Low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery

By using titanium compounds and trisodium citrate salt to inhibit hydrolysis, combined with three-dimensional porous electrodes, the problem of hydrolysis and dissolution of titanium sources in flow batteries is solved, reducing the cost of all-vanadium flow batteries, improving battery performance, and advancing vanadium Commercial applications of titanium flow batteries.

CN114824399BActive Publication Date: 2024-10-01CHANGSHA UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202210530232.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-16
Publication Date
2024-10-01
Estimated Expiration
2042-05-16

AI Technical Summary

Technical Problem

The development of all-vanadium flow batteries has been limited by high cost, low energy density and easy corrosion. In particular, the titanium source is easily hydrolyzed or has a slow dissolution rate in the electrolyte, resulting in reduced battery efficiency and difficulties in commercial production.

Method used

Low-cost titanium compounds are used to replace vanadium compounds as the negative active material, and trisodium citrate salt is used as a stabilizer to inhibit the hydrolysis of titanium and improve its solubility and electrochemical activity. It is assembled by combining three-dimensional porous electrodes and acid treatment technology. Low-cost and high-performance vanadium-titanium flow battery.

Benefits of technology

Significantly reduces battery costs, improves battery cycle stability and efficiency, solves the hydrolysis and dissolution problems of titanium sources in flow batteries, achieves high energy density and long cycle life, and promotes the commercial application of flow batteries .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114824399B_ABST
    Figure CN114824399B_ABST
Patent Text Reader

Abstract

The present invention discloses a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery, comprising: a positive electrode electrolyte comprising a vanadium compound and an auxiliary acid solution; a negative electrode electrolyte comprising a titanium compound, an auxiliary acid solution, and a stabilizer; the titanium compound comprises any one or more of TiO2, Ti(SO4)2, TiCl4, TiOSO4, TiOCl2, and TiCl3; and the stabilizer is trisodium citrate. The present invention uses a titanium compound as an active substance in the negative electrode electrolyte, and uses trisodium citrate as a negative electrode electrolyte stabilizer, which effectively inhibits the hydrolysis process of the titanium compound and promotes the TiO 2+ The increase in the solubility of the compound solves a series of problems that restrict the use of titanium as an active material for the negative electrode of liquid flow batteries, and effectively improves the performance of the overall liquid flow battery system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of redox flow batteries, in particular to a low-cost, high-performance, large-scale energy storage vanadium-titanium flow battery. Background Art

[0002] In energy storage technology, flow batteries have attracted much attention due to their unique characteristics of independent power and capacity, long life, safety and reliability, and flexible scale settings. The electrolyte of a flow battery consists of dissolved active molecules and corresponding supporting electrolytes, which are stored in the positive and negative electrode storage tanks, respectively, and circulated between the positive and negative electrodes and the storage tanks by pumps. Among them, all-vanadium redox flow batteries can not only avoid cross-contamination of ions of different elements, but also reduce the possibility of electrolyte precipitation, making it one of the most mature commercial flow batteries. However, all-vanadium flow batteries are limited by high cost (~US$600 / kWh), low energy density (~26WhL −1 ) and corrosion (vanadium flow batteries require acid as a supporting electrolyte) have limited their development.

[0003] Providing a low-cost and inexpensive negative electrode pair to pair with a vanadium positive electrode pair to form a new low-cost battery has become a feasible improvement direction. However, the vanadium pair has high requirements for the negative electrode pair: (1) In a high-concentration acid environment, the negative electrode pair must be stable and have good electrochemical activity; (2) Because V-valent vanadium will precipitate V2O5 when the temperature rises, the negative electrode pair must have good electrochemical activity and high solubility at a lower temperature; (3) The negative electrode pair of the new system is cheaper and easier to obtain than the titanium pair.

[0004] Titanium is abundant in the earth's crust and is cheap. Compared with all-vanadium liquid flow batteries, it can effectively reduce the cost of the entire battery and promote commercial development. Titanium has more than two valence states and can exist stably under acidic conditions. + It can also inhibit the hydrolysis of titanium to a certain extent. At the same time, it has high electrochemical activity at low temperatures and is suitable for reactions at low temperatures, matching the V-valent vanadium. Titanium is a better choice as a negative electrode pair.

[0005] However, as the negative electrode active material, titanium source inevitably has the problem of being easily hydrolyzed or having a very slow dissolution rate in the electrolyte, which is a major factor restricting titanium from matching vanadium as a negative electrode pair. For example, titanium sulfate or titanyl sulfate, in which IV valence titanium exists in the form of Ti 4+ and TiO 2+ , while Ti 4+ It is very easy to hydrolyze in water. At room temperature (25°C), 0.1 mol / L Ti 4+ At pH = 1, it will hydrolyze to form a water-insoluble precipitate, which makes Ti 4+Liquid flow batteries, which are the negative electrode active materials, are prone to hydrolysis and deposition and aggregation on the electrodes during the cycle, causing the battery efficiency to decrease, and even clogging the pipeline and causing the battery to fail. 2+ However, it is difficult to dissolve in aqueous solution, dissolves slowly, and undergoes hydrolysis during the dissolution process, which restricts its commercial production.

[0006] In summary, it is urgent to solve the problem of easy hydrolysis or slow dissolution rate of titanium sources participating in vanadium redox flow battery systems, and provide a new type of low-cost, high-energy density, high-performance, large-scale flow battery system for development. Summary of the invention

[0007] The purpose of the present invention is to propose a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery, which uses low-cost titanium compounds instead of expensive vanadium compounds as the negative electrode active material of the liquid flow battery, significantly reducing the battery cost while having good electrochemical activity and stability, solving the problems existing in the prior art.

[0008] The technical solution of the present invention is as follows: a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery, comprising:

[0009] Positive electrode electrolyte: comprising a vanadium compound and an auxiliary acid solution; the vanadium compound comprises one or more of vanadium dioxide, vanadium pentoxide, and vanadyl sulfate, and the concentration thereof is 0.1 mol / L to 3 mol / L; the auxiliary acid solution comprises sulfuric acid or hydrochloric acid, and the concentration thereof is 1 mol / L to 6 mol / L;

[0010] Negative electrode electrolyte: including titanium compounds, auxiliary acid solution, and stabilizer; the titanium compound includes any one or more of TiO2, Ti(SO4)2, TiCl4, TiOSO4, TiOCl2, and TiCl3, and its concentration is 0.1mol / L~3mol / L; the auxiliary acid solution includes sulfuric acid or hydrochloric acid, and its concentration is 1mol / L~6mol / L; the stabilizer is trisodium citrate, and its concentration is 0.01mol / L~0.3mol / L.

[0011] Furthermore, the concentration of the vanadium compound is 1 mol / L to 1.5 mol / L.

[0012] Furthermore, the concentration of the titanium compound is 1 mol / L to 2 mol / L.

[0013] Furthermore, the compound of titanium is: Ti 4+ Compounds and TiO 2+ Mixture of compounds, TiO 2+ Compounds and Ti 3+ A mixture of compounds.

[0014] Furthermore, the preparation method of the negative electrode electrolyte comprises the following steps:

[0015] Add the stabilizer to the auxiliary acid solution with a concentration of 1mol / L~6mol / L, and the concentration of the stabilizer is 0.01mol / L~0.3mol / L;

[0016] Weigh a titanium compound and add it evenly to the auxiliary acid solution added with a stabilizer in 5 to 20 times. The whole system is placed in an ice-water bath and magnetically stirred at the same time. The interval between each addition is 10 minutes to 30 minutes. After the addition is completed, the system is ultrasonically treated in an ice-water bath for 20 minutes to 60 minutes, and then continues to stand in the ice-water bath for 1 hour to 3 hours. The volume is fixed using a volumetric flask to obtain the negative electrode electrolyte.

[0017] Furthermore, it also includes a diaphragm treated with acid solution, wherein the treatment method is: placing the diaphragm in 1 mol / L~3 mol / L acid solution, and treating it at a constant temperature of 50°C~80°C for 1h~3h, and the obtained product is obtained by washing and drying.

[0018] Furthermore, the diaphragm includes: Nafion membrane, PP membrane, PE membrane, PEO membrane, SPEEK membrane, SPES membrane, PVDF membrane, PTFE membrane or PBI membrane; the acid solution includes hydrochloric acid or sulfuric acid.

[0019] Furthermore, it also includes a three-dimensional porous electrode; the three-dimensional porous electrode includes one of nickel mesh, graphite felt or carbon felt, and the thickness is 1mm~8mm.

[0020] Compared with the prior art, the present invention has the following significant advantages and beneficial effects:

[0021] (1) The present invention uses titanium compounds as active substances in the negative electrode electrolyte, which are non-toxic, harmless, and environmentally friendly, effectively reducing environmental pollution. At the same time, trisodium citrate is used as a negative electrode electrolyte stabilizer to effectively inhibit the hydrolysis process of titanium compounds and promote the synthesis of TiO 2+ The increase in the solubility of the compound has solved a series of problems that restrict the use of titanium as an active material for the negative electrode of liquid flow batteries. When matched with vanadium, it is assembled into a long-cycle, high-efficiency, low-cost vanadium-titanium liquid flow battery, which effectively reduces the cost of all-vanadium liquid flow batteries and improves the performance of the overall liquid flow battery system. It is expected to become one of the next generation of large-scale energy storage technologies.

[0022] (2) The equipment price of the entire preparation process of the embodiment of the present invention is low, the raw material source is abundant, the preparation process flow is simple, and the operation is convenient, which is conducive to industrialization and practicality, and is conducive to promoting the progress of industrial and commercialization of liquid flow batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 The figure shows the relationship between the coulombic efficiency, voltage efficiency and energy efficiency and the number of cycles of the low-concentration vanadium-titanium liquid flow battery according to the embodiment of the present invention.

[0025] Figure 2 The figures are the rate performance test results of the high-concentration vanadium-titanium liquid flow battery at different current densities according to the embodiment of the present invention.

[0026] Figure 3 The ultra-high concentration vanadium-titanium liquid flow battery of the present invention is 100 mA cm -2 The relationship between the coulombic efficiency, voltage efficiency and energy efficiency and the number of cycles at the current density.

[0027] Figure 4 This is a cost comparison chart of the negative electrode electrolyte of the ultra-high concentration vanadium-titanium liquid flow battery and the negative electrode electrolyte of the all-vanadium liquid flow battery according to the embodiment of the present invention.

[0028] Figure 5 Graph showing the relationship between voltage, power density and current of the ultra-high concentration vanadium-titanium liquid flow battery according to an embodiment of the present invention.

[0029] Figure 6 The figure shows the relationship between the coulombic efficiency, voltage efficiency and energy efficiency and the number of cycles of the ultra-high concentration vanadium-titanium liquid flow battery of the embodiment of the present invention. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The design concept of the present invention is: using three-dimensional porous materials as battery electrolyte reaction carriers, using vanadium and titanium as the positive and negative active materials of the battery respectively, and trisodium citrate as the negative electrode electrolyte stabilizer, to propose a low-cost, high-efficiency, high-stability liquid flow battery system, which promotes the dissolution of titanium while effectively inhibiting the hydrolysis of titanium, and can also improve the reversibility and stability of the electrolyte, thereby improving battery performance. By assembling a single cell, it is proved that it has high coulomb efficiency, energy efficiency and ultra-long cycle stability. This method of using titanium electrolyte instead of vanadium electrolyte in the negative electrode of the all-vanadium liquid flow battery can effectively reduce battery costs, while improving battery stability and cycle performance, and is expected to become one of the next generation of large-scale energy storage technologies.

[0032] The present invention uses a vanadium compound and an auxiliary acid solution as a positive electrode electrolyte, a titanium compound and an auxiliary acid solution as a negative electrode electrolyte, trisodium citrate as a negative electrode electrolyte stabilizer, an ion exchange membrane as a diaphragm, and a three-dimensional porous material as an electrode to assemble a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery. The preparation method includes the following steps:

[0033] (1) Treatment method of diaphragm material: place the diaphragm in 1mol / L~3mol / L acid solution, and treat it at a constant temperature of 50℃~80℃ for 1h~3h. After taking it out, wash it with deionized water, dry it in a constant temperature drying oven at 70℃~90℃ for 2h~4h, take it out, and soak it in deionized water for later use. The acid solution includes hydrochloric acid or sulfuric acid.

[0034] The liquid flow battery system of the present invention uses H + As the positive and negative electrode ion conductor, the diaphragm is treated with acid before use to fill the diaphragm with H + , fully activated, can effectively improve the early cycle performance. The diaphragm includes: Nafion membrane, PP membrane, PE membrane, PEO membrane, SPEEK membrane, SPES membrane, PVDF membrane, PTFE membrane or PBI membrane, which can conduct H + The diaphragm is ready for use.

[0035] (2) Preparation of positive electrode electrolyte: preparing the positive electrode electrolyte using vanadium compound, auxiliary acid solution and deionized water;

[0036] Among them, vanadium compounds are used as positive electrode active materials, including one or more of vanadium dioxide, vanadium pentoxide, and vanadyl sulfate; the concentration of the vanadium compound is 0.1mol / L~3mol / L; the concentration of the vanadium compound is preferably 1mol / L~1.5mol / L, at which the vanadium compound is easier to dissolve, and the acid concentration required for dissolution is not high. If the concentration of the vanadium compound continues to increase, a higher auxiliary acid concentration is required, which increases the cost and affects the viscosity of the solution, causing the performance of the liquid flow battery system to decline; the auxiliary acid includes sulfuric acid or hydrochloric acid; the auxiliary acid concentration is 1mol / L~6mol / L, and the concentration is selected according to the concentration of the vanadium compound.

[0037] In a strong acid environment, vanadium pentavalent vanadium is present in the solution as VO2 + If the pH rises, V2O5 will precipitate, which is not only highly toxic, but also causes capacity loss and pipe clogging. Therefore, the vanadium liquid flow battery of the present invention uses acid as the supporting electrolyte.

[0038] (3) Preparation of negative electrode electrolyte: The negative electrode electrolyte is prepared using titanium compounds, auxiliary acid, stabilizer and deionized water.

[0039] Titanium compounds are negative electrode active materials, including any one or more of titanium dioxide (TiO2), titanium sulfate (Ti(SO4)2), titanium tetrachloride (TiCl4), titanyl sulfate (TiOSO4), titanium oxychloride (TiOCl2), and titanium trichloride (TiCl3). The concentration is 0.1 mol / L~3 mol / L, preferably 1 mol / L~2 mol / L. If the concentration is too low, the solution hydrolysis will be aggravated, and if the concentration is too high, the dissolution time will be long.

[0040] The auxiliary acid solution includes sulfuric acid or hydrochloric acid; the concentration of the auxiliary acid solution is 1 mol / L~6 mol / L, and its concentration is determined according to the concentration of the positive electrode acid and the concentration of the negative electrode active material, and water migration is adjusted.

[0041] The stabilizer is trisodium citrate, which can inhibit the formation of TiO 2+ The hydrolysis process is TiO 2+ —>TiO2 can be used as an additive in this process, and the concentration of trisodium citrate solution is 0.01mol / L~0.3mol / L.

[0042] The specific preparation method of the negative electrode electrolyte is as follows: adding concentrated sulfuric acid or concentrated hydrochloric acid to deionized water, mixing evenly, and preparing an auxiliary acid solution with a concentration of 1 mol / L to 6 mol / L; after cooling to room temperature, adding the stabilizer to the auxiliary acid solution, the preparation concentration of the stabilizer is 0.01 mol / L to 0.3 mol / L; weighing the titanium compound, adding it evenly to the auxiliary acid solution with the stabilizer added in 5 to 20 times, placing the whole system in an ice water bath, and magnetic stirring is performed at the same time, each addition interval is 10 min to 30 min, after the addition is completed, the system is ultrasonically treated in the ice water bath for 20 min to 60 min (the hydrolysis process is endothermic, if the temperature is high, it will promote hydrolysis, this step ultrasound promotes the dissolution of the solute, and the ice water bath inhibits hydrolysis), and then continue to stand in the ice water bath for 1h to 3h (continue to inhibit hydrolysis at low temperature), and use a volumetric flask to adjust the volume to obtain the negative electrode electrolyte.

[0043] When using titanium compounds as negative electrode active materials, it is necessary to increase their dissolution rate and inhibit their hydrolysis process.

[0044] The titanium in TiO2, Ti(SO4)2 and TiCl4 exists in the form of Ti 4+ , its hydrolysis reaction is:

[0045] Ti(SO4)2 + H2O = TiOSO4 + H2SO4;

[0046] TiOSO4 + 2H2O = H2TiO3 + H2SO4.

[0047] The titanium in TiOSO4 and TiOCl2 exists in the form of TiO 2+ , its hydrolysis reaction is:

[0048] TiOSO4 + 2H2O = H2TiO3 + H2SO4.

[0049] Ti 4+ It takes a certain amount of time for the compound to reach reaction equilibrium, which will reduce the performance and stability of the first few cycles, and Ti 4+ Compounds are more 2+ The compound is easy to hydrolyze and form insoluble precipitates. 2+ In water with OH - The binding force is small and the degree of hydrolysis is less than that of Ti 4+ After dissolving, the existing form is relatively stable and it is not easy to generate water-insoluble precipitation. In terms of cost, TiO 2+ The cost of the compound is only Ti 4+ One seventh of a compound.

[0050] The present invention preferably uses TiO2+ Compounds, TiO 2+ Compounds and Ti 4+ Mixture of compounds, TiO 2+ Compounds and Ti 3+ The mixture of compounds is used as the negative electrode active material. The mixed valence negative electrode electrolyte can quickly reach equilibrium in the initial cycle, thereby improving the stability of subsequent cycles.

[0051] In this step, trisodium citrate is added as a stabilizer to increase H + concentration, effectively inhibiting the hydrolysis process of titanium compounds, inhibiting the formation of insoluble precipitates, and improving the performance of negative electrode active materials.

[0052] On the other hand, TiO 2+ In water with OH - The binding capacity of TiO2 is small, which makes it difficult to dissolve in aqueous solution and the dissolution process is slow, which is not conducive to large-scale production. In the present invention, trisodium citrate is added to the negative electrode electrolyte as a negative electrode stabilizer. The trisodium citrate reacts with TiO2 in the solution. 2+ Complexation has stronger binding ability with water, which is beneficial to promote the 2+ It dissolves in water without causing hydrolysis, allowing it to exist stably at the negative electrode for a long time. And the titanium molecules complexed with trisodium citrate are more reversible during the reaction on the electrode.

[0053] The present invention improves TiO 2+ The dissolution process of the compound to improve its solubility in water: in the dissolution of TiO 2+ In the process of preparing the compound, a certain concentration of acid solution is first prepared, and then trisodium citrate is added to prepare TiO 2+ The negative electrode electrolyte. Add TiO 2+ Compounds, using rotor magnetic stirring, when a small amount of TiO 2+ After the compound is added to the solution, a small amount of TiO 2+ Rapidly forms a complex with trisodium citrate, TiO 2+ This process was carried out in an ice water bath. 2+ The hydrolysis reaction of TiO is an endothermic process. 2+ The hydrolysis process of TiO becomes slow, which can effectively inhibit 2+ The hydrolysis of TiO2 was finally carried out by ultrasonic treatment. With the cooperation of trisodium citrate, the TiO2 2+ The dissolution time of the compound can be reduced, and pure TiO2 without hydrolysis products can be obtained. 2+The solution solved a major problem that restricted the large-scale preparation of vanadium-titanium liquid flow battery systems.

[0054] Use constant current to precharge the flow battery system so that the negative electrode electrolyte SOC is 10%~90%, that is, a certain amount of Ti 3+ and TiO 2+ Mix the solution, re-introduce the negative electrode electrolyte and the positive electrode electrolyte after the previous charge treatment into the battery, and perform battery testing to ensure that the SOC state of the negative electrode electrolyte is always maintained between 10% and 90%. During the battery charging and discharging process, there is always a certain amount of Ti in the solution. 3+ and TiO 2+ , making the Nernst potential of the negative electrode pair relatively stable without large fluctuations, keeping the efficiency stable and improving the overall stability of the battery; and during the charging and discharging process of the battery, the Ti in the solution 3+ and TiO 2+ It can promote the charging reaction and discharging reaction respectively, keep the negative electrode electrolyte at the intermediate state SOC, and effectively improve the efficiency of the battery. These make the assembled vanadium-titanium liquid flow battery highly stable, and can maintain stable efficiency and efficient operation in more than 3,000 cycles.

[0055] When a mixed-valence negative electrode electrolyte is used, the ratio of different valence states in the mixed-valence electrolyte can be adjusted accordingly according to the concentration and volume of the positive electrode vanadium electrolyte. The ratio of different valence states is preferably (1~9):(9~1), which can be regulated by direct mixing or by pre-charging or the first charging cycle, so that during the final charge and discharge cycle, the negative electrode SOC is maintained between 10% and 90%, effectively improving the stability of the battery.

[0056] The initial valence of the negative electrode titanium is determined by the initial valence of the vanadium added to the positive electrode. If the positive electrode uses tetravalent vanadium, the negative electrode uses tetravalent Ti. 4+ and TiO 2+ If the positive electrode uses pentavalent vanadium, the negative electrode uses trivalent Ti 3+ Mixed-valent titanium can also be used for the negative electrode, such as 4-valent Ti 4+ 、TiO 2+ and trivalent Ti 3+ Mixed valence, mixed valence negative electrode electrolyte can quickly reach equilibrium in the initial cycle, which helps to stabilize the cycle of the liquid flow battery system.

[0057] (4) Battery assembly and testing:

[0058] The single cell of the present invention is composed of an end plate, a sealing gasket, a current collector, a diaphragm, an electrode, a liquid storage tank, a pipeline and a peristaltic pump. The three-dimensional porous electrode includes one of a nickel mesh, a graphite felt or a carbon felt, and the thickness is 1mm~8mm. The three-dimensional porous electrode is used as the positive electrode and the negative electrode of the vanadium-titanium liquid flow battery, and the working load is connected to the positive working electrode through the positive current collector, and is connected to the negative working electrode through the negative current collector. On the positive side, the positive working electrode, the positive current collector, the sealing gasket, and the positive end plate are arranged in sequence from the inside to the outside, and on the negative side, the negative working electrode, the negative current collector, the sealing gasket, and the negative end plate are arranged in sequence from the inside to the outside. The positive working electrode and the negative working electrode are separated by a diaphragm. A flow channel hole is arranged on the upper side of the positive electrode, which is connected to the top of the liquid storage tank through a pipeline, and a flow channel hole is arranged on the lower side of the positive electrode, which is connected to the bottom of the liquid storage tank through a pipeline and a peristaltic pump. A flow channel hole is set on the upper side of the negative electrode, which is connected to the top of the liquid storage tank through a pipe. A flow channel hole is set on the lower side of the negative electrode, which is connected to the bottom of the liquid storage tank through a pipe and a peristaltic pump. The positive and negative electrolytes are stored in the positive and negative liquid storage tanks respectively, and are transported into the flow channel hole on the lower side of the electrode through the bottom of the liquid storage tank by the peristaltic pump, thereby entering the electrode. After the electrolyte is passed into the battery, the battery constant current charge and discharge test, battery rate performance test, and battery polarization performance test are performed on the battery test system.

[0059] (5) Assembly and testing of battery stack:

[0060] Assembly and testing of battery stack: The three-dimensional porous electrode is used as the positive electrode and negative electrode of the vanadium-titanium liquid flow battery. The thickness of the three-dimensional porous electrode is 1mm~8mm and the size is 4mm×4mm. The workload is connected to the positive working electrode through the positive current collector and to the negative working electrode through the negative current collector. The battery stack is composed of 2~6 single cells in series. In the single cell, the positive working electrode, positive current collector, and sealing gasket are arranged from the inside to the outside on the positive side, and the negative working electrode, negative current collector, and sealing gasket are arranged from the inside to the outside on the negative side. The positive and negative working electrodes of the single cell are separated by a diaphragm. A flow channel hole is set on the upper side of the positive electrode of the single cell, and a shunt is used to connect it to the top of the positive electrode storage tank through a pipeline. A flow channel hole is set on the lower side of the positive electrode, and a shunt is used to connect it to the bottom of the positive electrode storage tank through a pipeline and a peristaltic pump. A flow channel hole is set on the upper side of the negative electrode, and a flow diverter is used to connect it to the top of the liquid storage tank through a pipeline. A flow channel hole is set on the lower side of the negative electrode, and a flow diverter is used to connect it to the bottom of the liquid storage tank through a pipeline and a peristaltic pump. The positive and negative electrolytes are stored in the positive and negative liquid storage tanks respectively, and are transported by the peristaltic pump through the bottom of the liquid storage tank through the flow channel hole on the lower side of the positive and negative electrodes of each single cell through the flow diverter, thereby entering the electrode. After the electrolyte is passed into the battery stack, the battery constant current charge and discharge test is performed on the battery test system.

[0061] The low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery prepared by the present invention was tested as follows:

[0062] (1) Battery constant current charge and discharge test: The battery test system is used to perform constant current charge and discharge tests on the vanadium titanium liquid flow battery to test its cycle performance and stability.

[0063] (2) Battery rate performance test: A battery testing system is used to perform charge and discharge tests on vanadium-titanium liquid flow batteries at different current densities to test their rate performance.

[0064] (3) Battery polarization: The battery testing system is used to discharge the vanadium-titanium liquid flow battery to test the relationship between its voltage, power density and current.

[0065] Example 1

[0066] The method for preparing a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery in this embodiment comprises the following steps:

[0067] (1) Processing of diaphragm materials:

[0068] A 50 μm thick Nafion 212 membrane was placed in a 1 mol / L sulfuric acid solution, and treated in a water bath at 80°C for 2 h. After being taken out, it was cleaned with deionized water, dried in a constant temperature drying oven at 80°C for 3 hours, taken out, soaked in deionized water for 6 hours, and then taken out for use.

[0069] (2) Preparation of positive electrode electrolyte:

[0070] The active material is VOSO4 with a concentration of 0.1 mol / L, and the supporting electrolyte is H2SO4 solution with a concentration of 3 mol / L; the volume of the positive electrode electrolyte is 10 ml, which is placed in the positive electrode storage tank.

[0071] (3) Preparation of negative electrode electrolyte:

[0072] The active substance is a TiOSO4 solution with a concentration of 1 mol / L, the supporting electrolyte is a H2SO4 solution with a concentration of 3 mol / L, and the stabilizer is trisodium citrate with a concentration of 0.1 mol / L.

[0073] The specific configuration method is as follows: Take 16.3ml of 98% concentrated sulfuric acid, add it to a beaker containing 50ml of deionized water, mix well, cool to room temperature, take 2.58g of trisodium citrate, add it to the diluted H2SO4 solution, stir well, take 17.1g of TiOSO4, add it to the diluted H2SO4 solution evenly in 10 times, stir it with a magnetic stirrer in an ice-water bath, and the interval between each addition is 20min. After all the additions, place the solution in ice water for ultrasonic treatment for 40min, then continue to stand in the ice-water bath for 2h, and add a 100ml volumetric flask to make the solution 100ml. Take 60ml as the negative electrode electrolyte and place it in the negative electrode storage tank.

[0074] (4) Battery assembly:

[0075] The three-dimensional porous carbon felt is used as the positive electrode and negative electrode of the vanadium-titanium liquid flow battery. The carbon felt has a thickness of 5.5 mm and a size of 3×4.5 mm. The working load is connected to the positive working electrode through the positive current collector and to the negative working electrode through the negative current collector. The positive working electrode, the positive current collector, the sealing gasket, and the positive terminal plate are arranged in sequence from the inside to the outside on the positive side, and the negative working electrode, the negative current collector, the sealing gasket, and the negative terminal plate are arranged in sequence from the inside to the outside on the negative side. The positive working electrode and the negative working electrode are separated by a diaphragm. A flow channel hole is arranged on the upper side of the positive electrode, which is connected to the top of the liquid storage tank through a pipeline, and a flow channel hole is arranged on the lower side of the positive electrode, which is connected to the bottom of the liquid storage tank through a pipeline and a peristaltic pump. A flow channel hole is arranged on the upper side of the negative electrode, which is connected to the top of the liquid storage tank through a pipeline, and a flow channel hole is arranged on the lower side of the negative electrode, which is connected to the bottom of the liquid storage tank through a pipeline and a peristaltic pump. The positive and negative electrolytes are stored in the positive and negative electrode storage tanks respectively, and are transported into the flow channel holes on the lower side of the electrode through the bottom of the storage tank by a peristaltic pump, thereby entering the electrode.

[0076] (5) Battery pre-charge:

[0077] The liquid flow battery system is charged using a constant current to make the SOC of the negative electrode electrolyte 50%, and the treated negative electrode electrolyte and positive electrode electrolyte are reintroduced into the battery.

[0078] (6) Battery testing:

[0079] After the electrolyte is passed into the battery, the electrochemical performance test of the battery is carried out on the battery testing system.

[0080] The vanadium-titanium liquid flow battery system obtained in this embodiment has good battery performance. Figure 1 Shown: At 50mA / cm 2 At a current density of , after 1000 cycles, the coulombic efficiency of the battery is close to 100%, and the energy efficiency remains above 80%.

[0081] Example 2

[0082] The method for preparing a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery in this embodiment comprises the following steps:

[0083] Except for (2), the active substance is VOSO4 with a concentration of 1 mol / L.

[0084] The rest are the same as in Example 1.

[0085] The high concentration vanadium-titanium liquid flow battery obtained in this embodiment is Figure 2 As shown, at 40mA / cm 2 Up to 200mA / cm 2 At different current densities, the vanadium-titanium flow battery maintained a coulombic efficiency close to 100%. 2 At a current density of 40 mA / cm, the energy efficiency is still maintained at more than 70%, and it returns to 40 mA / cm 2 After the current density reaches , the energy efficiency does not decay, indicating that its stability is good.

[0086] Example 3

[0087] The method for preparing a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery in this embodiment comprises the following steps:

[0088] Except for (2), the active substance is VOSO4 at a concentration of 1.5 mol / L.

[0089] In (3), the active substance is a 2 mol / L TiOSO4 solution, and the stabilizer is 0.2 mol / L trisodium citrate. In the specific configuration method, the added mass of trisodium citrate is 5.16 g, and the added mass of TiOSO4 is 34.2 g, which are evenly added to the diluted H2SO4 solution in 20 times. Take 30 ml as the negative electrode electrolyte and place it in the negative electrode storage tank.

[0090] The rest are the same as in Example 1.

[0091] The high concentration vanadium-titanium liquid flow battery obtained in this embodiment is Figure 3 As shown, at 100mA / cm 2 At a current density of , the coulombic efficiency of the battery is close to 100%, and after 100 cycles, the energy efficiency remains above 77%. Figure 4 As shown, under the same conditions, the cost of the negative electrode electrolyte of the vanadium-titanium liquid flow battery in this embodiment is approximately 17.2% of the cost of the negative electrode electrolyte of the all-vanadium liquid flow battery. Figure 5 As shown, the high concentration vanadium titanium liquid flow battery obtained in this embodiment is first charged at 100 mA / cm 2 , 50mA / cm2 , 20mA / cm 2 and 10mA / cm 2 The battery was charged with a constant current density of 1000 mW / cm2. After being fully charged, the battery was discharged with a gradually increasing current density to test the battery polarization performance. The vanadium-titanium liquid flow battery in this embodiment has a high capacity and a power density of 537 mW / cm2. 2 , good performance.

[0092] Example 4

[0093] The method for preparing a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery in this embodiment comprises the following steps:

[0094] Except for (2), the supporting electrolyte is 6 mol / L HCl solution.

[0095] In (3), the supporting electrolyte is a 6 mol / L HCl solution. In the specific configuration method, take 50 ml of 37% concentrated hydrochloric acid. Take 30 ml as the negative electrode electrolyte and place it in the negative electrode storage tank.

[0096] The rest is the same as Example 3.

[0097] The high concentration of vanadium-titanium liquid flow battery obtained in this example is 100mA / cm 2 It can still work normally at a current density of 1.50 W, with good performance, high cycle stability and coulombic efficiency close to 100%.

[0098] Example 5

[0099] The method for preparing a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery in this embodiment comprises the following steps:

[0100] Except for (2), the active substance is VO2 with a concentration of 0.1 mol / L and the supporting electrolyte is H2SO4 solution with a concentration of 1 mol / L.

[0101] In (3), the active substance is a Ti(SO4)2 solution with a concentration of 0.1 mol / L, and the stabilizer is trisodium citrate with a concentration of 0.01 mol / L.

[0102] The rest are the same as in Example 1.

[0103] The high concentration of vanadium-titanium liquid flow battery obtained in this example is 100mA / cm 2 The capacity can still work normally at a current density of 1.5 % and rises after a short drop in the early cycle (due to Ti 4+ With TiO 2+ The battery performance is good and the coulombic efficiency is close to 100%.

[0104] Example 6

[0105] The method for preparing a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery in this embodiment comprises the following steps:

[0106] Except for (3), the active substances are TiOSO4 solution with a concentration of 1 mol / L and Ti(SO4)2 with a concentration of 1 mol / L.

[0107] The rest are the same as in Example 1.

[0108] The high concentration of vanadium-titanium liquid flow battery obtained in this example is 100mA / cm 2 The capacity can still work normally at a current density of 1.5 % and rises after a short drop in the early cycle (due to Ti 4+ With TiO 2+ The equilibrium is reached, and due to the presence of Ti in the solution 4+ and TiO 2+ , this embodiment reaches equilibrium faster than embodiment 5), and tends to be stable, the battery performance is good, and the coulombic efficiency is close to 100%.

[0109] Example 7

[0110] The method for preparing a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery in this embodiment comprises the following steps:

[0111] Except for (2), the active substance is V2O5 with a concentration of 1.5 mol / L and the supporting electrolyte is H2SO4 solution with a concentration of 3 mol / L.

[0112] Except for (3), the active material is a TiCl3 solution with a concentration of 2.5 mol / L, and the supporting electrolyte is a HCl solution with a concentration of 6 mol / L.

[0113] Except for (5), the flow battery system is discharged using a constant current so that the SOD of the negative electrode electrolyte is 50%.

[0114] The rest are the same as in Example 1.

[0115] The high concentration of vanadium-titanium liquid flow battery obtained in this example is 100mA / cm 2 It can still work normally at a current density of 1.50 W, with good performance, high cycle stability and coulombic efficiency close to 100%.

[0116] Example 8

[0117] The method for preparing a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery in this embodiment comprises the following steps:

[0118] Except for (3), the active substances are 0.8 mol / L titanium oxychloride TiOCl2 solution and 0.8 mol / L TiCl3 solution. The supporting electrolyte is 6 mol / L HCl solution;

[0119] Remove step (5);

[0120] The rest are the same as in Example 1.

[0121] The high concentration of vanadium-titanium liquid flow battery obtained in this example is 100mA / cm 2 It can still work normally at a current density of 1.50 W, with good performance, high cycle stability and coulombic efficiency close to 100%.

[0122] Example 9

[0123] The method for preparing a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery in this embodiment comprises the following steps:

[0124] Except for (3), the active substances are 1.5 mol / L TiOSO4 solution and 1.5 mol / L Ti2(SO4)3 solution;

[0125] Remove step (5);

[0126] The rest are the same as in Example 1.

[0127] The high concentration of vanadium-titanium liquid flow battery obtained in this example is 100mA / cm 2 It can still work normally at a current density of 1.50 W, with good performance, high cycle stability and coulombic efficiency close to 100%.

[0128] Example 10

[0129] The method for preparing a low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery in this embodiment comprises the following steps:

[0130] Except in (2), the volume of the positive electrode electrolyte is 30 ml and is placed in the positive electrode storage tank;

[0131] (4) The thickness of the three-dimensional porous carbon felt is 5.5 mm and the size is 4 mm × 4 mm;

[0132] The rest is the same as Example 3.

[0133] In this embodiment, the vanadium-titanium liquid flow battery stack is composed of three single cells, such as Figure 6 As shown, at 200mA / cm 2 At a current density of , the Coulombic efficiency of the vanadium-titanium liquid flow battery stack is 100% and the energy efficiency is 72%. After 1,000 cycles, the Coulombic efficiency still remains at 100%, indicating that it can be applied on a large scale.

[0134] Comparative Example 1

[0135] A method for preparing a vanadium-titanium liquid flow battery comprises the following steps:

[0136] Except for (3), no trisodium citrate is added;

[0137] The rest is the same as Example 3.

[0138] The vanadium-titanium liquid flow battery assembled in this comparative example undergoes hydrolysis during the dissolution process and the battery cycle process, generating TiO2 precipitates that are partially insoluble in the supporting electrolyte, resulting in a decrease in capacity and low coulombic efficiency, which can even cause pipe blockage and battery failure.

[0139] Comparative Example 2

[0140] A method for preparing a vanadium-titanium liquid flow battery comprises the following steps:

[0141] Except for (3), the entire system is operated at room temperature during the preparation of the negative electrode electrolyte;

[0142] The rest is the same as Example 3.

[0143] The vanadium-titanium liquid flow battery assembled in this comparative example showed hydrolysis during the dissolution process, and the active material was lost. After being assembled into a battery, the 2 The battery can still work normally at a current density of , and has good performance, high cycle stability, and a coulombic efficiency close to 100%, but the capacity is reduced compared with Example 3.

[0144] The results of the embodiments of the present invention show that the low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery prepared by the present invention has the advantages of good cycle performance and high stability, which effectively solves the problem of high cost of traditional all-vanadium liquid flow batteries, and can still maintain excellent performance after forming a battery stack. In short, the low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery of the present invention has the advantages of low cost and high performance, and can promote the commercial application and development of liquid flow batteries.

[0145] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0146] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. A low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery, characterized in that: include: Positive electrode electrolyte: comprising a vanadium compound and an auxiliary acid solution; the vanadium compound comprises one or more of vanadium dioxide, vanadium pentoxide, and vanadyl sulfate, and the concentration thereof is 0.1 mol / L to 3 mol / L; the auxiliary acid solution comprises sulfuric acid or hydrochloric acid, and the concentration thereof is 1 mol / L to 6 mol / L; Negative electrolyte: including titanium compounds, auxiliary acid solution, and stabilizer; the titanium compound includes any one or more of TiO2, Ti(SO4)2, TiCl4, TiOSO4, TiOCl2, and TiCl3, and its concentration is 0.1mol / L~3mol / L; the auxiliary acid solution includes sulfuric acid or hydrochloric acid, and its concentration is 1mol / L~6mol / L; the stabilizer is trisodium citrate, and its concentration is 0.01mol / L~0.3mol / L; The method for preparing the negative electrode electrolyte comprises the following steps: Adding the stabilizer to the auxiliary acid solution with a concentration of 1 mol / L to 6 mol / L, wherein the stabilizer is prepared at a concentration of 0.01 mol / L to 0.3 mol / L; The titanium compound is weighed and evenly added to the auxiliary acid solution with the stabilizer in 5 to 20 times. The whole system is placed in an ice-water bath and magnetically stirred at the same time. The interval between each addition is 10 min to 30 min. After the addition is completed, the system is ultrasonically treated in the ice-water bath for 20 min to 60 min, and then continues to stand in the ice-water bath for 1 h to 3 h. The volume is fixed using a volumetric flask to obtain the negative electrode electrolyte.

2. A low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery according to claim 1, characterized in that: The concentration of the vanadium compound is 1 mol / L to 1.5 mol / L.

3. A low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery according to claim 1, characterized in that: The concentration of the titanium compound is 1 mol / L to 2 mol / L.

4. A low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery according to claim 3, characterized in that: The titanium compound is: Ti 4+ Compounds and TiO 2+ Mixture of compounds, TiO 2+ Compounds and Ti 3+ A mixture of compounds.

5. A low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery according to claim 1, characterized in that: It also includes a diaphragm treated with acid solution, and the treatment method is: placing the diaphragm in 1mol / L~3mol / L acid solution, and treating it at a constant temperature of 50℃~80℃ for 1h~3h, and the obtained product is obtained by washing and drying.

6. A low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery according to claim 5, characterized in that: The diaphragm includes: Nafion membrane, PP membrane, PE membrane, PEO membrane, SPEEK membrane, SPES membrane, PVDF membrane, PTFE membrane or PBI membrane; the acid solution includes hydrochloric acid or sulfuric acid.

7. A low-cost, high-performance, large-scale energy storage vanadium-titanium liquid flow battery according to claim 1, characterized in that: It also includes a three-dimensional porous electrode; the three-dimensional porous electrode includes one of nickel mesh, graphite felt or carbon felt, and has a thickness of 1mm to 8mm.

Citation Information

Cited By

  • Manganese-vanadium-titanium electrolyte and application thereof in flow battery

    CN122762755A