A compound containing phenanthrene and triazine structure and its application
By using compounds containing phenanthrene and triazine structures in OLED devices, the problems of device voltage, current efficiency and lifespan are solved, and the effects of low voltage, high efficiency and long lifespan are achieved, especially under high temperature and high current density conditions. Significantly improved device performance.
Patent Information
- Application Number
- CN202110143043.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-02
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-02-02
AI Technical Summary
Existing triplet light-emitting OLED devices have needs for improvement in terms of device voltage, current efficiency and lifespan. In particular, the efficiency roll-off is serious at high current densities, and the turn-on voltage and high-temperature lifespan are insufficient.
Provides a compound containing phenanthrene and triazine structures for use as a light-emitting layer or electron transport layer material. By introducing carbazole and dibenzofuran groups, the asymmetry of the molecule is increased, the crystallinity of the molecule is reduced, and the branched chain Deuterium atoms are introduced into the molecule to improve the three-dimensionality and high-temperature stability of the molecule, and enhance the electron mobility and energy transfer efficiency.
It improves the photoelectric performance and life of the OLED device, reduces the driving voltage and turn-on voltage, significantly improves high temperature stability and chemical stability, reduces the efficiency roll-off at high current density, and extends the device life.
Smart Images

Figure CN114835686B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a compound containing phenanthrene and triazine structures and application thereof. Background Art
[0002] There may be a hole transport region between the anode and the light-emitting layer of the organic electroluminescent device, and there may be an electron transport region between the light-emitting layer and the cathode. Holes from the anode may migrate to the light-emitting layer through the hole transport region, and electrons from the cathode may migrate to the light-emitting layer through the electron transport region, and the holes and electrons recombine in the light-emitting layer to generate excitons. According to the principles of quantum mechanics, organometallic compound materials as doping materials can achieve an internal quantum yield of 100%.
[0003] Nevertheless, for triplet-luminescent phosphorescent OLEDs, there is still a need for improvement in device voltage, current efficiency and life. The performance of the host material in the light-emitting layer usually affects the above-mentioned key properties of the organic electroluminescent device to a large extent. According to the prior art, the compounds used as host materials usually contain triazine groups. When the existing triazine derivatives are used as host materials, there is a need for improvement in device voltage, current efficiency, especially in turn-on voltage and device life. The present invention provides a host replacement material with low voltage, high efficiency, long life, especially low turn-on voltage and long high-temperature life.
[0004] For phosphorescent OLED, there is usually an imbalance between holes and electrons in the light-emitting layer, and the device efficiency roll-off is serious under high current density. The present invention also provides a combination of two host materials, which can effectively solve the above-mentioned drawbacks. Summary of the invention
[0005] In view of the above problems existing in the prior art, a compound containing a phenanthrene and a triazine structure is provided. The provided compound can effectively improve the photoelectric performance of an OLED device and the life of the OLED device.
[0006] The technical solution of the present invention is as follows:
[0007] A compound containing phenanthrene and triazine structures, wherein the compound structure is shown in general formula (1):
[0008]
[0009] R represents the structure shown in general formula (2), and general formula (2) is connected to general formula (1) through any site indicated by the * mark;
[0010]
[0011] Ar1 and Ar2 are independently represented by the structure shown in general formula (3), general formula (4) or general formula (5); at least one of Ar1 and Ar2 is represented by the structure shown in general formula (4) or general formula (5);
[0012] Each occurrence of Z1, Z2, and Z3 is independently represented by C-R1, and each occurrence of R1 is independently represented by one of H, deuterium atom, phenyl, biphenyl, naphthyl, phenanthryl, dibenzofuranyl, and carbazole; Z1, Z2, and Z3 at the connection are represented by C;
[0013]
[0014] In a preferred embodiment, the compound structure is represented by any one of the general formulas (II-1) to (II-3):
[0015]
[0016] In a preferred embodiment, the compound structure is represented by any one of the general formulas (III-1) to (III-4):
[0017]
[0018] In the general formulae (III-1) to (III-4), Z1, Z2, and Z3 are each independently represented by C-R1, and R1 represents H or a deuterium atom.
[0019] In a preferred embodiment, at least one of the R1 is represented by a deuterium atom.
[0020] In a preferred embodiment, the specific structure of the compound is any one of the following structures:
[0021]
[0022]
[0023]
[0024]
[0025]
[0026]
[0027]
[0028]
[0029]
[0030]
[0031] An organic electroluminescent device comprises a cathode, an anode and a functional layer, wherein the functional layer is located between the cathode and the anode and contains the compound containing phenanthrene and triazine structures.
[0032] In a preferred embodiment, the functional layer includes a light-emitting layer, wherein the light-emitting layer contains a light-emitting host material, wherein the light-emitting host material is a mixture of any one or more of the compound containing phenanthrene and triazine structures and compounds GH-1 to GH-170, and the specific structures of the compounds GH-1 to GH-170 are:
[0033]
[0034]
[0035]
[0036]
[0037]
[0038]
[0039]
[0040] In a preferred embodiment, the functional layer includes an electron transport layer, and the electron transport layer contains the compound containing phenanthrene and triazine structures.
[0041] A lighting or display element, comprising the organic electroluminescent device.
[0042] Compared with the prior art, the beneficial technical effects of the present invention are:
[0043] 1) The compound provided by the present invention has suitable HOMO and LUMO energy levels, which can ensure efficient injection and recombination of carriers in the light-emitting layer, and the device has high efficiency.
[0044] 2) The compound provided by the present invention has a relatively high T1 energy level, which can ensure the energy transfer efficiency between the host and the guest.
[0045] 3) When compounds with high symmetry are used to produce OLED displays, they are prone to crystallization and block the crucible mouth used for evaporation. The introduction of carbazole and dibenzofuran groups in the compounds provided by the present invention increases the asymmetry of the molecules, the material has a high Tg, and the crystallinity of the molecules is low, which helps to improve the high temperature stability of the device.
[0046] 4) The introduction of specific phenanthrene substituent groups into the compounds provided by the present invention helps to improve the stereoscopic nature of the molecular structure and reduce the intermolecular interaction force, so that the molecules are not easy to crystallize, the evaporation temperature is low, the film-forming property is good, and it has excellent industrial processing performance.
[0047] 5) Cross-talk risk (because the blue and green light pixels have higher turn-on voltage than red light, there is a risk of turning on adjacent red light pixels while turning on blue and green light pixels) has always troubled OLED display manufacturers. The combined connection mode between the triazine fragment and the side chain in the compound provided by the present invention can further increase the electron mobility, and the application in the main material of the light-emitting layer or the electron transport layer material can help significantly reduce the driving voltage and turn-on voltage of the device.
[0048] 6) Device life, especially high-temperature device life, has always restricted the promotion of OLED displays in various application fields. Compared with the compounds in the prior art, the compounds provided by the present invention have high chemical stability, low efficiency roll-off at high current density, and long device life and high-temperature device life.
[0049] 7) The compound provided by the present invention further introduces deuterium atoms in the side chain, and its application in the light-emitting layer helps to improve the efficiency roll-off problem of the device at high current density and increase the device life. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 This is a schematic diagram of the structure of an OLED device in which the materials listed in the present invention are applied;
[0051] Among them, 1 is a transparent substrate layer, 2 is an anode layer, 3 is a hole injection layer, 4 is a hole transport layer, 5 is an electron blocking layer, 6 is a light-emitting layer, 7 is an electron transport layer, 8 is an electron injection layer, 9 is a cathode layer, and 10 is a CPL layer. DETAILED DESCRIPTION
[0052] The raw materials involved in the synthesis examples of the present invention can all be purchased from the market.
[0053] Example 1: Synthesis of Compound 2:
[0054]
[0055] 0.01 mol of intermediate B-1 and 0.012 mol of intermediate A-1 were added to 150 mL of a mixed solvent of toluene:ethanol = 2:1 (volume ratio), 10 mL of a 2 mol / L sodium carbonate aqueous solution was added, and 5×10 - 5mol Pd(PPh3)4, heated to 110℃ for 8 hours, sampled, cooled naturally, filtered, and the filtrate was distilled under reduced pressure to remove the solvent, and the crude product was passed through a silica gel column to obtain compound 2; elemental analysis molecular formula (C 47 H 30 N4), theoretical value: C, 86.74; H, 4.65; N, 8.61; found value: C, 86.78; H, 4.63; N, 8.60. LC-MS: theoretical value: 650.25; found value ([M+H] + ):651.34.
[0056] The preparation process in Example 1 was repeated to synthesize the following target compounds; the reaction conditions were the same, except that the intermediate B and intermediate A listed in Table 1 below were used; detailed characterization data are shown in Table 1.
[0057] Table 1
[0058]
[0059]
[0060]
[0061]
[0062] The synthetic route of intermediate A-1 is as follows:
[0063]
[0064] 1) Add 0.01 mol of raw material D1, 0.012 mol of raw material C1, and 100 ml of toluene, stir and mix, add 0.02 mol of sodium tert-butoxide, 5×10 -5 mol Pd2(dba)3,5×10 -5 mol tri-tert-butylphosphine, stirred and heated to 115°C, refluxed for 8 hours, sampled and plated, showing no intermediate C1 remaining, the reaction was complete; cooled naturally to room temperature, filtered, the filtrate was vacuum evaporated until no fraction was left, passed through a neutral silica gel column, and intermediate A-1 was obtained; LC-MS: theoretical value: 356.08; measured value: 357.17 ([M+H] + ).
[0065] The preparation process of intermediate A-1 was repeated to synthesize the following intermediate A; the reaction conditions were similar, except that the intermediates listed in Table 2 below were used; detailed characterization data are shown in Table 2.
[0066] Table 2
[0067]
[0068] The synthetic route of intermediate A-2 is as follows:
[0069]
[0070] 1) 0.01 mol of raw material D2 and 0.012 mol of raw material C1 were added to 120 mL of a mixed solvent of toluene:ethanol = 2:1 (volume ratio), 10 mL of a 2 mol / L sodium carbonate aqueous solution was added, and 5×10 -5 molPd(PPh3)4, heated to 110℃ for 6 hours, sampled, cooled naturally, filtered, and the filtrate was distilled under reduced pressure to remove the solvent. The crude product was passed through a silica gel column to obtain intermediate A-2; LC-MS: theoretical value: 357.07; measured value: 358.27 ([M+H] + ).
[0071] Referring to the synthesis method of the above intermediates, intermediates A-3, A-4, A-6, A-7, A-8, A-9 and A-11 were prepared; the reaction conditions were similar, except that the raw materials listed in Table 3 below were used; the characterization data are shown in Table 3.
[0072] Table 3
[0073]
[0074]
[0075] The synthetic route of intermediate B-1 is as follows
[0076]
[0077] 1) 0.01 mol of raw material F1 and 0.012 mol of raw material E1 were added to 120 mL of a mixed solvent of toluene:ethanol = 2:1 (volume ratio), 10 mL of a 2 mol / L sodium carbonate aqueous solution was added, and 5×10 -5 molPd(PPh3)4, heated to 110℃ for 6 hours, sampled, cooled naturally, filtered, and the filtrate was distilled under reduced pressure to remove the solvent. The crude product was passed through a silica gel column to obtain intermediate I1; LC-MS: theoretical value: 364.10; measured value: 365.22 ([M+H] + ).
[0078] 2) 0.01 mol of intermediate I1, 0.02 mol of biboric acid pinacol ester, 0.03 mol of potassium acetate, 5×10 - 51 mol Pd(dppf)Cl2 and 100 mL 1,4-dioxane were stirred and mixed, heated to 80°C, reacted for 6 hours, and the sampling point plate showed that no intermediate I1 remained, indicating that the reaction was complete; it was naturally cooled to room temperature, and solid precipitated after adding water. It was filtered, and the filter cake was dried in a vacuum drying oven, and then passed through a neutral silica gel column to obtain the borate ester compound intermediate B-1; LC-MS: theoretical value: 456.23; measured value: 457.37 ([M+H] + ).
[0079] Referring to the synthesis method of intermediate B-1, intermediate B-2, B-3, B-4 or B-5 were prepared; the reaction conditions were similar, except that the raw materials listed in Table 4 below were used; detailed characterization data are shown in Table 4.
[0080] Table 4
[0081]
[0082]
[0083] The compounds of the present invention are used in light-emitting devices and can be used as light-emitting layer or electron transport layer materials. The compounds prepared in the above embodiments of the present invention were tested for their physicochemical and photoelectric properties, and the test results are shown in Table 5:
[0084] Table 5
[0085]
[0086] Note: The triplet energy level T1 is tested by Horiba's Fluorolog-3 series fluorescence spectrometer, and the material test sample is 2*10 -5 mol / L toluene solution; the glass transition temperature Tg is measured by differential scanning calorimetry (DSC, DSC204F1 differential scanning calorimeter of NETZSCH, Germany), with a heating rate of 10°C / min; the highest occupied molecular orbital HOMO energy level is tested by an ionization energy test system (IPS-3), and the test is an atmospheric environment; Eg is tested by a double-beam UV-visible spectrophotometer (model: TU-1901), LUMO=HOMO+Eg. The electron mobility test is to make the material of the present invention into a single-charge device and measure it by the SCLC method.
[0087] From the data in the above table, it can be seen that the organic compound of the present invention has a high glass transition temperature (Tg), which can improve the phase stability and high temperature stability of the material film; the organic compound of the present invention has suitable HOMO and LUMO energy levels, which can reduce the injection barrier of carriers, reduce the device voltage and improve the device efficiency. The organic compound of the present invention has a high T1 energy level, and its use as a main material can ensure the energy transfer efficiency between the host and the guest and inhibit energy loss. (Corresponding to the conventional technical effect)
[0088] Surprisingly, the organic compounds of the present invention have high electron mobility, which helps to improve the device voltage, especially the turn-on voltage and current efficiency.
[0089] The following describes in detail the application effect of the OLED material synthesized by the present invention in the device through device examples 1-36 and device comparative examples 1-5. The device manufacturing process of the device embodiments 1-36 and device comparative examples 1-5 of the present invention is exactly the same as that of device embodiment 18, and the same substrate material and electrode material are used, and the film thickness of the electrode material is also the same. The difference is that the light-emitting layer or the electron transport layer in the device is replaced.
[0090] Device Example 18
[0091] like Figure 1As shown, the transparent substrate layer 1 is a transparent PI film, and the anode layer 2 (ITO (15nm) / Ag (150nm) / ITO (15nm)) is washed, that is, washed with a detergent (SemiClean M-L20), washed with pure water, dried, and then washed with ultraviolet-ozone to remove organic residues on the surface of the anode layer. On the anode layer 2 after the above washing, HT-1 and P-1 are evaporated on the anode layer 2 using a vacuum evaporation device as a hole injection layer 3, with a film thickness of 10nm, and a mass ratio of HT-1 to P-1 of 97:3. Then HT-1 is evaporated as a hole transport layer 4 with a thickness of 130nm. Subsequently, EB-1 is evaporated as an electron blocking layer 5 with a thickness of 40nm. After the above-mentioned electron blocking layer material is evaporated, the light-emitting layer 6 of the OLED light-emitting device is prepared, and its structure includes the compound 2 and GH-1 used in the OLED light-emitting layer 6 as the main materials, GD-1 as the guest material, the mass ratio of compound 2, GH-1, and GD-1 is 47:47:6, and the thickness of the light-emitting layer is 40nm. After the above-mentioned light-emitting layer 6, ET-1 and Liq are vacuum evaporated, the mass ratio of ET-1 and Liq is 1:1, the film thickness is 35nm, and this layer is the electron transport layer 7. On the electron transport layer 7, a LiF layer with a film thickness of 1nm is prepared by a vacuum evaporation device, and this layer is the electron injection layer 8. On the electron injection layer 8, a Mg:Ag electrode layer with a film thickness of 15nm is prepared by a vacuum evaporation device, and the mass ratio of Mg and Ag is 1:9, and this layer is the cathode layer 9. On the cathode layer 9, CP-1 is vacuum evaporated as the CPL layer 10, with a thickness of 70nm. An organic electroluminescent device 1 is obtained.
[0092] The molecular structure formula of the relevant materials is shown below:
[0093]
[0094] After the OLED light-emitting device is completed as described above, the anode and cathode are connected with a known driving circuit, and the voltage, current efficiency, luminescence spectrum and device life of the device are measured. The device examples and comparative examples prepared by the same method are shown in Table 6; the voltage, current efficiency and 20 mA / cm 2 The test results of LT95 life under the conditions are shown in Table 7.
[0095] Table 6
[0096]
[0097]
[0098]
[0099]
[0100] Table 7
[0101]
[0102]
[0103] Note: Voltage, current efficiency and color coordinates are obtained at a current density of 10 mA / cm 2 The test was conducted under the following conditions: IVL (current-voltage-luminance) test system (Suzhou Fushida Scientific Instrument Co., Ltd.); the life test system was EAS-62C OLED device life tester from Japan System Technology Co., Ltd.; the device life LT95 refers to the device life under the condition of current density of 20mA / cm 2 The device brightness decays to 95% of the initial brightness when the current density is 20mA / cm 2 When the temperature is 85°C, the time taken for the device brightness to decay to 95% of the initial brightness; the start-up voltage refers to the driving voltage of the device when the device brightness is 1 nit.
[0104] It can be seen from the device data results in Table 7 that, compared with the device comparison example, the organic light-emitting device of the present invention is improved in terms of device voltage, device efficiency and device life relative to OLED devices of known materials, especially the device's turn-on voltage and high-temperature life are significantly improved.
[0105] In order to compare the efficiency attenuation of different devices at high current density, the efficiency attenuation coefficient of each device is defined where μ m Expressed as the maximum current efficiency of the device, μ 50 Indicates that the driving current is 50mA / cm 2 The current efficiency of the device. The larger the value, the more serious the efficiency roll-off of the device. Conversely, it means that the problem of rapid attenuation of the device at high current density has been controlled. The present invention measures the efficiency attenuation coefficient of the device obtained in device embodiments 1, 4, 5, 7, 10, 12, 13, 15, 16, 17, 18, 19, 21, 24, 26, 27, 35 and device comparison examples 1-5. The results are shown in Table 8:
[0106] Table 8
[0107] It can be seen from the data in Table 8 that the organic light-emitting device prepared using the compound of the present invention has a smaller efficiency attenuation coefficient than that of the comparative example, indicating that the organic electroluminescent device prepared using the compound of the present invention can effectively reduce the efficiency roll-off of the device at high current density.
[0108] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A compound containing phenanthrene and triazine structure, It is characterized in that The compound structure is shown in general formula (1): R represents the structure shown in general formula (2), and general formula (2) is connected to general formula (1) through any site indicated by the * mark; Ar 1 ,Ar 2 are independently represented by the structure shown in general formula (3), general formula (4) or general formula (5); Ar 1 ,Ar 2 At least one of the structures is represented by the general formula (4) or the general formula (5); Z 1 , Z 2 , Z 3 Each occurrence is represented independently as CR 1 , R 1 Each occurrence is independently represented by one of H, deuterium atom, and phenyl; Z at the connection 1 , Z 2 , Z 3 It is represented by C; 2. The compound according to claim 1, It is characterized in that The structure of the compound is represented by any one of the general formulas (II-1) to (II-3):
3. The compound according to claim 1, It is characterized in that The compound structure is represented by any one of the general formulas (III-1) to (III-4): In the general formulae (III-1) to (III-4), Z 1 , Z 2 , Z 3 Each is independently represented as CR 1 , R 1 Represented by H or deuterium atoms.
4. The compound according to claim 1, It is characterized in that The R 1 At least one is represented as a deuterium atom.
5. The compound according to claim 1, It is characterized in that The specific structure of the compound is any one of the following structures:
6. An organic electroluminescent device comprising a cathode, an anode and a functional layer, wherein the functional layer is located between the cathode and the anode, It is characterized in that The functional layer contains the compound containing a phenanthrene and a triazine structure according to any one of claims 1 to 5.
7. The organic electroluminescent device according to claim 6, wherein the functional layer comprises a light-emitting layer. It is characterized in that The light-emitting layer contains a light-emitting host material, which is a mixture of the compound containing phenanthrene and triazine structure according to any one of claims 1 to 5 and any one or more of compounds GH-1 to GH-170. The specific structures of the compounds GH-1 to GH-170 are:
8. The organic electroluminescent device according to claim 6, wherein the functional layer comprises an electron transport layer. It is characterized in that The electron transport layer contains the compound containing phenanthrene and triazine structures according to any one of claims 1 to 5.
9. A lighting or display element, It is characterized in that The lighting or display element comprises the organic electroluminescent device according to any one of claims 6 to 8.
Citation Information
Patent Citations
Pyrimidine derivative and organic electroluminescent element
CN106573911A
Organic electroluminescent element
CN107112427A
Heterocyclic compound and organic light emitting element comprising same
CN107445945A
Novel heterocyclic compound and organic light-emitting device using same
CN108368078A
Organic light-emitting diode
CN111164777A