation by the average value. The results are shown in Tables 2 and 3.

[0148] (a) Tensile shear strength at 23°C

[0149] 28MPa and above: A

[0150] 25MPa or more, less than 28MPa: B

[0151] 20MPa or more, less than 25MPa: C

[0152] Less than 20MPa: D (unqualified)

[0153] (b) Tensile shear strength at 80°C

[0154] 16MPa or above: A

[0155] 13MPa or more, less than 16MPa: B

[0156] 10MPa or more, less than 13MPa: C

[0157] Less than 10MPa: D (unqualified)

[0158] (2) Interlaminar fracture toughness value (G IIC )

[0159] The prepreg [I] prepared above was cut into a predetermined size and stacked in a total of 20 sheets in such a manner that the reinforcing fibers were in the same direction. At this time, a release film for introducing precracks was sandwiched between the 10th and 11th sheets in the center to prepare a preform. The preform was placed in a press-forming mold, and a jig and a spacer were used as needed. While maintaining the shape, a pressure of 0.6 MPa was applied by a press machine, and heated at 180° C. for 120 minutes to obtain a laminate.

[0160] From the obtained laminate, a rectangular test piece with a length of 150 mm and a width of 20 mm was cut out with the reinforcing fiber axis as the length direction of the test piece, and dried in a vacuum oven at 60°C for 24 hours. The obtained test piece was evaluated for interlaminar fracture toughness value (G IIC ).

[0161] <Measurement of the mean roughness length RSm and the mean roughness height Rc of the prepreg and laminate>

[0162] Using the prepreg [I] prepared in the above, in a cross section cut perpendicular to the plane direction of the prepreg at an angle of 45 degrees when looking down at the prepreg relative to any fiber direction of [A] connected to the above two resin regions, an image of 1000 times was taken using an optical microscope. In an arbitrary 500 μm square observation range in the obtained image, the roughness average length RSm and the roughness average height Rc of the obtained cross-sectional curve element defined by JIS B0601 (2001) were measured using the above-mentioned cross-sectional curve element measurement method 1. In the obtained image, reinforcing fibers exist at the boundary surface between the resin region containing [C] and the resin region containing [B]. If the reinforcing fibers are connected to the resin region containing [C] and also to the resin region containing [B], it is assumed that there is a state of "reinforcing fibers that cross the boundary surface and are connected to the two resin regions". In the case of a laminate, the laminate described in (1) the method for measuring tensile shear bond strength is also used. An optical microscope is used to take a 1000x image of the observation cross section cut perpendicular to the plane direction, and then the measurement is performed in the same manner as in the case of the above-mentioned prepreg.

[0163] <Methods for producing laminates of Examples 1 to 14 and Comparative Examples 1 and 2>

[0164] In Examples 1 to 14 and Comparative Examples 1 and 2, laminates and integrated molded products were produced by the method described in (1) Measurement method of tensile shear bond strength.

[0165] <Method for producing laminates of Example 15 and Comparative Examples 3 to 5>

[0166] In Comparative Example 3, a film having a unit area weight of 50 g / m2 was attached to both sides of a reinforcing fiber sheet arranged in a plane in one direction. 2 A film of polyamide 6 ("Amilan" (registered trademark) CM1007 (manufactured by Toray Co., Ltd.)) was heated and pressed at 250°C to obtain a carbon fiber with a unit weight of 193 g / m 2 The obtained prepreg was cut into a predetermined size and used for bonding strength evaluation and compression strength evaluation at [0° / 90°] 2s The laminates were stacked in the same direction or 8 sheets were stacked in the same direction, and then a pressure of 3 MPa was applied by a press machine and heated at 250° C. for 10 minutes to obtain laminates. The tensile shear bonding strength was measured by the method described in the examples.

[0167] In Example 15, the above-mentioned prepreg [I] was cut into a predetermined size, a total of 20 sheets were stacked in such a manner that the reinforcing fibers were oriented in the same direction, and a release film for introducing a preliminary crack was sandwiched between the 10th and 11th sheets in the center to produce a preform.

[0168] In Comparative Example 4, the prepreg [II] (not containing the component [C]) was cut into a predetermined size and laminated in the same manner as in Example 15, with a release film interposed therebetween to obtain a preform.

[0169] In Comparative Example 5, on one side of a prepreg [II] (not including component [C]) cut into a predetermined size, the particle amount per unit area of ​​the prepreg was 7 g / m 2 Polyamide particles (SP-500, manufactured by Toray Co., Ltd.) were uniformly dispersed in a manner, and then laminated in the same manner as in Example 15, with a release film interposed therebetween to obtain a preform.

[0170] In Example 15 and Comparative Examples 4 and 5, a pressure of 0.6 MPa was applied to the obtained preform by a press machine and heated at 180° C. for 120 minutes to obtain a laminate. Then, the interlaminar fracture toughness value (G IIC ).

[0171] [Table 1]

[0172]

[0173] [Table 2]

[0174]

[0175] [Table 3]

[0176]

[0177] Description of Reference Numerals

[0178] 1: Prepreg or laminate

[0179] 2: Constituent elements [A]

[0180] 3: Component [C] and component [B] or component [D]

[0181] 4: Axial direction of any fiber bundle

[0182] 5: Observe the cross section

[0183] 6: Constituent elements [A]

[0184] 7: Resin area including component [C]

[0185] 8: Resin region containing component [B] or component [D]

[0186] 9: Observe the image

[0187] 10: Boundary surface

[0188] 11: Baseline

[0189] 12: Vertical Baseline

[0190] 13: Section curve

Claims

1. A prepreg comprising the following components [A], [B] and [C], wherein: [B] contains 10% by mass or more of a thermoplastic resin having an aromatic ring, a resin region containing [B] is present on one surface of the prepreg, and a resin region containing [C] is present on the other surface of the prepreg, and in the prepreg, there is [A] that straddles a boundary surface between the resin region containing [B] and the resin region containing [C] and is in contact with both resin regions, [A] Reinforcement fibers; [B] Thermosetting resin; [C] Thermoplastic resin, The resin region containing [B] and the resin region containing [C] are each formed in a layered manner and are adjacent to each other, thereby forming the boundary surface, In a process of heating at 1.5°C / min using a rheometer, the storage modulus of [B] at 90°C is 1.0 to 100 Pa, the minimum viscosity is 0.5 Pa·s or more, and the temperature at which the minimum viscosity is reached is in the range of 120°C or more, The prepreg satisfies at least one of the following [1] and [2], [1]: The thermoplastic resin having an aromatic ring is polyethersulfone or polyetherimide; [2]: The weight average molecular weight of the thermoplastic resin having an aromatic ring is 10,000 g / mol or more and 40,000 g / mol or less, [C] satisfies at least one of the following [3] and [4], [3]: one or more selected from the group consisting of polyamide, polyarylene ether ketone, polyphenylene sulfide, polyether sulfone and polyetherimide; [4]: In the case of a crystalline thermoplastic resin, the viscosity at a temperature 40°C higher than the melting point is 1,000 Pa·s to 100,000 Pa·s. In the case of an amorphous thermoplastic resin, the viscosity at a temperature 40°C higher than the glass transition temperature is 1,000 Pa·s to 100,000 Pa·s.

2. The prepreg according to claim 1, wherein In the prepreg blank viewed from above, when a cross section perpendicular to the prepreg plane containing the [A] is obtained from a direction that differs by 45 degrees from the fiber direction of any [A] that is connected to the two resin regions, the cross-sectional curve formed by the closely fitting boundary surfaces of the two resin regions in the cross section has a roughness average length RSm defined by JIS B0601 (2001) of less than 100 μm and a roughness average height Rc of more than 3.5 μm.

3. The prepreg according to claim 1 or 2, wherein: The content of the thermoplastic resin having an aromatic ring is 13% by mass or more.

4. The prepreg according to claim 1 or 2, wherein: The surface free energy measured by the Wilhelmy method is 10 to 50 mJ / m 2 The reinforcing fiber is used as [A].

5. A laminate, wherein: A cured product of the prepreg according to claim 1 or 2 constitutes at least a part of the layer.