Metal oxide particles coated with rare earth oxides and method for preparing the same by flame spray pyrolysis

The core/shell structure metal oxide particles prepared by flame spray pyrolysis technology solve the problem of instability of metal oxide particles in water in the existing technology, achieve the improvement of stability and optical properties in water, and are suitable for water-based formulations. products, and reduces the inconvenience caused by the increase in the amount of particles.

CN114845955BActive Publication Date: 2024-10-29LOREAL SA
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
CN202080089377.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-24
Publication Date
2024-10-29
Estimated Expiration
2040-12-24

AI Technical Summary

Technical Problem

Existing metal oxide particles are unstable in the presence of water, resulting in reduced photoprotective properties, and commonly used coating methods such as sol-gel process and fluorine compound grafting technology have problems with poor optical properties or environmental hazards.

Method used

M1-M2 oxide type metal oxide particles with core/shell structure are prepared through flame spray pyrolysis technology. The core is composed of the oxide of metal M1, and the surface covering is composed of element M2 (such as needle, yttrium, lanthanum, etc.) The inorganic compound coating covers more than 90% of the surface, improving the water resistance and optical properties of the particles.

Benefits of technology

It achieves improved stability and optical properties in water, maintains good UV absorption and visible light scattering properties, reduces UV radiation shielding capabilities, and avoids the use of hydrophobic coatings. It is suitable for water-based preparations and reduces the amount of particles. Increased inconvenience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114845955B_ABST
    Figure CN114845955B_ABST
Patent Text Reader

Abstract

The present invention relates to coated metal oxide particles, a process for preparing such coated particles by flame spray pyrolysis technology, metal oxide particles resulting from such a process, compositions comprising such particles and also uses thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to coated metal oxide particles, a process for preparing such coated particles by flame spray pyrolysis technology, metal oxide particles resulting from such a process, compositions comprising such particles and also uses thereof. Background Art

[0002] Metal oxides are used in many applications (cosmetics, paints, colorants, electronics, rubber, etc.) especially due to their optical properties. In particular, their light absorbing and / or light scattering properties are used to protect surfaces from UV radiation and / or to convert ambient light into electricity.

[0003] However, metal oxides have the disadvantage of being particularly unstable over time. For example, in the presence of water (either from the composition comprising it or from atmospheric moisture), zinc oxide can degrade to zinc hydroxide, or even ZnO. 2+ ions. This degradation results in partial or even complete dissolution of the zinc oxide in water and has the effect of greatly reducing or even removing the desirable properties of zinc oxide.

[0004] This instability is particularly problematic when the metal oxides are used in photoprotective cosmetic compositions. Indeed, as the metal oxide degrades, the protection against UV radiation decreases.

[0005] It has been envisaged to coat metal oxides with silicon dioxide, in particular using a sol-gel process, or to graft fluorine compounds onto metal oxides. However, these solutions are not entirely satisfactory. Metal oxides coated with silicon dioxide by a sol-gel process generally have worse optical properties than uncoated particles. As for the grafting technique, the use of fluorine compounds can be harmful to the environment and dangerous for the user.

[0006] It is also known to use the flame spray pyrolysis process (FSP process) to prepare metal oxide particles.

[0007] Flame spray pyrolysis or FSP is a now well-known process, which is essentially developed for the synthesis of ultrafine powders (with controlled morphology) of single or mixed oxides of various metals (for example SiO2, Al2O3, B2O3, ZrO2, GeO2, WO3, Nb2O5, SnO2, MgO, ZnO), and / or their deposition on various substrates, starting from a wide variety of metal precursors, which are generally in the form of organic or inorganic, preferably flammable, sprayable liquids; the liquid sprayed into the flame releases, by combustion, in particular nanoparticles of the metal oxides, which are sprayed by the flame itself onto these different substrates. For example, the principles of this approach are reviewed in a recent (2011) publication by Johnson Matthey entitled “Flame Spray Pyrolysis: a Unique Facility for the Production of Nanopowders,” Platinum Metals Rev., 2011, 55, (2), 149-151. Many variants of FSP processes and reactors are also described, for example, in the following patents or patent applications: US 5 958 361, US 2 268 337, WO 01 / 36332 or US 6 887 566, WO 2004 / 005184 or US 7 211 236, WO 2004 / 056927, WO 2005 / 103900, WO 2007 / 028267 or US 8182 573, WO 2008 / 049954 or US 8 231 369, WO 2008 / 019905, US 2009 / 0123357, US 2009 / 0126604, US 2010 / 0055340, WO 2011 / 020204.

[0008] However, this method applied to the preparation of metal oxides can still be improved, in particular in order to improve the stability of the metal oxide particles over time and more particularly their water resistance.

[0009] In addition, a scientific article by Han Gao et al. describes particles involving the application of a CeO2 layer on TiO2 particles in order to reduce the formation of free radicals caused by the interaction between TiO2, light and the external environment. However, this type of particle is coated with an extremely thin cerium oxide layer that does not completely cover the TiO2 core. (Ind. Eng. Chem. Res. [Industrial and Engineering Chemistry Research] 2014, 53 (1), 189-197). These particles are not suitable because the cerium oxide layer does not cover the TiO2 core, cannot prevent titanium oxide from contacting the external environment, and in particular, the release of titanium atoms is found in the particle core. Another scientific article involves combining an iron oxide core and a coating formed by cerium oxide and an acrylate polymer as a particle for the treatment and diagnosis of inflammatory diseases (Y. Wu et al. Journal of Materials Chemistry B [Journal of Materials Chemistry B]. 2018, 6, pp. 4937-4951). The coating located on the iron oxide core is a cluster of cerium oxide nanoparticles connected together by a polymer matrix based on acrylic monomers. This type of coating is not very stable, especially in water, because the acrylic polymer dissolves and the cerium oxide nanoparticles detach from the core surface, which then allows water free access to the iron oxide.

[0010] There is therefore a real need to develop metal oxide particles having good stability over time and very particularly good water resistance, while retaining good optical properties with regard to the absorption and / or scattering of light, more particularly with regard to UV radiation, and also to develop processes capable of preparing such particles. Summary of the invention

[0011] These aims are achieved with the present invention, a subject of which is in particular metal oxide particles, in particular metal oxide particles of the M1-M2 oxide type, of core / shell structure, comprising a core 1 and one or more upper coatings 2 covering said core 1, wherein:

[0012] (i) the core 1 is composed of an oxide of at least one metal M1, preferably in a crystalline state;

[0013] (ii) the upper coating 2 covers at least 90% of the surface of the core 1, preferably covers the entire surface of the core 1, and comprises one or more inorganic compounds containing one or more elements M2 and one or more oxygen atoms; and

[0014] (iii) the element M2 is different from the metal M1 and is selected from the group consisting of scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium, and mixtures thereof; and

[0015] It should be understood that:

[0016] - when the core 1 is made of titanium oxide and when the upper coating 2 is made of cerium oxide, the upper coating 2 is present in an amount greater than 1% by weight relative to the total weight of the particle; and

[0017] The particle is different from a particle comprising: a core 1 consisting of iron oxide Fe3O4 and a top coating 2 comprising cerium oxide CeO2.

[0018] It has been observed that the coated metal oxide particles according to the invention degrade only very little over time in the presence of water, even when they are formulated in aqueous compositions.

[0019] It has also been observed that the metal oxide particles according to the invention have good optical properties in terms of light absorption and / or light scattering. More particularly, they have high UV absorption and low or high visible light scattering, thus allowing uses such as sun protection and / or modifying the visual appearance, while benefiting from resistance in the presence of water.

[0020] Furthermore, the compositions comprising the coated metal oxide particles according to the invention exhibit good shielding capabilities, in particular with regard to long and short UV-A radiation.

[0021] Furthermore, the compositions comprising the coated metal oxide particles of the invention have a particularly high transparency, which can prove to be advantageous when the composition is applied to a coating and in particular to the skin and then allowed to dry.

[0022] Furthermore, since the coated metal oxide particles according to the invention do not require a hydrophobic coating, they can be used in a wide range of formulations (e.g. in completely aqueous formulations and / or formulations without surfactants). Furthermore, when the formulations thus obtained end up in water (washbasin drains, lakes or the sea), the risk of undue deposition (on washbasin rims, pipe walls or rocks) is reduced.

[0023] Another subject of the present invention relates to a method for preparing such metal oxide particles, in particular metal oxide particles of the M1-M2 oxide type with a core / shell structure, the method comprising at least the following steps:

[0024] a. preparing the composition (A) by adding one or more metal M1 precursors to a flammable solvent or a mixture of flammable solvents; and then

[0025] b. in a flame spray pyrolysis device, by injecting the composition (A) and an oxygen-containing gas to form a flame until an aggregate of metal M1 oxide is obtained; and

[0026] c. injecting a composition (B) comprising one or more element M2 precursors into a flame until a coating containing one or more elements M2 and one or more oxygen atoms is obtained on the surface of the metal M1 oxide aggregate; the element M2 is selected from scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium, and mixtures thereof, preferably selected from cerium, yttrium, lanthanum and mixtures thereof.

[0027] It has been observed that the process according to the invention makes it possible to obtain metal oxide particles coated with a layer of inorganic material based on an element M2 which are particularly stable over time and have good resistance to water.

[0028] Furthermore, unlike conventional coating methods, the method according to the invention has the advantage of maintaining the good intrinsic properties of the core despite the presence of the coating. In fact, due to the specific properties of the coating, for a given particle weight, the proportion of metal oxide can be reduced without reducing and / or negatively affecting the properties of said metal oxide.

[0029] Thus, the method of the present invention makes it possible to produce stable metal oxide particles while avoiding the inconvenience caused by an increase in the amount of particles, which is conventionally necessary in order to maintain good optical properties of the metal oxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The accompanying drawings are schematic diagrams. The drawings are not necessarily drawn to scale; rather, they are intended to illustrate the principles of the invention.

[0031] Figure 1 A cross-sectional view showing a metal oxide particle according to one embodiment of the present invention. DETAILED DESCRIPTION

[0032] Other subjects, features, aspects and advantages of the present invention will become even more clear after reading the following description and examples.

[0033] In this manual and unless otherwise indicated:

[0034] - the expression "at least one" is equivalent to the expression "one or more" and can be replaced by it;

[0035] - the expression "between" is equivalent to and can be replaced by the expression "extending from", and means that the limit values ​​are included;

[0036] - the expression "keratin material" refers in particular to the skin and also human keratin fibres, such as hair;

[0037] -Nucleus (1) is also called "center";

[0038] - The upper coating (2) is also called "outer layer", "shell" or "coating";

[0039] - "Alkyl" is understood to mean an "alkyl group", i.e., a C1 to C 10 , in particular C1 to C8, more particularly C1 to C6, and preferably C1 to C4 straight or branched hydrocarbon groups, such as methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl or tert-butyl;

[0040] - an "aryl" group is understood to mean a monocyclic or fused or non-fused carbon-based group containing from 6 to 22 carbon atoms, at least one of the rings being aromatic; preferably, aryl is phenyl, biphenyl, naphthyl, indenyl, anthracenyl or tetrahydronaphthyl, preferably phenyl;

[0041] -"arylate"group is understood to mean a group containing one or more -C(O)O - Aryl carboxylate groups (such as naphthalate or naphthenate);

[0042] - "complexed metal" is understood to mean that the metal atom forms a "metal complex" or "coordination compound" in which the metal ion corresponding to the central atom, i.e. M1, is chemically bonded to one or more electron donors (ligands);

[0043] - "ligand" is understood to mean a coordinating organic chemical group or compound, i.e., it contains at least one carbon atom and is capable of coordinating with the metal M1 and, once coordinated or complexed, produces a metal compound corresponding to the coordination sphere principle (internal complex or chelate) with a predetermined number of electrons - see Ullmann's Encyclopedia of Industrial Chemistry, "Metal complex dyes", 2005, pp. 1-42. More particularly, the ligand is an organic group which contains at least one group which donates electrons by inductive and / or mediating effects, more particularly carries at least one amino, phosphino, hydroxyl or mercapto electron-donating group, or the ligand is a stable carbene, in particular of the "Arduengo" type (imidazole-2-ylidene), or contains at least one carbonyl group. As ligands, mention may be made more particularly of: i) those containing at least one phosphorus atom -P<, i.e. a phosphine, such as triphenylphosphine; ii) bidentate ligands of the formula RC(X)-CR'R"-C(X)-R"', in which R and R"" are identical or different and represent linear or branched (C1-C6)alkyl, and R' and R" are identical or different and represent a hydrogen atom or a linear or branched (C1-C6)alkyl, preferably R' and R" represent a hydrogen atom, X represents an oxygen or sulfur atom, or an N(R) group, in which R represents a hydrogen atom or a linear or branched (C1-C6)alkyl, such as acetylacetone or β-diketone; iii) (poly)hydroxycarboxylic acid ligands of the formula [HO-C(O)]nAC(O)-OH and deprotonated forms thereof, in which when n is A represents a monovalent radical when it has the value zero, or, when n is greater than or equal to 1, a polyvalent radical, which radical is saturated or unsaturated, cyclic or acyclic and aromatic or non-aromatic, based on a hydrocarbon containing from 1 to 20 carbon atoms, optionally interrupted by one or more heteroatoms and / or optionally substituted (especially by one or more hydroxyl groups); preferably, A represents a monovalent (C1-C6) alkyl or polyvalent (C1-C6) alkylene radical optionally substituted by one or more hydroxyl groups; and n represents an integer between 0 and 10 and including the end values; preferably, n is between 0 and 5, for example between 0, 1 or 2; such as lactic acid, glycolic acid, tartaric acid, citric acid and maleic acid, and aryl radicals such as naphthalene dicarboxylate; and iv) C2 to C6 10 Polyol ligands containing from 2 to 5 hydroxyl groups, especially ethylene glycol, glycerol, more particularly still, the ligands carry carboxyl, carboxylate or amino groups, in particular, the ligands are selected from acetate, (C1-C6) alkoxylate, (di)(C1-C6) alkylamino, and aryl radicals, such as naphthalene dicarboxylate or cyclopentane dicarboxylate groups;

[0044] The term "fuel" is understood to mean a liquid compound which, together with molecular oxygen and energy, burns in a chemical reaction, generating heat: combustion. In particular, the liquid fuel is selected from: protic solvents, in particular alcohols, such as methanol, ethanol, isopropanol, n-butanol; aprotic solvents, which are particularly selected from esters such as methyl esters and those derived from acetates such as 2-ethylhexyl acetate, acids such as 2-ethylhexanoic acid (EHA), acyclic ethers such as diethyl ether, methyl tert-butyl ether (MTBE), methyl tert-amyl ether (TAME), methyl tert-hexyl ether (THEME), ethyl tert-butyl ether (ETBE), ethyl tert-amyl ether (TAEE), diisopropyl ether (DIPE), cyclic ethers such as tetrahydrofuran (THF), aromatic hydrocarbons or aromatic hydrocarbons such as xylene, non-aromatic hydrocarbons; and mixtures thereof. The fuel may optionally be selected from liquefied hydrocarbons, such as acetylene, methane, propane or butane; and mixtures thereof.

[0045] Metal oxide particles

[0046] The metal oxide particles according to the invention, in particular of the M1-M2 oxide type, of core / shell structure, comprise a core 1 consisting of an oxide of at least one metal M1, preferably in the crystalline state.

[0047] Preferably, the metal M1 is selected from the elements from column 2 of the periodic table, titanium, zinc, copper, scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium; more preferably selected from magnesium, calcium, titanium, zinc, copper, cerium and yttrium.

[0048] According to the invention, metal M1 is different from element M2.

[0049] The crystalline state of the core 1 and also its composition can be determined, for example, by conventional X-ray diffraction methods.

[0050] Advantageously, the core 1 of the particle according to the invention consists of one or more aggregates of crystalline primary particles of an oxide of at least one metal M1. In other words, the core 1 consists of several crystallites of an oxide of at least one metal M1.

[0051] according to Figure 1 The metal oxide particles have an average diameter D m A core 1 in a crystalline state is formed from an oxide of at least one metal M1 and comprises one or more aggregates of primary particles of an oxide of at least one metal M1.

[0052] according to Figure 1 The metal oxide particles further include a surface that completely covers the core 1 and has an average thickness d m The top coating 2.

[0053] The number average diameter D of core 1 mIt can be determined, for example, by transmission electron microscopy (TEM for short). Preferably, the number average diameter D of the core 1 of the particles according to the invention is m In the range extending from 3 to 1000 nm; more preferably from 6 to 50 nm, and still more preferably between 10 and 30 nm.

[0054] The metal oxide particles according to the invention comprise one or more top coatings 2 covering at least 90% of the surface of the core 1 .

[0055] The degree of coverage of the core by the top coating can be determined, for example, by visual analysis of the TEM-BF or STEM-HAADF type combined with STEM-EDX analysis.

[0056] Each analysis is performed on a statistical number of particles, in particular, at least 20 particles. The particles are deposited on a metal grid made of a metal different from any metal forming part of the particles (whether in the core or in the upper coating). For example, the grid is made of copper (except where it is desired to use copper in making the particles).

[0057] Visual analysis of TEM-BF and STEM-HAADF images allows one to infer, based on contrast, whether the coating completely surrounds the core of the particle. The degree of coverage of the core can be inferred by analyzing each of 20 (or more) images and then determining the average degree of coverage by taking the average.

[0058] STEM-EDX analysis makes it possible to verify that the coating does contain mainly or only the element M2. To do this, it is necessary to carry out measurements on the edges of the particles (at least on 20 particles). These measurements then reveal the element M2.

[0059] STEM-EDX analysis also makes it possible to verify that the core does contain metal M1. To do this, it is necessary to carry out measurements in the center of the particle (at least on 20 particles). These measurements then reveal metal M1 and element M2.

[0060] Preferably, the top coating 2 completely covers the surface of the core 1 .

[0061] The upper coating layer 2 comprises one or more inorganic compounds containing one or more elements M2 and one or more oxygen atoms.

[0062] The element M2 is different from the metal M1.

[0063] The element M2 belongs to the group of rare earth elements in the +III oxidation state and is chosen from scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium, and mixtures thereof.

[0064] Preferably, the element M2 is selected from cerium, yttrium, lanthanum and mixtures thereof.

[0065] According to a first specific embodiment of the present invention, the element M2 is preferably cerium.

[0066] According to another specific embodiment of the present invention, the element M2 is preferably yttrium.

[0067] According to yet another specific embodiment of the present invention, the element M2 is lanthanum.

[0068] According to yet another specific embodiment of the present invention, the metal oxide particles comprise a core 1 composed of yttrium oxide and an upper coating 2 comprising cerium oxide.

[0069] The average thickness of the coating layer is d m It can also be determined by transmission electron microscopy.

[0070] Preferably, the number average thickness d m In a range extending from 1 to 30 nm; more preferably from 1 to 15 nm, and still more preferably from 1 to 6 nm.

[0071] Advantageously, the top coating 2 is amorphous.

[0072] Preferably, the upper coating 2 is composed of one or more oxides of at least one element M2; the oxide of the at least one element M2 being different from the oxide of the at least one metal M1.

[0073] More preferably, the upper coating layer 2 is composed of cerium oxide CeO2, yttrium oxide Y2O3 and / or lanthanum oxide La2O3 and a mixture of these oxides.

[0074] Very particularly preferably, the particles according to the invention comprise a top coating 2 composed of an oxide of an element M2 selected from cerium oxide CeO 2 , yttrium oxide Y 2 O 3 and / or lanthanum oxide La 2 O 3 .

[0075] Advantageously, the metal oxide particles according to the invention comprise a specific (M1 / M2) for the particles according to the invention. 颗粒 Molar atomic ratio of metal M1 and element M2.

[0076] This ratio corresponds on the one hand to the molar amount of metal M1 atoms present in the particles according to the invention and on the other hand to the molar amount of element M2 present in the particles according to the invention.

[0077] This ratio can be determined by spectrometry according to one of the following two methods. According to the first method, the powder is spread and studied by X-ray fluorescence measurement using an X-ray spectrometer to deduce the metal ratio therefrom. According to another method, the particles of the invention are pre-dissolved in acid. The material obtained is then subjected to an elemental analysis by ICP-MS (Inductively Coupled Plasma Mass Spectrometry) to deduce the metal ratio therefrom.

[0078] Preferably, (M1 / M2) 颗粒 The molar atomic ratio is greater than or equal to 0.25; more preferably in a range extending from 0.25 to 99; still more preferably in a range extending from 1 to 80; and still better still in a range extending from 3 to 20.

[0079] Preferably, the sum of the content of metal M1 oxide and the content of element M2 oxide is at least equal to 99% by weight, relative to the total weight of the core 1 and the upper coating 2 .

[0080] The number average diameter of the particles according to the invention can also be determined by transmission electron microscopy. Preferably, the number average diameter of the particles according to the invention is in the range extending from 3 to 5000 nm; more preferably from 4 to 3000 nm; and still more preferably from 5 to 1000 nm.

[0081] Preferably, the BET specific surface area of ​​the particles according to the present invention is between 1 m 2 / g and 350m 2 / g; more preferably between 1m 2 / g and 200m 2 / g; and even more preferably between 30 and 100 m 2 / g.

[0082] According to a specific embodiment of the present invention, the metal oxide particles according to the present invention may optionally further comprise an additional coating covering the upper coating layer 2 and comprising at least one hydrophobic organic compound.

[0083] The hydrophobic organic compound comprised in the additional coating is more preferably chosen from silicones, in particular silicones comprising at least one fatty chain; carbon-based derivatives comprising at least 6 carbon atoms, in particular fatty acid esters; and mixtures thereof.

[0084] This additional coating can be produced by a liquid method or by a solid method. By a liquid method, the hydroxyl functional groups react with reactive functional groups of the compound that will form the coating (typically silanol functional groups of silicones or acid functional groups of carbon-based fatty substances). By a solid method, the particles are contacted with a liquid or pasty compound containing a hydrophobic substance.

[0085] Preferably, the metal oxide particles according to the present invention are obtained by the preparation method of the present invention as described below.

[0086] Method for preparing coated metal oxide particles

[0087] Another subject of the invention is a process for preparing metal oxide particles of the M1-M2 oxide type, in particular of a core / shell structure, comprising at least one step a.: preparing the composition (A); then a step b.: forming a flame; and a step c.: injecting the composition (B).

[0088] Step a. of the process according to the invention consists of preparing the composition (A) by adding one or more metal M1 precursors to a flammable solvent or a mixture of flammable solvents.

[0089] Preferably, the metal M1 is selected from the elements from column 2 of the periodic table, titanium, zinc, copper, scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium; more preferably selected from magnesium, calcium, titanium, zinc, copper, cerium and yttrium.

[0090] According to the invention, metal M1 is different from element M2.

[0091] The metal M1 precursor and the combustible solvent that can be used according to the present invention can be selected from the metal M1 precursors and combustible solvents conventionally used for flame spray pyrolysis.

[0092] Preferably, the metal M1 precursor comprised in composition (A) comprises one or more metal M1 atoms, optionally complexed with one or more ligands containing at least one carbon atom.

[0093] More preferably, the ligand is selected from acetate, (C1-C6) alcohol, (C2-C 10 )alkylcarboxylates, (di)(C1-C6)alkylamino and aryl radicals such as naphthenate or cyclopentanoate groups.

[0094] Preferably, the flammable solvent is selected from protic flammable solvents, aprotic flammable solvents and mixtures thereof; more preferably selected from alcohols, esters, acids, acyclic ethers, cyclic ethers, aromatic hydrocarbons or aromatic hydrocarbons, non-aromatic hydrocarbons, and mixtures thereof; and better still selected from 2-ethylhexyl acetate, 2-ethylhexanoic acid (EHA), ethyl ether, methyl tert-butyl ether (MTBE), methyl tert-amyl ether (TAME), methyl tert-hexyl ether (THEME), ethyl tert-butyl ether (ETBE), ethyl tert-amyl ether (TAEE), diisopropyl ether (DIPE), tetrahydrofuran (THF), xylene, and mixtures thereof.

[0095] Very particularly preferably, the flammable solvent is chosen from aprotic flammable solvents comprising at least three carbon atoms and mixtures thereof; and better still from xylene, tetrahydrofuran, 2-ethylhexyl acetate, 2-ethylhexanoic acid (EHA) and mixtures thereof.

[0096] Advantageously, the content of metal M1 precursor in composition (A) is between 1% and 60% by weight and preferably between 15% and 30% by weight relative to the total weight of composition (A).

[0097] The preparation method according to the present invention further comprises step b.: injecting the composition (A) and the oxygen-containing gas into a flame spray pyrolysis (FSP) device to form a flame.

[0098] During this step b., composition (A) and oxygen-containing gas are advantageously injected into the flame spray pyrolysis device through two injectors separated from each other. In other words, composition (A) and oxygen-containing gas are injected separately, that is, composition (A) and oxygen-containing gas are not injected through a single nozzle.

[0099] More specifically, the composition (A) is delivered through one tube, while the oxygen-containing gas (also referred to as "dispersed oxygen") is delivered through another tube. The inlets of the two tubes are arranged so that the oxygen-containing gas generates a negative pressure and the composition (A) is sucked and converted into droplets by the Venturi effect.

[0100] Step b. may optionally further comprise an additional injection of a "premix" mixture comprising oxygen and one or more combustible gases. This "premix" mixture (also referred to as "flame-supporting oxygen") is capable of generating a flame support intended to ignite and maintain the flame generated by composition A and the oxygen-containing gas (i.e., "dispersed oxygen").

[0101] Preferably, during step b., composition (A), oxygen-containing gas and optionally the "premix" mixture (when present) are injected into a reaction tube (also called "closed tube"). Preferably, the reaction tube is made of metal or quartz. Advantageously, the reaction tube has a height greater than or equal to 30 cm, preferably greater than or equal to 40 cm, and more preferably greater than or equal to 50 cm. Preferably, the length of the reaction tube is between 30 cm and 300 cm, in particular between 40 cm and 200 cm, and more particularly between 45 cm and 100 cm, for example 50 cm.

[0102] The weight ratio of the mass of solvent present in composition (A) on the one hand to the mass of oxygen-containing gas on the other hand is defined as follows: First, the amount of oxygen-containing gas (also called oxidant compound) is calculated so that the combination formed by composition (A) on the one hand (i.e., combustible solvent and metal M1 precursor) and oxygen-containing gas on the other hand can react together in a stoichiometric ratio in a combustion reaction (therefore without excess or deficiency of oxidant compound). Starting from this calculated amount of oxygen-containing gas (also called "calculated oxidant"), a new calculation is performed to deduce therefrom the amount of oxygen-containing gas to be injected (also called "oxidant to be injected") according to the following formula: Oxidant to be injected = calculated oxidant / in Preferably it is between 0.3 and 0.9, and more preferably between 0.4 and 0.65.

[0103] This approach is defined, inter alia, by Turns, SR, An Introduction to Combustion: Concepts and Applications, 3rd ed.; McGraw-Hill: New York, 2012.

[0104] The preparation method according to the invention further comprises a step c.: comprising injecting a composition (B) comprising one or more precursors of the element M2 into the flame formed during step b.

[0105] The injection of composition (A) and the injection of composition (B) are preferably simultaneous. In other words, the process of the invention is continuous and maintains the flame formed in step b.

[0106] Preferably, the flame formed during step b. has a temperature higher than or equal to 2000° C. in at least a portion of the flame.

[0107] At the point where composition (B) is injected into the flame formed in step b. and maintained in step c., ie during step c., the temperature is preferably between 200 and 800°C, and more preferably between 400 and 500°C.

[0108] Advantageously, during step c., composition (B) is injected through a spray ring placed above said reaction tube as described above, in particular in which the injection of composition (A) takes place. More preferably, an additional tube is placed in succession of said reaction tube and said spray ring, the additional tube then being placed above the spray ring, and the spray ring itself being placed above said reaction tube.

[0109] According to this preference, the additional tube is made of metal or quartz. Advantageously, the additional tube has the same diameter as the reaction tube and has a height greater than or equal to 30 cm, preferably greater than or equal to 40 cm, and more preferably greater than or equal to 50 cm. Preferably, the length of the additional tube is between 30 cm and 300 cm, in particular between 40 cm and 200 cm, and more particularly between 45 cm and 100 cm, for example 50 cm.

[0110] As mentioned above, the element M2 belongs to the group of rare earth elements in the +III oxidation state and is chosen from scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium, and mixtures thereof.

[0111] Preferably, the element M2 is selected from cerium, yttrium, lanthanum and mixtures thereof.

[0112] According to a first specific embodiment of the present invention, the element M2 is preferably cerium.

[0113] According to another specific embodiment of the present invention, the element M2 is preferably yttrium.

[0114] According to yet another specific embodiment of the present invention, the element M2 is lanthanum.

[0115] Preferably, the element M2 precursor comprises one or more atoms of the element M2, optionally complexed with one or more ligands.

[0116] Preferably, the ligand is selected from acetate, nitrate, (C1-C6) alcohol, (C2-C 10 )alkylcarboxylates, (di)(C1-C6)alkylamino and aryl radicals such as naphthenate or cyclopentanoate groups.

[0117] The element M2 precursor may be selected from halides of the element M2.

[0118] During the method according to the invention, it is possible to calculate (M1 / M2) 注射的 Molar atomic ratio. This ratio corresponds on the one hand to the molar amount of metal M1 atoms injected during step b. and on the other hand to the molar amount of element M2 injected during step c.

[0119] Preferably, (M1 / M2) 注射的 The molar atomic ratio is greater than or equal to 0.25; more preferably in a range extending from 0.25 to 120; still more preferably from 0.25 to 99, better in a range extending from 1 to 80; and still better in a range extending from 3 to 20.

[0120] Preferably, nitrogen (N2) is bubbled into the composition (B) as described above before injection during step c. The injection rate of the composition (B) can then be controlled by controlling the temperature and controlling the flow rate of the bubbler.

[0121] According to one particular embodiment of the invention, composition (B) as described above is brought to a temperature ranging from 25°C to 70°C, more preferably from 30°C to 60°C, before its injection during step c.

[0122] Preferably, the content of element M2 precursor in composition (B) injected during step c. of the process according to the invention is between 1% and 60% by weight, more preferably between 5% and 30% by weight relative to the total weight of composition (B).

[0123] Advantageously, composition (B) may also comprise one or more solvents. Preferably, the solvent present in composition (B) is chosen from polar protic solvents other than water; and more preferably from (C1-C8)alkanols. Still more preferably, composition (B) comprises ethanol.

[0124] According to a preferred embodiment of the present invention, the solvent present in composition (B) is chosen from solvents flammable at the flame temperature of step c., preferably from solvents flammable at a temperature between 200° C. and 800° C. and more preferably between 400° C. and 500° C. Even better, the solvent present in composition (B) has a boiling point higher than or equal to room temperature (25° C.), or even in a range extending from 50° C. to 120° C.

[0125] Preferably, the content of solvent present in the composition (B) injected during step c. of the process according to the invention is between 40% and 99% by weight, more preferably between 50% and 98% by weight and better still between 70% and 95% by weight relative to the total weight of composition (B).

[0126] According to a preferred embodiment of the present invention, the preparation method may further include step d.: calcining the metal oxide particles obtained after step c.

[0127] According to this embodiment, during the calcination step d.:

[0128] (i) calcination is preferably continued for between 60 and 400 minutes, more preferably between 60 and 180 minutes; and / or

[0129] (ii) The temperature range is preferably from 100°C to 600°C, more preferably from 300°C to 600°C.

[0130] According to a particular embodiment of the invention, the particles obtained by the preparation method according to the invention are doped. According to this embodiment, the composition (A) further comprises one or more precursors of an element D different from the metal M1 and the element M2, wherein D is selected from fluorine, vanadium, zirconium, hafnium, iron and tungsten.

[0131] Another subject of the present invention is a composition, preferably a cosmetic composition, comprising one or more metal oxide particles as described above and / or preferably obtained by the process according to the invention.

[0132] The composition of the invention may be in various galenic forms. Thus, the composition of the invention may be in the form of a powder (powdered) composition or a liquid composition, or in the form of a milk, cream, paste or aerosol composition.

[0133] The composition according to the invention is in particular a cosmetic composition, i.e. the material of the invention is in a cosmetic medium. The term "cosmetic medium" means a medium suitable for application to keratin materials, in particular human keratin materials such as the skin, which cosmetic medium is generally composed of water or a mixture of water and one or more organic solvents or a mixture of organic solvents.

[0134] The composition according to the invention is advantageously an aqueous composition.

[0135] Preferably, the composition comprises water, especially in a content ranging from 5% to 95% inclusive relative to the total weight of the composition.

[0136] The term "organic solvent" means an organic substance that is capable of dissolving another substance without chemically altering it.

[0137] Examples of organic solvents that may be mentioned include lower C2-C6 alkanols, such as ethanol and isopropanol, polyols and polyol ethers, for example 2-butoxyethanol, propylene glycol, propylene glycol monomethyl ether and diethylene glycol monoethyl ether and monomethyl ether, and also aromatic alcohols, for example benzyl alcohol or phenoxyethanol, and mixtures thereof.

[0138] Preferably, the organic solvent is present in the composition according to the invention in a content of between about 0.1% and 40% by weight, inclusive, relative to the total weight of the composition, and more preferably between about 1% and 30% by weight and even more particularly between 5% and 25% by weight, inclusive, relative to the total weight of the composition.

[0139] The composition according to the invention may contain a fatty phase and may be in the form of a direct or inverse emulsion.

[0140] The composition according to the invention can be prepared in the form of a simple or complex emulsion (oil-in-water, or abbreviated as O / W, water-in-oil or W / O, oil-in-water-in-oil or O / W / O, or water-in-oil-in-water or W / O / W) such as a cream, lotion or cream-gel according to techniques well known to those skilled in the art.

[0141] According to a particular embodiment of the invention, the composition according to the invention may also be in the form of an anhydrous composition, for example in the form of an oil. The term "anhydrous composition" is intended to mean a composition containing less than 2% by weight of water, preferably less than 1% by weight of water and even more preferably less than 0.5% by weight of water, relative to the total weight of the composition, or even a composition that is free of water. In compositions of this type, the water that may be present is not added during the preparation of the composition, but corresponds to the residual water provided by the mixed ingredients.

[0142] The metal oxide particles according to the invention can also be in dry form (powder, flakes, plates), as a dispersion or as a liquid suspension or as an aerosol.The metal oxide particles according to the invention can be used as such or mixed with other ingredients.

[0143] Preferably, the composition according to the invention contains between 0.1% and 40% by weight, more preferably between 0.5% and 20% by weight, still more preferably between 1% and 10% by weight and better still between 1.5% and 5% by weight of metal oxide particles according to the invention, relative to the total weight of the composition.

[0144] Another subject of the present invention is a composition, preferably a cosmetic composition, according to the invention for protecting the skin, preferably human skin, from visible radiation (i.e. wavelengths between 400 nm and 800 nm) and / or ultraviolet radiation (i.e. wavelengths between 100 nm and 400 nm), UV-A radiation (i.e. wavelengths between 320 nm and 400 nm) and / or UV-B radiation (i.e. wavelengths between 280 nm and 320 nm). The compositions according to the invention make it possible to effectively screen against solar radiation, they are broad-spectrum, in particular with respect to UV-A radiation (including long-wave UV-A radiation), while being particularly stable over time under UV exposure.

[0145] The composition according to the invention may optionally contain, in addition to the metal oxide particles according to the invention, one or more additional UV-screening agents selected from hydrophilic, lipophilic or insoluble organic UV-screening agents and / or one or more mineral pigments. It will preferably consist of at least one hydrophilic, lipophilic or insoluble organic UV-screening agent.

[0146] The composition of the invention can be used in a single application or in multiple applications. When the composition of the invention is intended for multiple applications, the content of the metal oxide particles of the invention is generally lower than in a composition intended for a single application.

[0147] For the purposes of the present invention, the term "single administration" means a single administration of the composition, which may be repeated several times a day with each administration separated from the next by one or more hours, or once a day as needed.

[0148] For the purposes of the present invention, the term "multiple administrations" means repeated administrations of the composition, usually 2 to 5 times, with each administration being separated from the next by a few seconds to a few minutes. Each multiple administration can be repeated several times a day, separated from the next administration by one or more hours, or every day, as desired.

[0149] Application method

[0150] The metal oxide particles according to the invention are agents for protection against UVA and UVB radiation. They significantly improve the overall shielding against UV radiation while maintaining good overall transmittance in the visible range and excellent transparency in the visible range (400-780 nm).

[0151] The metal oxide particles according to the invention are used in particular in cosmetic compositions, in particular for application to keratin materials, especially human keratin materials such as the skin, in a concentration preferably of between 0.1% and 40% by weight relative to the total weight of the composition in which they are contained; more preferably between 0.5% and 20% by weight relative to the total weight of the composition in which they are contained.

[0152] The composition may be in any galenical form.

[0153] The metal oxide particles of the present invention can be applied to the keratin material as a single application or as multiple applications. For example, the cosmetic composition comprising the metal oxide particles of the present invention can be applied once.

[0154] According to another variant, the application method involves several successive applications on the keratin material of a cosmetic composition comprising one or more metal oxide particles according to the invention.

[0155] They may also be related application methods, such as saturated single application, i.e. single application of a cosmetic composition with a high concentration of metal oxide particles according to the invention, or multiple applications of a cosmetic composition (at a lower concentration) comprising one or more metal oxide particles according to the invention. In the case of multiple applications, the cosmetic composition comprising at least one metal oxide particle according to the invention may be applied several times in succession, with or without delay between applications.

[0156] Another subject of the invention is a method for treating keratin materials, especially human keratin materials such as the skin, by applying to said material a composition as defined previously, preferably by 1 to 5 consecutive applications, leaving drying between the layers, the applications being by spraying or in some other way.

[0157] According to one embodiment of the invention, multiple applications are carried out on keratin materials with a drying step between successive applications of the cosmetic composition comprising the metal oxide particles of the invention. The drying step between successive applications of the cosmetic composition comprising at least one metal oxide particle of the invention can be carried out outdoors or manually, for example with a hot air drying system such as a hair dryer.

[0158] Another subject of the invention is the use of the metal oxide particles as described above and / or obtained by the preparation process as described above for formulating cosmetic or pharmaceutical compositions which have, in particular, an antiperspirant or pH-regulating effect on the skin or are intended to protect the skin from visible and / or UV radiation or to modify the appearance of the skin.

[0159] A further subject of the invention is the use of one or more of the inventive metal oxide particles as defined above as UV-A and UV-B screening agents for protecting keratin materials, in particular the skin.

[0160] The following examples serve to illustrate the invention but are not limiting in nature.

[0161] Examples

[0162] Example 1:

[0163] 1.1 First, a composition (A) of zinc naphthenate (550 mM) in xylene was prepared.

[0164] Uncoated zinc oxide particles P1 (outside the present invention) were then prepared using the conventional FSP preparation method Prep 1 with the pre-prepared composition (A).

[0165] Next, zinc oxide particles P2 coated with cerium dioxide (invention) were prepared using the same composition (A) and a composition (B) comprising cerium (III) nitrate hexahydrate (500 mM) and ethanol using the preparation method Prep 2 according to the invention.

[0166] The parameters of the Prep 1 method are as follows:

[0167] - Ratio (composition (A) / O2) = 5 mL / min of composition (A) and 7 L / min of gas (O2). To adjust the oxygen flow rate, use

[0168] The parameters of the Prep 2 method are as follows:

[0169] - Ratio (composition (A) / O2) = 5 mL / min of composition (A) and 7 L / min of gas (O2). To adjust the oxygen flow rate, use

[0170] In this Prep 2 process, a 40 cm high quartz tube was used to inject composition (A). A spray ring was placed above the quartz tube for injection of composition (B). The quartz tube and the spray ring had a diameter of 10 cm.

[0171] Furthermore, nitrogen was first bubbled through composition (B). When injecting composition (B), the nitrogen flow heated between 30°C and 40°C was adjusted so as to evaporate cerium (III) nitrate hexahydrate and make (Zn / Ce) 注射的 Molar atomic ratio = 5.7.

[0172] 1.2 Once the particles were prepared, it was observed that the zinc oxide particles obtained were crystalline.

[0173] Furthermore, the particles obtained according to the method Prep 2 according to the invention are coated with cerium dioxide and have a (Zn / Ce) ratio of 5.7. 颗粒 Molar atomic ratio.

[0174] The BET surface area of ​​the particles according to method Prep 2 is 50 m 2 / g.

[0175] The particles according to method Prep 2 had a number average diameter equal to 22 nm.

[0176] 1.3 Water resistance evaluation:

[0177] A first aqueous suspension S1 (pH=8, by adding sodium hydroxide) was prepared from particles P1 and water in a content of 1 g of P1 / L of water.

[0178] In the same way, a second aqueous suspension S2 (pH=8, by adding sodium hydroxide) was prepared from particles P2 and water in a content of 1 g of P2 / L of water.

[0179] Next, each of the suspensions S1 and S2 was placed in an ultrasonic bath at a power of 20 W for 10 min.

[0180] The Zn present in the suspension was then measured for each suspension by conventional anodic stripping voltammetry as a function of time and relative to the amount of zinc introduced. 2+ Ion content.

[0181] The results are summarized in the following table:

[0182]

[0183]

[0184] t0 corresponds to the first measurement performed less than 10 min after the end of the ultrasonic bath.

[0185] It should be noted that the coated zinc oxide particles P2 obtained according to the preparation method Prep 2 according to the invention have much better water resistance than the uncoated zinc oxide particles P1 obtained according to the comparative preparation method Prep 1.

[0186] In particular, no selective sedimentation (Ce vs. Zn) or selective dissolution was observed for the coated zinc oxide particles P2 (according to the invention) in the suspension S2.

[0187] Example 2:

[0188] 2.1 First, a composition (A) of zinc naphthenate (550 mM) in xylene was prepared.

[0189] The pre-prepared composition (A) was then used to prepare zinc oxide particles P3 coated with cerium dioxide (according to the invention) using the FSP preparation method Prep 3.

[0190] The parameters of the Prep 3 method are as follows:

[0191] - Ratio (composition (A) / O2) = 5 mL / min of composition (A) and 7 L / min of gas (O2). To adjust the oxygen flow rate, use

[0192] In this Prep 3 process, a 40 cm high quartz tube was used to inject composition (A). A spray ring was placed above the quartz tube for injecting composition (B). And an additional 30 cm high metal tube was placed above the spray ring. The quartz tube, the additional metal tube and the spray ring all had a diameter of 10 cm.

[0193] Furthermore, nitrogen was first bubbled through composition (B). When injecting composition (B), the nitrogen flow heated between 30°C and 40°C was adjusted so as to evaporate cerium (III) nitrate hexahydrate and make (Zn / Ce) 注射的 Molar atomic ratio = 5.7.

[0194] Next, a portion of the prepared particles P3 was taken out to be subjected to an additional calcination step at 500° C. for 1 hour, and thus zinc oxide particles P4 (the present invention) coated with cerium dioxide were obtained.

[0195] 2.2 Once the particles were prepared, it was observed that the zinc oxide particles P3 and P4 obtained were crystalline.

[0196] Furthermore, particles P3 and P4 according to the invention were coated with ceria and had a (Zn / Ce) ratio of 5.7. 颗粒 Molar atomic ratio.

[0197] The BET specific surface area of ​​particle P3 is 44 m 2 / g.

[0198] The BET surface area of ​​particle P4 is 40 m 2 / g.

[0199] The particles P3 have a number average diameter equal to 23 nm.

[0200] The particles P4 have a number average diameter equal to 26 nm.

[0201] 2.3 Water resistance evaluation:

[0202] A third aqueous suspension S3 (pH=8, by adding sodium hydroxide) was prepared from particles P3 and water in a content of 1 g of P3 / L of water.

[0203] In the same way, a fourth aqueous suspension S4 (pH=8, by adding sodium hydroxide) was prepared from particles P4 and water at a content of 1 g of P4 / L of water.

[0204] Next, each of the suspensions S3 and S4 was placed in an ultrasonic bath at a power of 20 W for 10 min.

[0205] The amount of Zn present in suspensions S3 and S4 and in suspension S1 of Example 1 above was then measured for each suspension as a function of time and relative to the amount of zinc introduced by conventional anodic stripping voltammetry. 2+ Ion content.

[0206] The results are summarized in the following table:

[0207]

[0208] t0 corresponds to the first measurement performed less than 10 min after the end of the ultrasonic bath.

[0209] It should be noted that the coated zinc oxide particles P3 and P4 according to the invention have better water resistance than the comparative uncoated zinc oxide particle P1.

[0210] In particular, no selective sedimentation (Ce vs. Zn) or selective dissolution was observed for the coated zinc oxide particles P3 and P4 (according to the invention) in suspensions S3 and S4, respectively.

[0211] Example 3

[0212] Particles P1, P2, P3 and P4 from the two previous examples were used.

[0213] 200 mg of one type of particles P1 to P4 were introduced into 1 L of water to produce formulations F1 (based on particles P1), F2 (based on particles P2), F3 (based on particles P3) and F4 (based on particles P4). Spectra of these formulations F1 to F4 in the UV and visible regions were then produced.

[0214] Record the following absorbance.

[0215]

[0216] Note that formulations F2 and F3 according to the invention absorb less UV radiation than formulation F1 (comparative).

[0217] It was observed that formulation F4 according to the invention absorbed more UV radiation than formulation F1 (comparative).

[0218] Raman studies were performed on particles P1 to P4. The Raman peak of the ZnO of particle P4 is much stronger (about 3 times) than that of the reference ZnO.

[0219] Raman peaks of ZnO were also observed for particles P2 and P3.

[0220] The invention thus makes it possible to adjust the barrier capacity of a composition while having good stability in water in all cases.

Claims

1. A metal oxide particle comprising a core (1) and one or more upper coating layers (2) covering the core (1), characterized in that: (i) the core (1) is composed of at least one oxide of a metal M1, (ii) the upper coating (2) covers at least 90% of the surface of the core (1) and comprises one or more inorganic compounds containing one or more elements M2 and one or more oxygen atoms; as well as (iii) the element M2 is different from the metal M1 and is selected from scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium, and mixtures thereof; and It should be understood that: - The BET specific surface area of ​​the particles is 30 m 2 / g to 200m 2 / g between; - when the core (1) is composed of titanium oxide and when the top coating (2) is composed of cerium oxide, the top coating (2) is present in an amount greater than 1% by weight relative to the total weight of the particle; and The particles are different from particles comprising: a core (1) consisting of iron oxide Fe3O4 and an upper coating (2) comprising cerium oxide CeO2.

2. The particle according to claim 1, characterized in that The metal M1 is selected from the group consisting of elements from column 2 of the periodic table, titanium, zinc, copper, scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium.

3. The particle according to claim 1 or 2, characterized in that The element M2 is selected from cerium, yttrium, lanthanum and mixtures thereof.

4. The particle according to claim 1 or 2, characterized in that The upper coating (2) is composed of one or more oxides of at least one element M2.

5. The particle according to claim 4, characterized in that The sum of the content of the metal M1 oxide and the content of the element M2 oxide is at least equal to 99% by weight relative to the total weight of the core (1) and the upper coating (2).

6. The particle according to claim 1 or 2, characterized in that The number average diameter Dm of the core (1) determined by transmission electron microscopy is in the range extending from 3 to 1 000 nm.

7. The particle according to claim 1 or 2, characterized in that The number average thickness d of the top coating (2) determined by transmission electron microscopy m It is in the range extending from 1 to 30nm.

8. The particle according to claim 1 or 2, characterized in that The number average diameter of the particles determined by transmission electron microscopy is in the range extending from 3 to 5 000 nm.

9. A method for preparing the metal oxide particles according to any one of claims 1 to 8, characterized in that: The method comprises at least the following steps: a. preparing composition A by adding one or more metal M1 precursors to a flammable solvent or a mixture of flammable solvents; then b. in a flame spray pyrolysis device, forming a flame by injecting the composition A and an oxygen-containing gas until an aggregate of metal M1 oxide is obtained; and c. injecting a composition B comprising one or more element M2 precursors into the flame until a coating containing one or more elements M2 and one or more oxygen atoms is obtained on the surface of the metal M1 oxide aggregate; the element M2 is selected from scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium, and mixtures thereof.

10. The method according to claim 9, characterized in that The metal M1 precursor comprises one or more metal M1 atoms optionally complexed with one or more ligands; the ligands are selected from the following groups: acetate, C1-C6 alcohol, C2-C 10 Alkyl carboxylates, C1-C6 alkylaminos, C1-C6 dialkylaminos and aryl radicals.

11. The method according to claim 9 or 10, characterized in that: The flammable solvent is selected from the group consisting of aprotic flammable solvents containing at least three carbon atoms and mixtures thereof.

12. The method according to claim 9 or 10, characterized in that: The element M2 precursor comprises one or more element M2 atoms optionally complexed with one or more ligands, the ligands being selected from the following groups: acetate, nitrate, C1-C6 alcohol, C2-C 10 Alkyl carboxylates, C1-C6 alkylaminos, C1-C6 dialkylaminos and aryl radicals.

13. The method according to claim 9 or 10, characterized in that: The composition B comprises one or more polar protic solvents other than water.

14. The method according to claim 9 or 10, characterized in that The method further comprises the step (d) of calcining the metal oxide particles obtained after step c at a temperature extending from 100°C to 600°C.

15. The particle according to any one of claims 1 to 8, characterized in that The particles are obtained by the method according to any one of claims 9 to 14.

16. A composition comprising one or more particles as claimed in any one of claims 1 to 8 and / or obtained by the method of any one of claims 9 to 14.

17. The composition according to claim 16, for use in protecting the skin from visible light and / or UV-A and / or UV-B ultraviolet radiation.

18. Use of the particles according to any one of claims 1 to 8 and / or obtained by the process according to any one of claims 9 to 14 for formulating a cosmetic or pharmaceutical composition.

Citation Information

Patent Citations

  • Method for making silica nanoparticles by flame spray pyrolysis adopting two-fluid nozzle

    US20090123357A1

  • Gas phase production of coated titania

    US20090126604A1

  • Method for Coating Core Ceramic Particles by Emulsion Flame Spray Pyrolysis

    US20100055340A1

  • Strap seal joint

    US2268337A

  • Ultrafine metal oxide powders by flame spray pyrolysis

    US5958361A