A natural fiber composite material and its preparation method and application
Through the method of melt mixing machine and molding of plunger injection molding machine, combined with the use of compatibilizers, the problem of low mechanical properties of natural fiber composite materials has been solved, significantly improved its mechanical properties and interface strength, and expanded its engineering Application in the field.
Patent Information
- Application Number
- CN202210289736.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-03-23
AI Technical Summary
The mechanical properties of natural fiber composites are lower than those of artificial fiber composites, and polar natural fibers are poorly compatible with traditional non-polar resins, which limits their application in the engineering field.
The natural fibers are melted and mixed with the thermoplastic resin by using a mixer, and molded through a plunger injection molding machine to retain the original length of the fibers and add compatibilizers to improve the interface performance.
It significantly improves the mechanical properties of natural fiber composite materials, enhances the interface bonding between fiber and resin matrix, and expands its application range in the field of engineering.
Smart Images

Figure CN114833989B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of composite material preparation, and in particular to a natural fiber composite material and a preparation method and application thereof. Background Art
[0002] With the increasing environmental awareness, the increasing scarcity of petroleum-based resources and the inherent advantages of natural fibers, such as low cost, light weight, renewable, degradable, high specific strength and specific modulus, natural fibers have gradually replaced artificial fibers to prepare composite materials. However, the strength and modulus of natural fiber composites are much lower than those of artificial fiber composites, and conventional natural fiber composites are often melt-mixed by a twin-screw extruder and then injection-molded by a screw injection molding machine. This screw processing method reduces the length of natural fibers and further reduces the mechanical properties of natural fiber composites. Polar natural fibers have poor compatibility with traditional non-polar resins, resulting in poor interfacial strength, which greatly limits the application of natural fiber composites in engineering fields. Therefore, the development of an environmentally friendly natural fiber composite with high mechanical properties has become an urgent need for the development of polymer composites, which just conforms to the trend of industrialization development and has broad application prospects in engineering fields such as automobiles, aerospace, packaging, sports, and construction. Summary of the invention
[0003] The purpose of the present invention is to provide a new natural fiber composite material and its preparation method and application, so as to solve the problem of low mechanical properties caused by existing screw extrusion injection molding, so as to expand the application scope of natural fiber composite materials in the engineering field.
[0004] To achieve the above object, the present invention adopts the following technical solution:
[0005] According to a first aspect of the present invention, there is provided a method for preparing a natural fiber composite material, comprising:
[0006] Step (1), shearing the natural fibers, and drying the natural fibers, the compatibilizer and the thermoplastic resin;
[0007] Step (2), preparing the natural fiber composite material by using an internal mixer, and shearing the natural fiber composite material into block-shaped composite materials;
[0008] Step (3), adding the block composite material into a plunger type injection molding machine for melting treatment and then injection molding a natural fiber composite material product.
[0009] Furthermore, in step (1), the natural fiber is one of flax, ramie, hemp, jute, sisal, wood fiber, cotton, kapok, coconut shell, and bamboo fiber.
[0010] Furthermore, in the step (1), the thermoplastic resin is one of polylactic acid (PLA), polybutylene adipate / terephthalate (PBAT), poly-β-hydroxybutyric acid (PHB), glycolic acid-hydroxyvaleric acid copolyester (PBHV), polycaprolactone (PCL), polypropylene (PP), polyethylene (PE), polyamide (PA), polybutylene succinate (PBS), starch and copolyesteramide (PEA).
[0011] Furthermore, in the step (1), the compatibilizer is one of maleic anhydride grafted PP, maleic anhydride grafted POE, polyvinyl alcohol, and triglycidyl isocyanurate (TGIC).
[0012] Furthermore, the step (1) specifically includes: cutting the natural fiber into 5 mm pieces, and drying the natural fiber, the compatibilizer and the thermoplastic resin at a drying temperature of 40-60° C. for 6-10 hours.
[0013] Furthermore, the step (2) specifically comprises: adding a thermoplastic resin into an internal mixer, adding a certain proportion of a compatibilizer and natural fiber after the thermoplastic resin is melted, mixing for 8-12 minutes, taking out the natural fiber composite material, and shearing it into block composite materials while it is hot.
[0014] Furthermore, in the step (2), the mass fraction of the natural fiber is 10-40wt.%, and the mass fraction of the compatibilizer is 0.5-5wt.%.
[0015] Furthermore, the step (3) specifically comprises: adding the block composite material into a plunger injection molding machine, heating the block composite material to a temperature of 150°C-210°C for a heating time of 5-10 minutes, and injecting the natural fiber composite material product after the block composite material is melted.
[0016] According to a second aspect of the present invention, a natural fiber composite material is provided. The natural fiber composite material is prepared by the preparation method according to any one of the above aspects.
[0017] According to a third aspect of the present invention, there is provided a use of the natural fiber composite material as described above in a secondary load-bearing component.
[0018] Beneficial effects of the present invention:
[0019] The present invention uses an internal mixer to melt and mix natural fibers and thermoplastic resins, and then uses a plunger injection molding machine to form composite products, thereby retaining the original length of the fibers to the greatest extent and improving the mechanical properties of natural fiber composite plastic parts. The addition of a compatibilizer improves the interface properties between the natural fibers and the resin matrix, thereby further improving the mechanical properties of the natural fiber composite material.
[0020] The natural fiber and the thermoplastic resin are melt-mixed by adopting an internal mixer, so that the natural fiber and the thermoplastic resin are melt-mixed more evenly.
[0021] By adopting the plunger injection molding method to manufacture composite products, longer natural fibers can be retained, thereby improving the mechanical properties of natural fiber composite plastic parts.
[0022] By adding a compatibilizer, the bonding force of the interface between the natural fiber surface and the resin matrix can be improved, thereby improving the performance of the interface between the natural fiber and the resin matrix, and further improving the mechanical properties of natural fiber composite plastic parts. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0024] Figure 1 The flowchart of the method for preparing a natural fiber composite material according to the technical solution of the present invention is shown.
[0025] Figure 2 A schematic diagram of a process for preparing a natural fiber composite material according to an embodiment of the present invention is shown.
[0026] Figure 3 A schematic diagram of a UL-94 combustion test of a flame retardant composite material according to an embodiment of the present invention is shown.
[0027] FIG. 4A to FIG. 4B A schematic diagram of a PLA / RF impact fracture according to an embodiment of the present invention is shown.
[0028] FIG. 5A to FIG. 5B A schematic diagram of a PLA / RF / 4EBA-GMA impact fracture according to an embodiment of the present invention is shown.
[0029] FIG. 6A to FIG. 6B A schematic diagram of a PLA / RF / 8EBA-GMA impact fracture according to an embodiment of the present invention is shown.
[0030] FIG. 7A to FIG. 7B A schematic diagram of a PLA / RF / 12EBA-GMA impact fracture according to an embodiment of the present invention is shown.
[0031] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0032] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present disclosure. Instead, they are merely examples of devices and methods consistent with some aspects of the present disclosure as detailed in the appended claims.
[0033] The terms "first", "second", etc. in the specification and claims of the present disclosure are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchanged where appropriate, so that the embodiments of the present disclosure described herein can be implemented in an order other than those illustrated or described herein, for example.
[0034] In addition, the terms "comprises," "comprising," and "having," and any variations thereof, are intended to cover non-exclusive inclusions. For example, a process, method, system, product, or apparatus that includes a series of steps or elements is not necessarily limited to those steps or elements explicitly listed, but may include other steps or elements not explicitly listed or inherent to such process, method, product, or apparatus.
[0035] Multiple includes two or more.
[0036] It should be understood that the term "and / or" used in this disclosure is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone.
[0037] The present invention discloses a novel natural fiber composite material injection molding method, wherein natural fibers of a certain length and thermoplastic resin are melt-mixed in a certain proportion through an internal mixer, and then the uniformly mixed composite material is sheared into a block composite material of a certain size by using residual heat, and finally injection molding is performed by a plunger injection molding machine. Figure 1 and 2 As shown, the method specifically includes:
[0038] Step 101, cutting the natural fiber into 5 mm pieces, and drying the natural fiber, compatibilizer and thermoplastic resin at a drying temperature of 40-60° C. for 6-10 hours.
[0039] Step 102, preparing a natural fiber composite material using an internal mixer: first add a thermoplastic resin, and after the thermoplastic resin is melted, add a certain proportion of a compatibilizer and natural fibers, mix for 8-12 minutes, take out the composite material, and cut the natural fiber composite material into block materials while it is hot.
[0040] Step 103, finally adding the block composite material into the plunger injection molding machine, heating the temperature to 150° C.-210° C., heating time to 5-10 min, and injecting the composite material product after the block composite material is melted.
[0041] The composite material formed by the present invention not only has the advantages of light weight, high strength, high modulus, etc., but also, compared with conventional twin-screw extrusion and screw injection molding, the new natural fiber composite material molding method can retain the original length of the natural fiber to the greatest extent and has excellent mechanical properties. In addition, adding a certain proportion of compatibilizer to the composite material can further improve the mechanical properties of the composite material.
[0042] Embodiment 1
[0043] The ramie fibers were cut into 5 mm lengths, and the ramie fibers and polylactic acid (PLA) were dried at 60 °C for 8 h.
[0044] The ramie fiber and polylactic acid (PLA) were melt-mixed in an internal mixer at a mass ratio of 1:9, and then the PLA / ramie fiber composite material was taken out and the composite material was sheared into block materials while hot;
[0045] Add the block composite material into the plunger injection molding machine, heat it to 210°C for 10 minutes, and after the block composite material is melted, injection mold the composite material product;
[0046] Comparative Example 1
[0047] The ramie fibers were cut into 5 mm lengths, and the ramie fibers and polylactic acid (PLA) were dried at 60 °C for 8 h.
[0048] The ramie fiber and polylactic acid (PLA) were melt-mixed in an internal mixer at a mass ratio of 1:9, and then the PLA / ramie fiber composite material was taken out and pressed into a sheet by a hot press;
[0049] The sheet-like composite material is crushed and extruded by a twin-screw extruder, and then the extruded molten composite material is directly injection molded.
[0050] Embodiment 2
[0051] The ramie fibers were cut into 5 mm lengths, and the ramie fibers and polylactic acid (PLA) were dried at 60 °C for 8 h.
[0052] The ramie fiber and polylactic acid (PLA) were melt-mixed in an internal mixer at a mass ratio of 2:8, and then the PLA / ramie fiber composite material was taken out and the composite material was sheared into block materials while hot;
[0053] Add the block composite material into the plunger injection molding machine, heat it to 210°C for 10 minutes, and after the block composite material is melted, injection mold the composite material product;
[0054] Comparative Example 2
[0055] The ramie fibers were cut into 5 mm lengths, and the ramie fibers and polylactic acid (PLA) were dried at 60 °C for 8 h.
[0056] The ramie fiber and polylactic acid (PLA) were melt-mixed in an internal mixer at a mass ratio of 2:8, and then the PLA / ramie fiber composite material was taken out and pressed into a sheet using a hot press;
[0057] The sheet-like composite material is crushed and extruded by a twin-screw extruder, and then the extruded molten composite material is directly injection molded.
[0058] Embodiment 3
[0059] The ramie fibers were cut into 5 mm lengths, and the ramie fibers and polylactic acid (PLA) were dried at 60 °C for 8 h.
[0060] The ramie fiber and polylactic acid (PLA) were melt-mixed in an internal mixer at a mass ratio of 3:7, and then the PLA / ramie fiber composite material was taken out and sheared into block materials while hot;
[0061] Add the block composite material into the plunger injection molding machine, heat it to 210°C for 10 minutes, and after the block composite material is melted, injection mold the composite material product;
[0062] Comparative Example 3
[0063] The ramie fibers were cut into 5 mm lengths, and the ramie fibers and polylactic acid (PLA) were dried at 60 °C for 8 h.
[0064] The ramie fiber and polylactic acid (PLA) were melt-mixed in an internal mixer at a mass ratio of 3:7, and then the PLA / ramie fiber composite material was taken out and pressed into a sheet by a hot press.
[0065] The sheet-like composite material is crushed and extruded by a twin-screw extruder, and then the extruded molten composite material is directly injection molded.
[0066] Capacity increase comparison
[0067] The ramie fiber was cut into 5 mm length, and the ramie fiber, triglycidyl isocyanurate (TGIC) and polylactic acid (PLA) were dried at 60 °C for 8 h.
[0068] Ramie fiber, polylactic acid (PLA) and TGIC were melt-mixed in an internal mixer at a mass ratio of 3:6.1:0.9, and then the PLA / ramie fiber composite material was taken out and the composite material was sheared into block materials while hot;
[0069] Add the block composite material into the plunger injection molding machine, heat it to 210°C for 10 minutes, and after the block composite material is melted, injection mold the composite material product;
[0070] Embodiment 4
[0071] The ramie fibers were cut into 5 mm lengths, and the ramie fibers and polylactic acid (PLA) were dried at 60 °C for 8 h.
[0072] The ramie fiber and polylactic acid (PLA) were melt-mixed in an internal mixer at a mass ratio of 4:6, and then the PLA / ramie fiber composite material was taken out and the composite material was sheared into block materials while hot;
[0073] Add the block composite material into the plunger injection molding machine, heat it to 210°C for 10 minutes, and after the block composite material is melted, injection mold the composite material product;
[0074] Comparative Example 4
[0075] The ramie fibers were cut into 5 mm lengths, and the ramie fibers and polylactic acid (PLA) were dried at 60 °C for 8 h.
[0076] The ramie fiber and polylactic acid (PLA) were melt-mixed in an internal mixer at a mass ratio of 4:6, and then the PLA / ramie fiber composite material was taken out and pressed into a sheet by a hot press;
[0077] The sheet-like composite material is crushed and extruded by a twin-screw extruder, and then the extruded molten composite material is directly injection molded.
[0078] The mechanical properties of the PLA / ramie fiber composite materials prepared in the example and the comparative example were tested, and the test results are shown in Table 1.
[0079]
[0080] Table 1
[0081] It can be seen from the test results in the above table that, under the premise of the same ramie fiber content, the comprehensive performance of the composite material prepared by the present invention is significantly higher than the mechanical properties of the composite material formed by conventional screw molding. This is mainly because the present invention adopts the internal mixer for melt mixing and the plunger injection molding method to retain the original length of the fiber to the greatest extent, thereby significantly improving the mechanical properties of the composite material, and the addition of the compatibilizer improves the interface strength between the natural fiber and the resin matrix, further improving the mechanical properties of the composite material.
[0082] PLA / RF vertical combustion and limiting oxygen index test
[0083] The vertical burning rating and limiting oxygen index combustion results of the composites are shown in Table 3. It can be seen that the PLA / RF composite without flame retardant failed the UL-94 vertical burning rating test, the limiting oxygen index was only 19.8%, and dripping occurred during the combustion process. When 30wt% of AlPi was added alone, the UL-94 vertical burning reached the V-2 level, and the corresponding LOI increased from 19.8% to 32.4%. When 30wt% of MCA was added alone, the composite did not pass the UL-94 vertical burning test, but the LOI increased from 19.8% to 27.3%. When AlPi:MCA=1:1, the UL-94 test reached the V-0 level, and the corresponding LOI reached 34.4%. The UL-94 and LOI test results of the PLA / RF / AM composites show that there is a synergistic effect between AlPi and MCA. As shown in Table 2, in the AlPi and MCA compound flame retardant system, as the content of flame retardant MCA increases, the UL-94 combustion level of the composite material increases first and then decreases. This is mainly because AlPi and MCA are mainly based on condensed phase and gas phase flame retardancy, respectively. Only when the condensed phase and gas phase are in a certain proportion can a good flame retardant effect be achieved. The limiting oxygen index and UL-94 test levels are completely opposite, which is mainly due to the different methods of UL-94 test and limiting oxygen index test.
[0084] Ramie fiber reinforced polylactic acid flame retardant composite material composition (wt%)
[0085]
[0086] Table 2
[0087] In the flame retardant compound of flame retardant A1Pi, MCA and SiO2, PLA / RF / A2MS and PLA / RF / AMS composite materials can reach V-0 flame retardant grade; however, compared with the compound flame retardant composite materials without SiO2, the flame retardant composite materials containing SiO2 have a lower limiting oxygen index, such as Figure 3As shown. Compared with the flame retardant grades of PLA / RF / 2AM and PLA / RF / A2M composites, PLA / RF / 2AMS and PLA / RF / A2MS have higher UL-94 combustion grades, which are increased to V-1 and V-0 grades respectively. However, when the flame retardant AlPi∶MCA∶SiO2 complex is 1∶1∶2, PLA / RF / AM2S did not pass the UL-94 combustion grade test, indicating that less SiO2 can better improve the firmness of the carbon layer on the surface of the composite material, thereby improving the flame retardant properties of the composite material; high content of SiO2 is not conducive to improving the flame retardant properties of the composite.
[0088] Vertical combustion level and limiting oxygen index
[0089]
[0090] Table 3
[0091] The figure below can more intuitively show the burning condition of the composite material after the UL-94 test. The PLA / RF composite material cannot be displayed because it burned violently and dripped severely. The PLA / RF / 3M composite material was burned out and twisted and deformed, while the PLA / RF / 2AM and PLA / RF / AM2S composite materials were fully burned. Compared with the PLA / RF / 3A and PLA / RF / 3M composite materials, the PLA / RF / AM composite material was burned less, further indicating that the flame retardants AlPi and MCA have a synergistic effect. After the addition of SiO2, it can be observed that the burning site has a significant expansion phenomenon, which is mainly because AlPi, MCA and SiO2 act as acid sources, gas sources and carbon sources respectively, and together constitute an intumescent flame retardant.
[0092] Impact toughness test of PLA / RF composites
[0093] The impact cross-section scanning electron microscopy images of PLA / RF composites and PLA / RF / compatibilizer EBA-GMA composites at 500-2000 times magnification are as follows: Figure 4A-4B to Figure 7A-7B. The composite surface has a lot of fiber debonding and pulling out phenomena, forming a lot of holes, reflecting the poor interfacial bonding strength between the polylactic acid resin matrix and the composite material. In the PLA / RF / EBA-GMA composite material, the PLA matrix and the reinforcing ramie fiber have good interfacial bonding, and the pulled-out fiber surface forms a matrix embedding phenomenon and even obvious damage and tearing phenomena. This phenomenon shows that the introduction of EBA-GMA significantly improves the interfacial bonding performance between the ramie fiber and the PLA resin matrix, improves the efficiency of stress transfer from the resin matrix to the ramie fiber during the material stress process, and then improves the bearing capacity of the ramie fiber in the composite material, which will cause the fiber to be damaged. The emergence of these phenomena also indicates that during the impact fracture of the material, the resin absorbs the impact energy through deformation, resulting in more energy dissipation, thereby improving the impact strength of the composite material.
[0094] The above embodiments are merely descriptions of the technical solutions of the present invention, rather than limiting its scope. Although ordinary technicians in the field can make various modifications with reference to the above embodiments, they should be within the protection scope of the present invention as long as they do not deviate from the design spirit of the present invention.
Claims
1. A method for preparing a natural fiber composite material, characterized in that: include: Step (1), cutting the natural fiber, and drying the natural fiber, the compatibilizer and the thermoplastic resin: cutting the natural fiber into 5 mm pieces, and drying the natural fiber, the compatibilizer and the thermoplastic resin at a drying temperature of 40-60° C. for 6-10 hours, wherein the compatibilizer is one of polyvinyl alcohol and triglycidyl isocyanurate (TGIC); Step (2), preparing a natural fiber composite material by using an internal mixer, and shearing the composite material into block-shaped blocks: adding a thermoplastic resin into the internal mixer, adding a certain proportion of a compatibilizer and natural fibers to melt and mix after the thermoplastic resin is melted, taking out the natural fiber composite material after mixing for 8-12 minutes, and shearing the composite material into block-shaped blocks of a certain size while it is hot; wherein the mass fraction of the natural fiber is 10-40wt.%, and the mass fraction of the compatibilizer is 0.5-5wt.%; Step (3), adding the block composite material into a plunger injection molding machine for melting treatment and then injection molding a natural fiber composite material product: adding the block composite material into a plunger injection molding machine, heating the block composite material to a temperature of 150°C-210°C for a heating time of 5-10 minutes, and injecting the natural fiber composite material product after the block composite material is melted.
2. The method for preparing a natural fiber composite material according to claim 1, characterized in that: In the step (1), the natural fiber is one of flax, ramie, hemp, jute, sisal, wood fiber, cotton, kapok, coconut shell, and bamboo fiber.
3. The method for preparing a natural fiber composite material according to claim 1, characterized in that: In the step (1), the thermoplastic resin is one of polylactic acid (PLA), polybutylene adipate / terephthalate (PBAT), poly-β-hydroxybutyric acid (PHB), glycolic acid-hydroxyvaleric acid copolyester (PBHV), polycaprolactone (PCL), polypropylene (PP), polyethylene (PE), polyamide (PA), polybutylene succinate (PBS), starch and copolyesteramide (PEA).
4. A natural fiber composite material, wherein the natural fiber composite material is prepared by the preparation method according to any one of claims 1 to 3.