Cationic emulsion composition of polyorganosiloxane and preparation method thereof
A cationic emulsion composition of polyorganosiloxane, using specific surfactants and an alkali catalyst, addresses the challenges of slow polymerization and stability, achieving high viscosity and durability for applications in fiber treatment agents and cosmetics.
Patent Information
- Application Number
- CN202080085540.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-13
- Filing Date
- 2020-11-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-11-27
AI Technical Summary
Existing methods for preparing cationic emulsions of highly polymerized polysiloxanes face challenges such as insufficient polymerization rates, stability issues, and prolonged processing times, particularly when using cationic surfactants like quaternary ammonium salts, and there is a need for improved durability in fiber treatment agents.
A cationic emulsion composition of polyorganosiloxane containing specific cationic and nonionic surfactants, combined with an alkali catalyst, is polymerized at controlled temperatures to achieve high viscosity and stability, using components like polydiorganosiloxane, cationic surfactants, and water, with a polymerization time of 1 to 150 hours.
The method results in a highly polymerized polyorganosiloxane emulsion with excellent stability and durability, suitable for applications in fiber treatment agents, release agents, water repellents, and cosmetics, while reducing polymerization time.
Smart Images

Figure CN114787282B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a cationic emulsion composition of polyorganosiloxane and a preparation method thereof. Background Art
[0002] Since it is possible to impart smoothness and water repellency by treating substrates with polyorganosiloxane, it is used in fiber treatment agents, release agents, water repellents, cosmetics, hair cosmetics, etc. Among them, the imparting effect of smoothness of highly polymerized polysiloxanes is excellent. In addition, it is known that if cationic surfactants such as quaternary ammonium salts are used as surfactants when emulsifying these polysiloxanes, the adsorptivity of polysiloxanes to substrates can be improved. Therefore, the requirements for the emulsion obtained by emulsifying highly polymerized polysiloxanes with cationic surfactants are relatively high.
[0003] A common method for emulsifying polysiloxane is to emulsify polysiloxane and a surfactant and disperse them in water using the mechanical shear force of an emulsifier. However, polysiloxane with a high degree of polymerization has an excessively high viscosity and the mechanical shear force cannot be applied uniformly, so a stable emulsion cannot be obtained.
[0004] As a method for obtaining a polysiloxane emulsion with a high degree of polymerization, an emulsion polymerization method is known in which an emulsion of a siloxane monomer is polymerized in an emulsion using an acid or base catalyst (Patent Documents 1, 2). However, when a cationic surfactant such as a quaternary ammonium salt represented by hexadecyltrimethylammonium chloride recorded in the literature is used in such an emulsion polymerization method, the polymerization rate is extremely slow, so it takes a long time to achieve a high degree of polymerization. Even if a polymerization of about 150 hours, which is considered to be the practical limit in industry, is carried out, polysiloxane can only be polymerized to a viscosity of tens of thousands of mPa·s after extraction.
[0005] As methods for obtaining cationic emulsions of highly polymerized polysiloxane, there have been proposed methods of polymerization using a silicon alkoxide catalyst (Patent Document 3) and a method of polymerization using an ammonium hydroxide catalyst (Patent Document 4), but the degree of polymerization is also insufficient.
[0006] In addition, a method has been proposed in which a highly polymerized polysiloxane emulsion is prepared using an anionic surfactant and then a cationic surfactant is added (Patent Documents 5 and 6). However, since an anionic surfactant is used simultaneously, there is a problem in terms of stability.
[0007] Furthermore, a method of carrying out polymerization under two-stage temperature conditions has been proposed (Patent Document 7), but there is a problem that a long polymerization time is required to achieve a high degree of polymerization.
[0008] In addition, in recent years, in the field of fiber treatment agents, there are increasing demands for washing durability that is difficult to achieve with high-polymerization polysiloxane alone. Although there are examples of adding a film-strengthening agent such as silica to an emulsion of high-polymerization polysiloxane to increase the strength of the film and thus improve durability, there are also problems such as decreased stability and increased manufacturing steps due to the addition of silica.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Publication No. 41-13995
[0012] Patent Document 2: Japanese Patent Publication No. 56-38609
[0013] Patent Document 3: Japanese Patent Application Laid-Open No. 08-104752
[0014] Patent Document 4: Japanese Patent Application Publication No. 2001-106787
[0015] Patent Document 5: Japanese Patent Application Laid-Open No. 09-137062
[0016] Patent Document 6: Japanese Patent Application Laid-Open No. 10-140480
[0017] Patent Document 7: Japanese Patent Application Laid-Open No. 09-278626 Summary of the invention
[0018] Technical Problems to be Solved by the Invention
[0019] The present invention has been made in view of the above circumstances, and its object is to provide a cationic emulsion composition of polyorganosiloxane having a high viscosity of 300,000 mPa·s or more and good stability and durability. The present invention also provides a method for preparing the emulsion composition which can polymerize the emulsion composition in a relatively short time.
[0020] Technical means to solve technical problems
[0021] In order to achieve the above object, the present invention provides a cationic emulsion composition of polyorganosiloxane, characterized in that it contains:
[0022] 100 parts by mass of (A) a polyorganosiloxane represented by the following average composition formula (1) and having a viscosity of 300,000 mPa·s or more at 25° C.,
[0023] [Chemical formula 1]
[0024]
[0025] In formula (1), R 1 are independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, R 2 are independently selected from the above R 1 The group, hydroxyl group or alkoxy group having 1 to 20 carbon atoms in the options, a, b, c, d are values such that the viscosity of the polyorganosiloxane at 25°C satisfies 300,000 mPa·s or more, and a≥2, c+d≥1;
[0026] 0.1 to 30 parts by mass of (B-1) cationic surfactant Q 1 3(CH3)N + ·X - ,
[0027] Among them, Q 1 are monovalent organic groups having 6 to 30 carbon atoms of the same or different types, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms;
[0028] 0.1 to 30 parts by mass of (B-2) cationic surfactant Q 2 (CH3)3N + ·X - ,
[0029] Among them, Q 2 is a monovalent organic group having 17 to 30 carbon atoms, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms;
[0030] 30 to 3,000 parts by mass of (C) water.
[0031] Such a cationic emulsion composition of polyorganosiloxane is a highly polymerized cationic emulsion composition of polyorganosiloxane having a relatively high viscosity, and has excellent stability and durability.
[0032] In this case, the emulsion composition of the present invention preferably further contains a nonionic surfactant.
[0033] Thus, by using the cationic surfactant and the nonionic surfactant simultaneously, the particle size of the emulsion can be easily reduced, thereby improving the stability of the emulsion.
[0034] Furthermore, the emulsion composition of the present invention preferably forms a coating after drying.
[0035] In this manner, the emulsion compound of the present invention can be dried to form a coating.
[0036] Furthermore, the present invention provides a fiber treating agent, characterized in that it comprises the cationic emulsion composition of the polyorganosiloxane.
[0037] In addition, the present invention provides a release agent, characterized in that it comprises the cationic emulsion composition of the polyorganosiloxane.
[0038] In addition, the present invention provides a water repellent, characterized in that it comprises the cationic emulsion composition of the polyorganosiloxane.
[0039] Furthermore, the present invention provides a cosmetic, characterized in that it comprises the cationic emulsion composition of the polyorganosiloxane.
[0040] Furthermore, the present invention provides a hair cosmetic comprising a cationic emulsion composition of the above-mentioned polyorganosiloxane.
[0041] Thus, the cationic emulsion composition of the polyorganosiloxane of the present invention can be suitably used as a component contained in a fiber treating agent, a release agent, a water repellent, a cosmetic, or a hair cosmetic.
[0042] In addition, the present invention provides a method for preparing a cationic emulsion composition of polyorganosiloxane, characterized in that the emulsion is polymerized at 0 to 30° C. for 1 to 150 hours in the presence of an alkali catalyst, and further neutralized, wherein the emulsion is obtained by emulsifying and dispersing the following components:
[0043] 100 parts by mass of (D) general formula HO-[R 1 2SiO] j -H represented by a polydiorganosiloxane having hydroxyl groups at both ends, wherein R 1 are independently hydrogen atoms or monovalent organic groups having 1 to 20 carbon atoms, and j is a value such that the viscosity of the polydiorganosiloxane having hydroxyl groups at both ends at 25° C. is less than 2,000 mPa·s;
[0044] 0 to 20 parts by mass of (E) any one or two or more of the following organoalkoxysilanes,
[0045] Si(OR 3 4. R 1 Si(OR 3 )3. R 1 2Si(OR 3 2. R 1 3Si(OR 3 ),
[0046] Among them, R 1 are independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, R 3 are independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms;
[0047] 0.1 to 30 parts by mass of (B-1) cationic surfactant Q 1 3(CH3)N + ·X - ,
[0048] Among them, Q 1 are monovalent organic groups having 6 to 30 carbon atoms of the same or different types, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms;
[0049] 0.1 to 30 parts by mass of (B-2) cationic surfactant Q 2 (CH3)3N + ·X - ,
[0050] Among them, Q 2 is a monovalent organic group having 17 to 30 carbon atoms, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms;
[0051] 30 to 3,000 parts by mass of (C) water.
[0052] According to such a method for preparing an emulsion composition, a cationic emulsion composition of a highly polymerized polyorganosiloxane having a relatively high viscosity can be polymerized in a relatively short period of time, and the emulsion composition has good stability and durability.
[0053] Effects of the Invention
[0054] The cationic emulsion composition of the polyorganosiloxane of the present invention is a cationic emulsion composition of a highly polymerized polyorganosiloxane with a relatively high viscosity, and has good stability and good durability. In addition, the emulsion composition can form a coating film alone, and further the durability of the coating film can be improved. Such an emulsion composition can be suitably used as a fiber treatment agent, a release agent, a water repellent, a cosmetic, a hair cosmetic, etc.
[0055] Furthermore, the method for preparing the cationic emulsion composition of polyorganosiloxane of the present invention enables the emulsion composition to be polymerized in a relatively short period of time and is therefore also industrially useful. DETAILED DESCRIPTION
[0056] The inventors of the present application have conducted intensive research to achieve the above-mentioned purpose, and have found that the emulsion can be polymerized in a relatively short time by polymerizing the emulsion at 0 to 30° C. for 1 to 150 hours in the presence of an alkali catalyst and further neutralizing the emulsion. The emulsion is obtained by emulsifying and dispersing the following components:
[0057] 100 parts by mass of (D) general formula HO-[R 1 2SiO]j -H represented by a polydiorganosiloxane having hydroxyl groups at both ends, wherein R 1 are independently hydrogen atoms or monovalent organic groups having 1 to 20 carbon atoms, and j is a value such that the viscosity of the polydiorganosiloxane having hydroxyl groups at both ends at 25° C. is less than 2,000 mPa·s;
[0058] 0 to 20 parts by mass of (E) any one or two or more of the following organoalkoxysilanes,
[0059] Si(OR 3 4. R 1 Si(OR 3 )3. R 1 2Si(OR 3 2. R 1 3Si(OR 3 ),
[0060] Among them, R 1 are independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, R 3 are independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms;
[0061] 0.1 to 30 parts by mass of (B-1) cationic surfactant Q 1 3(CH3)N + ·X - ,
[0062] Among them, Q 1 are monovalent organic groups having 6 to 30 carbon atoms of the same or different types, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms;
[0063] 0.1 to 30 parts by mass of (B-2) cationic surfactant Q 2 (CH3)3N + ·X - ,
[0064] Among them, Q 2 is a monovalent organic group having 17 to 30 carbon atoms, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms;
[0065] 30 to 3,000 parts by mass of (C).
[0066] The inventors of the present application have found that a cationic emulsion composition can be obtained, which contains a polysiloxane represented by the following average composition formula (1) and having a viscosity of 300,000 mPa·s or more at 25° C. as component (A), and that the emulsion composition has good stability and good durability, thereby completing the present invention.
[0067] [Chemical formula 2]
[0068]
[0069] In formula (1), R 1 are independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, R 2 are independently selected from the above R 1 The group, hydroxyl group or alkoxy group having 1 to 20 carbon atoms in the options, a, b, c, d are values such that the viscosity of the polyorganosiloxane at 25°C satisfies 300,000 mPa·s or more, and a≥2, c+d≥1.
[0070] Such a high viscosity polyorganosiloxane of 300,000 mPa·s or more is generally a polyorganosiloxane of high polymerization degree. Therefore, when explaining the present invention, it may be referred to as a cationic emulsion composition of a polyorganosiloxane of high polymerization degree.
[0071] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited thereto.
[0072] First, each component of the polyorganosiloxane cationic emulsion composition of the present invention will be described.
[0073] [(A) ingredient]
[0074] The component (A) is a polyorganosiloxane represented by the following average composition formula (1) and having a viscosity of 300,000 mPa·s or more at 25° C. The emulsion composition of the present invention contains 100 parts by mass of the component (A).
[0075] [Chemical formula 3]
[0076]
[0077] In formula (1), R 1 are independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, R 2 are independently selected from the above R 1 The group, hydroxyl group or alkoxy group having 1 to 20 carbon atoms in the options, a, b, c, d are values such that the viscosity of the polyorganosiloxane at 25°C satisfies 300,000 mPa·s or more, and a≥2, c+d≥1.
[0078] As mentioned above, R 1They are independently hydrogen atoms or monovalent organic groups having 1 to 20 carbon atoms. The monovalent organic groups having 1 to 20 carbon atoms may be straight chain, branched chain or cyclic. Specifically, they include: alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, cyclopentyl, cyclohexyl, cycloheptyl, etc.; aryl groups such as phenyl, tolyl, naphthyl, etc.; alkenyl groups such as vinyl, allyl, etc.; or groups in which some hydrogen atoms in the structures of these organic groups are replaced by organic groups containing polar groups such as halogen atoms, amino, acryloxy, methacryloyloxy, epoxy, mercapto, etc. Here, R is preferably selected from the group consisting of: 1 More than 80% of them are methyl groups.
[0079] In addition, as mentioned above, R 2 are independently selected from the above R 1 The alkoxy group having 1 to 20 carbon atoms may be any of a linear, branched or cyclic group, and specifically, methoxy, ethoxy, propoxy, butoxy, pentyloxy, hexyloxy, octyloxy, decyloxy, dodecyloxy, 2-ethylhexyloxy, etc. are listed, preferably methoxy, ethoxy, propoxy, butoxy, pentyloxy, and more preferably methoxy, ethoxy, and propoxy.
[0080] When a reactive functional group is present in the above average composition formula (1), the reactive functional group can react with other compounds. Specifically, when an amino group is present in the above average composition formula (1), a ring-opening reaction can be carried out with a polyoxyalkylene compound containing an epoxy group or an alkyl compound containing an epoxy group. In addition, an acetylation reaction can be carried out with a carboxylic anhydride such as acetic anhydride, propionic anhydride, oxalic anhydride, succinic anhydride, maleic anhydride, phthalic anhydride, and benzoic anhydride. In addition, when an epoxy group is present in the above average composition formula (1), a ring-opening reaction can be carried out with an amino-containing compound. In addition, the reaction with the reactive functional groups shown above is not limited to these reactions.
[0081] In the above average composition formula (1), a, b, c, and d are values such that the viscosity of the polyorganosiloxane at 25°C satisfies 300,000 mPa·s or more, more preferably such values such that the viscosity of the polyorganosiloxane at 25°C satisfies 400,000 mPa·s or more, and even more preferably such values such that the viscosity of the polyorganosiloxane at 25°C satisfies 500,000 mPa·s or more. In addition, the viscosity is an absolute viscosity, and when it can be measured in a liquid state, it is a value directly measured at 25°C using a rotational viscometer, and when the viscosity is too high to be measured, it is a value obtained by measuring the toluene solution viscosity at 25°C using a rotational viscometer. In addition, a≥2, c+d≥1.
[0082] b in the average composition formula (1) can typically be 50 or more, preferably 100 or more. However, as the c+d value increases, the crosslinking units increase, and thus the viscosity may be 300,000 mPa·s or more even when b is 50 or less.
[0083] As specific examples of the component (A), the following average composition formula can be cited, but it is not limited to these average composition formulas. In the following average composition formula, a, b, c, d, e, and f are values that satisfy the viscosity of the polyorganosiloxane at 25° C. of 300,000 mPa·s or more, and a ≥ 2, c + d ≥ 1. In addition, b + e + f in the following average composition formula can typically take a value of 50 or more, preferably a value of 100 or more.
[0084] [Chemical formula 4]
[0085]
[0086] [Chemical formula 5]
[0087]
[0088] [Chemical formula 6]
[0089]
[0090] [Component (B-1) and component (B-2)]
[0091] The components (B-1) and (B-2) are as follows.
[0092] (B-1) Cationic surfactant: Q 1 3(CH3)N + ·X - , where Q 1 are monovalent organic groups having 6 to 30 carbon atoms of the same or different types, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms.
[0093] (B-2) Cationic surfactant: Q 2 (CH3)3N + ·X - , where Q 2 is a monovalent organic group having 17 to 30 carbon atoms, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms.
[0094] The emulsion composition of the present invention contains 0.1 to 30 parts by mass of the component (B-1) and 0.1 to 30 parts by mass of the component (B-2) based on 100 parts by mass of the component (A).
[0095] The cationic surfactants as the components (B-1) and (B-2) are used to emulsify and disperse the polyorganosiloxane in water. However, the inventors of the present application believe that the action mechanism of the components (B-1) and (B-2) is not limited to the action mechanism as emulsifiers, but also includes the following action mechanism. It is believed that in the method for preparing the cationic emulsion composition of polyorganosiloxane of the present invention, when the polyorganosiloxane is emulsified and dispersed in water and then the alkali catalyst is added, the OH generated in the aqueous phase - By exchanging counter ions with the cationic surfactants as the components (B-1) and (B-2), the cationic surfactants themselves also function as catalysts, and as a result, the polyorganosiloxane as the component (A) can be more efficiently polymerized to a high degree.
[0096] As mentioned above, the cationic surfactant as component (B-1) is Q 1 3(CH3)N + ·X - The cationic surfactant represented by Q 1 are the same or different monovalent organic groups having 6 to 30 carbon atoms, preferably a monovalent organic group having 7 to 18 carbon atoms. 1 When the number of carbon atoms of Q is less than 6, the hydrophilicity of the surfactant is too strong, and the contact frequency with the polyorganosiloxane of component (A) decreases, and a long time of polymerization is required to make the polyorganosiloxane highly polymerized. 1 When the carbon number of the polyol is greater than 30, the emulsifying power as a surfactant is weak, and a stable emulsion may not be obtained.
[0097] As Q 1 Specific examples include: alkyl groups such as hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, docosyl, cyclopentyl, cyclohexyl, and cycloheptyl; aryl groups such as phenyl, benzyl, tolyl, and naphthyl; alkenyl groups such as octadecyl, etc. Among them, octyl, dodecyl, hexadecyl, and octadecyl are preferred.
[0098] In addition, X - is a halogen ion or a monovalent carboxylic acid ion having 1 to 6 carbon atoms, and specifically includes: Cl - Br - ,I - Halogen ions such as HCOO - 、CH3COO - 、C2H5COO - Among them, Cl -HCOO - 、CH3COO - .
[0099] Specific examples of the component (B-1) include trihexylmethylammonium chloride, triheptylmethylammonium chloride, trioctylmethylammonium chloride, trinonylmethylammonium chloride, tridecylmethylammonium chloride, trilaurylmethylammonium chloride, trioctylmethylammonium acetate, and trilaurylmethylammonium acetate, but are not limited to these examples.
[0100] The amount of the cationic surfactant as component (B-1) can be 0.1 to 30 parts by mass, preferably 0.5 to 20 parts by mass, and more preferably 1 to 15 parts by mass relative to 100 parts by mass of component (A). When the amount is less than 0.1 parts by mass, component (A) may not be efficiently polymerized to a high degree during the polymerization process, and when the amount is more than 30 parts by mass, the stability of the emulsion may become unstable.
[0101] As mentioned above, the cationic surfactant of component (B-2) is Q 2 (CH3)3N + ·X - The cationic surfactant represented by can improve the stability of the emulsion. 2 is a monovalent organic group having 17 to 30 carbon atoms, preferably a monovalent organic group having 18 to 28 carbon atoms. 2 When the number of carbon atoms of Q is less than 17, the compatibility with the cationic surfactant represented by (B-1) is poor, and the stability of the emulsion may decrease. 2 When the number of carbon atoms is greater than 30, 1 As with the case of Q, the emulsifying power of the surfactant is weak and sometimes a stable emulsion cannot be obtained. 2 X - With the above Q 1 X - same.
[0102] Specific examples of the component (B-2) include octadecyltrimethylammonium chloride, eicosyltrimethylammonium chloride, behenyltrimethylammonium chloride, octadecyltrimethylammonium acetate, eicosyltrimethylammonium acetate, behenyltrimethylammonium acetate, etc., but are not limited to these examples.
[0103] The amount of the cationic surfactant as component (B-2) can be 0.1 to 30 parts by mass, preferably 0.5 to 20 parts by mass, and more preferably 1 to 15 parts by mass relative to 100 parts by mass of component (A). When the amount is less than 0.1 parts by mass, the stability of the emulsion tends to become unstable, and when the amount is more than 30 parts by mass, component (A) may not be efficiently polymerized to a high degree during the polymerization process.
[0104] Compared with component (B-2), component (B-1) has higher hydrophobicity, so the contact frequency with the polyorganosiloxane of component (A) is high, and the effect of further accelerating the polymerization rate can be expected, but sometimes the hydrophobicity is too high, resulting in poor emulsification ability. Therefore, when only (B-1) is used, the time stability of the emulsion sometimes deteriorates due to the composition, particle size, viscosity, pH and other conditions of the emulsion. Therefore, compared with component (B-1), by using component (B-2) with higher emulsification ability at the same time, the stability of the emulsion can be improved when the polymerization rate is accelerated.
[0105] In addition, in the cationic emulsion composition of the polyorganosiloxane of the present invention, by using a cationic surfactant and a nonionic surfactant simultaneously, the emulsion is easily reduced in particle size, thereby improving the stability of the emulsion. As nonionic surfactants, polyoxyalkylene alkyl ethers, polyoxyalkylene alkylphenyl ethers, polyoxyalkylene alkyl esters, polyoxyalkylene sorbitan alkyl esters, polyethylene glycol, polypropylene glycol, diethylene glycol, etc. can be exemplified, and one or more of them can be used alone or appropriately selected for use. Among them, the nonionic surfactant represented by the following general formula (2) is preferred.
[0106] R 4 O(EO) P (PO) q H(2)
[0107] In formula (2), R 4 is a linear or branched alkyl group having 8 to 30 carbon atoms, EO represents an oxyethylene group, PO represents an oxypropylene group, and the arrangement of these groups may be block-shaped or random. p and q are independently integers of 0 to 100, and p+q>0. In particular, in the above general formula (2), R 4 It is preferably a linear or branched alkyl group having 8 to 18 carbon atoms, and p and q are preferably independently 0 to 25 and 0<p+q≤50.
[0108] In addition, there is no problem in adding the following surfactants for the purpose of improving the stability of the emulsion, etc.: cationic surfactants such as quaternary ammonium salts and alkylamine acetates other than components (B-1) and (B-2); and amphoteric surfactants such as alkyl betaines and alkyl imidazolines.
[0109] [(C) ingredient]
[0110] The emulsion composition of the present invention contains 30 to 3,000 parts by mass of water as the component (C), preferably 40 to 2,400 parts by mass of water as the component (C), relative to 100 parts by mass of the component (A). If the amount of water is too small, a water-in-oil emulsion cannot be formed, and if it is too large, it is uneconomical.
[0111] [Method for preparing emulsion composition]
[0112] Next, the preparation method of the emulsion composition of the present invention is as follows. That is, in the presence of an alkali catalyst, the emulsion is polymerized at 0 to 30° C. for 1 to 150 hours, and further neutralized, and the emulsion is obtained by emulsifying and dispersing the following components:
[0113] 100 parts by mass of (D) general formula HO-[R 1 2SiO] j -H represented by a polydiorganosiloxane having hydroxyl groups at both ends, wherein R 1 are independently hydrogen atoms or monovalent organic groups having 1 to 20 carbon atoms, and j is a value such that the viscosity of the polydiorganosiloxane having hydroxyl groups at both ends at 25° C. is less than 2,000 mPa·s;
[0114] 0 to 20 parts by mass of (E) any one or two or more of the following organoalkoxysilanes,
[0115] Si(OR 3 4. R 1 Si(OR 3 )3. R 1 2Si(OR 3 2. R 1 3Si(OR 3 ),
[0116] Among them, R 1 are independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, R 3 are independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms;
[0117] 0.1 to 30 parts by mass of (B-1) cationic surfactant Q 1 3(CH3)N + ·X- ,
[0118] Among them, Q 1 are monovalent organic groups having 6 to 30 carbon atoms of the same or different types, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms;
[0119] 0.1 to 30 parts by mass of (B-2) cationic surfactant Q 2 (CH3)3N + ·X - ,
[0120] Among them, Q 2 is a monovalent organic group having 17 to 30 carbon atoms, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms;
[0121] 30 to 3,000 parts by mass of (C) water.
[0122] [(D) ingredient]
[0123] First, the general formula HO-[R 1 2SiO] j -H-terminated hydroxyl polydiorganosiloxane is a raw material of the polyorganosiloxane as the component (A). 1 Each of the groups is independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, and j is a value such that the viscosity of the polydiorganosiloxane having hydroxyl groups at both ends at 25° C. is less than 2,000 mPa·s.
[0124] In the above general formula, j can typically take a value of 1 to 400.
[0125] As specific examples of the component (D), the following average composition formula can be cited, but it is not limited to these average composition formulas. In the following average composition formula, j, k+l, and k+l+m are values that satisfy the viscosity of the polydiorganosiloxane having hydroxyl groups at both ends at 25°C less than 2,000 mPa·s. In addition, j, k+l, and k+l+m in the following general formula can typically take values of 1 to 400.
[0126] [Chemical formula 7]
[0127]
[0128] [(E) ingredient]
[0129] The organoalkoxysilane as the component (E) is a raw material for the polyorganosiloxane as the component (A), and is any one or two or more organoalkoxysilanes of the following general formula.
[0130] Si(OR3 4. R 1 Si(OR 3 )3. R 1 2Si(OR 3 2. R 1 3Si(OR 3 ),
[0131] Among them, R 1 They are independently hydrogen atoms or monovalent organic groups having 1 to 20 carbon atoms. Examples of monovalent organic groups having 1 to 20 carbon atoms include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, cyclopentyl, cyclohexyl, and cycloheptyl; aryl groups such as phenyl, tolyl, and naphthyl; alkenyl groups such as vinyl and allyl; or groups in which some hydrogen atoms in the structure of these organic groups are replaced by halogen atoms or organic groups containing polar groups such as amino, acryloyloxy, methacryloyloxy, epoxy, and mercapto groups. Here, R is preferably selected from the viewpoints of industry and properties. 1 More than 80% of the R 3 are independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 3 The monovalent organic group having 1 to 20 carbon atoms and the above R 1 The same is preferred, and methyl, ethyl, propyl and butyl are preferred, and methyl and ethyl are more preferred.
[0132] The amount of component (E) used is 0 to 20 parts by mass, preferably 0 to 15 parts by mass, relative to 100 parts by mass of the polydiorganosiloxane having hydroxy groups at both ends as component (D). If the amount of component (E) is too large, the film may become brittle during coating and the durability may decrease.
[0133] Specific examples of the component (E) include methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, decyltrimethoxysilane, trifluoropropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-phenylyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxy Propyl trimethoxysilane, 3-methacryloxypropyl methyl diethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-acryloxypropyl trimethoxysilane, N-2-(aminoethyl)-3-aminopropyl methyl dimethoxysilane, N-2-(aminoethyl)-3-aminopropyl trimethoxysilane, 3-aminopropyl trimethoxysilane, 3-aminopropyl triethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butenyl) propylamine, N-phenyl-3-aminopropyl trimethoxysilane, 3-ureapropyl triethoxysilane, 3-mercaptopropyl methyl dimethoxysilane, 3-mercaptopropyl trimethoxysilane, bis(triethoxysilylpropyl) tetrasulfide, 3-isocyanate propyl triethoxysilane, etc., but are not limited to these examples.
[0134] [Component (B-1), component (B-2), component (C)]
[0135] The (B-1) component, the (B-2) component, and the (C) component used in the method for producing the emulsion composition of the present invention are the same as described above.
[0136] The polydiorganosiloxane having hydroxy groups at both ends as the component (D), the organoalkoxysilane as the component (E), the cationic surfactant as the components (B-1) and (B-2), and water as the component (C) are prepared into a uniform emulsion using an emulsifier such as a homomixer, a homogenizer, a colloid mill, a homodisper, or a line mixer, and then a base catalyst is added to carry out polymerization at 0 to 30° C. for 1 to 150 hours.
[0137] Here, examples of the base catalyst include sodium hydroxide, potassium hydroxide, lithium hydroxide, potassium fluoride, ammonia, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, benzyltrimethylammonium hydroxide, tetrabutylphosphonium hydroxide, trifluoromethylphenyltrimethylammonium hydroxide, etc. Among them, sodium hydroxide, potassium hydroxide, ammonia, tetramethylammonium hydroxide, tetrabutylammonium hydroxide, benzyltrimethylammonium hydroxide, and tetrabutylphosphonium hydroxide are preferred.
[0138] The amount of the base catalyst used is preferably 0.01 to 5 parts by mass, more preferably 0.03 to 5 parts by mass, relative to 100 parts by mass of the organosiloxane having hydroxyl groups at both ends as the component (D).
[0139] In addition, when the cationic surfactants as components (B-1) and (B-2) are converted into quaternary ammonium hydroxide using an ion exchange resin, the quaternary ammonium hydroxide itself functions as an alkali catalyst component, and thus there is no need to add an alkali catalyst separately. In this way, when component (B-1) or component (B-2) itself functions as an alkali catalyst component, it is also equivalent to polymerizing the emulsion obtained by emulsifying and dispersing the above-mentioned components (D), (E), (B-1), (B-2) and (C) in the presence of an alkali catalyst in the preparation method of the emulsion composition of the present invention.
[0140] In addition, the polymerization temperature is 0 to 30°C. When it is lower than 0°C, the polymerization proceeds slowly and is not practical, and when it is higher than 30°C, the stability of the emulsion becomes unstable. Preferably, the polymerization temperature is 5 to 25°C. In addition, the polymerization time is 1 to 150 hours. When it is less than 1 hour, the polymerization is insufficient, and when it is longer than 150 hours, it becomes unsuitable for industry. The polymerization time is preferably 5 to 120 hours.
[0141] After a predetermined polymerization time, neutralization is performed to stop the polymerization reaction. Neutralization here can be performed using an acidic compound. Examples of the acidic compound include hydrochloric acid, formic acid, acetic acid, propionic acid, etc., preferably hydrochloric acid, formic acid, and acetic acid. In addition, ion exchange resins can be used instead of acidic compounds for neutralization.
[0142] The cationic emulsion composition of the high-polymerization organosiloxane of the present invention obtained by the above method can be suitably used as a fiber treatment agent, a mold release agent, a water repellent, a cosmetic raw material, etc., and can be given excellent softness, lubricity, water repellency, volume, etc. by treating various fibers, leather, paper, hair, etc. In addition, as fibers, there can be listed: natural fibers such as cotton, linen, silk, and wool; synthetic fibers such as polyester, polyamide, polyacrylonitrile, polyethylene, polypropylene, vinylon (vinylon), polyvinyl chloride, spandex (spandex), etc.; semi-synthetic fibers such as acetate fibers, etc., but are not limited to these fibers.
[0143] Various thickeners, pigments, dyes, penetrants, antistatic agents, defoamers, flame retardants, antibacterial agents, preservatives, water repellents, crosslinking agents, adhesion enhancers or other silicone oils, silicone resins, silica, acrylic resins, polyurethane resins, etc. can be appropriately blended into the cationic emulsion composition of the high polymerization degree organosiloxane of the present invention.
[0144] The cationic emulsion composition of the high-polymerization organosiloxane of the present invention can form a coating after drying, and can be used to treat the surface of various substrates such as fiber, paper, metal, wood, rubber, plastic, glass, etc. The method of coating on the substrate can be various coating methods known in the past such as dipping, spraying, roller coating, rod coating, brush coating, etc.
[0145] Example
[0146] Hereinafter, the present invention will be specifically described with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples. In the following examples, "%" means "mass %".
[0147] [Example 1]
[0148] Use a homogenizer and a disperser to mix 300 g of a mixture of the general formula HO-[(CH3)2SiO] n -H) (component (D)) (where n is about 310 and the viscosity at 25°C is 1,500 mPa·s), 4.3 g of triethoxyphenylsilane (component (E)), 24.0 g of trioctylmethylammonium chloride (component (B-1)) whose active ingredient is a 75% IPA (isopropyl alcohol) solution (TOMAC-75: manufactured by Lion Specialty Chemicals Co., Ltd.), 18.0 g of behenyltrimethylammonium chloride (component (B-2)) whose active ingredient is an 80% ethanol product (LIPOQUAD22-80: manufactured by Lion Specialty Chemicals Co., Ltd.), and 239.3 g of ion exchange water (component (C)) were uniformly emulsified and dispersed to obtain an emulsion. To this emulsion, 6.6 g of a 30% aqueous ammonia solution (alkaline catalyst) was added. Then, the liquid temperature was lowered to 15° C., and polymerization was carried out for 24 hours, followed by neutralization with 7.8 g of acetic acid, whereby emulsion A was obtained.
[0149] [Example 2]
[0150] Emulsion B was obtained in the same manner as in Example 1 except that the ion exchange water in Example 1 was changed to 215.3 g and 24.0 g of polyoxyethylene alkyl ether EMULGEN 109P (manufactured by Kao Corporation) was further added as a nonionic emulsifier.
[0151] [Example 3]
[0152] Emulsion C was obtained in the same manner as in Example 2 except that the IPA solution containing 75% of trioctylmethylammonium chloride as an active ingredient (TOMAC-75: manufactured by Lion Specialty Chemicals Co., Ltd.) in Example 2 was changed to 3.0 g and the ion exchange water was changed to 236.3 g.
[0153] [Example 4]
[0154] Emulsion D was obtained in the same manner as in Example 2 except that the IPA solution containing 75% of trioctylmethylammonium chloride as an active ingredient (TOMAC-75: manufactured by Lion Specialty Chemicals Co., Ltd.) in Example 2 was changed to 12.0 g and the ion exchange water was changed to 227.3 g.
[0155] [Example 5]
[0156] Emulsion E was obtained in the same manner as in Example 4 except that the polymerization conditions in Example 4 were set to polymerization at 15° C. for 48 hours.
[0157] [Example 6]
[0158] Emulsion F was obtained in the same manner as in Example 4 except that the ion exchange water in Example 4 was changed to 231.6 g and 2.3 g of 85% KOH was added instead of the 30% ammonia aqueous solution.
[0159] [Comparative Example 1]
[0160] Emulsion G was obtained in the same manner as in Example 1, except that the triethoxyphenylsilane in Example 1 was changed to 1.1 g, the ion exchange water was changed to 258.7 g, and the IPA solution containing 75% of trioctylmethylammonium chloride as an active ingredient (TOMAC-75: manufactured by Lion Specialty Chemicals Co., Ltd.) and the ethanol product containing 80% of behenyltrimethylammonium chloride as an active ingredient (LIPOQUAD 22-80: manufactured by Lion Specialty Chemicals Co., Ltd.) were further changed to 25.8 g of an aqueous solution containing 30% of hexadecyltrimethylammonium chloride as an active ingredient (QUARTAMIN 60W: manufactured by Kao Corporation).
[0161] [Comparative Example 2]
[0162] Emulsion H was obtained in the same manner as in Comparative Example 1 except that the polymerization conditions in Comparative Example 1 were set to polymerization at 15° C. for 96 hours.
[0163] [Comparative Example 3]
[0164] Emulsion I was obtained in the same manner as in Comparative Example 1 except that the triethoxyphenylsilane in Comparative Example 1 was changed to 4.3 g, and the ion exchange water was changed to 255.5 g.
[0165] [Comparative Example 4]
[0166] Emulsion J was obtained in the same manner as in Comparative Example 3, except that the aqueous solution containing 30% of the active ingredient of hexadecyltrimethylammonium chloride (QUARTAMIN60W: manufactured by Kao Corporation) in Comparative Example 3 was changed to 24.0 g of an IPA solution containing 75% of the active ingredient of trioctylmethylammonium chloride (TOMAC-75: manufactured by Lion Specialty Chemicals Co., Ltd.), and the ion-exchanged water was changed to 257.3 g.
[0167] [Comparative Example 5]
[0168] The same method as in Comparative Example 4 was followed except that 25.8 g of an aqueous solution containing 30% of the active ingredient of cetyltrimethylammonium chloride (QUARTAMIN 60W: manufactured by Kao Corporation) was added and the ion-exchanged water was changed to 231.5 g. However, since emulsion K could not be produced with this composition, physical properties and characteristic evaluations were not carried out.
[0169] [Comparative Example 6]
[0170] Emulsion L was obtained by uniformly emulsifying and dispersing 300 g of linear dimethyl silicone oil having a viscosity of 800,000 mPa·s at 25° C., 21.6 g of an aqueous solution containing 30% of the active ingredient of cetyltrimethylammonium chloride (QUARTAMIN 60W: manufactured by Kao Corporation), and 235.2 g of ion-exchanged water using a homogenizer and a disperser.
[0171] The physical properties and characteristics of the emulsions obtained in Examples 1 to 6 and Comparative Examples 1 to 6 were measured by the following evaluation methods. The results are shown in Tables 1 and 2.
[0172] (Viscosity of extracted polysiloxane)
[0173] 300 g of emulsions A to L were added to 2 L of IPA while stirring, thereby breaking the emulsion to extract polydiorganosiloxane, and the polydiorganosiloxane was dried at 105° C. for 3 hours, and then the viscosity was measured at 25° C. using a BH type rotational viscometer. In addition, when the viscosity can be measured in liquid form, it is directly measured. When the viscosity is too high to be measured, the 10% toluene solution viscosity is measured. When the viscosity is too high to be measured, the viscosity is always 300,000 mPa·s or more.
[0174] (Whether a film is formed)
[0175] 20 g of emulsions A to L were dispensed into PP (polypropylene) trays, dried at 25° C. for 48 hours, and then further dried at 105° C. for 1 hour, and the formation of a coating was evaluated.
[0176] ○: Film formed
[0177] ×: No film was formed (remained liquid)
[0178] (Storage stability)
[0179] The appearance after standing at 25°C for 1 month was evaluated visually.
[0180] ○: No separation
[0181] △: Slightly separated
[0182] ×: Completely separated
[0183] (Texture of processed cloth)
[0184] Emulsions A to L were diluted with ion exchange water to prepare treatment solutions so that the polyorganosiloxane concentration was 1%. Polyester cotton plain weave cloth (T / C broadcloth) was immersed in the treatment solution for 10 seconds, then squeezed with a roller at a squeeze rate of 100%, and dried at 150°C for 2 minutes. The treated cloth was then evaluated for feel, and compared with untreated cloth for softness and smoothness.
[0185] ○: Good
[0186] ×: Untreated fabric grade
[0187] (Washing durability of treated cloth)
[0188] Emulsions A to L were diluted with ion exchange water to prepare a treatment solution so that the polyorganosiloxane concentration was 1%. After the polyester-cotton plain weave cloth was immersed in the treatment solution for 10 seconds, it was squeezed out using a roller at a squeeze rate of 100%, and dried at 150°C for 2 minutes. Then, the treated cloth was cut into half, and one of the treated cloths was washed once using a washing machine according to the method based on JIS L0217 103, and then dried at room temperature for one day. The amount of polysiloxane residue on the fiber surface of the treated cloth before and after washing was measured using an X-ray fluorescence analyzer (manufactured by Rigaku Corporation), and the residual rate (%) after washing was calculated.
[0189] [Table 1]
[0190]
[0191] [Table 2]
[0192]
[0193] As shown in Tables 1 and 2, the cationic emulsion composition of the high-polymerization polyorganosiloxane of the present invention can be polymerized in a relatively short time even if it has a high viscosity, and has the ability to form a film, so it has excellent durability when treating fibers, and the texture of the treated cloth is also good. Further, the cationic emulsion composition of the high-polymerization polyorganosiloxane of the present invention also has excellent storage stability. In contrast, the cationic emulsion composition obtained by the composition of the comparative example has high stability, but does not have the ability to form a film, and has poor durability when treating fibers, or has the ability to form a film, but the stability of the emulsion is low and it separates quickly.
[0194] Industrial Applicability
[0195] By using the cationic emulsion composition of the high-polymerization polyorganosiloxane of the present invention as a fiber treatment agent, it is possible to impart good softness to the fiber, and the fiber also has excellent durability, so that the fiber can maintain good softness even after washing. Furthermore, when the cationic emulsion composition of the high-polymerization polyorganosiloxane of the present invention is treated and dried, the film formed has high durability, so it is also excellent in versatility, and can be widely used in release agents, water repellents, cosmetics, hair cosmetics, etc. in addition to fiber treatment agents.
Claims
1. A cationic emulsion composition of polyorganosiloxane, characterized in that: It contains: 100 parts by mass of (A) a polyorganosiloxane represented by the following average composition formula (1) and having a viscosity of 300,000 mPa·s or more at 25° C., In formula (1), R 1 are independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, R 2 are independently selected from the above R 1 The group, hydroxyl group or alkoxy group having 1 to 20 carbon atoms in the options, a, b, c, d are values such that the viscosity of the polyorganosiloxane at 25°C satisfies 300,000 mPa·s or more, and a≥2, c+d≥1; 0.7 to 15 parts by mass of (B-1) cationic surfactant Q 1 3(CH3)N + ·X - , Among them, Q 1 are monovalent organic groups having 6 to 30 carbon atoms of the same or different types, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms; 1 to 15 parts by mass of (B-2) cationic surfactant Q 2 (CH3)3N + ·X-, Among them, Q 2 is a monovalent organic group having 17 to 30 carbon atoms, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms; 30 to 3,000 parts by mass of (C) water.
2. The cationic emulsion composition of polyorganosiloxane according to claim 1, characterized in that: It further comprises a nonionic surfactant.
3. The cationic emulsion composition of polyorganosiloxane according to claim 1, characterized in that: After drying, a coating is formed.
4. The cationic emulsion composition of polyorganosiloxane according to claim 2, characterized in that: After drying, a coating is formed.
5. A fiber treating agent, characterized in that A cationic emulsion composition comprising the polyorganosiloxane according to any one of claims 1 to 4.
6. A release agent, characterized in that A cationic emulsion composition comprising the polyorganosiloxane according to any one of claims 1 to 4.
7. A water repellent, characterized in that A cationic emulsion composition comprising the polyorganosiloxane according to any one of claims 1 to 4.
8. A cosmetic, characterized in that: A cationic emulsion composition comprising the polyorganosiloxane according to any one of claims 1 to 4.
9. A hair cosmetic, characterized in that: A cationic emulsion composition comprising the polyorganosiloxane according to any one of claims 1 to 4.
10. A method for preparing a cationic emulsion composition of polyorganosiloxane, characterized in that: In the presence of an alkali catalyst, the emulsion is polymerized at 0 to 30° C. for 1 to 150 hours and further neutralized. The emulsion is obtained by emulsifying and dispersing the following components: 100 parts by mass of (D) general formula HO-[R 1 2SiO] j -H represented by a polydiorganosiloxane having hydroxyl groups at both ends, wherein R 1 are independently hydrogen atoms or monovalent organic groups having 1 to 20 carbon atoms, and j is a value such that the viscosity of the polydiorganosiloxane having hydroxyl groups at both ends at 25° C. is less than 2,000 mPa·s; parts by mass of (E) any one or two or more of the following organoalkoxysilanes, Si(OR 3 )4、R 1 Si(OR 3 )3、R 1 2Si(OR 3 )2、R 1 3Si(OR 3 ), Among them, R 1 are independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, R 3 are independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms; 0.7 to 15 parts by mass of (B-1) cationic surfactant Q 1 3(CH3)N + ·X-, Among them, Q 1 are monovalent organic groups having 6 to 30 carbon atoms of the same or different types, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms; 1 to 15 parts by mass of (B-2) cationic surfactant Q 2 (CH3)3N + ·X-, Among them, Q 2 is a monovalent organic group having 17 to 30 carbon atoms, and X is a halogen atom or a monovalent carboxyl group having 1 to 6 carbon atoms; 30 to 3,000 parts by mass of (C) water.