A manganese-based denitration catalyst and its preparation method and application
By adding cerium and titanium to the manganese oxide to form a bimetal single atom Ce-Ti modified manganese oxide catalyst, the problems of poor performance of manganese-based denitrification catalyst under low temperature conditions are solved, and the water and sulfur resistance effect is poor is achieved. Efficient NOx conversion and environmentally friendly low-cost preparation.
Patent Information
- Application Number
- CN202210258431.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-16
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-03-16
AI Technical Summary
The existing manganese-based denitrification catalysts have poor performance, poor water and sulfur resistance under low temperature conditions, complex preparation process, high environmental pollution, and high production costs, making it difficult to meet the needs of industrial applications.
Using a catalyst with manganese oxide as the main body, by adding cerium and titanium sources, bimetallic single atoms Ce and Ti work together in the manganese oxide crystal lattice to prepare a manganese-based denitrification catalyst with good water and sulfur resistance. The process is simple. , low cost and pollution-free.
It achieves high-efficiency NOx conversion under low temperature conditions. The NO conversion rate of the catalyst below 100℃ can reach more than 40.2%, and the NO conversion rate of the catalyst below 150℃ can reach more than 93.3%, and has excellent water and sulfur resistance. Simple process, environmentally friendly and low cost.
Smart Images

Figure CN114797840B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to low temperature NH 3 - The technical field of SCR denitration catalytic materials and their preparation, relates to a manganese-based denitration catalyst and its preparation method and application. Background Art
[0002] Ammonia selective catalytic reduction technology (NH 3 -SCR) is the most mature technology currently used in the field of fixed source flue gas denitrification and mobile source tail gas denitrification, and the denitrification efficiency can reach more than 90%. 2 O 5 -WO 3 (MoO 3 ) / TiO 2 As a typical commercial SCR catalyst, it has been widely used in power plants, steel mills, glass kilns and other fields. However, since the operating temperature of traditional SCR is generally 300-400℃ or even higher, SO will occur in the flue gas at this temperature. 2 and NH 3 In addition, due to the use of waste heat power generation and energy-saving equipment, the flue gas emission temperature of many industrial boilers (kilns) in operation in my country (such as industrial boilers, glass and ceramic kilns, cement kilns, steel metallurgical sintering furnaces, etc.) and processes involving the production and use of nitric acid is relatively low (120-300℃), making it difficult to directly use medium and high temperature SCR catalytic processes to treat NO. x The low-temperature SCR technology catalyst has an operating temperature below 250°C, and the reactor can be placed after desulfurization and dust removal, thus avoiding SO 2 , smoke and high temperature. Compared with high-temperature SCR technology, low-temperature SCR technology has higher economic practicality. The development of efficient low-temperature SCR catalyst is the core of low-temperature SCR denitrification technology and the current research focus in the field of SCR denitrification at home and abroad.
[0003] The transition metal oxides reported in the current research, such as Mn, Fe and Ce-based oxides, have good NH 3 -SCR activity. Among them, Mn-based denitrification catalytic materials have excellent denitrification activity at low temperatures due to their superior redox ability. However, Mn-based denitrification catalytic materials have the disadvantage of being intolerant to sulfur and water in the low temperature range, which greatly hinders the application of SCR denitrification catalysts.
[0004] Many researchers have introduced other elements into manganese oxide to improve its water and sulfur resistance.
[0005] Jin et al. (Applied Catalysis B: Environmental, 2014, 148-149: 582-588) reported a sol-gel method for preparing Mn-Ce / TiO 2 The method comprises the following steps: 2 The catalyst exhibits good water and sulfur resistance in low-temperature denitrification reactions, but its water vapor content is only 3%, and the catalyst preparation cycle is long, so its industrial application is of little significance.
[0006] CN104289227A discloses a supported four-component metal catalyst for low-temperature flue gas denitration and a preparation method thereof. The catalyst is prepared by calcining nitrates of elements such as Mn, Co, and Ce on nano-scale P25 using an impregnation method, and the NO conversion rate is higher than 90% in the low temperature range of 150-200°C.
[0007] CN104785246A discloses a supported low-temperature SCR catalyst and a preparation method thereof. 2 O 3 As the carrier, manganese oxide as the active ingredient, cerium oxide as the modifier, the activity reaches 100% under the reaction conditions of 120-240°C. However, the active temperature window of these two types of catalysts is narrow, and the water and sulfur resistance of the catalysts have not been studied.
[0008] CN111992203A discloses a Mn-Ce-O / TiO 2 The preparation method of the catalyst comprises dissolving manganese nitrate, cerium nitrate and fuel in deionized water, and adding TiO 2 The product was placed in a preheated combustion chamber and burned rapidly, and then continued to be roasted for a certain period of time to obtain Mn-Ce-O / TiO 2 Denitration catalyst. The catalyst prepared by this method exhibits good water and sulfur resistance in low-temperature denitration reactions, but the preparation method is complicated and dangerous, and the raw materials need to be burned during the preparation process, which causes great environmental pollution.
[0009] The manganese-based catalyst described in the above scheme has the disadvantages of poor low-temperature performance, poor sulfur and water resistance, long preparation process, difficult operation, environmental pollution and high production cost. Therefore, a simple preparation method and low-temperature NH 3 -SCR denitrification efficiency is high, sulfur and water resistance is good, and the cost is low. Manganese-based catalysts are very necessary. Summary of the invention
[0010] The object of the present invention is to provide a manganese-based denitration catalyst and a preparation method and application thereof. The catalyst of the present invention is 3- It has good low temperature activity and strong water and sulfur resistance in SCR denitration reaction. The preparation method of the catalyst is simple, low cost, pollution-free and easy to implement.
[0011] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0012] In a first aspect, the present invention provides a method for preparing a manganese-based denitration catalyst, the preparation method comprising the following steps:
[0013] (1) mixing a manganese source, a cerium source, a titanium source and a solvent to obtain a mixed solution;
[0014] (2) grinding the mixed solution obtained in step (1), washing, and drying to obtain a precursor;
[0015] (3) calcining the precursor obtained in step (2) to obtain the manganese-based denitration catalyst.
[0016] In the preparation method of the manganese-based denitration catalyst of the present invention, manganese oxide is used as the main body, cerium source and titanium source are added, bimetallic single atoms Ce and Ti are confined in the manganese oxide lattice, and the synergistic effect of Ce-Ti bimetallic single atoms improves the manganese-based catalyst in low temperature NH 3 - Water and sulfur resistance in SCR denitrification reaction.
[0017] Preferably, the manganese source in step (1) comprises potassium permanganate and divalent manganese salt.
[0018] Preferably, the divalent manganese salt includes any one of manganese nitrate, manganese acetate, manganese chloride or manganese sulfate, or a combination of at least two thereof.
[0019] Preferably, the manganese source comprises potassium permanganate and manganese nitrate.
[0020] Preferably, the cerium source includes any one of cerium nitrate, cerium carbonate, cerium chloride or cerium acetate, or a combination of at least two thereof.
[0021] Preferably, the titanium source includes any one of titanium tetrachloride, tetrabutyl titanate or titanyl sulfate, or a combination of at least two thereof.
[0022] Preferably, the solvent comprises deionized water.
[0023] Preferably, the molar ratio of potassium permanganate to divalent manganese salt is 1:(0.5-2), for example: 1:0.5, 1:0.8, 1:1, 1:1.2, 1:1.5 or 1:2, etc.
[0024] Preferably, the mass ratio of the manganese source, cerium source and titanium source in step (1) is (0.5-2):(0.0007-0.05):(0.002-0.13), for example: 0.8:0.001:0.002, 1:0.005:0.01, 1.2:0.008:0.05, 1.5:0.009:0.008, 1:0.01:0.02 or 1:0.03:0.13, etc.
[0025] Preferably, the grinding treatment in step (2) comprises ball milling.
[0026] Preferably, the ball milling speed is 100 to 1000 rpm, such as 200 rpm, 400 rpm, 600 rpm, 800 rpm or 1000 rpm, etc., preferably 400 to 600 rpm.
[0027] Preferably, the ball milling time is 0.5 to 6 h, such as 0.5 h, 1 h, 2 h, 4 h, 5 h or 6 h, etc., preferably 0.5 to 3 h.
[0028] Preferably, during the grinding process in step (2), the mass ratio of the grinding beads to the solute in the mixed solution is (10-40):1, for example: 10:1, 15:1, 20:1, 30:1 or 40:1, etc., preferably (10-20):1.
[0029] Preferably, the temperature of the calcination treatment in step (3) is 300-600°C, for example, 300°C, 400°C, 500°C or 600°C, preferably 300-400°C.
[0030] Preferably, the calcination treatment time is 2 to 6 hours, such as 2 hours, 3 hours, 4 hours, 5 hours or 6 hours, preferably 3 to 5 hours.
[0031] As a preferred embodiment of the present invention, the preparation method comprises the following steps:
[0032] (1) mixing a manganese source, a cerium source, and a titanium source with a solvent in a mass ratio of 1:(0.001-3):(0.001-3) to obtain a mixed solution;
[0033] (2) grinding the mixed solution obtained in step (1) at 400-600 rpm for 0.5-3 h, washing and drying to obtain a precursor;
[0034] (3) The precursor obtained in step (2) is calcined at 300-400° C. for 3-5 hours to obtain the manganese-based denitration catalyst.
[0035] In a second aspect, the present invention provides a manganese-based denitration catalyst, which is prepared by the method described in the first aspect.
[0036] Preferably, the mass proportion of titanium in the manganese-based denitration catalyst is 0.1-3%, for example: 0.1%, 0.2%, 0.5%, 1%, 2% or 3%, etc., preferably 0.1-1%;
[0037] Preferably, the mass proportion of cerium in the manganese-based denitration catalyst is 0.1-3%, for example: 0.1%, 0.2%, 0.5%, 1%, 2% or 3%, etc., preferably 0.1-1%.
[0038] In a third aspect, the present invention provides an application of the manganese-based denitration catalyst as described in the second aspect, wherein the manganese-based denitration catalyst is used for low-temperature NH 3 -SCR denitrification reaction.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] (1) The catalyst of the present invention is 3 - It has good low temperature activity and strong water and sulfur resistance in SCR denitration reaction. The preparation method of the catalyst is simple, low cost, pollution-free and easy to implement.
[0041] (2) The manganese-based denitration catalyst of the present invention has a NO conversion rate of more than 40.2% at 100°C, a NO conversion rate of more than 93.3% at 150°C, a NO conversion rate of more than 94.3% at 200°C, a NO conversion rate of more than 92.3% at 250°C, and a NO conversion rate of more than 92.8% at 300°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a spherical aberration electron microscope image of the manganese-based denitration catalyst prepared in Example 1 of the present invention.
[0043] Figure 2 is NH of Example 1 of the present invention and Comparative Examples 1-4 3 -SCR water and sulfur resistance performance diagram. DETAILED DESCRIPTION
[0044] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0045] Example 1
[0046] This embodiment provides a manganese-based denitration catalyst, and the preparation method of the manganese-based denitration catalyst is as follows:
[0047] (1) Weighing 1.5 g of potassium permanganate, 1.23 g of manganese chloride, 0.02 g of cerium acetate, 0.03 g of titanyl sulfate and 3.5 ml of deionized water to obtain a mixed solution;
[0048] (2) The mixed solution obtained in step (1) was mixed with 125.6 g of ball mill beads, and the mixed raw materials were ball milled at a speed of 580 rpm for 4 h to obtain a solid powder, which was washed several times with deionized water and dried;
[0049] (3) calcining in a tubular furnace at 400° C. for 6 h to obtain the manganese-based denitration catalyst, wherein the loading amount of Ce is 1% and the loading amount of Ti is 1%.
[0050] The spherical aberration electron microscope image of the manganese-based denitrification catalyst is as follows Figure 1 shown.
[0051] Example 2
[0052] This embodiment provides a manganese-based denitration catalyst, and the preparation method of the manganese-based denitration catalyst is as follows:
[0053] (1) Weigh 1.5 g of potassium permanganate, 2.3 g of manganese sulfate, 0.19 g of cerium carbonate, and 0.08 g of titanium tetrachloride and mix with 2 ml of deionized water to obtain a mixed solution;
[0054] (2) The mixed solution obtained in step (1) was mixed with 60.7 g of ball mill beads, and the mixed raw materials were ball milled at a speed of 500 rpm for 4 h to obtain a solid powder, which was washed several times with deionized water and dried;
[0055] (3) The manganese-based denitration catalyst is calcined in a tubular furnace at 450° C. for 6 h, wherein the loading amount of Ce is 3% and the loading amount of Ti is 1%.
[0056] Example 3
[0057] This embodiment provides a manganese-based denitration catalyst, and the preparation method of the manganese-based denitration catalyst is as follows:
[0058] (1) Weighing 1.5 g of potassium permanganate, 4.9 g of manganese acetate, 0.18 g of cerium nitrate, and 0.014 g of tetrabutyl titanate and mixing them with 1.5 ml of deionized water to obtain a mixed solution;
[0059] (2) The mixed solution obtained in step (1) was mixed with 78.1 g of ball mill beads, and the mixed raw materials were ball milled at a speed of 100 rpm for 0.5 h to obtain a solid powder, which was washed several times with deionized water and dried;
[0060] (3) Calcination in a tubular furnace at 300° C. for 6 h to obtain the manganese-based denitration catalyst, wherein the loading amount of Ce is 3% and the loading amount of Ti is 0.1%.
[0061] Example 4
[0062] This embodiment provides a manganese-based denitration catalyst, and the preparation method of the manganese-based denitration catalyst is as follows:
[0063] (1) Weighing 1.5 g of potassium permanganate, 2.9 g of manganese chloride, 0.18 g of cerium nitrate, and 0.24 g of titanium tetrachloride and mixing them with 3 ml of deionized water to obtain a mixed solution;
[0064] (2) The mixed solution obtained in step (1) was mixed with 80.9 g of ball mill beads, and the mixed raw materials were ball milled at a speed of 580 rpm for 4 h to obtain a solid powder, which was washed several times with deionized water and dried;
[0065] (3) calcining in a tubular furnace at 500° C. for 2 h to obtain the manganese-based denitration catalyst, wherein the loading amount of Ce is 3% and the loading amount of Ti is 3%.
[0066] Example 5
[0067] This embodiment provides a manganese-based denitration catalyst, and the preparation method of the manganese-based denitration catalyst is as follows:
[0068] (1) Weighing 1.5 g of potassium permanganate, 2.3 g of manganese sulfate, 0.003 g of cerium chloride, and 0.21 g of titanyl sulfate and mixing them with 3 ml of deionized water to obtain a mixed solution;
[0069] (2) The mixed solution obtained in step (1) was mixed with 104.2 g of ball mill beads, and the mixed raw materials were ball milled at a speed of 600 rpm for 4 h to obtain a solid powder, which was washed several times with deionized water and dried;
[0070] (3) calcining at 350° C. for 2 h in a tubular furnace to obtain the manganese-based denitration catalyst, wherein the loading amount of Ce is 0.1% and the loading amount of Ti is 3%.
[0071] Example 6
[0072] This embodiment provides a manganese-based denitration catalyst, and the preparation method of the manganese-based denitration catalyst is as follows:
[0073] (1) Weighing 1.5 g of potassium permanganate, 5.4 g of manganese nitrate, 0.06 g of cerium nitrate, 0.04 g of titanium tetrachloride and 3.5 ml of deionized water to obtain a mixed solution;
[0074] (2) The mixed solution obtained in step (1) was mixed with 162.1 g of ball mill beads, and the mixed raw materials were ball milled at a speed of 800 rpm for 4 h to obtain a solid powder, which was washed several times with deionized water and dried;
[0075] (3) calcining in a tubular furnace at 600° C. for 2 h to obtain the manganese-based denitration catalyst, wherein the loading amount of Ce is 1% and the loading amount of Ti is 0.5%.
[0076] Example 7
[0077] This embodiment provides a manganese-based denitration catalyst, and the preparation method of the manganese-based denitration catalyst is as follows:
[0078] (1) Weighing 1.5 g of potassium permanganate, 2.3 g of manganese sulfate, 0.04 g of cerium chloride, and 0.23 g of titanium tetrachloride and mixing them with 4 ml of deionized water to obtain a mixed solution;
[0079] (2) The mixed solution obtained in step (1) was mixed with 161.4 g of ball mill beads, and the mixed raw materials were ball milled at a speed of 1000 rpm for 4 h to obtain a solid powder, which was washed several times with deionized water and dried;
[0080] (3) calcining in a tubular furnace at 500° C. for 5 h to obtain the manganese-based denitration catalyst, wherein the loading amount of Ce is 1% and the loading amount of Ti is 3%.
[0081] Example 8
[0082] This embodiment provides a manganese-based denitration catalyst, and the preparation method of the manganese-based denitration catalyst is as follows:
[0083] (1) Weighing 1.5 g of potassium permanganate, 3.6 g of manganese acetate, 0.12 g of cerium nitrate, and 0.14 g of tetrabutyl titanate and mixing them with 2.5 ml of deionized water to obtain a mixed solution;
[0084] (2) The mixed solution obtained in step (1) was mixed with 154.3 g of ball mill beads, and the mixed raw materials were ball milled at a speed of 400 rpm for 1 h to obtain a solid powder, which was washed several times with deionized water and dried;
[0085] (3) calcining in a tubular furnace at 400° C. for 2 h to obtain the manganese-based denitration catalyst, wherein the loading amount of Ce is 2% and the loading amount of Ti is 1%.
[0086] Example 9
[0087] This embodiment provides a manganese-based denitration catalyst, and the preparation method of the manganese-based denitration catalyst is as follows:
[0088] (1) Weighing 1.5 g of potassium permanganate, 3.1 g of manganese oxalate, 0.06 g of cerium chloride, and 0.13 g of titanyl sulfate and mixing them with 2.5 ml of deionized water to obtain a mixed solution;
[0089] (2) The mixed solution obtained in step (1) was mixed with 165.1 g of ball mill beads, and the mixed raw materials were ball milled at a speed of 600 rpm for 6 h to obtain a solid powder, which was washed several times with deionized water and dried;
[0090] (3) calcining at 350° C. for 3 h in a tubular furnace to obtain the manganese-based denitration catalyst, wherein the loading amount of Ce is 2% and the loading amount of Ti is 2%.
[0091] Example 10
[0092] This embodiment provides a manganese-based denitration catalyst, and the preparation method of the manganese-based denitration catalyst is as follows:
[0093] (1) Weighing 1.5 g of potassium permanganate, 2.9 g of manganese chloride, 0.06 g of cerium nitrate, and 0.28 g of tetrabutyl titanate and mixing them with 2.5 ml of deionized water to obtain a mixed solution;
[0094] (2) The mixed solution obtained in step (1) was mixed with 180.2 g of ball mill beads, and the mixed raw materials were ball milled at a speed of 700 rpm for 2 h to obtain a solid powder, which was washed several times with deionized water and dried;
[0095] (3) calcining at 600° C. for 3 h in a tubular furnace to obtain the manganese-based denitration catalyst, wherein the loading amount of Ce is 1% and the loading amount of Ti is 2%.
[0096] Comparative Example 1
[0097] The difference between this comparative example and Example 1 is that only Ce is loaded, and other parameters and conditions are exactly the same as in Example 1, to obtain a single-atom Ce-modified manganese oxide catalyst, wherein the Ce loading is 1%, and other conditions and parameters are the same as in Example 1.
[0098] Comparative Example 2
[0099] The only difference between this comparative example and Example 1 is that only Ti is loaded, and the other parameters and conditions are exactly the same as those in Example 1, thereby obtaining a single-atom Ti-modified manganese oxide catalyst, wherein the loading amount of Ti is 1%.
[0100] Comparative Example 3
[0101] The only difference between this comparative example and Example 1 is that Ce and Ti are not loaded, and other parameters and conditions are exactly the same as those in Example 1, to obtain a manganese oxide catalyst.
[0102] Comparative Example 4
[0103] This comparative example is commercial MnO 2 catalyst.
[0104] Performance Testing:
[0105] The catalysts obtained in Examples 1-10 and Comparative Examples 1-4 were subjected to NH 3 -SCR catalytic activity test, the catalyst performance test is carried out in a micro fixed bed device, specifically including: weighing a certain amount of catalyst and quartz sand respectively, mixing them evenly, placing the above mixture in a laboratory-made fixed bed reactor, and ensuring that the catalyst filling volume is 1.5mL. Then, 600ppm NO / 600ppm NH 3 / 6%O 2 SO 2 / 50ppm and 10%H 2 O,N 2 As a balance gas, the space velocity (GHSV) is 40000h -1 The reactor temperature was raised from 100°C to 300°C at a rate of 5°C / min. After each test temperature point was stable for 30 minutes, the NO concentration was recorded by the testo 350 flue gas analyzer. The NO conversion rate was calculated as follows:
[0106]
[0107] Where [NO] in Refers to the NO concentration at the reactor inlet, [NO] out Refers to the NO concentration at the reactor outlet. Test results
[0108] The test results are shown in Table 1:
[0109] Table 1
[0110]
[0111]
[0112] As can be seen from Table 1, from Examples 1-10, the manganese-based denitration catalyst of the present invention can achieve a conversion rate of catalytic denitration of NO of more than 40.2% at 100°C, a conversion rate of catalytic denitration of NO of more than 93.3% at 150°C, a conversion rate of catalytic denitration of NO of more than 94.3% at 200°C, a conversion rate of catalytic denitration of NO of more than 92.3% at 250°C, and a conversion rate of catalytic denitration of NO of more than 92.8% at 300°C.
[0113] By comparing Example 1 with Examples 2-10, it can be seen that the mass ratio of cerium to titanium in the manganese-based denitration catalyst of the present invention affects its performance. When the mass ratio of cerium to titanium in the manganese-based denitration catalyst is controlled at 0.1-1%, the catalytic effect of the manganese-based denitration catalyst is better.
[0114] In the preparation method of the present invention, the calcination temperature will affect the catalytic performance of the obtained manganese-based denitration catalyst. The calcination temperature is controlled at 300-400°C, and the catalytic performance of the obtained manganese-based denitration catalyst is better. If the calcination temperature is too low, the precursor salt will be incompletely decomposed, and the grain size of manganese oxide will deteriorate, and the side reactions will increase during the reaction, resulting in a decrease in the selectivity of the product N2; if the calcination temperature is too high, single atoms are prone to agglomeration and sintering, and the grain size will increase, and the activity of the catalyst will decrease.
[0115] From the comparison between Example 1 and Comparative Examples 1-4, it can be seen that the adjacent bimetallic single atoms Ce and Ti in the catalyst of the present invention are confined in the manganese oxide lattice, and the synergistic effect of the Ce-Ti bimetallic single atoms improves the low-temperature NH 3 - Water and sulfur resistance in SCR denitrification reaction.
[0116] The water resistance and sulfur resistance of the catalysts obtained in Examples 1-10 and Comparative Examples 1-4 were tested in NH 3 -SCR reaction device. The specific operation of the experiment is the same as that of NH 3 -SCR experiment is basically the same, but the reaction atmosphere is changed to 600ppm NO / 600ppm NH 3 / 6%O 2 / 50ppm SO 2 / 10%H 2 O / N 2 , the experimental temperature is 150℃. Figure 2 The catalyst was in the presence of 10% H 2 O and 50 ppm SO 2 Activity changes under atmosphere, by Figure 2It can be seen that within 10 hours, the NO conversion rate of Example 1 is significantly better than that of the four comparative examples. It can be seen that the manganese oxide catalyst modified with Ce-Ti bimetallic single atoms obtained by the preparation method of the present invention has very excellent low-temperature denitrification activity and water and sulfur resistance, which is mainly attributed to the synergistic effect between Ce-Ti bimetallic single atoms in the catalyst.
[0117] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a manganese-based denitration catalyst, characterized in that: The preparation method comprises the following steps: (1) mixing a manganese source, a cerium source, a titanium source and a solvent to obtain a mixed solution; (2) grinding the mixed solution obtained in step (1), washing, and drying to obtain a precursor; (3) calcining the precursor obtained in step (2) to obtain the manganese-based denitration catalyst; The manganese source in step (1) comprises potassium permanganate and divalent manganese salt, the molar ratio of the potassium permanganate to the divalent manganese salt is 1:(0.5-2), and the molar ratio of the manganese source, the cerium source and the titanium source is (0.5-2):(0.0007-0.05):(0.002-0.13); The divalent manganese salt includes any one of manganese nitrate, manganese acetate, manganese chloride or manganese sulfate, or a combination of at least two of them; the cerium source includes any one of cerium nitrate, cerium carbonate, cerium chloride or cerium acetate, or a combination of at least two of them; the titanium source includes any one of titanium tetrachloride, tetrabutyl titanate or titanyl sulfate, or a combination of at least two of them; The grinding treatment in step (2) includes ball milling, the ball milling speed is 400-600 rpm, and the ball milling time is 0.5-3 h.
2. The preparation method according to claim 1, characterized in that The solvent includes deionized water.
3. The preparation method according to claim 1, characterized in that: During the grinding process in step (2), the mass ratio of the grinding beads to the solute in the mixed solution is (10-40):
1.
4. The preparation method according to claim 3, characterized in that: During the grinding process, the mass ratio of the grinding beads to the solute in the mixed solution is (10-20):
1.
5. The preparation method according to claim 1, characterized in that: The temperature of the calcination treatment in step (3) is 300-600°C.
6. The preparation method according to claim 5, characterized in that: The calcination temperature is preferably 300-400°C.
7. The preparation method according to claim 1, characterized in that: The calcination time is 2 to 6 hours.
8. The preparation method according to claim 7, characterized in that: The calcination time is 3 to 5 hours.
9. A manganese-based denitration catalyst, characterized in that: The manganese-based denitration catalyst is prepared by the method according to any one of claims 1 to 8.
10. The manganese-based denitration catalyst according to claim 9, characterized in that: The mass proportion of titanium in the manganese-based denitration catalyst is 0.1-3%.
11. The manganese-based denitration catalyst according to claim 10, characterized in that The mass proportion of titanium in the manganese-based denitration catalyst is 0.1-1%.
12. The manganese-based denitration catalyst according to claim 9, characterized in that: The mass proportion of cerium in the manganese-based denitration catalyst is 0.1-3%.
13. The manganese-based denitration catalyst according to claim 12, characterized in that: The mass proportion of cerium in the manganese-based denitration catalyst is 0.1-1%.
14. Use of the manganese-based denitration catalyst according to any one of claims 9 to 13, characterized in that: The manganese-based denitration catalyst is used for low-temperature NH3-SCR denitration reaction.