Method for manufacturing zipper bag
By using isocyanate and polyol components to form a solvent-free adhesive composition, the problems of attachment damage and solvent release of zipper bags at high temperatures are solved, the heat resistance and sealing strength are improved, and the production cost is reduced.
Patent Information
- Application Number
- CN202080088642.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-11-09
AI Technical Summary
Existing zipper bags are easily damaged when attaching the zipper structure at high temperatures, and the use of solvent-based high-performance adhesives can lead to the release of volatile organic compounds, increasing costs and production difficulties.
A solvent-free adhesive composition is formed using an isocyanate component and a polyol component by applying its layer to a polyethylene terephthalate layer and a polyethylene layer at a temperature of 200°C or higher Contact with zipper structure to form a heat-resistant laminate.
Damage during the attachment process of the zipper structure is effectively avoided and solvent residue is reduced, improving the heat resistance and sealing strength of the laminate and reducing production costs.
Smart Images

Figure CN114846046B_ABST
Abstract
Description
[0001] A desirable container for packaging food is a zipper bag, which has a closure configuration (called a "zipper") that can be sealed by applying pressure with the fingers, then opened manually, and then closed again by applying pressure with the fingers. The sides of the body of the zipper bag are polymer laminates, and the zipper structure is also made of one or more polymers. The zipper structure is attached to the sides of the bag body by applying pressure at relatively high temperatures.
[0002] Due to the high temperatures involved, the process of attaching the zipper structure to the bag body will typically damage the laminates that make up the sides of the bag body, for example by causing wrinkles and / or blistering. This damage can sometimes be avoided when the laminate is formed by combining the layers with a high-performance adhesive composition having very good heat resistance. In the past, many such high-performance adhesives were solvent-based; that is, when applied to a substrate, the adhesive was in the form of a solution in an organic solvent. The use of such solvents causes problems (e.g., the release of volatile organic compounds (VOCs)) and / or difficulties (such as, increased costs and / or lower productivity resulting from the use of methods for limiting VOC release).
[0003] WO 2015 / 125160 describes a bag for carrying water made of a laminate which in turn is made of a polyethylene terephthalate (PET) layer adhered to a polyolefin polymer layer using an adhesive composition which may be solvent-free.
[0004] It would be desirable to provide a method of making a zipper bag made from a laminate, wherein the method avoids the use of solvents to make the laminate, and wherein the laminate resists damage from the process of attaching a zipper structure to the laminate.
[0005] The following is a summary of the present invention.
[0006] A first aspect of the present invention is a method for forming a zipper bag, wherein the method comprises
[0007] A) forming a first laminate by a method comprising:
[0008] i) combining a polyisocyanate component and a polyol component to form an adhesive composition,
[0009] wherein the polyisocyanate component comprises a polyisocyanate prepolymer, and
[0010] wherein the polyol component comprises a phosphate functional compound,
[0011] wherein the adhesive composition comprises 0 wt % to 10 wt % of a solvent based on the weight of the adhesive composition,
[0012] wherein the adhesive composition comprises 0 wt % to 0.01 wt % of the silane compound based on the weight of the adhesive composition,
[0013] ii) applying a layer of the adhesive composition to the polyethylene terephthalate layer,
[0014] iii) then contacting the adhesive composition layer with a polyethylene layer having a thickness of 80 micrometers or more,
[0015] B) contacting the polymeric zipper structure with the first laminate at a temperature of 200°C or higher.
[0016] The second aspect of the present invention is a zipper bag manufactured by the method of the first aspect of the present invention.
[0017] The following is a brief description of the accompanying drawings.
[0018] Figure 1 is a top view of one embodiment of a zipper bag according to the present invention. Figure 2 is a cross section of a zipper construction of one embodiment of the zipper bag according to the present invention.
[0019] The following is a detailed description of the present invention.
[0020] As used herein, the following terms have the designated definitions unless the context clearly indicates otherwise.
[0021] As used herein, "isocyanate" is any compound containing two or more isocyanate groups. An isocyanate monomer is an isocyanate having a molecular weight of 550 or less. An aromatic isocyanate is an isocyanate containing one or more aromatic rings. Aliphatic isocyanates do not contain aromatic rings.
[0022] As used herein, a polyol is a compound having two or more hydroxyl groups. A polyol having exactly two hydroxyl groups is a diol, and a polyol having exactly three hydroxyl groups is a triol. The functionality of a polyol is the number of hydroxyl groups per molecule, represented by the letter "f". Polyester polyols are polyols having two or more ester bonds. Polyether polyols are polyols having two or more ether bonds. Polyester polyether polyols are polyols having both two or more ester bonds and two or more ether bonds. Polyester polyols or polyether polyols are typically present as a mixture of several compounds. The molecular weight of such a mixture is the number average molecular weight, and the functional group of such a mixture is the number average functionality.
[0023] Compounds having isocyanate groups can be characterized by the parameter "% NCO", which is the amount of isocyanate groups by weight, based on the weight of the compound. The parameter % NCO is measured by the method of ASTM D 2572-97 (2010).
[0024] A polymer is a molecule with a number average molecular weight of 10,000 Daltons or more. Polymers are made of bonded smaller units of polymerized units known as monomers. Polymers can be homopolymers, where all polymerized units are identical, or copolymers, where two or more different types of polymerized units are present. Polymers can be linear, branched, cross-linked, or a combination thereof.
[0025] Polyethylene is a polymer containing 75% or more of ethylene polymerized units, based on the weight of the polymer, as shown in structure I:
[0026]
[0027] Polyethylene terephthalate is a polymer containing 50% by weight or more, based on the weight of the polymer, of polymerized units having the structure of a monoester of terephthalic acid and ethylene glycol as shown in Structure II:
[0028]
[0029] Phosphate functional compounds are compounds having structure III:
[0030]
[0031] wherein R is any atom or group of atoms, including, for example, hydrogen, an organic group, an inorganic group, or any combination thereof.
[0032] A "film" is any structure that is 0.5 mm or less in one dimension and 1 cm or more in both other dimensions. A polymer film is a film made from a polymer or a polymer mixture.
[0033] The ratios presented herein are characterized as follows. For example, if a ratio is referred to as 3:1 or greater, then the ratio may be 3:1 or 5:1 or 100:1, but not 2:1. The characterization may be stated generally as follows. When a ratio is referred to herein as X:1 or greater, it is meant that the ratio is Y:1, where Y is greater than or equal to X. For another example, if a ratio is referred to as 15:1 or less, then the ratio may be 15:1 or 10:1 or 0.1:1, but may not be 20:1. In general, when a ratio is referred to herein as W:1 or less, it is meant that the ratio is Z:1, where Z is less than or equal to W.
[0034] The present invention relates to the use of an isocyanate component. The isocyanate component contains one or more isocyanate prepolymers, which are the reaction product of reactants ("prepolymer reactants") comprising at least one isocyanate monomer and at least one polyol. The at least one polyol contains one or more polyols selected from the group consisting of one or more polyester polyols, one or more polyether polyols, one or more polyether polyester polyols, and one or more mixtures thereof.
[0035] Suitable isocyanate monomers for prepolymer reactants can be selected from the group consisting of aromatic isocyanates, aliphatic isocyanates and / or combinations thereof. Examples of aromatic isocyanates suitable for use according to the present disclosure include, but are not limited to, isomers of methylene diphenyl diisocyanate ("MDI") (such as 4,4-MDI, 2,4-MDI and 2,2'-MDI) or modified MDI (such as carbodiimide-modified MDI or allophanate-modified MDI); isomers of toluene-diisocyanate ("TDI") (such as 2,4-TDI, 2,6-TDI), isomers of naphthalene diisocyanate ("NDI") (such as 1,5-NDI), and mixtures and / or combinations thereof. Examples of aliphatic isocyanates suitable for use in accordance with the present disclosure include, but are not limited to, isomers of hexamethylene diisocyanate ("HDI"), isomers of isophorone diisocyanate ("IPDI"), isomers of xylene diisocyanate ("XDI"), and combinations thereof. Preferred are aromatic isocyanate monomers.
[0036] The preferred amount of isocyanate monomer in the prepolymer reactant is at least 10 wt %, more preferably at least 20 wt %, more preferably at least 30 wt %, based on the total weight of the prepolymer reactant. The preferred amount of isocyanate monomer in the prepolymer reactant is no more than 80 wt %, more preferably no more than 70 wt %, more preferably no more than 65 wt %, based on the total weight of the prepolymer reactant.
[0037] The prepolymer reactant preferably contains one or more polyester polyols. The molecular weight of the preferred polyester polyol does not exceed 4,000 g / mol. The preferred polyester polyol has a hydroxyl functionality of at least 1.5 and not more than 3 (i.e., 1.5≤f≤3). Preferably, the polyester polyol has a viscosity of 2,000 mPa-s at 23° C., as measured by the method of ASTM D2196.
[0038] Suitable polyester polyols for prepolymer reactants are polycondensates of diols and optionally also higher polyols (e.g., triols, tetraols) and dicarboxylic acids and optionally also polycarboxylic acids (e.g., tricarboxylic acids, tetracarboxylic acids) or hydroxycarboxylic acids or lactones. Instead of free polycarboxylic acids, the polyester polyols can also be derived from the corresponding polycarboxylic anhydrides or the corresponding lower alcohol polycarboxylates.
[0039] Suitable glycols for preparing polyester polyols include, but are not limited to, ethylene glycol, butylene glycol, diethylene glycol, triethylene glycol, polyalkylene glycols (such as polyethylene glycol) and 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,6-hexanediol and neopentyl glycol. In order to achieve a polyester polyol functionality greater than 2, a polyol having a functionality of 3 may be optionally included in the adhesive composition (e.g., trimethylolpropane, glycerol, erythritol, pentaerythritol, trimethylolbenzene or trishydroxyethyl isocyanurate).
[0040] Suitable dicarboxylic acids for preparing polyester polyols include but are not limited to aliphatic acids, aromatic acids and / or combinations thereof. The example of suitable aromatic acids includes phthalic acid, isophthalic acid, terephthalic acid and tetrahydrophthalic acid. The example of aliphatic acids includes hexahydrophthalic acid, cyclohexanedicarboxylic acid, adipic acid, azelaic acid, sebacic acid, glutaric acid, tetrachlorophthalic acid, maleic acid, fumaric acid, itaconic acid, malonic acid, suberic acid, 2-methylsuccinic acid, 3,3-diethylglutaric acid, 2,2-dimethylsuccinic acid and trimellitic acid. As used herein, the term "acid" also includes any anhydride of the acid. In addition, monocarboxylic acids, such as benzoic acid and hexanecarboxylic acid, should be reduced or excluded from the disclosed composition as much as possible. Saturated aliphatic acids and / or aromatic acids are preferred, such as adipic acid or isophthalic acid.
[0041] Based on the total weight of the prepolymer reactant, the preferred amount of polyester polyol in the prepolymer reactant is more preferably at least 2wt%, more preferably at least 5wt%, more preferably at least 10wt%. Based on the total weight of the prepolymer reactant, the preferred amount of polyester polyol in the prepolymer reactant is no more than 45wt%, more preferably no more than 40wt%, more preferably no more than 35wt%.
[0042] The prepolymer reactant preferably comprises one or more polyether polyols. The molecular weight of the preferred polyether polyol does not exceed 5,000 g / mol. Preferably, the polyether polyol has a hydroxyl functionality of at least 1.5 and not more than 4 (i.e., 1.5≤f≤4). The preferred polyether polyol has a viscosity of 1,000 mPa-s or less at 23°C, as measured by the method of ASTM D2196.
[0043] Suitable polyether polyols for use in the prepolymer reactants are optionally polyaddition products of ethylene oxide, propylene oxide, tetrahydrofuran, butylene oxide, or co-addition or grafting products thereof, as well as polyether polyols obtained by condensation of polyols or mixtures thereof. Examples of suitable polyether polyols for use may include, but are not limited to, polypropylene glycol (PPG), polyethylene glycol (PEG), polybutylene glycol, and polytetramethylene ether glycol (PTMEG).
[0044] The preferred amount of polyether polyol in the prepolymer reactant is at least 5 wt%, more preferably at least 10 wt%, more preferably at least 25 wt%, based on the total weight of the prepolymer reactant. The preferred amount of polyether polyol in the prepolymer reactant is no more than 45 wt%, more preferably no more than 40 wt%, more preferably no more than 35 wt%, based on the total weight of the prepolymer reactant.
[0045] The prepolymer reactants may optionally further comprise one or more bio-based polyols, such as castor oil, one or more modified castor oils, or one or more other known bio-based polyols, or mixtures thereof. Preferred bio-based polyols have a hydroxyl functionality of at least 1.5 and not more than 4 (i.e., 1.5≤f≤4). Preferred bio-based polyols are modified castor oil.
[0046] When optionally included in the prepolymer reactant, the preferred amount of bio-based polyol in the isocyanate component is at least 0.3 wt%, more preferably at least 1 wt%, more preferably at least 3 wt%, by weight based on the total weight of the prepolymer reactant. When optionally included in the prepolymer reactant, the preferred amount of bio-based polyol in the prepolymer reactant is no more than 15 wt%, more preferably no more than 10 wt%, more preferably no more than 5 wt%, by weight based on the total weight of the prepolymer reactant.
[0047] Preferably, the NCO% of the isocyanate component is at least 3wt%, more preferably at least 5wt%, more preferably at least 7wt%. Preferably, the NCO% of the isocyanate component does not exceed 30wt%, more preferably does not exceed 25wt%, more preferably does not exceed 22wt%, more preferably does not exceed 20wt%.
[0048] Preferably, the isocyanate component has a viscosity of 300 to 20,000 mPa-s at 25°C as measured by the method of ASTM D2196.
[0049] The isocyanate component may optionally contain one or more catalysts. Suitable examples include, but are not limited to, dibutyltin dilaurate, zinc acetate, 2,2-dimorpholine diethyl ether, and combinations thereof.
[0050] The adhesive composition also contains a polyol component. The polyol component preferably contains a mixture of two or more polyols plus one or more phosphate functional compounds. Preferably, the polyol component contains one or more polyester polyols. Preferably, the amount of all polyester polyols is 10% or more by weight based on the weight of the polyol component; more preferably 20% or more. Preferably, the amount of all polyester polyols is 50% or less by weight based on the weight of the polyol component; more preferably 40% or less.
[0051] Preferably, the polyol component contains one or more polyether polyols. Preferably, the amount of all polyether polyols is 50% or more by weight based on the weight of the polyol component; more preferably 60% or more. Preferably, the amount of all polyester polyols is 90% or less by weight based on the weight of the polyol component; more preferably 80% by weight or less.
[0052] Preferably, the amount of the phosphate functional compound is 1% or more by weight based on the weight of the polyol component; more preferably 2% or more. Preferably, the amount of the phosphate functional compound is 15% or less by weight based on the weight of the polyol component; more preferably 10% or less;
[0053] Preferably, the weight ratio of the isocyanate component to the polyol component is 1:1 or higher, more preferably 1.5:1 or higher; more preferably 1.8:1 or higher. Preferably, the weight ratio of the isocyanate component to the polyol component is 5:1 or lower, more preferably 4.5:1 or lower, more preferably 4:1 or lower.
[0054] Preferably, the adhesive composition is solvent-free. As used herein, a solvent is a liquid at 25°C and is capable of forming a solution having an adhesive composition dissolved in the solvent such that the amount of the adhesive composition dissolved in the solvent is a compound or mixture of compounds of 10% by weight or more based on the weight of the solution. The adhesive composition is considered to be solvent-free herein if the total weight of all solvents in the adhesive composition is 10% or less by weight based on the weight of the adhesive composition. Preferably, the total weight of all solvents in the adhesive composition is 5% or less by weight based on the weight of the adhesive composition; more preferably 2% or less; more preferably 1% or less.
[0055] It is expected that the isocyanate component and the polyol component of the adhesive composition can be prepared separately and, if necessary, stored until the adhesive composition is desired to be used. In some embodiments, the isocyanate component and the polyol component are each liquid at 25°C. When it is desired to use the adhesive composition, the isocyanate component and the polyol component are contacted with each other and mixed together. It is expected that when the two components are contacted, the curing reaction begins, wherein the isocyanate group reacts with the hydroxyl group to form a carbamate chain segment. The adhesive composition formed by contacting the two components can be referred to as a "curable mixture".
[0056] A method for forming a laminate using an adhesive composition is also disclosed. In some embodiments, the adhesive composition (such as the adhesive composition discussed above) is liquid. In some embodiments, the composition is liquid at 25°C. Even if the composition is solid at 25°C, it is acceptable to heat the composition as needed to convert it into a liquid state or to heat the composition as needed to reduce the viscosity of the liquid adhesive composition. The composition layer is applied to the surface of the first film. In some embodiments, the thickness of the layer of the curable mixture is 1 to 5 microns.
[0057] In some embodiments, the surface of the second film is contacted with a layer of the curable mixture to form an uncured laminate. Preferably, the uncured laminate is made when the amount of unreacted polyisocyanate groups present in the adhesive composition is more preferably at least 50%, more preferably at least 75%, more preferably at least 90% on a molar basis compared to the amount of polyisocyanate groups present in the isocyanate component prior to contact with the polyol component. Preferably, the uncured laminate is made when the amount of unreacted polyisocyanate groups present in the curable mixture is less than 100%, more preferably less than 97%, more preferably less than 95%.
[0058] The curable mixture is then cured or allowed to cure. The uncured laminate may be subjected to pressure, for example by passing through nip rollers, which may or may not be heated. The film optionally has a surface printed with an image with ink; the ink may be in contact with the adhesive composition.
[0059] The composition of the first film includes polyethylene terephthalate (PET). PET can be a homopolymer in which all polymerized units have structure II, or PET can be a copolymer in which some polymerized units have structures other than structure II. Some suitable comonomers are, for example, monoesters of a diacid and a diol, in which the diacid is different from terephthalic acid, or the diol is different from ethylene glycol, or the diacid is different from terephthalic acid and the diacid is different from ethylene glycol. Some suitable diacids include, for example, phthalic acid, isophthalic acid, and mixtures thereof. Some suitable diols include, for example, olefin diols other than ethylene glycol. Preferably, the amount of polymerized units in PET having structure II is 75% or more by weight based on the weight of PET; more preferably 85% or more; more preferably 95% or more.
[0060] Preferably, the amount of PET in the first film is 60% or more by weight based on the weight of the first film; more preferably 80% or more; more preferably 90% or more; more preferably 95% or more.
[0061] The second film comprises polyethylene (PE). PE may be linear or branched. PE may be chlorinated, sulfonated and / or cross-linked. Preferably, PE is not chlorinated. Preferably, PE is not sulfonated. Preferably, PE is not cross-linked.
[0062] PE may be a homopolymer, in which all polymerized units have structure I, or PE may be a copolymer. Suitable comonomers include, for example, unsaturated olefins (including dienes) other than ethylene and unsaturated esters. Unsaturated esters have structure R 1 -C(O)OR 2 , where R 1 and / or R 2 One or both of them contain carbon-carbon double bonds. Some suitable unsaturated esters include, for example, vinyl esters, acrylates, and mixtures thereof. Vinyl esters in R 1 contains one or more carbon-carbon double bonds and includes, for example, vinyl acetate. Acrylates in R 2 The PE has one or more carbon-carbon double bonds, and includes, for example, acrylic acid, methacrylic acid, alkyl esters of acrylic acid or methacrylic acid, and mixtures thereof. Preferably, the amount of polymerized units in the PE having structure I is 75% or more by weight based on the weight of the PE; more preferably 85% or more; more preferably 95% or more.
[0063] Preferably, the amount of PE in the second film is 50% or more by weight based on the weight of the second film; more preferably 75% or more; more preferably 90% or more; more preferably 95% or more.
[0064] The laminate is used to make zipper bags. Zipper bags can have any shape. Zipper bags include a zipper structure that allows the bag to be opened and closed multiple times. Figure 1 One embodiment of a zipper bag 1 is shown in FIG. In the embodiment shown, the zipper bag has an opening 2 along the top edge; sealed sides 4 and bottom 5; and the bag can be opened and then closed using a zipper structure 3. A suitable method of making the illustrated embodiment is to form two rectangles of the same size of the laminate of the present invention, as described above. The two rectangles can have the same composition or can be different. Preferably, the two rectangles have the same composition as each other. The two rectangles can be brought into contact with all edges of one rectangle against the edge of the other rectangle; then, the sides 4 or bottom 5 can be sealed, for example, by heat sealing. The zipper structure can then be placed between the two rectangles of the laminate and then bonded in place, for example, by applying heat and pressure.
[0065] Figure 2A cross section of a bag 1 is shown, and an embodiment of a zipper structure 3 is shown. The zipper structure 3 is located between an upper layer 10 of a laminate and a lower layer 11 of a laminate. The zipper structure 3 includes a pocket 6 and a track 7. In some embodiments, the pocket 6 is extruded, and the track 7 is also extruded, wherein the extrusion direction is perpendicular to the Figure 2 The track 7 and the bag 6 may each independently be of uniform composition, or the composition of either or both of the bag 6 and the track 7 may vary in the direction of extrusion. Preferably, the track is sufficiently rigid, and the bag is sufficiently flexible, that the track can be pulled out of the bag and then reinserted into the bag with only hand pressure, and these operations can be performed multiple times without damaging the zipper structure. The bag is bonded to the top laminate 10, and the track is bonded to the bottom laminate 11.
[0066] In some embodiments, the zipper structure will include two or more tracks and a bag structure where the tracks are parallel to each other. In some embodiments, the bottom 5 of the bag will have an additional laminate (not shown) bonded to the top laminate 10 and the bottom laminate 11 to form a gusset that allows the bag to stand upright so that the bag stands upright on the gusseted bottom 5 resting on a horizontal surface.
[0067] Regardless of the other details of how the zipper bag is constructed, the step of bonding the zipper structure to the laminate is preferably performed by applying pressure to force the zipper structure against the laminate while exposing the assembly so formed to a temperature of: 200° C. or higher; more preferably 220° C. or higher; more preferably 240° C. or higher. The zipper structure may be bonded to both the top laminate and the bottom laminate at the same time, or the zipper structure may be bonded to the first laminate and then to the other laminate.
[0068] The following are examples of the present invention. Unless otherwise stated, operations were carried out at room temperature (approximately 23°C).
[0069] Lamination was done manually using a K-bar coater and a hot roll laminator.
[0070] The processing conditions for lamination with solvent-based adhesives (adhesives with more than 10% solvent by weight) are as follows. The adhesive is coated on the printed PET and then laminated with PE; thereafter, it is immediately dried by a hot air gun (temperature 60°C-80°C) and laminated using a hot roll laminator and then cured at room temperature (25°C-35°C) for 24 hours. The adhesive coating weight obtained is 1.9+ / -0.2 grams per square meter (GSM). Lamination is carried out at a roll temperature of 60°C. The roll pressure is 4.0 bar and the roll speed is a machine setting of 5.0.
[0071] The processing conditions for laminating with solvent-free adhesive are as follows. The isocyanate component and the polyol component are heated in separate reservoirs of a metering and mixing distributor (isocyanate at 48°C, polyol at 38°C). The adhesive is then transported to a static mixer via a heated hose (40°C), whereby the isocyanate and polyol are uniformly mixed before the resulting mixture is distributed between heated adhesive sheet rollers. The heated adhesive is applied to the film using a coating roller, followed by another film roll (lamination) on a hot press roller. The adhesive is applied to printed PET, then laminated with PE, and cured under 50°C hot room conditions. The metering roller is at -40°C, and the coating roller is at 47°C, and the laminating roller is at 50°C. The mixing ratio of the isocyanate component to the polyol component is 100 parts by weight of the isocyanate component and 42 to 43 parts by weight of the polyol component. When the PE is 80 microns thick, the coating weight is 1.9 to 2.1 GSM; when it is 130 microns thick, the coating weight is 2.2 to 2.4 GSM.
[0072] Laminates used for laboratory testing in the form of laminated sheets were allowed to stand at 50°C for 24 hours before testing. Those laminates to be made into bags were allowed to stand at 50°C for 4 days before being made into bags.
[0073] The laminates were tested as follows.
[0074] Adhesive Strength: To determine the adhesive strength, 15 mm or 25 mm wide strips of the test laminate were cut. These strips were immersed in an ethyl acetate solvent, in which the adhesive dissolved. These strips were then separated and the samples were tested on a universal testing machine (UTM). The maximum force required to separate the two layers is referred to as the adhesive strength. Test conditions: 25 mm jaw length, test speed 100 mm / min, test unit: grams / 15 mm or 25 mm width, under ambient conditions.
[0075] Seal Strength: 15mm or 25mm wide strips of the test laminate were cut. These strips were tested on a Universal Testing Machine (UTM). The maximum force required to break the specimen is called the seal strength. Test conditions: 25mm jaw length, test speed 150mm / min, test unit: kg / 15 or 25mm, pressure: 3.0kg / cm 2 , temperature: 150℃.
[0076] Heat Resistance Test: Cut rectangular strips, approximately 100 to 150 mm on each side. Subject the laminate to the heat seal jaws of a sealing machine from 150°C to 260°C in 10°C increments or until the laminate breaks. Visual observations are then made for piping / tunneling / bubbling or other physical deformities. Test Conditions: 0.5-1.0 second dwell time, 3.0 kg / cm2 pressure. Ambient conditions (25°C to 35°C). Samples without physical deformities are considered "passed". Report the highest temperature the laminate passed.
[0077] The materials used are as follows: Adhesives with labels ending in "C" are comparative. "Adh." means "Adhesive." "Promoter" means "Adhesion Promoter." "Phosphorylated?" means "Is there a phosphate functional compound in the polyol component?"
[0078] <![CDATA[ Adh ]]> <![CDATA[ Isocyanate component ]]> <![CDATA[ Polyol components ]]> <![CDATA[ Phosphorylation? ]]> <![CDATA[ Solvent wt% ]]> <![CDATA[ Accelerator ]]> A1 <![CDATA[PACACEL (TM) 968 (1) ]]> <![CDATA[PacAcel (TM) C108 (1) ]]> yes none Non-Si A2C <![CDATA[MORFREE (TM) MF698A (1) ]]> <![CDATA[MORFREE (TM) C411 (1) ]]> none none Non-Si A3C <![CDATA[MORFREE (TM) 899 (1) ]]> <h2 style=";text-align:left;direction:ltr"><![CDATA[MORFREE <h2 style=";text-align:left;direction:ltr"> (TM) <h2 style=";text-align:left;direction:ltr"> C99<h2 style=";text-align:left;direction:ltr"> (1) <h2 style=";text-align:left;direction:ltr"> ]]><h2 style=";text-align:left;direction:ltr"> none none Non-Si A4C <![CDATA[ADCOTE (TM) Cat-F (1) ]]> <![CDATA[ADCOTE (TM) 545EA (1) ]]> none >20% Non-Si A5C <![CDATA[ADCOTE (TM) Cat-F (1) ]]> <![CDATA[ADCOTE (TM) 811A (1) ]]> none >20% Si A6C <![CDATA[Henkel 1511A (2) ]]> <![CDATA[Henkel 2511 (2) ]]> none >20% unknown A7C <![CDATA[Henkel 7720 (2) ]]> <![CDATA[Henkel 6028 (2) ]]> none none unknown A8C <![CDATA[CA-7918 (3) ]]> <![CDATA[SF-7660 (3) ]]> none none unknown
[0079] (1) Dow Chemical Company
[0080] (2) Henkel Corporation
[0081] (3) Coim Company (weight ratio of isocyanate component to polyol component is 0.7:1)
[0082] It is believed that comparative adhesives A6C, A7C or A8C do not contain phosphate functional compounds.In all of Examples A1, A2C, A3C, A4C, A5C, A6C and A7C, the weight ratio of the isocyanate component to the polyol component is 1:1 or greater.
[0083] The first test was performed using PET 12 micron thick and PE 130 micron thick. The samples were cured for 48 hours at ambient conditions (25°C to 30°C). The bond strength samples were 15 mm wide.
[0084] Table 1: Results of the first test
[0085] <![CDATA[ Example ]]> <![CDATA[ Adhesion strength (g) ]]> <![CDATA[ Sealing strength(kg) ]]> <![CDATA[ Heat resistance ]]> A1 550-657 5.5-6.3 260℃ A2C 468-531 5.4-5.9 240℃ A3C 400-439 4.7-4.9 220℃ A4C 550-590 5.5-5.8 260℃ A5C 610-645 5.8-6.4 260℃
[0086] The results show that the inventive working example A1 performs better in all measurements than the solvent-free comparative samples A2C and A3C. The solvent-only based samples A4C and A5C also perform as well as or better than the working example A1.
[0087] A second test was performed using PE of varying thickness. PET was printed and PE was white with a thickness of 12 microns. The test strip was 15 mm wide. "Str" means "Strength". "CF" means "Cohesive Failure". "PT" means "PET Tear", which indicates the mode of failure during the adhesive strength test. "ND" means "Not Tested".
[0088] Table 2: Strength results of the second test
[0089]
[0090] The samples from the second test were also tested for heat resistance.At each test temperature, the laminates were observed and given a rating of 1 (poor) to 5 (excellent).
[0091] Table 3: Heat resistance results of the second test (rating)
[0092]
[0093] The results in Tables 2 and 3 show that the working examples of the present invention performed better in all tests than all other samples except solvent-based adhesive A5C. That is, A1 outperformed all other solvent-free adhesives.
[0094] Gas chromatography was performed on two laminate samples from the second test to determine the amount of solvent remaining in the laminate. Four replicates were run on each sample and the average values are reported below.
[0095] Table 4: Solvent retention by gas chromatography analysis
[0096] <![CDATA[ Example ]]> <![CDATA[ Solvent concentration (mg / m 2 ) ]]> A1 2.3 A6C 5.2
[0097] The results in Table 4 show that solvent-free adhesive A1 resulted in a laminate with less residual solvent than solvent-based adhesive A6C.
Claims
1. A method for preparing a zipper bag, wherein the method comprises: A) forming a first laminate by a method comprising: i) combining a polyisocyanate component and a polyol component to form a solvent-free adhesive composition, wherein the polyisocyanate component comprises a polyisocyanate prepolymer, and wherein the polyol component comprises from 1 wt % to 15 wt % of a phosphate functional compound, based on the weight of the polyol component, The weight ratio of the polyisocyanate component to the polyol component in the adhesive composition is 1.5:1 to 4.5:1, ii) applying a layer of said adhesive composition to a layer of polyethylene terephthalate, iii) then contacting said layer of said adhesive composition with a polyethylene layer having a thickness of 80 micrometers or more, B) contacting a polymer zipper structure comprising a pocket and a track with the first laminate at a temperature of 200°C or higher.
2. The method of claim 1, wherein the polyol component further comprises 10 to 50 wt % of one or more polyester polyols, based on the weight of the polyol component, and 50 to 90 wt % of one or more polyether polyols, based on the weight of the polyol component.
3. The method of claim 2, wherein the method comprises the additional step of contacting the zipper structure with a second laminate at a temperature of 200° C. or higher, wherein the second laminate is formed by a method comprising the steps of: i) combining a polyisocyanate component and a polyol component to form a solvent-free adhesive composition, wherein the polyisocyanate component comprises a polyisocyanate prepolymer, and wherein the polyol component comprises from 1 wt % to 15 wt % of a phosphate functional compound based on the weight of the polyol component, The weight ratio of the polyisocyanate component to the polyol component in the adhesive composition is 1.5:1 to 4.5:1, ii) applying a layer of said adhesive composition to a layer of polyethylene terephthalate, iii) then contacting said layer of said adhesive composition with a polyethylene layer having a thickness of 80 micrometers or more, The second laminate may have the same composition as the first laminate or may have a different composition than the first laminate.
4. A zipper bag manufactured by the method according to claim 1.
Citation Information
Patent Citations
Phosphate adhesion promoters