A lithium carbon dioxide battery positive electrode material catalyst and its preparation method and application

By using porous carbon nanotubes as cathode material catalysts for lithium carbon dioxide batteries, the problems of high overpotential and poor cycle stability of lithium carbon dioxide batteries are solved, and low-cost and efficient battery performance improvements are achieved.

CN114824321BActive Publication Date: 2024-10-18BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210231930.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-09
Publication Date
2024-10-18
Estimated Expiration
2042-03-09

AI Technical Summary

Technical Problem

Lithium carbon dioxide batteries have high overpotential, poor cycle stability and low energy efficiency due to the irreversible formation of insulation discharge product lithium carbonate. The synthesis process of existing carbon-based material catalysts is complex and consumes huge amounts of energy, which limits the development of lithium carbon dioxide batteries.

Method used

Porous carbon nanotubes are used as cathode material catalysts for lithium carbon dioxide batteries. A porous structure with sidewall openings is formed through thermal oxidation and acid treatment, which increases the physical surface area and active sites, and reduces preparation costs and energy consumption.

Benefits of technology

The electrochemical performance of lithium carbon dioxide batteries is improved, showing low overpotential and long-term cycle stability, increasing discharge capacity, simplifying the catalyst preparation process, and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114824321B_ABST
    Figure CN114824321B_ABST
Patent Text Reader

Abstract

The present invention discloses a positive electrode material catalyst for a lithium carbon dioxide battery, and a preparation method and application thereof. The positive electrode material catalyst for a lithium carbon dioxide battery is a porous carbon nanotube; the side wall of the porous carbon nanotube has an opening. The present invention also provides a preparation method and application of a positive electrode material catalyst for a lithium carbon dioxide battery. The positive electrode material catalyst for a lithium carbon dioxide battery provided by the present invention adopts a porous carbon nanotube, and the openings on the side wall thereof lead to an increase in the physical surface area, pore volume and active sites, which can store more discharge product lithium carbonate and promote its decomposition, and the preparation method is simple and efficient, with low energy consumption, which effectively reduces the cost; the electrochemical performance of the lithium carbon dioxide battery prepared by the catalyst is significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium carbon dioxide batteries, and more specifically, to a lithium carbon dioxide battery positive electrode material catalyst, a preparation method and application thereof. Background Art

[0002] As the demand for energy in modern industry continues to increase, fossil fuels have been overused worldwide, producing a large amount of carbon dioxide, leading to energy shortages and the greenhouse effect. Many chemical and physical technologies, such as carbon dioxide capture, carbon dioxide conversion, and metal carbon dioxide batteries, have been developed to reduce the concentration of carbon dioxide in the atmosphere.

[0003] Among them, based on the redox reaction between the lithium anode and the carbon dioxide cathode (4Li+3CO 2 =2Li 2 CO 3 +C) lithium carbon dioxide batteries are considered to be the most promising, as they have a high discharge potential (2.8 V) and a high theoretical energy density (1876 Wh kg-1).

[0004] However, the irreversible formation of the insulating discharge product lithium carbonate leads to problems such as high battery overpotential, poor cycle stability and low energy efficiency, which limits the development of lithium carbon dioxide batteries. Although several high-performance carbon-based catalysts for lithium carbon dioxide batteries have been reported in the literature, the synthesis process of such carbon-based catalysts is complex and energy-intensive. Therefore, reducing the battery overpotential and improving the battery cycle performance are important issues that need to be solved urgently.

[0005] Therefore, it is necessary to provide a catalyst that is easy to synthesize and has low energy consumption as a positive electrode material catalyst for a lithium carbon dioxide battery to solve one of the above problems. Summary of the invention

[0006] The first object of the present invention is to provide a positive electrode material catalyst for a lithium carbon dioxide battery.

[0007] The second object of the present invention is to provide a method for preparing a positive electrode material catalyst for a lithium carbon dioxide battery.

[0008] The third object of the present invention is to provide an application of a lithium carbon dioxide battery positive electrode material catalyst in the preparation of a lithium carbon dioxide battery positive electrode material.

[0009] The fourth object of the present invention is to provide a positive electrode material for a lithium carbon dioxide battery.

[0010] A fifth object of the present invention is to provide an application of a lithium carbon dioxide battery positive electrode material in the preparation of a lithium carbon dioxide battery.

[0011] A sixth object of the present invention is to provide a lithium carbon dioxide battery.

[0012] In order to achieve the above object, the present invention adopts the following technical solutions:

[0013] A lithium carbon dioxide battery positive electrode material catalyst, the lithium carbon dioxide battery positive electrode material catalyst is a porous carbon nanotube; the side wall of the porous carbon nanotube has an opening.

[0014] Preferably, the diameter of the porous carbon nanotube is 40-60 nm, more preferably 50 nm.

[0015] Preferably, the pore diameter of the side wall opening is 30-40 nm.

[0016] Preferably, the specific surface area of ​​the porous carbon nanotubes is 174 cm 2 / g.

[0017] As another aspect of the present invention, the present invention also provides a method for preparing the above-mentioned lithium carbon dioxide battery positive electrode material catalyst, comprising the following steps:

[0018] The multi-walled carbon nanotube powder is heated and oxidized, the heated product is mixed with an acid to obtain a mixture, the mixture is heated to reflux, and the lithium carbon dioxide battery positive electrode material catalyst is obtained through filtering, washing, drying and heat treatment.

[0019] Preferably, the conditions for heating and oxidizing the multi-walled carbon nanotube powder are: a heating rate of 1 to 10°C / min -1 , heating to 400-450°C, and keeping warm for 5-10 hours; in some preferred embodiments, the heating rate is, for example, 1-5°C·min -1 、5~10℃·min -1 etc.; heating to 400-430°C, 430-450°C, etc.; keeping time for 5-8 hours, 8-10 hours, 10-12 hours, etc.

[0020] Preferably, the step of heating and oxidizing the multi-walled carbon nanotube powder comprises placing the multi-walled carbon nanotube powder in an alumina ceramic boat and heating it in a tubular furnace with openings at both ends.

[0021] Preferably, the diameter of the multi-walled carbon nanotube powder is 40-60 nm. In certain preferred embodiments, the diameter of the multi-walled carbon nanotube powder is, for example, 40-50 nm, 50-60 nm, etc., and more preferably 50 nm.

[0022] Preferably, the acid is hydrochloric acid, sulfuric acid or nitric acid.

[0023] Preferably, the concentration of the acid is 5-10 mol / L; in certain preferred embodiments, the concentration of the acid is, for example, 5-6 mol / L, 5-8 mol / L, 6-8 mol / L, 6-10 mol / L, 8-10 mol / L, etc., more preferably 6 mol / L.

[0024] Preferably, the dosage ratio of the multi-walled carbon nanotube powder to the acid is 50 mg: 80-150 mL; in certain preferred embodiments, the dosage ratio is, for example, 50 mg: 80-100 mL, 50 mg: 80-120 mL, 50 mg: 100-120 mL, 50 mg: 100-150 mL, 50 mg: 120-150 mL, etc.; more preferably 50 mg: 100 mL.

[0025] Preferably, the conditions for heating the mixture to reflux are: the reflux temperature is 100-150°C, and the reflux time is 20-30 hours; in certain preferred embodiments, the temperature for heating the mixture to reflux is, for example, 100-120°C, 120-150°C, etc., and the time for heating the mixture to reflux is, for example, 20-24 hours, 24-30 hours, etc.

[0026] Preferably, the reagent used for washing is deionized water, and the number of washing times is at least six times.

[0027] Preferably, the drying conditions are: vacuum drying at a temperature of 60°C to 80°C for 10 to 15 hours; in some preferred embodiments, the drying temperature is, for example, 60°C, and the drying time is, for example, 10 to 12 hours, 12 to 15 hours, etc.

[0028] Preferably, the heat treatment is maintained at 800-1200°C in an Ar atmosphere for 0.5-2 hours; more preferably, the heat treatment temperature is, for example, 800-1000°C, 1000-1200°C, and the holding time is 0.5-1 hour, 1-2 hours, etc.

[0029] As another aspect of the present invention, the present invention also provides a use of the above-mentioned lithium carbon dioxide battery positive electrode material catalyst in the preparation of lithium carbon dioxide battery positive electrode material.

[0030] Preferably, the use of the lithium carbon dioxide battery positive electrode material catalyst in the preparation of a lithium carbon dioxide battery positive electrode material comprises the following steps:

[0031] A lithium carbon dioxide battery positive electrode material catalyst, a binder and an organic solvent are mixed to obtain a slurry, and the slurry is coated on carbon paper to prepare a lithium carbon dioxide battery positive electrode material.

[0032] Preferably, the binder is a naphthol solution or polyvinylidene fluoride, and more preferably, the binder is a naphthol solution.

[0033] Preferably, the concentration of the naphthol solution is 0.2-0.6 wt.%, more preferably 0.5 wt.%.

[0034] Preferably, the usage ratio of the lithium carbon dioxide battery positive electrode material catalyst, binder and solvent is 1 mg to 3 mg: 10 μL: 1 mL, more preferably 2 mg: 10 μL: 1 mL.

[0035] Preferably, the organic solvent is isopropanol or N-methylpyrrolidone, more preferably isopropanol.

[0036] Preferably, the coating amount of the slurry coated on the carbon paper is 0.09-0.27 mg / cm 2 More preferably, the coating amount is 0.18 mg / cm 2 .

[0037] As another aspect of the present invention, the present invention also provides a lithium carbon dioxide battery positive electrode material prepared from the above lithium carbon dioxide battery positive electrode material catalyst.

[0038] As another aspect of the present invention, the present invention also provides a use of the above-mentioned lithium carbon dioxide battery positive electrode material in the preparation of a lithium carbon dioxide battery.

[0039] Preferably, the use of the lithium carbon dioxide battery positive electrode material in the preparation of a lithium carbon dioxide battery comprises the following steps:

[0040] A lithium carbon dioxide battery is assembled in a glove box filled with argon, wherein the positive electrode of the battery adopts the positive electrode material of the lithium carbon dioxide battery.

[0041] Preferably, the battery negative electrode of the lithium carbon dioxide battery is a lithium sheet, the separator is a glass fiber paper, and the electrolyte is a 1.0 mol / L lithium bis(trifluoromethanesulfonyl)imide / 0.3 mol / L sodium nitrate / dimethyl sulfoxide solution (LiTFSI / NaNO 3 / DMSO).

[0042] As another aspect of the present invention, the present invention also provides a lithium carbon dioxide battery made from the above lithium carbon dioxide battery positive electrode material.

[0043] In addition, unless otherwise specified, any range described in the present invention includes the end value and any numerical value between the end values ​​and any sub-range formed by the end value or any numerical value between the end values.

[0044] The beneficial effects of the present invention are as follows:

[0045] (1) The positive electrode material catalyst of the lithium carbon dioxide battery provided by the present invention adopts porous carbon nanotubes, and the openings on the side walls thereof lead to an increase in physical surface area, pore volume and active sites, which can store more discharge product lithium carbonate and promote its decomposition.

[0046] (2) The preparation method of the positive electrode material catalyst of the lithium carbon dioxide battery provided by the present invention is simple and efficient, has low energy consumption, and effectively reduces the cost.

[0047] (3) The lithium carbon dioxide battery positive electrode material catalyst provided by the present invention does not use an external catalyst during the preparation process. Instead, the catalytic residue encapsulated in the nanotube cavity during the carbon nanotube generation process is used to catalyze the gasification of the nanotube wall carbon to generate holes. The preparation process is simple and energy consumption is low. The generation of holes increases the specific surface area of ​​the catalyst and increases the degree of defects in the carbon nanotubes, which is conducive to the storage and decomposition of more discharge products, lithium carbonate.

[0048] (4) The electrochemical performance of the lithium carbon dioxide battery provided by the present invention is significantly improved. -1 The overpotential is 1.18V to 1.25V at a current density of 100mA·g -1 , cut-off capacity is 500mA·h·g -1 It has a surprising long-term cycle stability of 1400h to 1500h at 0.5A·g -1 Excellent current density of 16000 ~ 17500mA·h·g -1 The full discharge capacity (based on catalyst mass) provides an effective reference for the practical application and promotion of lithium carbon dioxide batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0050] Figure 1 The X-ray diffraction pattern of the positive electrode material catalyst of the lithium carbon dioxide battery prepared in Example 1 is shown;

[0051] Figure 2 The low-magnification microscopic morphology of the lithium carbon dioxide battery cathode material catalyst prepared in Example 1 under a scanning electron microscope is shown;

[0052] Figure 3 The high-magnification microscopic morphology of the lithium carbon dioxide battery cathode material catalyst prepared in Example 1 under a transmission electron microscope is shown;

[0053] Figure 4 The porous structure distribution diagram of the positive electrode material catalyst of the lithium carbon dioxide battery prepared in Example 1 is shown;

[0054] Figure 5 The cyclic voltammogram of the lithium carbon dioxide battery prepared in Example 5 is shown;

[0055] Figure 6 The lithium carbon dioxide batteries prepared in Example 5, Comparative Example 5 and Comparative Example 6 have a high conductivity at 100 mA·g -1 Comparison of the first cycle charge and discharge curves at current density;

[0056] Figure 7 A comparison chart of the full discharge capacity of the lithium carbon dioxide batteries prepared in Example 5 and Comparative Example 5 is shown;

[0057] Figure 8 A comparison chart of the rate performance of the lithium carbon dioxide batteries prepared in Example 5, Comparative Example 5 and Comparative Example 6 at different current densities is shown;

[0058] Fig. 9 The long cycle performance diagram of the lithium carbon dioxide battery prepared in Example 5 is shown. DETAILED DESCRIPTION

[0059] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0060] In the present invention, the preparation methods are conventional methods unless otherwise specified. The raw materials used are available from public commercial sources unless otherwise specified, and the percentages are by mass unless otherwise specified.

[0061] Example 1

[0062] This embodiment provides a preparation method of a positive electrode material catalyst for a lithium carbon dioxide battery, and the steps are as follows:

[0063] (1) 50 mg of multi-walled carbon nanotube powder (diameter 50 nm) was placed in an alumina porcelain boat and heated in a tube furnace with both ends open to allow it to be oxidized by air at a heating rate of 5 °C min. -1 , keep warm at 430℃ for 10 hours;

[0064] (2) adding the product obtained in step (1) to 100 mL of 6 mol / L HCl to obtain a mixture, and reflux the mixture at 120° C. for 24 hours; then filtering the slurry, repeatedly washing the solid with deionized water for 6 times, and vacuum drying at 60° C. for 12 hours;

[0065] (3) The product obtained in step (2) was placed in a tube furnace at 5°C min -1The temperature was raised to 1000°C at a heating rate and kept in argon for 1 hour to obtain porous carbon nanotubes, which are the positive electrode material catalyst of lithium carbon dioxide batteries and are named porous CNTs.

[0066] In this embodiment, the first step is air oxidation. During this process, the catalyst encapsulated inside the carbon nanotubes will catalyze the reaction between the outer wall of the carbon nanotubes and the oxygen in the air, partially vaporizing to form holes and partially forming oxygen-containing groups, such as hydroxyl and carbonyl groups. The second step is heating, which is thermal reduction in an argon atmosphere to remove the hydroxyl carbonyl groups formed after air oxidation, thereby ensuring the consistency of the oxygen content with the comparison sample.

[0067] Figure 1 The X-ray diffraction pattern of the positive electrode material catalyst of the lithium carbon dioxide battery prepared in this embodiment is shown; Figure 1 It can be seen that the product obtained in Example 1 is pure porous carbon nanotubes, and only the diffraction peaks of carbon nanotubes appear in the XRD graph.

[0068] Figure 2 The low-magnification microscopic morphology of the lithium carbon dioxide battery cathode material catalyst prepared in this embodiment under a scanning electron microscope is shown; Figure 3 The high-magnification microscopic morphology of the transmission electron microscope is shown; Figure 4 Figure 2 shows the distribution of porous structures of porous carbon nanotubes. Figure 2 and Figure 3 Some shallow pits (about 20-30 nm in diameter) appeared on the surface of the porous carbon nanotubes prepared in this embodiment, mainly located on the surface, and occasionally some penetrated the tube wall. Obviously, there were no residual metal particles, indicating that the prepared catalyst had high purity and the porous structure was conducive to storing the discharge product lithium carbonate; see Figure 4 The material structure prepared in this embodiment is a mesoporous and macroporous structure, which is conducive to storing the discharge product lithium carbonate.

[0069] Example 2

[0070] This embodiment provides a preparation method for a positive electrode material catalyst of a lithium carbon dioxide battery. The steps are the same as those of embodiment 1, except that the insulation temperature in step (1) is changed from 430° C. to 400° C. to prepare a positive electrode material catalyst of a lithium carbon dioxide battery.

[0071] Example 3

[0072] This embodiment provides a preparation method for a positive electrode material catalyst of a lithium carbon dioxide battery. The steps are the same as those of embodiment 1, except that the insulation temperature in step (1) is changed from 430° C. to 450° C. to prepare a positive electrode material catalyst of a lithium carbon dioxide battery.

[0073] Example 4

[0074] This embodiment provides a preparation method of a positive electrode material for a lithium carbon dioxide battery, and the specific steps are as follows:

[0075] 2 mg of the lithium carbon dioxide battery positive electrode material catalyst prepared in Example 1 and 6 μL of naphthol solution (0.5 wt.%) were dispersed in 1 mL of isopropanol and ultrasonicated for 60 minutes to obtain a slurry; the slurry was dripped onto carbon paper (Toray TGP-H-060, cut into discs with a diameter of 9 mm) at 80° C. to obtain electrode sheets, wherein the mass loading of each sheet was 0.2 mg; the electrode sheets were then placed in a vacuum oven and dried at 80° C. for 12 hours to obtain a lithium carbon dioxide battery positive electrode material.

[0076] Example 5

[0077] This embodiment provides a preparation of a lithium carbon dioxide battery, and the specific steps are as follows:

[0078] In a glove box filled with argon, the positive electrode material of the lithium carbon dioxide battery prepared in Example 4 was used as the cathode and the lithium sheet was used as the anode to assemble a CR2032 button battery with 19 holes on the cathode side; wherein the cathode and the anode were separated by glass fiber (19 mm), and 100 μL of 1.0 mol / L LiTFSI and 0.3 mol / L LiNO were added dropwise. 3 DMSO solution was used as the electrolyte.

[0079] The lithium carbon dioxide battery prepared in this example was tested by placing the assembled button cells in a sealed bottle and heating them with CO 2 Inflate for 30 minutes to obtain pure CO 2 Atmosphere, constant current charge and discharge tests were performed using a battery testing station (Land), and all specific capacity values ​​were calculated based on the weight of the lithium carbon dioxide battery cathode material catalyst.

[0080] See also Figure 5 The cyclic voltammetry curve of the lithium carbon dioxide battery prepared in this embodiment begins to show reduction peaks and oxidation peaks at potentials of 2.8V and 4.0V; see Figure 6 The lithium carbon dioxide battery prepared in this embodiment has the smallest overpotential compared with the comparative example; see Figure 7 , battery 500mA·g -1 The discharge capacity can reach 17500mA·h·g -1 ; See Figure 8 , lithium carbon dioxide batteries using porous carbon nanotubes as catalysts have good rate performance; see Fig. 9 The above battery is at 100mA·g -1 The cycle time is up to 1400 hours at a current density of 1.

[0081] Comparative Example 1

[0082] This comparative example provides a preparation method for a positive electrode material catalyst of a lithium carbon dioxide battery, and the specific steps are as follows:

[0083] 50 mg of multi-walled carbon nanotubes were dispersed in 100 mL of 6 mol / L HCl, and the mixture was refluxed at 120°C for 24 hours. The slurry was then filtered, the solid was repeatedly washed with deionized water for 6 times, and vacuum dried at 60°C for 12 hours to obtain a lithium carbon dioxide battery cathode material catalyst, named CNTs.

[0084] Compared with Example 1, the cathode material catalyst of the lithium carbon dioxide battery prepared in this comparative example is a carbon nanotube without a porous structure, with a smaller specific surface area and a lower degree of defects.

[0085] Comparative Example 2

[0086] This comparative example provides a preparation method for a positive electrode material catalyst of a lithium carbon dioxide battery, and the specific steps are as follows:

[0087] 50 mg of multi-walled carbon nanotubes were dispersed in 100 mL of 6 mol / L HCl, and the mixture was refluxed at 120°C for 24 hours. The slurry was filtered, the solid was repeatedly washed with deionized water for 6 times, vacuum dried at 60°C for 12 hours, and then the solid was kept at 1000°C for 1 hour under argon atmosphere to obtain a lithium carbon dioxide battery positive electrode material catalyst, named r-CNTs.

[0088] Comparative Example 3

[0089] This comparative example provides a preparation method for a positive electrode material for a lithium carbon dioxide battery. The steps are the same as those of Example 4, except that this comparative example uses the positive electrode material catalyst for a lithium carbon dioxide battery prepared in Comparative Example 1 to prepare the positive electrode material for a lithium carbon dioxide battery.

[0090] Comparative Example 4

[0091] This comparative example provides a preparation method for a positive electrode material for a lithium carbon dioxide battery. The steps are the same as those of Example 4, except that this comparative example uses the positive electrode material catalyst for a lithium carbon dioxide battery prepared in Comparative Example 2 to prepare the positive electrode material for a lithium carbon dioxide battery.

[0092] Comparative Example 5

[0093] This comparative example provides a preparation method for a lithium carbon dioxide battery. The steps are the same as those of Example 5, except that this comparative example uses the lithium carbon dioxide battery positive electrode material prepared in Comparative Example 3 to prepare the lithium carbon dioxide battery positive electrode.

[0094] from Figure 8 It can be seen that the rate performance of the lithium carbon dioxide battery prepared in this comparative example is poor.-1 The discharge platform is as low as 2.5V at a current density of Figure 7 It can be seen that the lithium carbon dioxide battery prepared in this comparative example has a high -1 The discharge capacity of the battery at the current density is only 8800mA·h·g -1 When the capacity is limited to 500mA·h·g -1 When the current density is 100mA·g -1 Under these conditions, the electrode can only be charged and discharged 20 times.

[0095] Comparative Example 6

[0096] This comparative example provides a preparation method for a lithium carbon dioxide battery. The steps are the same as those of Example 5, except that this comparative example uses the lithium carbon dioxide battery positive electrode material prepared in Comparative Example 4 to prepare the lithium carbon dioxide battery positive electrode.

[0097] from Figure 6 It can be seen that the polarization of the lithium carbon dioxide battery prepared in this comparative example is greater than that of Example 5; Figure 8 It can be seen that the rate performance of the lithium carbon dioxide battery prepared in this comparative example is poor. -1 The discharge platform is as low as 2.5V at a current density of 1.5V.

[0098] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A lithium carbon dioxide battery cathode material catalyst, It is characterized in that The positive electrode material catalyst of the lithium carbon dioxide battery is a porous carbon nanotube; the side wall of the porous carbon nanotube has an opening; The method for preparing the positive electrode material catalyst of the lithium carbon dioxide battery comprises the following steps: The multi-walled carbon nanotube powder is heated and oxidized, the heated product is mixed with an acid to obtain a mixture, the mixture is heated to reflux, and the mixture is filtered, washed, dried, and heat-treated to obtain the lithium carbon dioxide battery positive electrode material catalyst; The conditions for heating and oxidizing the multi-walled carbon nanotube powder are as follows: the heating rate is 1 to 10°C·min -1 , raise the temperature to 400-450°C and keep warm for 5-10 hours; The conditions for heating the mixture to reflux are: reflux temperature of 100 to 150° C., and reflux time of 20 to 30 hours; The heat treatment is carried out in an Ar atmosphere at a temperature of 800 to 1200° C. for 0.5 to 2 hours.

2. The lithium carbon dioxide battery cathode material catalyst according to claim 1, It is characterized in that The diameter of the multi-walled carbon nanotube powder is 40-60 nm.

3. The lithium carbon dioxide battery cathode material catalyst according to claim 1, It is characterized in that The acid is hydrochloric acid, sulfuric acid or nitric acid.

4. The lithium carbon dioxide battery cathode material catalyst according to claim 1, It is characterized in that The concentration of the acid is 5-10 mol / L.

5. The lithium carbon dioxide battery cathode material catalyst according to claim 1, It is characterized in that The dosage ratio of the multi-walled carbon nanotube powder to the acid is 50 mg: 80-150 mL.

6. The lithium carbon dioxide battery cathode material catalyst according to claim 1, It is characterized in that The drying conditions are: vacuum drying at a temperature of 60 to 80° C. for 10 to 15 hours.

7. Use of the lithium carbon dioxide battery positive electrode material catalyst according to any one of claims 1 to 6 in the preparation of lithium carbon dioxide battery positive electrode material.

8. A positive electrode material for a lithium carbon dioxide battery, It is characterized in that The lithium carbon dioxide battery positive electrode material is prepared from the lithium carbon dioxide battery positive electrode material catalyst according to any one of claims 1-6.

9. A lithium carbon dioxide battery, It is characterized in that The lithium carbon dioxide battery is made from the lithium carbon dioxide battery positive electrode material according to claim 8.