A red light flip-chip Micro-LED chip and a manufacturing method thereof

By growing an AlGaInP-based epitaxial structure on a GaAs substrate layer and etching to form an n-GaAs point contact array, the problem of large electrode spacing and low light extraction efficiency of red Micro-LED chips is solved, and efficient light extraction and good electrical properties are achieved. performance.

CN114843386BActive Publication Date: 2024-10-15SHENZHEN HONGKAIHONG INFORMATION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210362012.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-07
Publication Date
2024-10-15
Estimated Expiration
2042-04-07

AI Technical Summary

Technical Problem

The traditional red AlGaInP-based thin film Micro-LED chip has a large distance between the P electrode and the N electrode, making it difficult to form a flip-chip structure. The GaAs ohmic contact layer has low absorption efficiency of red light photons, resulting in low light extraction efficiency.

Method used

An AlGaInP-based epitaxial structure is grown on an accurately lattice-matched GaAs substrate layer, and an n-GaAs point contact array is formed by selectively etching the heavily doped n-GaAs ohmic contact layer, and a through-hole double-layer electrode structure is designed. Reduce the absorption of red light photons by the GaAs layer.

Benefits of technology

Significantly improve the light extraction efficiency of the AlGaInP-based red flip-chip Micro-LED chip, improve the current expansion performance of the chip, reduce the process difficulty, and ensure good electrical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114843386B_ABST
    Figure CN114843386B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of Micro-LED chip technology, and discloses a red flip-chip Micro-LED chip and a manufacturing method thereof. The present invention selectively etches the heavily doped n-GaAs ohmic contact layer to form an n-GaAs point contact array corresponding to the N-type through hole, which can effectively reduce the absorption of red light photons by the GaAs layer and significantly improve the light extraction efficiency of the AlGaInP-based red flip-chip Micro-LED chip. The present invention adopts a through-hole double-layer electrode to solve the problem that the p-electrode and n-electrode of the traditional AlGaInP-based red Micro-LED chip are too far apart to form a flip-chip structure, and can improve the current expansion performance of the chip and reduce the process difficulty.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of Micro-LED chips, and more specifically, relates to a red light flip-chip Micro-LED chip and a manufacturing method thereof. Background Art

[0002] Full-color displays based on AlGaInP-based red thin-film micro-light-emitting diodes (Micro-LEDs) and InGaN-based blue / green thin-film Micro-LEDs have the advantages of high resolution, high brightness, long life, wide color gamut, wide operating temperature range, strong anti-interference ability, fast response speed and low power consumption, and have been highly valued by scientific researchers in the industry and academia at home and abroad. In Micro-LED full-color displays, red, green and blue Micro-LED chips usually adopt a flip-chip structure. The P-electrode and N-electrode spacing of traditional red light AlGaInP-based thin-film Micro-LED chips is large, making it difficult to form a flip-chip structure. Moreover, in the red light AlGaInP-based thin-film Micro-LED chip, the photons emitted from the active area will be emitted from the GaAs ohmic contact layer, but the GaAs ohmic contact layer has a strong absorption effect on red light photons, resulting in low light extraction efficiency of the red light AlGaInP-based thin-film flip-chip Micro-LED chip. Therefore, how to design a reasonable red light AlGaInP-based flip-chip Micro-LED chip structure and reduce the absorption of red light by the GaAs ohmic contact layer is the current technical difficulty. Summary of the invention

[0003] The present invention provides a red light flip-chip Micro-LED chip and a manufacturing method thereof, thereby solving the problems in the prior art that a P-electrode and an N-electrode of a red light AlGaInP-based thin film Micro-LED chip have a large spacing, making it difficult to form a flip-chip structure, and the light extraction efficiency of the red light AlGaInP-based thin film flip-chip Micro-LED chip is low.

[0004] The present invention provides a method for manufacturing a red light flip-chip Micro-LED chip, comprising the following steps:

[0005] Step 1, growing an AlGaInP-based epitaxial structure on a GaAs substrate layer with accurate lattice matching, wherein the AlGaInP-based epitaxial structure comprises, from bottom to top, an n-InGaP etching stop layer, a heavily doped n-GaAs ohmic contact layer, an n-AlGaInP layer, a GaInP / AlGaInP multi-quantum well layer, a p-AlGaInP layer, a p-GaP layer, and a heavily doped p-GaP contact layer;

[0006] Step 2, etching the AlGaInP-based epitaxial structure to form an N-type through hole directly reaching the heavily doped n-GaAs ohmic contact layer;

[0007] Step 3, depositing a first layer of P electrode on the heavily doped p-GaP contact layer;

[0008] Step 4, depositing an insulating layer on the surface of the first layer of P electrodes, the sidewalls of the AlGaInP-based epitaxial structure, and the sidewalls of the N-type through holes;

[0009] Step 5, depositing a first layer of N-electrodes in the N-type through holes;

[0010] Step 6, depositing a passivation layer, and etching the passivation layer to form an N-electrode interconnection hole and a P-electrode contact hole;

[0011] Step 7, evaporating a second layer of electrodes; separating the second layer of electrodes into a second layer of N electrodes and a second layer of P electrodes, and the first layer of N electrodes and the second layer of N electrodes are interconnected through the N electrode interconnection holes;

[0012] Step 8, etching the GaAs substrate layer and the n-InGaP etching stop layer;

[0013] Step 9: selectively etching the heavily doped n-GaAs ohmic contact layer to form an n-GaAs point contact array; the number, shape and size of the n-GaAs point contacts included in the n-GaAs point contact array are the same as those of the N-type through holes.

[0014] Preferably, the first layer of P electrode in step 3 is a AuZn / Ag / TiW / Pt / Ti / Pt / Ti / Pt / Ti metal stack layer; the total thickness of the AuZn / Ag / TiW / Pt / Ti / Pt / Ti / Pt / Ti metal stack layer is 3.6 to 4 μm.

[0015] Preferably, the doping concentration of the heavily doped n-GaAs ohmic contact layer is 1×10 19 ~1×10 20 cm -3 .

[0016] Preferably, the insulating layer in step 4 is composed of 12 pairs of TiO2 / SiO2, the thickness of each TiO2 layer is 100-150 nm, and the thickness of each SiO2 layer is 50-100 nm.

[0017] Preferably, the first N electrode layer in step 5 is a AuGe / Ni / Au metal layer; the material of the passivation layer in step 6 is SiO2 or SiN x ; The second electrode layer in step 7 is a Cr / Pt / Au metal layer.

[0018] Preferably, in step 9, the number of n-GaAs point contacts included in the n-GaAs point contact array is 4 to 9.

[0019] Preferably, in step 9, the shape of a single n-GaAs point contact in the n-GaAs point contact array is circular, with a radius of 1 to 6 μm.

[0020] Preferably, the radius of a single n-GaAs point contact is 1 μm, and the light extraction efficiency of the resulting red flip-chip Micro-LED chip is 55%.

[0021] Preferably, the thickness of the n-InGaP etching stop layer is 60 to 100 nm, the thickness of the heavily doped n-GaAs ohmic contact layer is 300 to 400 nm, the thickness of the n-AlGaInP layer is 1 to 1.5 μm, the thickness of the GaInP / AlGaInP multiple quantum well layer is 0.5 to 0.7 μm, the thickness of the p-AlGaInP layer is 0.7 to 0.9 μm, the thickness of the p-GaP layer is 4.5 to 5 μm, and the thickness of the heavily doped p-GaP contact layer is 5 to 10 nm.

[0022] On the other hand, the present invention provides a red light flip-chip Micro-LED chip, which is obtained by using the above-mentioned red light flip-chip Micro-LED chip manufacturing method.

[0023] One or more technical solutions provided in the present invention have at least the following technical effects or advantages:

[0024] In the present invention, the heavily doped n-GaAs ohmic contact layer is selectively etched to form an n-GaAs point contact array corresponding to the N-type through hole, which can effectively reduce the absorption of red light photons by the GaAs layer and significantly improve the light extraction efficiency of the AlGaInP-based red light flip-chip Micro-LED chip. The existing red light flip-chip usually adopts a design of depositing an ITO transparent conductive electrode on the surface of the heavily doped p-GaP contact layer and depositing a metal stack on the other side of the ITO transparent conductive electrode to form a P electrode, which will result in a very thick P electrode, a high process difficulty, and poor current expansion performance of the chip. In response to the above problems, the present invention adopts a through-hole double-layer electrode to solve the problem that the p-electrode and n-electrode of the traditional AlGaInP-based red light Micro-LED chip are too far apart to form a flip-chip structure, and can improve the current expansion performance of the chip and reduce the process difficulty. In addition, the present invention heavily dopes the n-GaAs ohmic contact layer to ensure that the AlGaInP-based red light flip-chip Micro-LED chip still has good electrical properties after etching the n-GaAs ohmic contact layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A schematic diagram of the result of growing an AlGaInP-based epitaxial layer structure on a GaAs substrate layer provided by an embodiment of the present invention;

[0026] Figure 2 A schematic diagram of the result of etching an AlGaInP-based epitaxial structure to form an N-type through hole provided by an embodiment of the present invention;

[0027] Figure 3 A schematic diagram of the result of depositing a first layer of P electrode on a heavily doped p-GaP contact layer provided in an embodiment of the present invention;

[0028] Figure 4 A schematic diagram of the result of depositing an insulating layer on the surface of the first layer P electrode, the side wall of the AlGaInP-based epitaxial structure and the side wall of the N-type through hole provided by an embodiment of the present invention;

[0029] Figure 5 A schematic diagram of the result of depositing a first layer of N-electrodes in an N-type through hole provided by an embodiment of the present invention;

[0030] Figure 6 A schematic diagram of the result of depositing a passivation layer and etching to form an N-electrode interconnection hole and a P-electrode contact hole provided in an embodiment of the present invention;

[0031] Figure 7 A schematic diagram of the result of evaporating a second layer of electrode and separating it into a second layer of N electrode and a second layer of P electrode provided by an embodiment of the present invention;

[0032] Figure 8 A schematic diagram of the results of etching a GaAs substrate layer and an n-InGaP etching stop layer provided in an embodiment of the present invention;

[0033] Fig. 9 A schematic diagram of the result of selectively etching a heavily doped n-GaAs ohmic contact layer provided by an embodiment of the present invention;

[0034] Fig.10 is a schematic diagram of an n-GaAs point contact array formed in the present invention;

[0035] Fig.11 The light distribution curves of the Micro-LED chip corresponding to etching the heavily doped n-GaAs ohmic contact layer into a point contact array and not etching the heavily doped n-GaAs ohmic contact layer into a point contact array;

[0036] Fig.12 This is a diagram of the light extraction efficiency of the Micro-LED chip corresponding to n-GaAs point contact arrays of different sizes in the present invention.

[0037] Among them, 1-GaAs substrate layer, 2-n-InGaP etching stop layer, 3-heavily doped n-GaAs ohmic contact layer, 4-n-AlGaInP layer, 5-GaInP / AlGaInP multiple quantum well layer, 6-p-AlGaInP layer, 7-p-GaP layer, 8-heavily doped p-GaP contact layer, 9-first layer P electrode, 10-insulating layer, 11-first layer N electrode, 12-passivation layer, 13-second layer N electrode, 14-second layer P electrode. DETAILED DESCRIPTION

[0038] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0039] Embodiment 1:

[0040] Embodiment 1 provides a method for manufacturing a red flip-chip Micro-LED chip, which specifically includes the following steps:

[0041] Step 1: Figure 1 As shown, an AlGaInP-based epitaxial structure is grown on a GaAs substrate layer 1 with accurate lattice matching by a MOCVD method, and the AlGaInP-based epitaxial structure includes, from bottom to top: an n-InGaP etching stop layer 2, a heavily doped n-GaAs ohmic contact layer 3, an n-AlGaInP layer 4, a GaInP / AlGaInP multiple quantum well layer 5, a p-AlGaInP layer 6, a p-GaP layer 7 and a heavily doped p-GaP contact layer 8.

[0042] The area of ​​the GaAs substrate layer 1 is 2 inches, the thickness of the n-InGaP etching stop layer 2 is 60-100 nm, the thickness of the heavily doped n-GaAs ohmic contact layer 3 is 300-400 nm, the thickness of the n-AlGaInP layer 4 is 1-1.5 μm, the thickness of the GaInP / AlGaInP multi-quantum well layer 5 is 0.5-0.7 μm, the thickness of the p-AlGaInP layer 6 is 0.7-0.9 μm, the thickness of the p-GaP layer 7 is 4.5-5 μm, and the thickness of the heavily doped p-GaP contact layer 8 is 5-10 nm; the doping concentration of the heavily doped n-GaAs ohmic contact layer 3 is 1×10 19 ~1×10 20 cm -3 .

[0043] Step 2: Figure 2 As shown, the AlGaInP-based epitaxial structure is etched using a BCl 3 / Cl 2 mixed gas to form an N-type through hole directly reaching the heavily doped n-GaAs ohmic contact layer 3 .

[0044] Step 3: Figure 3 As shown, on the heavily doped p-GaP contact layer 8 is deposited

[0045] The AuZn / Ag / TiW / Pt / Ti / Pt / Ti / Pt / Ti metal stack layer forms a first layer of P electrode 9, wherein the AuZn alloy forms an ohmic contact with the heavily doped p-GaP contact layer 8, and the total thickness of the AuZn / Ag / TiW / Pt / Ti / Pt / Ti / Pt / Ti metal stack layer is 3.6-4μm. That is, the AuZn / Ag / TiW / Pt / Ti / Pt / Ti / Pt / Ti metal stack layer is used as a high-reflectivity, low-resistance p-type ohmic contact.

[0046] Step 4: Figure 4 As shown, an insulating layer 10 is deposited on the surface of the AuZn / Ag / TiW / Pt / Ti / Pt / Ti / Pt / Ti metal stack layer, the sidewall of the AlGaInP-based epitaxial structure and the sidewall of the N-type through hole, and the insulating layer 10 is composed of 12 pairs of TiO2 / SiO2, and the thickness of each TiO2 layer is 100 to 150 nm, and the thickness of each SiO2 layer is 50 to 100 nm.

[0047] Step 5: Figure 5 As shown, an AuGe / Ni / Au metal layer is deposited in the N-type through hole to form a first layer of N-electrode 11 .

[0048] Step 6: Figure 6 As shown, the passivation layer 12 is deposited by PECVD, and the passivation layer 12 is wet-etched by BOE to form N-electrode interconnection holes and P-electrode contact holes; wherein the material of the passivation layer 12 can be SiO2 or SiNx.

[0049] Step 7: Figure 7 As shown, a Cr / Pt / Au metal layer is deposited by electron beam to form a second layer electrode, and the second layer electrode is separated into a second layer N electrode 13 and a second layer P electrode 14 by wet etching. The first layer N electrode 11 and the second layer N electrode 13 are interconnected through the N electrode interconnection hole.

[0050] Step 8, see Figure 1 , Figure 8 The GaAs substrate layer 1 is etched by using a mixed solution of NH4OH and H2O2, and the n-InGaP etching stop layer 2 is etched by using a mixed solution of H3PO4 / HCl.

[0051] Step 9: Fig. 9As shown, the heavily doped n-GaAs ohmic contact layer 3 is selectively etched using a mixed solution of NH4OH and H2O2 to form an n-GaAs point contact array; the number, shape, and size of the n-GaAs point contacts contained in the n-GaAs point contact array are the same as those of the N-type through holes.

[0052] Embodiment 2:

[0053] Embodiment 2 provides a red flip-chip Micro-LED chip, which is obtained by the manufacturing method provided in Embodiment 1. The structure of the chip corresponds to that of Embodiment 1, and please refer to the description of Embodiment 1 for details.

[0054] The red light flip-chip Micro-LED chip structure finally obtained in Example 2 includes, from top to bottom, a heavily doped n-GaAs ohmic contact layer, an n-AlGaInP layer, a GaInP / AlGaInP multiple quantum well layer, a p-AlGaInP layer, a p-GaP layer, a heavily doped p-GaP contact layer, a first layer of P electrode, an insulating layer, a first layer of N electrode, a passivation layer, a second layer of N electrode and a second layer of P electrode.

[0055] The heavily doped n-GaAs ohmic contact layer is selectively etched to form an n-GaAs point contact array; the number, shape, and size of the n-GaAs point contacts contained in the n-GaAs point contact array are the same as those of the N-type through holes. The AuZn / Ag / TiW / Pt / Ti / Pt / Ti / Pt / Ti metal stack is used as a high-reflectivity, low-resistance p-type ohmic contact. The red flip-chip Micro-LED chip provided in Example 2 adopts a through-hole double-layer electrode structure.

[0056] like Fig.10 As shown, the size of a single n-GaAs point contact in the n-GaAs point contact array in Example 1 or Example 2 is R, the spacing between two adjacent n-GaAs point contacts is L, and the number of the n-GaAs point contacts is the same as the number of the N-type through holes. If there are too many N-type through holes in the active area, the area of ​​the active area will be reduced, the radiation recombination rate of the active area will be reduced, and the luminous efficiency of the red flip-chip Micro-LED chip will be reduced. Considering all factors, the number of N-type through holes is preferably 4 to 9.

[0057] The effect evaluation and performance testing of the present invention are as follows:

[0058] Fig.11The light distribution curves of the red flip-chip Micro-LED chip obtained by simulation using lightTools are: the heavily doped n-GaAs ohmic contact layer is etched into an n-GaAs point contact array (including the cases where the contact point radius is 1μm, 2μm, 3μm, 4μm, 5μm, and 6μm) and the heavily doped GaAs ohmic contact layer is not etched into an n-GaAs point contact array. Fig.11 It can be found that after the heavily doped n-GaAs ohmic contact layer is etched into an n-GaAs point contact array, the top luminescence intensity of the red flip-chip Micro-LED chip is significantly enhanced, which indicates that etching the heavily doped n-GaAs ohmic contact layer into an n-GaAs point contact array can effectively improve the top light extraction efficiency of the red Micro-LED chip.

[0059] Fig.12 This is a diagram of the light extraction efficiency of red flip-chip Micro-LED chips with n-GaAs point contact arrays of different sizes obtained using lightTools simulation. Fig.12 It can be found that as the radius of the n-GaAs contact point decreases, the light extraction efficiency of the red flip-chip Micro-LED chip increases, which indicates that reducing the size of the n-GaAs point contact array can effectively improve the light extraction efficiency of the red flip-chip Micro-LED chip. However, in order to ensure that the red flip-chip Micro-LED chip still has good electrical properties after etching the heavily doped n-GaAs ohmic contact layer, the size R of the designed n-GaAs point contact array cannot be less than 1μm. For example, the radius of a single n-GaAs point contact can be 1μm, and the light extraction efficiency of the obtained red flip-chip Micro-LED chip is 55%.

[0060] In summary, the present invention proposes a red flip-chip Micro-LED chip and a manufacturing method thereof, which not only solves the problem that the p-electrode and n-electrode of the traditional AlGaInP-based red Micro-LED chip have a large distance between them and is difficult to form a flip-chip structure, but also after etching the heavily doped n-GaAs ohmic contact layer into an n-GaAs point contact array, the absorption effect of the GaAs ohmic contact layer on red light photons is weakened, and the light extraction efficiency of the AlGaInP-based red flip-chip Micro-LED chip is significantly improved. In addition, the number, shape, and size of the designed n-GaAs point contact array are the same as those of the N-type through hole, which can ensure that the AlGaInP-based red flip-chip Micro-LED chip still has good electrical performance after etching the n-GaAs ohmic contact layer.

[0061] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for manufacturing a red flip-chip Micro-LED chip, characterized in that: The following steps are involved: Step 1, growing an AlGaInP-based epitaxial structure on a GaAs substrate layer with accurate lattice matching, wherein the AlGaInP-based epitaxial structure comprises, from bottom to top, an n-InGaP etching stop layer, a heavily doped n-GaAs ohmic contact layer, an n-AlGaInP layer, a GaInP / AlGaInP multi-quantum well layer, a p-AlGaInP layer, a p-GaP layer, and a heavily doped p-GaP contact layer; Step 2, etching the AlGaInP-based epitaxial structure to form an N-type through hole directly reaching the heavily doped n-GaAs ohmic contact layer; Step 3, depositing a first layer of P electrode on the heavily doped p-GaP contact layer; Step 4, depositing an insulating layer on the surface of the first layer of P electrodes, the sidewalls of the AlGaInP-based epitaxial structure, and the sidewalls of the N-type through holes; Step 5, depositing a first layer of N-electrodes in the N-type through holes; Step 6, depositing a passivation layer, and etching the passivation layer to form an N-electrode interconnection hole and a P-electrode contact hole; Step 7, evaporating a second layer of electrodes; separating the second layer of electrodes into a second layer of N electrodes and a second layer of P electrodes, and the first layer of N electrodes and the second layer of N electrodes are interconnected through the N electrode interconnection holes; Step 8, etching the GaAs substrate layer and the n-InGaP etching stop layer; Step 9: selectively etching the heavily doped n-GaAs ohmic contact layer to form an n-GaAs point contact array; the number, shape and size of the n-GaAs point contacts included in the n-GaAs point contact array are the same as those of the N-type through holes.

2. The method for manufacturing a red flip-chip Micro-LED chip according to claim 1, characterized in that: The first layer of P electrode in step 3 is a AuZn / Ag / TiW / Pt / Ti / Pt / Ti / Pt / Ti metal stack layer; the total thickness of the AuZn / Ag / TiW / Pt / Ti / Pt / Ti / Pt / Ti metal stack layer is 3.6 to 4 μm.

3. The method for manufacturing a red flip-chip Micro-LED chip according to claim 1, characterized in that: The doping concentration of the heavily doped n-GaAs ohmic contact layer is 1×10 19 ~1×10 20 cm -3 .

4. The method for manufacturing a red flip-chip Micro-LED chip according to claim 1, characterized in that: The insulating layer in step 4 is composed of 12 pairs of TiO2 / SiO2, the thickness of each TiO2 layer is 100-150nm, and the thickness of each SiO2 layer is 50-100nm.

5. The method for manufacturing a red flip-chip Micro-LED chip according to claim 1, characterized in that: The first N electrode layer in step 5 is a AuGe / Ni / Au metal layer; the material of the passivation layer in step 6 is SiO2 or SiN x ; The second electrode layer in step 7 is a Cr / Pt / Au metal layer.

6. The method for manufacturing a red flip-chip Micro-LED chip according to claim 1, characterized in that: In step 9, the number of n-GaAs point contacts included in the n-GaAs point contact array is 4 to 9.

7. The method for manufacturing a red flip-chip Micro-LED chip according to claim 1, characterized in that: In the step 9, the shape of a single n-GaAs point contact in the n-GaAs point contact array is circular, with a radius of 1 to 6 μm.

8. The method for manufacturing a red flip-chip Micro-LED chip according to claim 7, characterized in that: The radius of a single n-GaAs point contact is 1 μm, and the light extraction efficiency of the resulting red flip-chip Micro-LED chip is 55%.

9. The method for manufacturing a red flip-chip Micro-LED chip according to claim 1, characterized in that: The thickness of the n-InGaP etching stop layer is 60 to 100 nm, the thickness of the heavily doped n-GaAs ohmic contact layer is 300 to 400 nm, the thickness of the n-AlGaInP layer is 1 to 1.5 μm, the thickness of the GaInP / AlGaInP multiple quantum well layer is 0.5 to 0.7 μm, the thickness of the p-AlGaInP layer is 0.7 to 0.9 μm, the thickness of the p-GaP layer is 4.5 to 5 μm, and the thickness of the heavily doped p-GaP contact layer is 5 to 10 nm.

10. A red flip-chip Micro-LED chip, characterized in that: The method for manufacturing a red flip-chip Micro-LED chip is adopted as described in any one of claims 1 to 9.