An electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester additive and its preparation and application
By adding ethylene glycol 3-isopropylphenylborate additive to the lithium-ion battery electrolyte to form a protective film, the problem of insufficient rate performance of lithium-ion battery is solved, and efficient electrochemical performance improvement and cycle stability are achieved. Enhanced.
Patent Information
- Application Number
- CN202210379394.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-04-12
AI Technical Summary
The rate performance of lithium-ion batteries in high-power electrical appliances is insufficient, the commercial cathode materials used in the prior art are costly and have low working efficiency, and there is a lack of effective electrolyte additives to improve the cathode electrochemical performance.
Add ethylene glycol 3-isopropylphenyl borate as a functional additive to form a protective film by oxidizing and decomposing it in advance on the surface of the positive electrode material, optimizing the positive electrode/electrolyte interface, improving the transfer speed of lithium ions and suppressing electrolysis Catalytic oxidation and decomposition of liquid.
It significantly improves the high-voltage rate performance and cycle stability of lithium-ion batteries, especially under high voltage conditions, which extends the battery's cycle life and improves capacity utilization.
Smart Images

Figure CN114824475B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of lithium ion batteries, and particularly relates to an electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester additive, and a preparation method and application thereof. Background Art
[0002] Among commercial secondary batteries, lithium-ion batteries have the highest specific energy, the best cycle performance, and strong safety performance. The electrode material selection is diverse, so it has broad development prospects as an energy storage battery. However, with the advancement of technology and the continuous development of the market, the battery rate performance has hindered the development of lithium-ion batteries in high-power electrical appliances. Therefore, improving the rate performance of lithium batteries has become another new topic that troubles scientific researchers.
[0003] Most of the commercial cathode materials currently used are lithium cobalt oxide (145 mAh g -1 ), lithium iron phosphate (165mAh g -1 ), etc., can no longer meet the needs of high-power electrical appliances in high-current charging and discharging. Developing new battery materials with excellent kinetic properties is a way to solve the problem of insufficient rate performance. However, this method has the disadvantages of requiring huge capital investment, high cost, and low work efficiency. Adding additives to the electrolyte that effectively improve the electrode kinetic performance can also effectively improve the rate performance of the battery. This method is simple and effective, so finding an electrolyte that can match the high-rate charging and discharging rules is another more economical and effective method. Additives that optimize the electrode interface can be added to carbonate electrolytes to achieve the purpose of improving rate performance. At present, many additives have been studied that form a protective film on the surface of the material by generating decomposition products through early oxidation, but the 3-isopropylphenyl boric acid ethylene glycol ester of the present invention has not been added as a functional additive to improve the positive electrode electrochemical properties of lithium-ion batteries. Summary of the invention
[0004] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide an electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester additive, which can be oxidized and decomposed in advance on the material surface and form a film on the positive electrode.
[0005] Another object of the present invention is to provide a method for preparing the electrolyte containing the above-mentioned 3-isopropylphenylboronic acid ethylene glycol ester additive.
[0006] Another object of the present invention is to provide the use of the electrolyte containing the above-mentioned 3-isopropylphenylboronic acid ethylene glycol ester additive in lithium ion batteries.
[0007] The purpose of the present invention is achieved through the following solutions:
[0008] An electrolyte containing 3-isopropylbenzene boric acid ethylene glycol ester additive consists of a common electrolyte and a functional additive, wherein the functional additive is 3-isopropylbenzene boric acid ethylene glycol ester.
[0009] The addition of the functional additive optimizes the positive electrode / electrolyte interface, increases the transfer speed of lithium ions, and reduces the surface catalytic activity of the positive electrode, inhibiting the catalytic oxidation decomposition of the electrolyte. Therefore, the present invention can improve the performance of high voltage (>4.2V) LiNi 0.8 Co 0.15 Al 0.05 The high voltage rate performance and cycle stability of lithium-ion batteries with O2 material as the positive electrode material.
[0010] The content of the functional additive is 3-7% of the mass of the ordinary electrolyte, preferably 5%.
[0011] Preferably, the common electrolyte includes a cyclic carbonate solvent, a linear carbonate solvent and an ion-conducting lithium salt; wherein the cyclic carbonate solvent is ethylene carbonate or propylene carbonate; the linear carbonate solvent includes at least one of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate and methyl propyl carbonate; the ion-conducting lithium salt is selected from at least one of LiPF6, LiBF4, LiBOB, LiDFOB, LiSO3CF3, LiCLO4, LiAsF6, Li(CF3SO2)2N and LiC(CF3SO2)3.
[0012] In the common electrolyte, the mass ratio of the cyclic carbonate solvent to the linear carbonate solvent is (1:3) to (3:2); the solubility of the ion-conducting lithium salt in the common electrolyte is 0.8 to 1.2 mol / L.
[0013] A method for preparing the electrolyte containing the above-mentioned 3-isopropylphenyl boric acid ethylene glycol ester additive comprises the following steps: adding a functional additive to a common electrolyte to obtain a lithium ion battery electrolyte containing the 3-isopropylphenyl boric acid ethylene glycol ester additive.
[0014] The preparation method of the common electrolyte comprises the following steps: mixing a cyclic carbonate solvent and a linear carbonate solvent, purifying and removing impurities and water, and adding an ion-conducting lithium salt thereto at room temperature to obtain the common electrolyte.
[0015] The purification, impurity removal and water removal refer to treatment by any one or more of molecular sieve, activated carbon, calcium hydride, lithium hydride, anhydrous calcium oxide, calcium chloride, phosphorus pentoxide, alkali metal or alkaline earth metal; the molecular sieve adopts 3A type, 4A type or 5A type.
[0016] The room temperature is 25-30°C.
[0017] The electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester additive is used to manufacture lithium ion batteries, and the obtained batteries have good cycle stability.
[0018] A lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, an electrolyte and a diaphragm; wherein the electrolyte is the electrolyte containing 3-isopropylphenyl borate ethylene glycol ester additive as mentioned above, the positive electrode sheet is made of lithium nickel cobalt aluminum oxide material, lithium nickel cobalt manganese oxide material or LiCoO2, the negative electrode sheet is made of metallic lithium, and the diaphragm between the positive electrode sheet and the negative electrode sheet is a polyethylene film.
[0019] The functional additive used in the present invention can form a stable protective film on the surface of the positive electrode material during the charge and discharge process of 3-4.35V. The additive can optimize the interface of the positive electrode, increase the transfer speed of lithium ions, and inhibit the oxidative decomposition of the high-voltage electrolyte, thereby protecting the structure of the positive electrode material and improving the rate performance and cycle stability of the lithium-ion battery.
[0020] The mechanism of the present invention is:
[0021] The invention improves the rate performance and cycle stability of the battery by adding 3-isopropylphenylboronic acid ethylene glycol ester to the electrolyte, which is convenient and economical. At the same time, the electrolyte can significantly improve the cycle stability of the lithium ion battery under high voltage conditions.
[0022] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0023] The present invention uses an additive containing 3-isopropylphenyl boric acid ethylene glycol ester as a high-rate interface film-forming additive for lithium ion electrolyte. Since the additive has a lower oxidation potential, it can be oxidized and decomposed in advance during the first charging process, and its decomposition products form a protective film on the positive electrode surface. This protective film can optimize the interface of the positive electrode material / electrolyte under high pressure, allowing lithium ions to pass smoothly, and inhibiting the oxidative decomposition of the electrolyte, which can significantly improve the rate performance and cycle performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a comparison chart of the cycle performance of lithium ion batteries made from the electrolytes prepared in Examples 1, 2, 3 of the present invention and Comparative Example 1 after 100 cycles.
[0025] Figure 2 It is a comparison chart of the rate performance of lithium ion batteries prepared in Example 2 of the present invention and in Comparative Example 1.
[0026] Figure 3 It is a comparison chart of the rate performance of lithium-ion batteries made in Example 4 of the present invention and in Comparative Example 2.
[0027] Figure 4 It is a comparison chart of the rate performance of lithium ion batteries made in Example 5 of the present invention and in Comparative Example 3. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0029] Unless otherwise specified, the reagents used in the examples can be purchased from the market.
[0030] Example 1
[0031] (1) At room temperature, cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a mass ratio of EC:EMC:DEC=3:5:2, stirred evenly, and purified by molecular sieve to remove impurities and water;
[0032] (2) at room temperature, dissolving the ion-conducting lithium salt LiPF6 in the solvent obtained in step (1) to a final solubility of 1.0 mol / L, stirring evenly, and obtaining a common electrolyte;
[0033] (3) The amount of 3-isopropylphenyl boric acid ethylene glycol ester additive added to the ordinary electrolyte prepared in step (1) is 3% of the mass of the ordinary electrolyte, thereby obtaining a high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive.
[0034] (4) Using layered lithium nickel cobalt aluminum oxide LiNi 0.8 Co 0.15 Al 0.05 O2 is used as the positive electrode material, metallic lithium is used as the negative electrode material, Ceglard 2500 is used as the battery separator, and the high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive prepared in step (3) is added to obtain a lithium-ion battery containing a high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive.
[0035] Example 2
[0036] (1) At room temperature, cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a mass ratio of EC:EMC:DEC=3:5:2, stirred evenly, and purified by molecular sieve to remove impurities and water;
[0037] (2) at room temperature, dissolving the ion-conducting lithium salt LiPF6 in the solvent obtained in step (1) to a final solubility of 1.0 mol / L, stirring evenly, and obtaining a common electrolyte;
[0038] (3) The amount of 3-isopropylphenyl boric acid ethylene glycol ester additive added to the ordinary electrolyte prepared in step (1) is 5% of the mass of the ordinary electrolyte, thereby obtaining a high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive.
[0039] (4) Using layered lithium nickel cobalt aluminum oxide LiNi 0.8 Co 0.15 Al 0.05 O2 is used as the positive electrode material, metallic lithium is used as the negative electrode material, Ceglard 2500 is used as the battery separator, and the high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive prepared in step (3) is added to obtain a lithium-ion battery containing a high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive.
[0040] Example 3
[0041] (1) At room temperature, cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a mass ratio of EC:EMC:DEC=3:5:2, stirred evenly, and purified by molecular sieve to remove impurities and water;
[0042] (2) at room temperature, dissolving the ion-conducting lithium salt LiPF6 in the solvent obtained in step (1) to a final solubility of 1.0 mol / L, stirring evenly, and obtaining a common electrolyte;
[0043] (3) The amount of 3-isopropylphenyl boric acid ethylene glycol ester additive added to the ordinary electrolyte prepared in step (1) is 7% of the mass of the ordinary electrolyte, thereby obtaining a high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive.
[0044] (4) Using layered lithium nickel cobalt aluminum oxide LiNi 0.8 Co 0.15 Al 0.05 O2 is used as the positive electrode material, metallic lithium is used as the negative electrode material, Ceglard 2500 is used as the battery separator, and the high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive prepared in step (3) is added to obtain a lithium-ion battery containing a high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive.
[0045] Example 4
[0046] (1) At room temperature, cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a mass ratio of EC:EMC:DEC=3:5:2, stirred evenly, and purified by molecular sieve to remove impurities and water;
[0047] (2) at room temperature, dissolving the ion-conducting lithium salt LiPF6 in the solvent obtained in step (1) to a final solubility of 1.0 mol / L, stirring evenly, and obtaining a common electrolyte;
[0048] (3) The amount of 3-isopropylphenyl boric acid ethylene glycol ester additive added to the ordinary electrolyte prepared in step (1) is 5% of the mass of the ordinary electrolyte, thereby obtaining a high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive.
[0049] (4) Using layered lithium nickel cobalt manganese oxide LiNi 0.8 Co 0.1 Mn 0.1 O2 is used as the positive electrode material, metallic lithium is used as the negative electrode material, Ceglard 2500 is used as the battery separator, and the high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive prepared in step (3) is added to obtain a lithium-ion battery containing a high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive.
[0050] Example 5
[0051] (1) At room temperature, cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a mass ratio of EC:EMC:DEC=3:5:2, stirred evenly, and purified by molecular sieve to remove impurities and water;
[0052] (2) at room temperature, dissolving the ion-conducting lithium salt LiPF6 in the solvent obtained in step (1) to a final solubility of 1.0 mol / L, stirring evenly, and obtaining a common electrolyte;
[0053] (3) The amount of 3-isopropylphenyl boric acid ethylene glycol ester additive added to the ordinary electrolyte prepared in step (1) is 5% of the mass of the ordinary electrolyte, thereby obtaining a high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive.
[0054] (4) Using lithium cobalt oxide LiCoO2 as the positive electrode material, metallic lithium as the negative electrode material, Ceglard 2500 as the battery separator, and adding the high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive prepared in step (3) to obtain a lithium-ion battery containing a high-rate electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive.
[0055] Comparative Example 1
[0056] (1) At room temperature, cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a mass ratio of EC:EMC:DEC=3:5:2, stirred evenly, and purified by molecular sieve to remove impurities and water;
[0057] (2) at room temperature, dissolving the ion-conducting lithium salt LiPF6 in the solvent obtained in step (1) to a final solubility of 1.0 mol / L, stirring evenly, and obtaining a common electrolyte;
[0058] (3) Using layered lithium nickel cobalt aluminum oxide LiNi 0.8 Co 0.15 Al 0.05 O2 is used as the positive electrode material, metallic lithium is used as the negative electrode material, Ceglard 2500 is used as the battery separator, and the common electrolyte prepared in step (2) is added to form a lithium-ion battery with the common electrolyte.
[0059] Comparative Example 2
[0060] (1) mixing cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) in a mass ratio of EC:EMC:DEC=3:5:2, stirring evenly, and purifying with molecular sieve to remove impurities and water;
[0061] (2) at room temperature, dissolving the ion-conducting lithium salt LiPF6 in the solvent obtained in step (1) to a final solubility of 1.0 mol / L, stirring evenly, and obtaining a common electrolyte;
[0062] (3) Using layered lithium nickel cobalt manganese oxide LiNi 0.8 Co 0.1 Mn 0.1 O2 is used as the positive electrode material, metallic lithium is used as the negative electrode material, Ceglard 2500 is used as the battery separator, and the common electrolyte prepared in step (2) is added to form a lithium-ion battery with the common electrolyte.
[0063] Comparative Example 3
[0064] (1) mixing cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) in a mass ratio of EC:EMC:DEC=3:5:2, stirring evenly, and purifying and removing impurities and water by using molecular sieve;
[0065] (2) at room temperature, dissolving the ion-conducting lithium salt LiPF6 in the solvent obtained in step (1) to a final solubility of 1.0 mol / L, stirring evenly, and obtaining a common electrolyte;
[0066] (3) Using lithium cobalt oxide LiCoO2 as the positive electrode material, metallic lithium as the negative electrode material, Ceglard 2500 as the battery separator, and adding the common electrolyte prepared in step (2), a lithium-ion battery with the common electrolyte.
[0067] The cycle performance comparison of lithium ion batteries made of the electrolytes prepared in Examples 1, 2, and 3 of the present invention and Comparative Example 1 after 100 cycles is shown in the figure below: Figure 1 As shown, from Figure 1 It can be seen that in the charge-discharge cycle with a charge-discharge range of 3.0 to 4.35 V, the capacity retention rate of Example 2 after 100 cycles is 96%, which is significantly better than 79% of Comparative Example 1.
[0068] The comparison of the rate performance of the lithium ion battery prepared in Example 2 of the present invention and in Comparative Example 1 is shown in the figure below: Figure 2 As shown, from Figure 2 It can be seen that in the charge and discharge range of 3.0 to 4.35 V, Example 2 has better capacity utilization and cycle stability at a larger charge and discharge current.
[0069] The comparison of the rate performance of lithium ion batteries prepared in Example 4 of the present invention and Comparative Example 2 is shown in the figure below. Figure 3 As shown, from Figure 3 It can be seen that in the charge and discharge range of 3.0 to 4.35 V, Example 4 has better capacity utilization and cycle stability at any charge and discharge current.
[0070] The comparison of the rate performance of lithium ion batteries prepared in Example 5 of the present invention and Comparative Example 3 is shown in the figure below. Figure 4 As shown, from Figure 4 It can be seen that in the charge and discharge range of 3.0 to 4.35 V, Example 5 has better capacity utilization and cycle stability at any charge and discharge current.
[0071] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. An electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester additive, characterized in that It is composed of a common electrolyte and a functional additive, wherein the functional additive is 3-isopropylphenyl boric acid ethylene glycol ester; The common electrolyte comprises a cyclic carbonate solvent, a linear carbonate solvent and an ion-conducting lithium salt.
2. The electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester additive according to claim 1, characterized in that: The content of the functional additive is 3-7% of the mass of ordinary electrolyte.
3. The electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester additive according to claim 1, characterized in that: The content of the functional additive is 5% of the mass of ordinary electrolyte.
4. The electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester additive according to claim 1, characterized in that: The cyclic carbonate solvent is ethylene carbonate or propylene carbonate; the linear carbonate solvent includes at least one of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate and methyl propyl carbonate; the ion-conducting lithium salt is selected from at least one of LiPF6, LiBF4, LiBOB, LiDFOB, LiSO3CF3, LiCLO4, LiAsF6, Li(CF3SO2)2N and LiC(CF3SO2)3.
5. The electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester additive according to claim 1, characterized in that: In the common electrolyte, the mass ratio of the cyclic carbonate solvent to the linear carbonate solvent is (1:3) to (3:2); the solubility of the ion-conducting lithium salt in the common electrolyte is 0.8 to 1.2 mol / L.
6. A method for preparing an electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester as an additive according to any one of claims 1 to 5, characterized in that The following steps are involved: By adding the functional additive into the common electrolyte, the lithium ion battery electrolyte containing 3-isopropylphenyl boric acid ethylene glycol ester additive is obtained.
7. The method for preparing an electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester as an additive according to claim 6, characterized in that: The preparation method of the common electrolyte comprises the following steps: mixing a cyclic carbonate solvent and a linear carbonate solvent, purifying and removing impurities and water, and adding an ion-conducting lithium salt thereto at room temperature to obtain the common electrolyte.
8. The method for preparing an electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester as an additive according to claim 7, characterized in that: The purification, impurity removal and water removal refer to treatment by any one or more of molecular sieve, activated carbon, calcium hydride, lithium hydride, anhydrous calcium oxide, calcium chloride, phosphorus pentoxide, alkali metal or alkaline earth metal; the molecular sieve adopts 3A type, 4A type or 5A type.
9. Use of the electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester additive according to any one of claims 1 to 5 in the manufacture of lithium ion batteries.
10. A lithium ion battery, characterized in that The invention comprises a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator; wherein the electrolyte is the electrolyte containing 3-isopropylphenylboronic acid ethylene glycol ester additive as claimed in any one of claims 1 to 5.