tire
By optimizing the proportion of isoprene structural rubber, modified SBR, silica filler with moderate nitrogen adsorption specific surface area, and hydrogenated resin in the rubber composition, the difficulty in achieving the balance between wet grip and rolling resistance in the existing technology is solved. problem, improving the tire's grip performance and wear resistance.
Patent Information
- Application Number
- CN202080087337.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-19
- Filing Date
- 2020-09-30
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Existing rubber compositions are difficult to achieve a balance between improving wet grip and reducing rolling resistance, and have problems with reduced elastic modulus and insufficient wear resistance.
A rubber composition containing a rubber with an isoprene structure, a modified SBR with a low bound styrene content, a silica filler with a nitrogen adsorption specific surface area of 130m2/g to 330m2/g, a hydrogenated resin and carbon black is used. Optimize the proportion and structure of these ingredients to improve the compatibility and strength of the rubber.
It achieves excellent wet grip and low rolling resistance of the tire, while improving the mechanical strength and wear resistance of the tire.
Smart Images

Figure BDA0003695965330000081 
Figure BDA0003695965330000101 
Figure BDA0003695965330000102
Abstract
Description
Technical Field
[0001] The present invention relates to tires. Background Art
[0002] From the viewpoint of improving vehicle safety, various studies have been conducted to improve the braking performance and driving performance of tires on dry roads and various roads such as wet roads, ice and snow roads, etc. For example, as a rubber composition capable of producing a tread rubber having high braking performance on dry roads and even on wet roads such as manholes that are more prone to slipping than asphalt, a rubber composition is disclosed, which is prepared by mixing a rubber component (A) including 70% by mass or more of a natural component, and mixing 5 to 50 parts by mass of at least one thermoplastic resin (B) selected from C5-based resins, C5 to C9-based resins, C9-based resins, terpene-based resins, terpene aromatic compound-based resins, rosin-based resins, dicyclopentadiene resins, and alkylphenol-based resins with respect to 100 parts by mass of the rubber component, and wherein the silica content in the filler (C) is 50% to 100% by mass (see, for example, PTL 1).
[0003] In addition, as a rubber composition for tires capable of improving grip performance on dry roads without impairing grip performance on wet roads, a rubber composition for tires is disclosed, which comprises: relative to 100 parts by mass of a diene rubber component including 70 parts by mass or more of styrene-butadiene rubber having a styrene content percentage of 20% to 60% by mass in the rubber component, each filler from a filler group comprises 50 to 300 parts by mass of silica, 0 to 150 parts by mass of an inorganic agent represented by the general formula: mM1·xSiOy·zH2O, and 0 to 150 parts by mass of carbon black, so that the total amount of silica and the inorganic agent is 200 to 350 parts by mass, and the total amount of silica, the inorganic agent, and the carbon black is 200 to 350 parts by mass, the rubber composition for tires comprises a softener in an amount of 70% by mass or more relative to the total amount of the filler, and further comprises 5 to 60 parts by mass of at least one of resins having a softening point of 145°C or less (see, for example, PTL 2).
[0004] Reference List
[0005] Patent Literature
[0006] PTL 1: WO 2015 / 079703
[0007] PTL 2: JP 2008-184505 A Summary of the invention
[0008] Problem that the invention aims to solve
[0009] However, in the rubber compositions disclosed in PTL 1 and PTL 2, there is a need to further improve the balance between the increase in wet grip performance and the reduction in rolling resistance.
[0010] An object of the present invention is to provide a tire having excellent wet grip and low rolling resistance, and the present invention is intended to achieve this object.
[0011] Solutions for solving problems
[0012] <1> A tire obtained by using a rubber composition,
[0013] The rubber composition comprises:
[0014] A rubber component comprising a rubber having an isoprene structure and an aminoalkoxysilane-modified styrene-butadiene rubber having a bound styrene amount of 15% or less;
[0015] Filler, comprising a nitrogen adsorption specific surface area (BET method) of 130 m 2 / g or more and less than 330m 2 / g of silica, and the amount of the filler is 40 to 125 parts by mass relative to 100 parts by mass of the rubber component; and
[0016] The hydrogenated resin has a softening point higher than 110° C. and a weight average molecular weight of 200 to 1200 g / mol in terms of polystyrene, and the amount of the hydrogenated resin is 5 to 50 parts by mass based on 100 parts by mass of the rubber component.
[0017] <2> according to <1> The tire, wherein the content of the modified styrene-butadiene rubber in the rubber component is 10 mass % to 90 mass %.
[0018] <3> according to <1> or <2> The tire, wherein the content of the rubber having an isoprene structure in the rubber component is 10 mass % to 90 mass %.
[0019] <4> according to <1> to <3> The tire described in any one of the preceding claims, wherein the rubber component further comprises a modified styrene-butadiene rubber having a bound styrene amount of 30% or more.
[0020] <5> according to <1> to <4> The tire described in any one of the preceding claims, wherein the filler further contains carbon black, and the content of the silica in the filler is 70% by mass or more.
[0021] <6> according to <1> to <5> The tire described in any one of the preceding claims, wherein the hydrogenated resin is at least one selected from the group consisting of hydrogenated C5-based resins, hydrogenated C5-C9-based resins, and hydrogenated dicyclopentadiene-based resins.
[0022] <7> according to <1> to <6> The tire described in any one of the preceding claims, wherein the rubber composition further comprises a silane coupling agent having a mercapto group.
[0023] Effects of the Invention
[0024] According to the present invention, it is possible to provide a tire having excellent wet grip and low rolling resistance. DETAILED DESCRIPTION
[0025] <Rubber Composition>
[0026] The rubber composition according to the present invention comprises:
[0027] A rubber component comprising a rubber having an isoprene structure and an aminoalkoxysilane-modified styrene-butadiene rubber having a bound styrene amount of 15% or less;
[0028] Filler, comprising a nitrogen adsorption specific surface area (BET method) of 130 m 2 / g or more and less than 330m 2 / g of silica, and the amount of the filler is 40 to 125 parts by mass relative to 100 parts by mass of the rubber component; and
[0029] The hydrogenated resin has a softening point higher than 110° C. and a weight average molecular weight of 200 to 1200 g / mol in terms of polystyrene, and the amount of the hydrogenated resin is 5 to 50 parts by mass based on 100 parts by mass of the rubber component.
[0030] "Styrene-butadiene rubber modified with aminoalkoxysilane having a bound styrene content of 15% or less" may be referred to as "modified SBR having a low bound styrene content". In addition, "a hydrogenated resin having a softening point of more than 110°C and a weight average molecular weight of 200 to 1200 g / mol in terms of polystyrene" may be referred to as "the hydrogenated resin of the present invention".
[0031] In addition, the nitrogen adsorption specific surface area (BET method) is a nitrogen adsorption method specific surface area (N2SA) measured according to the BET method defined in ASTM D4567-03 (2007), and may be referred to as a "BET specific surface area".
[0032] In the prior art, wet grip has been improved by inorganic fillers such as silica. However, such fillers have the problem of increased energy loss. In addition, research has been conducted to provide a rubber composition for tire treads, which achieves an excellent balance between wet grip performance and low rolling resistance performance without compromising the wear resistance of the tire by blending rubbers with different glass transition temperatures (Tg); however, there are also disadvantages in terms of low loss and wear resistance.
[0033] In addition, in recent years, various studies have been conducted on mixing a large amount of thermoplastic resin in a rubber composition, mixing a high silica ratio in a filler material, and mixing by using a modified polymer with highly dispersed silica, etc.; however, the trade-off solution is limited. In particular, in the technology of mixing a large amount of a softener including a thermoplastic resin, there is also a problem of a decrease in the elastic modulus of the rubber.
[0034] In contrast, since the rubber composition according to the present invention has the above-mentioned constitution, the tire obtained from the rubber composition according to the present invention has excellent wet grip and low rolling resistance.
[0035] The reason for this is not clear; however, it is speculated that this phenomenon is caused by the following reasons.
[0036] The weight average molecular weight of the hydrogenated resin of the present invention is 1200 or less in terms of polystyrene conversion, and since the hydrogenated resin has a low molecular weight, it is highly compatible with the rubber component. In addition, since the hydrogenated resin of the present invention has a high softening point, it is believed that the hydrogenated resin reinforces the rubber component and increases the elastic modulus of the vulcanized rubber, and it is presumed that the rolling resistance of the tire is reduced. At the same time, the hydrogenated resin of the present invention can impart the tire with the flexibility required for road grip due to its high compatibility, and it is believed that the grip on a slippery road surface, i.e., wet grip, can be improved.
[0037] Since the styrene-butadiene rubber included in the rubber composition according to the present invention is modified, the styrene-butadiene rubber has a high interaction with the silica as a reinforcing filler, and since the bound styrene amount is 15% or less and the elastic modulus of the tire is not excessively increased, it is considered that the wet grip is further improved. On the other hand, since the nitrogen adsorption specific surface area (BET method) of silica is 130 m 2 / g or more and less than 330m 2 / g and has a small particle size, it is believed that silica improves the strength of the tire and further reduces rolling resistance. In addition, since the rubber composition according to the present invention includes a rubber having an isoprene structure, it is believed that the rubber composition improves the mechanical strength of the tire and also has excellent wear resistance.
[0038] From the above, it is considered that the tire obtained from the rubber composition of the present invention has excellent wet grip performance and low rolling resistance.
[0039] In the following description, the rubber composition according to the present invention will be described in detail.
[0040] [Rubber component]
[0041] The rubber component contains a rubber having an isoprene structure and an aminoalkoxysilane-modified styrene-butadiene rubber having a bound styrene content of 15% or less (modified SBR having a low bound styrene content).
[0042] The rubber component may further include a rubber component other than the rubber having an isoprene structure and the modified SBR having a low bound styrene amount, for example, a modified styrene-butadiene rubber having a bound styrene amount of 30% or more.
[0043] (Rubber with isoprene structure)
[0044] Since the rubber component contains a rubber having an isoprene structure, the breaking strength of the vulcanized rubber can be increased. As a result, the rolling resistance of the tire can be reduced, and the wear resistance of the vulcanized rubber is excellent.
[0045] Examples of the rubber having an isoprene structure include natural components (NR) and polyisoprene rubber (IR).
[0046] The content of rubber having an isoprene structure in the rubber component further reduces the rolling resistance of the tire, and from the viewpoint of improving the wear resistance of the vulcanized rubber, the rubber content is preferably 10% to 90% by mass, more preferably 20% to 70% by mass, even more preferably 30% to 65% by mass, still more preferably 35% to 60% by mass, and even more preferably 41% to 57% by mass.
[0047] (Modified styrene-butadiene rubber)
[0048] The rubber component contains an aminoalkoxysilane-modified styrene-butadiene rubber having a bound styrene content of 15% or less (modified SBR having a low bound styrene content).
[0049] The bound styrene amount of the styrene-butadiene rubber means the ratio of styrene units included in the styrene-butadiene rubber.
[0050] When the rubber component contains a modified SBR with a low bound styrene amount, excellent wet grip is obtained. The bound styrene amount of the modified SBR with a low bound styrene amount is preferably 14% or less, more preferably 13% or less, and even more preferably 12% or less. In addition, the bound styrene amount of the modified SBR with a low bound styrene amount is preferably 5% or more, more preferably 7% or more, and even more preferably 8% or more.
[0051] From the viewpoint of improving wet grip and further reducing rolling resistance, the content of the modified SBR having a low bound styrene amount in the rubber component is preferably 10% by mass to 90% by mass, more preferably 15% by mass to 70% by mass, even more preferably 20% by mass to 60% by mass, still more preferably 23% by mass to 58% by mass, even more preferably 28% by mass to 53% by mass, still more preferably 28% by mass to 48% by mass, and even more preferably 31% by mass to 45% by mass.
[0052] It is preferred that the rubber component further contains a modified styrene-butadiene rubber having a bound styrene amount of 30% or more (hereinafter, may be referred to as "modified SBR having a high bound styrene amount").
[0053] Since the rubber component further contains a modified SBR having a high bound styrene amount in addition to the modified SBR having a low bound styrene amount, the rolling resistance can be further reduced.
[0054] From the viewpoint of further reducing rolling resistance, the bound styrene amount of the modified SBR having a high bound styrene amount is more preferably 35% or more, even more preferably 38% or more, and still more preferably 39% or more. In addition, the bound styrene amount of the modified SBR having a high bound styrene amount is more preferably 60% or less, even more preferably 50% or less, still more preferably 45% or less, even more preferably 43% or less, and still more preferably 42% or less.
[0055] When the rubber component contains a modified SBR having a high bound styrene amount, the ratio of natural component / modified SBR having a low bound styrene amount / modified SBR having a high bound styrene amount is preferably 20 to 70 / 15 to 65 / 5 to 50, more preferably 20 to 50 / 20 to 55 / 5 to 40, and even more preferably 30 to 50 / 30 to 55 / 15 to 40 on a mass basis from the viewpoint of respectively improving rolling performance, wet performance and wear performance.
[0056] The bound styrene amount of the modified SBR can be adjusted by the amount of the monomer used for polymerization of the modified SBR and the degree of polymerization, etc. In addition, the bound styrene amount of the modified SBR can be determined by an infrared method (Morero method).
[0057] Incidentally, the bound styrene amount and the bound vinyl amount of a polymer such as modified SBR may be referred to as the microstructure of the polymer.
[0058] Aminoalkoxysilane modification is a general term for modification groups each having a functional group including at least one nitrogen atom and at least one alkoxysilane group. In the following description, a functional group including at least one nitrogen atom may be referred to as a nitrogen atom-containing group.
[0059] It is preferred that the functional group including at least one nitrogen atom (nitrogen atom-containing group) is selected from the following.
[0060] That is, it is preferred that the nitrogen atom-containing group is a monovalent group having a functional group selected from the group consisting of a primary amino group, a primary amino group protected with a hydrolyzable protecting group, an onium salt residue of a primary amine, an isocyanate group, a thioisocyanate group, an imine group, an imine residue, an amide group, a secondary amino group protected with a hydrolyzable protecting group, a cyclic secondary amino group, an onium salt residue of a cyclic secondary amine, a non-cyclic secondary amino group, an onium salt residue of a non-cyclic secondary amine, an isocyanurate triester residue, a cyclic tertiary amino group, a non-cyclic tertiary amino group, a nitrile group, a pyridine residue, an onium salt residue of a cyclic tertiary amine, and an onium salt residue of a non-cyclic tertiary amine.
[0061] The group containing nitrogen atoms may further include at least one selected from the group consisting of a hydrocarbon group and a heteroatom. Here, the hydrocarbon group may be a monovalent hydrocarbon group having 1 to 30 carbon atoms and including a straight chain, a branched chain, an alicyclic ring or an aromatic ring. In addition, the heteroatom may be at least one heteroatom selected from the group consisting of an oxygen atom, a sulfur atom, and a phosphorus atom.
[0062] The modified site of the aminoalkoxysilane-modified SBR having a bonded styrene content of 15% or less may be the molecular terminal as described above, or may be the main chain.
[0063] According to the methods described in, for example, WO 2003 / 046020 and JP 2007-217562 A, SBR having modified molecular terminals can be produced by reacting various modifiers with the terminals of SBR having active terminals.
[0064] According to one suitable embodiment, according to the method described in WO 2003 / 046020 and JP 2007-217562 A, an aminoalkoxysilane-modified SBR in which the amount of bound styrene having been modified at the molecular terminal is 15% or less can be produced by reacting the terminal of SBR having an active terminal and an amount of cis-1,4-bonds of 75% or more with an aminoalkoxysilane compound and then reacting the terminal with a carboxylic acid partial ester of a polyol to stabilize the terminal.
[0065] The carboxylic acid partial ester of a polyol is an ester of a polyol and a carboxylic acid, and means a partial ester having one or more hydroxyl groups. Specifically, it is preferred to use an ester of a sugar or modified sugar having 4 or more carbon atoms and a fatty acid. The ester may more preferably be: (1) a fatty acid partial ester of a polyol, in particular a partial ester of a saturated higher fatty acid or unsaturated higher fatty acid having 10 to 20 carbon atoms and a polyol (which may be any of a monoester, a diester, and a triester); and (2) an ester compound obtained by bonding 1 to 3 units of a partial ester of a polycarboxylic acid and a higher alcohol to a polyol; etc.
[0066] As for the polyol used as a raw material of the partial ester, it is preferred to use a sugar having 5 or 6 carbon atoms and having at least 3 hydroxyl groups (which may be hydrogenated or unhydrogenated), a diol, and a polyol, etc. In addition, the raw material fatty acid is preferably a saturated or unsaturated fatty acid having 10 to 20 carbon atoms, and, for example, stearic acid, lauric acid, and palmitic acid are used.
[0067] Among the fatty acid partial esters of polyols, sorbitan fatty acid esters are preferred, and specific examples thereof include sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan tristearate, sorbitan monooleate, and sorbitan trioleate.
[0068] The aminoalkoxysilane compound is not particularly limited; however, it is more preferred that the aminoalkoxysilane compound is an aminoalkoxyalkoxysilane compound represented by the following general formula (i).
[0069] R 11 a -Si-(OR 12 ) 4-a (i)
[0070] In the general formula (i), R 11 and R 12 Each independently represents a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms; R 11 and R 12 At least one of them is substituted with an amino group; a is an integer from 0 to 2; when there are multiple OR 12 When each OR 12 may be the same as or different from each other; and active protons are not included in the molecule.
[0071] It is preferred that the modifying group having at least one nitrogen atom-containing functional group, at least one alkoxy group, and at least one silane atom is more specifically a modifying group derived from a hydrocarbyloxysilane compound represented by the following general formula (II).
[0072]
[0073] In the general formula (II), n1+n2+n3+n4=4 (provided that n2 represents an integer of 1 to 4; and n1, n3 and n4 each represent an integer of 0 to 3); A 1 represents at least one functional group selected from a saturated cyclic tertiary amine compound residue, an unsaturated cyclic tertiary amine compound residue, a ketimine residue, a nitrile group, a (thio)isocyanate group (representing an isocyanate group or a thioisocyanate group; hereinafter, the same), a (thio)epoxy group, a trialkyl isocyanurate group, a dialkyl carbonate group, a nitrile group, a pyridine group, a (thio)keto group, a (thio)aldehyde group, an amide group, a (thio)carboxylate group, a metal salt of a (thio)carboxylate, a carboxylic anhydride residue, a carboxylic acid halogen compound residue, and a primary or secondary amino group or a mercapto group having a hydrolyzable group. When n4 is 2 or more, A 1 Can be the same or different; A 1 It can be a divalent group that combines with Si and forms a ring structure; R 21 represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and when n1 is 2 or more, R 21 Can be the same or different; R 23 represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, or a halogen atom (fluorine, chlorine, bromine or iodine), when n3 is 2 or more, R 23 Can be the same or different; R 22 represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, all of which may contain nitrogen atoms and / or silicon atoms. When n2 is 2 or more, R 22 may be the same or different from each other, or R 22 can combine together to form a ring; R 24 represents a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and when n4 is 2 or more, R 24 Can be the same or different.
[0074] The hydrolyzable group in the primary or secondary amino group having a hydrolyzable group or the mercapto group having a hydrolyzable group is preferably a trimethylsilyl group or a tert-butyldimethylsilyl group, and particularly preferably a trimethylsilyl group.
[0075] Incidentally, according to the present invention, "a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms" means "a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms or a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms". The same applies to the case of a divalent hydrocarbon group.
[0076] As a specific example of the hydrocarbyloxysilane compound represented by the general formula (II), [N,N-bis(trimethylsilyl)-(3-amino-1-propyl)](methyl)(diethoxy)silane may be suitably mentioned.
[0077] In addition, it is more preferable that the hydrocarbyloxysilane compound represented by the general formula (II) is a hydrocarbyloxysilane compound represented by the following general formula (III).
[0078]
[0079] In the general formula (III), p1+p2+p3=2 (provided that p2 represents an integer from 1 to 2; and p1 and p3 each represent an integer from 0 to 1); and A 2 R represents NRa (Ra represents a monovalent hydrocarbon group, a hydrolyzable group, or a nitrogen-containing organic group. The hydrolyzable group is preferably a trimethylsilyl group or a tert-butyldimethylsilyl group, and particularly preferably a trimethylsilyl group), or sulfur. 25 R represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 27 R represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, or a halogen atom (fluorine, chlorine, bromine or iodine). 26 represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, or a nitrogen-containing organic group, all of which may contain nitrogen atoms and / or silicon atoms, and when p2 is 2, R 26 may be the same or different from each other, or R 26 Can combine together to form a ring. 28 It represents a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms.
[0080] In addition, it is more preferred that the hydrocarbyloxysilane compound represented by the general formula (II) is a hydrocarbyloxysilane compound represented by the following general formula (IV) or (V).
[0081]
[0082] In the general formula (IV), q1+q2=3 (provided that q1 represents an integer of 0 to 2; and q2 represents an integer of 1 to 3). 31 R represents a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 32 and R 33Each independently represents a hydrolyzable group, a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 34 represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and when q1 is 2, R 34 Can be the same or different. 35 represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and when q2 is 2 or more, R 35 Can be the same or different.
[0083]
[0084] In the general formula (V), r1+r2=3 (provided that r1 represents an integer of 1 to 3; and r2 represents an integer of 0 to 2). 36 R represents a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 37 represents dimethylaminomethyl, dimethylaminoethyl, diethylaminomethyl, diethylaminoethyl, methylsilyl(methyl)aminomethyl, methylsilyl(methyl)aminoethyl, methylsilyl(ethyl)aminomethyl, methylsilyl(ethyl)aminoethyl, dimethylsilylaminomethyl, dimethylsilylaminoethyl, a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and when r1 is 2 or more, R 37 Can be the same or different. 38 represents a hydrocarbonoxy group having 1 to 20 carbon atoms, a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and when r2 is 2, R 38 Can be the same or different.
[0085] Furthermore, it is preferred that the modifier is a hydrocarbyloxysilane compound having two or more nitrogen atoms, which is represented by the following general formula (VI) or (VII).
[0086]
[0087] In the general formula (VI), TMS represents a trimethylsilyl group. 40 R represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 41R represents a hydrocarbyloxy group having 1 to 20 carbon atoms, a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 42 It represents a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms.
[0088]
[0089] In the general formula (VII), TMS represents a trimethylsilyl group. 43 and R 44 Each independently represents a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 45 represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 45 Can be the same or different.
[0090] Furthermore, it is more preferred that the hydrocarbyloxysilane compound represented by the general formula (II) is a hydrocarbyloxysilane compound represented by the following general formula (VIII).
[0091]
[0092] In the general formula (VIII), r1+r2=3 (provided that r1 represents an integer of 0 to 2; and r2 represents an integer of 1 to 3). TMS represents a trimethylsilyl group. 46 R represents a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 47 and R 48 Each independently represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 47 or R 48 Can be the same or different.
[0093] Furthermore, it is preferable that the above-mentioned modifier is a hydrocarbyloxysilane compound represented by the following general formula (IX).
[0094]
[0095] In the general formula (IX), X represents a halogen atom (fluorine, chlorine, bromine or iodine). 49 R represents a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 50 and R 51Each independently represents a hydrolyzable group, a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, or R 50 and R 51 can combine to form a divalent organic group, and R 52 and R 53 Each independently represents a halogen atom (fluorine, chlorine, bromine or iodine), a hydrocarbonoxy group, a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 50 and R 51 Each is preferably a hydrolyzable group, and the hydrolyzable group is preferably a trimethylsilyl group or a tert-butyldimethylsilyl group, and particularly preferably a trimethylsilyl group.
[0096] Furthermore, it is preferred that the modifier is a compound having a structure represented by any one of the following general formulae (X) to (XIII).
[0097]
[0098]
[0099] Here, the symbols U and V included in formulas (X) to (XII) each represent an integer of 0 to 2, which satisfies the equation: U+V=2. In addition, R in formulas (X) to (XIII) 54 ~R 92 They may be the same or different, and each represents a monovalent or divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent or divalent aromatic hydrocarbon group having 6 to 18 carbon atoms. In addition, α and β in formula (XIII) each represent an integer of 0 to 5.
[0100] In addition, among the compounds satisfying formulas (X) to (XII), N1,N1,N7-tetramethyl-4-((trimethoxysilyl)methyl)-1,7-heptane, 2-((hexyl-dimethoxysilyl)methyl)-N1,N1,N3,N3-2-pentamethylpropane-1,3-diamine, N1-(3-(dimethylamino)propyl)-N3,N3-dimethyl-N1-(3-(trimethoxysilyl)propyl)propane-1,3-diamine, and 4-(3-(dimethylamino)propyl)-N1,N1,N7,N7-tetramethyl-4-((trimethoxysilyl)methyl)heptane-1,7-diamine are particularly preferred.
[0101] Among the compounds satisfying formula (XIII), N,N-dimethyl-2-(3-(dimethoxymethylsilyl)propoxy)ethylamine, N,N-bis(trimethylsilyl)-2-(3-(trimethoxysilyl)propoxy)ethylamine, N,N-dimethyl-2-(3-(trimethoxysilyl)propoxy)ethylamine, and N,N-dimethyl-3-(3-(trimethoxysilyl)propoxy)propan-1-amine are particularly preferred.
[0102] It is preferred that the hydrocarbyloxysilane compounds represented by the above general formulae (II) to (XIII) are used as the modifier in the case of a modified polymer produced by anionic polymerization which may be contained in a polymer phase having the lowest peak temperature in a tan δ temperature dispersion curve.
[0103] Furthermore, it is preferred that the hydrocarbyloxysilane compound represented by the general formulae (II) to (XIII) is an alkoxysilane compound.
[0104] Regarding the rubber composition according to the present invention, it is preferred that the modified conjugated diene polymer (A1) is formed by reacting a conjugated diene polymer with a coupling agent represented by the following general formula (1). In this case, the low loss property and wear resistance of the rubber composition can be further improved.
[0105]
[0106] In formula (1), R 1 , R 2 , and R 3 Each independently represents a single bond or an alkylene group having 1 to 20 carbon atoms. 4 , R 5 , R 6 , R 7 , and R 9 Each independently represents an alkyl group having 1 to 20 carbon atoms. 8 and R 11 Each independently represents an alkylene group having 1 to 20 carbon atoms. 10 represents an alkyl group or a trialkylsilyl group each having 1 to 20 carbon atoms. m represents an integer of 1 to 3, and p represents 1 or 2. 1 ~R 11 , m, and p, when a plurality of these groups exist, they are independent of each other. i, j, and k each independently represent an integer of 0 to 6. However, (i+j+k) represents an integer of 3 to 10. A represents a hydrocarbon group or an organic group having at least one atom selected from the group consisting of oxygen atoms, nitrogen atoms, silicon atoms, sulfur atoms, and phosphorus atoms and having no active hydrogen, and both the hydrocarbon group and the organic group have 1 to 20 carbon atoms.
[0107] Generally, when compared with a linear polymer having the same absolute molecular weight, a branched polymer tends to have a smaller molecular size, and the shrinkage factor (g') is an index of the ratio of the size occupied by the molecule of the linear polymer assumed to have the same absolute molecular weight. That is, as the degree of branching of the polymer increases, the shrinkage factor (g') tends to decrease. In the present embodiment, the intrinsic viscosity is used as an indicator of the molecular size, and for a linear polymer, the following is used to follow the intrinsic viscosity [η] = -3.883M 0.771 The contraction factor (g') of the modified conjugated diene polymer at each absolute molecular weight was calculated, and the absolute molecular weight was 100×10 4 ~200×10 4 The average value of the shrinkage factors (g') at the time of 0.05 % was designated as the shrinkage factor (g') of the modified conjugated diene polymer.
[0108] Here, when a polymer is directly or indirectly bonded to other polymers, a "branch" is formed. In addition, the "degree of branching" is the number of polymers that are directly or indirectly bonded to each other relative to one branch. For example, when five conjugated diene polymer chains described later are indirectly bonded to each other by coupling residues described later, the degree of branching is 5. Incidentally, the coupling residue is a constituent unit of a modified conjugated diene polymer, which is bonded to the conjugated diene polymer chain, and the coupling residue is, for example, a structural unit derived from a coupling agent, which is manufactured by reacting the conjugated diene polymer described below with a coupling agent. In addition, the conjugated diene polymer chain is a constituent unit of a modified conjugated diene polymer, and is, for example, a structural unit derived from a conjugated diene polymer, which is manufactured by reacting the conjugated diene polymer described below with a coupling agent.
[0109] The shrinkage factor (g') is less than 0.64, preferably 0.63 or less, more preferably 0.60 or less, even more preferably 0.59 or less, and still more preferably 0.57 or less. In addition, the lower limit of the shrinkage factor (g') is not particularly limited, and may be less than or equal to the detection limit; however, the lower limit is preferably 0.30 or more, more preferably 0.33 or more, even more preferably 0.35 or more, and still more preferably 0.45 or more. By using a modified conjugated diene polymer (A1) having a shrinkage factor (g') within this range, the processability of the rubber composition is improved.
[0110] Since the shrinkage factor (g') tends to depend on the degree of branching, for example, the shrinkage factor (g') can be controlled by using the degree of branching as an index. Specifically, when a modified conjugated diene polymer having a degree of branching of 6 is used, its shrinkage factor (g') tends to be 0.59 or more and 0.63 or less, and when a modified conjugated diene polymer having a degree of branching of 8 is used, its shrinkage factor (g') tends to be 0.45 or more and 0.59 or less. The shrinkage factor (g') is measured by the method described in the examples described later.
[0111] Preferably, the modified conjugated diene polymer (A1) has a side chain, and the degree of branching is more than 5. In addition, it is more preferred that the modified conjugated diene polymer (A1) has more than one coupling residue and a conjugated diene polymer chain combined with the coupling residue, and the side chain includes a side chain in which more than 5 of the conjugated diene polymer chain units are combined with 1 coupling residue unit. By setting the degree of branching to more than 5, and by specifying the structure of the modified conjugated diene polymer, the side chain includes a side chain in which more than 5 of the conjugated diene polymer chain units are combined with 1 coupling residue unit, and the contraction factor (g') can be more reliably adjusted to less than 0.64. Incidentally, the number of conjugated diene polymer chains bonded to a coupling residue can be confirmed by the value of the contraction factor (g').
[0112] In addition, it is more preferred that the modified conjugated diene polymer (A1) has a branched chain, and the degree of branching is 6 or more. In addition, it is even more preferred that the modified conjugated diene polymer (A1) has one or more coupling residues and a conjugated diene polymer chain combined with the coupling residue, and the branched chain includes a branched chain in which 6 or more of the conjugated diene polymer chain units are combined with 1 of the coupling residue units. By setting the degree of branching to 6 or more, and by specifying the structure of the modified conjugated diene polymer, the branched chain includes a branched chain in which 6 or more of the conjugated diene polymer chain units are combined with 1 of the coupling residue units, the contraction factor (g') can be adjusted to less than 0.63.
[0113] In addition, it is even more preferred that the modified conjugated diene polymer (A1) has a branched chain, and the degree of branching is 7 or more, and it is even more preferred that the degree of branching is 8 or more. The upper limit of the degree of branching is not particularly limited; however, it is preferred that the upper limit is 18 or less. In addition, it is also more preferred that the modified conjugated diene polymer (A1) has one or more coupling residues and a conjugated diene polymer chain combined with the coupling residue, and the branched chain includes a branched chain in which more than 7 of the conjugated diene polymer chain units are combined with 1 of the coupling residue units, and it is particularly preferred that the branched chain includes a branched chain in which more than 8 of the conjugated diene polymer chain units are combined with 1 of the coupling residue units. By setting the degree of branching to more than 8, and by specifying the structure of the modified conjugated diene polymer, the branched chain includes a branched chain in which more than 8 of the conjugated diene polymer chain units are combined with 1 of the coupling residue units, the shrinkage factor (g') can be adjusted to less than 0.59.
[0114] Preferably, the modified conjugated diene polymer (A1) has a nitrogen atom and a silicon atom. In this case, the processability of the rubber composition is improved, and the low loss and wear resistance of the rubber composition can be further improved. Incidentally, whether the modified conjugated diene polymer (A1) has a nitrogen atom can be confirmed by the method described in the embodiments described later by being adsorbed on a specific column. In addition, whether the modified conjugated diene polymer (A1) has a silicon atom can be confirmed by the method described in the embodiments described later by metal analysis.
[0115] Preferably, at least one end of the conjugated diene polymer chain is each combined with a silicon atom possessed by the coupling residue. In this case, the ends of a plurality of conjugated diene polymer chains may be combined with one silicon atom. In addition, the ends of the conjugated diene polymer chain and an alkoxy or hydroxyl group having 1 to 20 carbon atoms may be combined with one silicon atom, and therefore, one silicon atom may constitute an alkoxysilyl or silanol group having 1 to 20 carbon atoms.
[0116] The modified conjugated diene copolymer (A1) can be produced as an oil-extended polymer to which an extender oil is added. The modified conjugated diene copolymer (A1) may be unextended or oil-extended; however, from the viewpoint of wear resistance, the Mooney viscosity measured at 100° C. is preferably 20 or more and 100 or less, and more preferably 30 or more and 80 or less. Incidentally, the Mooney viscosity is measured by the method described in Examples described later.
[0117] The weight average molecular weight (Mw) of the modified conjugated diene polymer (A1) is 20×10 4 Above and 300×10 4 Below, preferably 50×10 4 More preferably 64×104 More than 80×10 4 In addition, the weight average molecular weight is preferably 250×10 4 Below, more preferably 180×10 4 Below, and even more preferably 150×10 4 When the weight average molecular weight is less than 20×10 4 When the weight average molecular weight is greater than 300×10 4 The weight average molecular weight of the modified conjugated diene polymer (A1) and the conjugated diene polymer described later is measured by the method described in the Examples described later.
[0118] The modified conjugated diene polymer (A1) includes 0.25% by mass or more and 30% by mass or less of a molecular weight of 200×10 4 Above and 500×10 4 The following modified conjugated diene polymer (hereinafter, also referred to as "specific high molecular weight component") When the content of the specific high molecular weight component is less than 0.25 mass % or more than 30 mass %, the low loss property and wear resistance of the rubber composition cannot be sufficiently improved.
[0119] The modified conjugated diene polymer (A1) preferably comprises a specific high molecular weight component in a ratio of 1.0% by mass or more, more preferably 1.4% by mass or more, even more preferably 1.75% by mass or more, still more preferably 2.0% by mass or more, particularly preferably 2.15% by mass or more, and extremely preferably 2.5% by mass or more. In addition, the modified conjugated diene polymer (A1) preferably comprises a specific high molecular weight component in a ratio of 28% by mass or less, more preferably 25% by mass or less, even more preferably 20% by mass or less, and still more preferably 18% by mass or less.
[0120] Incidentally, the "molecular weight" according to this specification is a molecular weight converted to standard polystyrene obtained by GPC (gel permeation chromatography). In order to obtain a modified conjugated diene polymer (A1) having a content of a specific high molecular weight component within this range, it is preferred to control the reaction conditions of the polymerization step and the reaction step, which will be described later. For example, in the polymerization step, the amount of an organic monolithium compound as a polymerization initiator can be adjusted, which will be described later. In addition, in the polymerization step, a method with a residence time distribution is used for continuous and intermittent polymerization modes, that is, it is desired to broaden the time distribution of the growth reaction.
[0121] Regarding the modified conjugated diene polymer (A1), the molecular weight distribution (Mw / Mn) represented by the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is preferably 1.6 or more and 3.0 or less. When the molecular weight distribution of the modified conjugated diene polymer (A1) is within this range, the processability of the rubber composition is improved.
[0122] Incidentally, the number average molecular weight, weight average molecular weight, molecular weight distribution, and content of specific high molecular weight components of the modified conjugated diene polymer (A1) and the conjugated diene polymer described later are measured by the method described in Examples described later.
[0123] The method for producing the modified conjugated diene polymer (A1) is not particularly limited; however, it is preferred that the method has a polymerization step of polymerizing at least a conjugated diene compound by using an organic monolithium compound as a polymerization initiator and obtaining a conjugated diene polymer; and a reaction step of reacting the active end of the conjugated diene polymer with a pentafunctional or higher-functional reactive compound (hereinafter, may also be referred to as a "coupling agent"). It is preferred that the coupling agent reacts with a pentafunctional or higher-functional reactive compound having a nitrogen atom and a silicon atom.
[0124] Preferably, the modified conjugated diene polymer (A1) is formed by reacting a conjugated diene polymer with a coupling agent represented by the general formula (1). By using the modified conjugated diene polymer (A1) formed by reacting with a coupling agent, the low loss property and wear resistance of the rubber composition can be further improved.
[0125] In the general formula (1), R 1 , R 2 , and R 3 Each independently represents a single bond or an alkylene group having 1 to 20 carbon atoms; R 4 , R 5 , R 6 , R 7 , and R 9 Each independently represents an alkyl group having 1 to 20 carbon atoms; R 8 and R 11 Each independently represents an alkylene group having 1 to 20 carbon atoms; R 10 represents an alkyl group or trialkylsilyl group having 1 to 20 carbon atoms; m represents an integer of 1 to 3; p represents 1 or 2; when there are multiple R 1 ~R 11, m, and p, they are each independent; i, j, and k each independently represent an integer from 0 to 6, provided that (i+j+k) represents an integer from 3 to 10; and A represents a hydrocarbon group having 1 to 20 carbon atoms or an organic group having at least one atom selected from the group consisting of oxygen atoms, nitrogen atoms, silicon atoms, sulfur atoms, and phosphorus atoms and having no active hydrogen.
[0126] Here, in the general formula (1), the hydrocarbon group represented by A includes saturated, unsaturated, aliphatic and aromatic hydrocarbon groups. Examples of the organic group having no active hydrogen include organic groups not containing functional groups having active hydrogen such as hydroxyl (-OH), secondary amino (>NH), primary amino (-NH2), and mercapto (-SH).
[0127] The polymerization step is preferably polymerization by a growth reaction of a living anionic polymerization reaction, whereby a conjugated diene polymer having an active terminal can be obtained, and a modified diene polymer (A1) having a high modification rate can be obtained.
[0128] The conjugated diene polymer is obtained by polymerizing at least a conjugated diene compound, and is obtained by copolymerizing both the conjugated diene compound and a vinyl-substituted aromatic compound as necessary.
[0129] The conjugated diene compound is preferably a conjugated diene compound having 4 to 12 carbon atoms, and more preferably a conjugated diene compound having 4 to 8 carbon atoms. Examples of such conjugated diene compounds include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 3-methyl-1,3-pentadiene, 1,3-hexadiene, and 1,3-hexadiene. Among them, from the perspective of ease of industrial availability, 1,3-butadiene and isoprene are preferred. With regard to these conjugated diene compounds, one of them can be used alone, or two or more of them can be used in combination.
[0130] In addition, the vinyl-substituted aromatic compound is preferably a monovinyl aromatic compound. Examples of monovinyl aromatic compounds include styrene, p-methylstyrene, α-methylstyrene, vinylethylbenzene, vinylxylene, vinylnaphthalene, and diphenylethylene. Among them, styrene is preferred from the viewpoint of ease of industrial availability. Regarding these vinyl-substituted aromatic compounds, one of them can be used alone, or two or more of them can be used in combination.
[0131] Preferably, the amount of the organic monolithium compound as a polymerization initiator is determined by the molecular weight of the target conjugated diene polymer or the modified conjugated diene polymer. Relative to the amount of the polymerization initiator, the amount of monomers such as conjugated diene compounds is related to the degree of polymerization, that is, to the number average molecular weight and / or weight average molecular weight. Therefore, in order to increase the molecular weight, it can be adjusted in the direction of reducing the polymerization initiator, and in order to reduce the molecular weight, it can be adjusted in the direction of increasing the amount of the polymerization initiator.
[0132] From the viewpoint of ease of industrial availability and ease of controlling polymerization, the organic monolithium compound is preferably an alkyl lithium compound. In this case, a conjugated diene polymer having an alkyl group at the polymerization initiation terminal is obtained. Examples of alkyl lithium compounds include, for example, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, n-hexyl lithium, benzyl lithium, phenyl lithium, and stilbene lithium. From the viewpoint of ease of industrial availability and ease of controlling polymerization, the alkyl lithium compound is preferably n-butyl lithium and sec-butyl lithium. With regard to these organic monolithium compounds, one of them can be used alone, or two or more of them can be used in combination.
[0133] In the polymerization step, examples of polymerization reaction modes include intermittent and continuous polymerization reaction modes. Regarding the continuous type, one or more connected reactors can be used. Regarding the continuous reactor, for example, a tank reactor and a tubular reactor with an agitator are used. Regarding the continuous type, preferably, monomers, inert solvents, and polymerization initiators are continuously fed into the reactor, a polymer solution containing polymers is obtained in the reactor, and the polymer solution is continuously discharged. Regarding the intermittent reactor, for example, a tank reactor with an agitator is used. Regarding the intermittent type, preferably, monomers, inert solvents, and polymerization initiators are fed, monomers are continuously or intermittently added as needed during the polymerization, a polymer solution containing polymers is obtained in the reactor, and the polymer solution is discharged after the polymerization is completed. According to the present embodiment, in order to obtain a high proportion of conjugated diene polymers with active ends, a continuous type in which the polymer can be continuously discharged and subsequent reactions are carried out in a short time is preferred.
[0134] In the polymerization step, it is preferred that the polymerization is carried out in an inert solvent. Examples of solvents include hydrocarbon solvents such as saturated hydrocarbons and aromatic hydrocarbons. Specific examples of hydrocarbon solvents are not limited to the following; however, examples include hydrocarbons composed of aliphatic hydrocarbons, such as butane, pentane, hexane, and heptane; alicyclic hydrocarbons, such as cyclopentane, cyclohexane, methylcyclopentane, and methylcyclohexane; aromatic hydrocarbons, such as benzene, toluene, and xylene; and mixtures thereof. When allenes and acetylenes as impurities are treated with an organic metal compound before being supplied to the polymerization reaction, it is preferred because a high concentration of conjugated diene polymers having active terminals and a modified conjugated diene polymer having a high modification rate are tended to be obtained.
[0135] In the polymerization step, a polar compound may be added. By adding the polar compound, the aromatic vinyl compound can be randomly copolymerized with the conjugated diene compound, and there is a tendency that the polar compound can also function as a vinylating agent to control the microstructure of the conjugated diene portion.
[0136] As for polar compounds, for example, ethers such as tetrahydrofuran, diethyl ether, dioxane, ethylene glycol dimethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, diethylene glycol dibutyl ether, dimethoxybenzene, and 2,2-bis(2-oxolanyl)propane; tertiary amine compounds such as tetramethylethylenediamine, dipiperidylethane, trimethylamine, triethylamine, pyridine, and quinuclidine; alkali metal alkoxide compounds such as potassium tert-amylate, potassium tert-butyrate, sodium tert-butyrate, sodium amylate; and; phosphine compounds such as triphenylphosphine can be used. As for these polar compounds, one of them can be used alone, or two or more of them can be used in combination.
[0137] In the polymerization step, from the viewpoint of productivity, the polymerization temperature is preferably 0° C. or higher, more preferably 120° C. or lower, and particularly preferably 50° C. or higher and 100° C. or lower. When the polymerization temperature is within this range, there is a tendency that a sufficient reaction amount of the coupling agent relative to the active terminal after completion of the polymerization can be ensured.
[0138] The bound conjugated diene amount in the conjugated diene polymer or modified conjugated diene polymer (A1) is not particularly limited; however, the bound conjugated diene amount is preferably 40% by mass or more and 100% by mass or less, and more preferably 55% by mass or more and 80% by mass or less.
[0139] Furthermore, the amount of bound aromatic vinyl in the conjugated diene polymer or modified conjugated diene polymer (A1) is not particularly limited; however, the amount of bound aromatic vinyl is preferably 0 mass % or more and 60 mass % or less, and more preferably 20 mass % or more and 45 mass % or less.
[0140] When the bound conjugated diene amount and the bound aromatic vinyl amount are within the above ranges, the low loss property and the wear resistance of the rubber composition can be further improved.
[0141] Incidentally, the bound aromatic vinyl amount can be measured by ultraviolet absorption of phenyl groups, and thereby the bound conjugated diene amount can also be determined. Specifically, the bound aromatic vinyl amount is measured according to the method described in Examples described later.
[0142] The amount of vinyl bonds in the conjugated diene-based polymer or the modified conjugated diene-based polymer (A1) is not particularly limited; however, the amount of vinyl bonds is preferably 10 mol% or more and 75 mol% or less, and more preferably 20 mol% or more and 65 mol% or less. When the amount of vinyl bonds is within the above range, the low loss property and wear resistance of the rubber composition can be further improved.
[0143] Incidentally, when the modified conjugated diene polymer (A1) is a copolymer of butadiene and styrene, the amount of vinyl bonds (amount of 1,2-bonds) in the butadiene bonding unit can be determined by the Hampton method [RR Hampton, Analytical Chemistry, 21, 923 (1949)]. Specifically, the amount of vinyl bonds is measured by the method described in the Examples described later.
[0144] The modified conjugated diene polymer (A1) preferably has a glass transition temperature (Tg) of -45°C to -15°C. When the glass transition temperature (Tg) of the modified conjugated diene polymer (A1) is within the range of -45°C to -15°C, the low loss property and wear resistance of the rubber composition can be further improved.
[0145] Incidentally, regarding the glass transition temperature, a DSC curve is recorded while increasing the temperature within a predetermined temperature range according to ISO 22768: 2006, and the peak top (inflection point) of the DSC differential curve is designated as the glass transition temperature. Specifically, the glass transition temperature is measured by the method described in Examples described later.
[0146] Preferably, the reactive compound (coupling agent) is a pentafunctional or higher functional reactive compound having a nitrogen atom and a silicon atom, and preferably, the reactive compound has at least three silicon-containing functional groups. A more preferred coupling agent is a compound in which at least one silicon atom constitutes an alkoxysilyl group or a silanol group having 1 to 20 carbon atoms, and the coupling agent is more preferably a compound represented by the above general formula (1).
[0147] The alkoxysilyl group possessed by the coupling agent reacts with the active end of, for example, a conjugated diene polymer to dissociate the alkoxylithium, and tends to form a bond between the end of the conjugated diene polymer chain and the silicon of the coupling residue. The value obtained by subtracting the number of SiOR reduced by the reaction from the total number of SiOR possessed by one molecule of the coupling agent is the number of alkoxysilyl groups possessed by the coupling residue. In addition, the azasilyl ring group possessed by the coupling agent forms a bond between the>N-Li bond and the end of the conjugated diene polymer and the silicon of the coupling residue. Incidentally, the>N-Li bond tends to easily become>NH and LiOH due to water, etc. at the time of completion. In addition, with respect to the coupling agent, there is a tendency that the residual unreacted alkoxysilyl group can easily become a silanol (Si-OH group) due to water, etc. at the time of completion.
[0148] The reaction temperature of the reaction step is preferably a temperature similar to the polymerization temperature of the conjugated diene polymer, and the reaction temperature is more preferably 0° C. or higher and 120° C. or lower, and even more preferably 50° C. or higher and 100° C. or lower. In addition, the temperature change occurring after the polymerization step until the coupling agent is added is preferably 10° C. or lower, and more preferably 5° C. or lower.
[0149] The reaction time of the reaction step is preferably 10 seconds or more, and more preferably 30 seconds or more. From the viewpoint of coupling rate, it is preferred that the time from completion of the polymerization step to start of the reaction step is shorter; however, the time is more preferably 5 minutes or less.
[0150] The mixing of the reaction step can be achieved by any of mechanical stirring and static mixer stirring, etc. When the polymerization step is a continuous process, it is preferred that the reaction step is also a continuous process. Regarding the reactor of the reaction step, for example, a tank type reactor, a tubular type reactor with a stirrer is used. The coupling agent can be diluted with an inert solvent and continuously supplied to the reactor. When the polymerization step is a batch process, even in a method in which the coupling agent is introduced into a polymerization reactor, the reaction step can be performed after the reactor contents are transferred to another reactor.
[0151] In the general formula (1), A is preferably represented by any one of the following general formulae (2) to (5). When A is represented by any one of the general formulae (2) to (5), a modified conjugated diene polymer (A1) having excellent properties can be obtained.
[0152]
[0153] In the general formula (2), B 1 represents a single bond or a hydrocarbon group having 1 to 20 carbon atoms; and a represents an integer from 1 to 10. 1 , they are independent of each other.
[0154]
[0155] In the general formula (3), B 2 represents a single bond or a hydrocarbon group having 1 to 20 carbon atoms; B 3 represents an alkyl group having 1 to 20 carbon atoms; and a represents an integer of 1 to 10. When there are multiple B 2 and multiple B 3 , they are independent of each other.
[0156]
[0157] In general formula (4), B 4 represents a single bond or a hydrocarbon group having 1 to 20 carbon atoms; and a represents an integer from 1 to 10. 4 , they are independent of each other.
[0158]
[0159] In the general formula (5), B 5 represents a single bond or a hydrocarbon group having 1 to 20 carbon atoms; and a represents an integer from 1 to 10. 5 , they are independent of each other.
[0160] Incidentally, regarding B in the general formulas (2) to (5), 1 , B 2 , B 4 , and B 5 , the hydrocarbon group having 1 to 20 carbon atoms may be an alkylene group having 1 to 20 carbon atoms, etc.
[0161] Preferably, in the general formula (1), A is represented by the general formula (2) or (3); and k represents 0.
[0162] More preferably, in the general formula (1), A is represented by the general formula (2) or (3); k represents 0, and in the general formula (2) or (3), a represents an integer of 2 to 10.
[0163] Even more preferably, in the general formula (1), A is represented by the general formula (2), k represents 0, and in the general formula (2), a represents an integer of 2-10.
[0164] Examples of such coupling agents include bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]amine, tris(3-trimethoxysilylpropyl)amine, tris(3-triethoxysilylpropyl)amine, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propylenediamine, tetrakis ...
[0063] The preferred embodiments of the present invention include bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-methyl-1,3-propylenediamine, tetrakis(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane, tris(3-trimethoxysilylpropyl)-methyl-1,3-propylenediamine, and bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trimethoxysilylpropyl)-methyl-1,3-propylenediamine, and among them, tetrakis(3-trimethoxysilylpropyl)-1,3-propylenediamine and tetrakis(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane are particularly preferred.
[0165] The amount of the compound represented by the general formula (1) as a coupling agent can be adjusted so that the molar number of the conjugated diene polymer and the molar number of the coupling agent react in a desired stoichiometric ratio, thereby tending to achieve a desired degree of branching. Preferably, the specific molar number of the polymerization initiator is preferably 5.0 times mol or more, and more preferably 6.0 times mol or more relative to the molar number of the coupling agent. In this case, in the general formula (1), the number of functional groups of the coupling agent ((m-1)×i+p×j+k) is preferably an integer of 5 to 10, and more preferably an integer of 6 to 10.
[0166] In order to obtain a modified conjugated diene polymer (A1) having a specific polymer component, the molecular weight distribution (Mw / Mn) of the conjugated diene polymer is preferably set to 1.5 or more and 2.5 or less, and more preferably 1.8 or more and 2.2 or less. In addition, the obtainable modified conjugated diene polymer (A1) is preferably such that one peak is detected from the molecular weight curve obtained by GPC.
[0167] When the peak molecular weight of the modified conjugated diene polymer (A1) obtained by GPC is represented by Mp1, and the peak molecular weight of the conjugated diene polymer is represented by Mp2, it is preferred that the following formula holds.
[0168] (Mp1 / Mp2)<1.8×10-12×(Mp2-120×10 4 ) 2 +2
[0169] More preferably, Mp2 is 20×104 Above and 80×10 4 Below, and Mp1 is 30×10 4 Above and 150×10 4 Hereinafter, Mp1 and Mp2 are determined by the method described in the Examples described later.
[0170] The modification rate of the modified conjugated diene polymer (A1) is preferably 30% by mass or more, more preferably 50% by mass or more, and even more preferably 70% by mass or more. When the modification rate is 30% by mass or more, the low loss and wear resistance of the rubber composition can be further improved. Incidentally, the modification rate is measured by the method described in the examples described later.
[0171] After the reaction step, a deactivating agent, a neutralizing agent, and the like may be added to the copolymer solution as needed. The deactivating agent is not limited to the following; however, examples thereof include water; and alcohols such as methanol, ethanol, and isopropanol. The neutralizing agent is not limited to the following; however, examples thereof include carboxylic acids such as stearic acid, oleic acid, and versatic acid (a highly branched carboxylic acid mixture having 9 to 11, mainly 10 carbon atoms); an aqueous solution of an inorganic acid, and carbon dioxide gas.
[0172] Furthermore, from the viewpoint of preventing gel formation after polymerization and from the viewpoint of improving stability during processing, it is preferred that an antioxidant such as 2,6-di-tert-butyl-4-hydroxytoluene (BHT), n-octadecyl-3-(4'-hydroxy-3',5'-di-tert-butylphenyl)propionate, or 2-methyl-4,6-bis[(octylthio)methyl]phenol is added to the modified conjugated diene polymer (A1).
[0173] As for the method for obtaining the modified conjugated diene polymer (A1) from the polymer solution, a known method can be used. Examples of the method include a method in which the solvent is separated by steam stripping, the polymer is subsequently separated by filtration, and the polymer is dehydrated and dried to obtain the polymer; a method in which the polymer solution is concentrated in a rinse tank and devolatilized by exhaust extrusion or the like; a method in which the polymer solution is directly devolatilized by a drum dryer or the like.
[0174] The modified conjugated diene polymer (A1) is obtained by reacting a coupling agent represented by the general formula (1) with a conjugated diene polymer represented by, for example, the following general formula (6).
[0175]
[0176] In the general formula (6), D represents a conjugated diene polymer chain, and preferably, the weight average molecular weight of the conjugated diene polymer chain is 10×10 4 ~100×10 4The conjugated diene polymer chain is a constituent unit of the modified conjugated diene polymer, and is, for example, a constituent unit derived from a conjugated diene polymer, which is produced by reacting the conjugated diene polymer with a coupling agent.
[0177] R 12 , R 13 , and R 14 Each independently represents a single bond or an alkylene group having 1 to 20 carbon atoms; R 15 and R 18 Each independently represents an alkyl group having 1 to 20 carbon atoms; R 16 , R 19 , and R 20 Each independently represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms; R 17 and R 21 Each independently represents an alkylene group having 1 to 20 carbon atoms; and R 22 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. m and x each represent an integer of 1 to 3; x≤m; p represents 1 or 2; y represents an integer of 1 to 3; y≤(p+1); and z represents an integer of 1 or 2. 12 ~R 22 , m, p, x, y, and z, they are independent of each other and may be the same or different. In addition, i represents an integer of 0 to 6; j represents an integer of 0 to 6; k represents an integer of 0 to 6; (i+j+k) represents an integer of 3 to 10; and ((x×i)+(y×j)+(z×k)) represents an integer of 5 to 30. A represents a hydrocarbon group having 1 to 20 carbon atoms, or an organic group having at least one atom selected from the group consisting of oxygen atoms, nitrogen atoms, silicon atoms, sulfur atoms, and phosphorus atoms and having no active hydrogen. The hydrocarbon group represented by A includes saturated, unsaturated, aliphatic and aromatic hydrocarbon groups. Examples of organic groups without active hydrogen include organic groups that do not contain functional groups having active hydrogen such as hydroxyl (-OH), secondary amino groups (>NH), primary amino groups (-NH2), and mercapto groups (-SH).
[0178] In the general formula (6), A is preferably represented by any one of the general formulas (2) to (5). When A is represented by any one of the general formulas (2) to (5), the low loss property and wear resistance of the rubber composition can be further improved.
[0179] At least one selected from the modified styrene-butadiene rubber is modified by at least one selected from the group consisting of N,N-bis(trimethylsilyl)-3-[diethoxy(methyl)silyl]propylamine, N-(1,3-dimethylbutylene)-3-triethoxysilyl-1-propylamine, and tetrakis(3-trimethoxysilylpropyl)-1,3-propylenediamine.
[0180] The modification site of the aminoalkoxysilane-modified SBR may be the molecular terminal or may be the main chain; however, it is preferred that the terminal of the styrene-butadiene rubber (SBR) is modified.
[0181] As described above, it is preferred that the rubber component contains a modified styrene-butadiene rubber having a bound styrene amount of 30% or more (modified SBR having a high bound styrene amount).
[0182] From the viewpoint of having high affinity for fillers (eg, silica), the modified SBR is preferably such that the terminal of the SBR is modified with a silane compound. Examples of the silane compound include a silane compound having a glycidoxy group, an alkoxysilane, and a hydrocarbyloxysilane compound.
[0183] When the terminal of SBR is modified with a silane compound, the interaction of the modified SBR with silica increases.
[0184] The modified site of the modified SBR may be a molecular terminal or may be the main chain; however, it is preferred that the terminal of the styrene-butadiene rubber (SBR) is modified.
[0185] The rubber component may include other rubber components in addition to the rubber having an isoprene structure, the modified SBR having a low bound styrene content, and the modified SBR having a high bound styrene content.
[0186] Examples of other rubber components include modified styrene-butadiene rubber having a bound styrene amount of greater than 15% and less than 30%, unmodified styrene-butadiene rubber, chloroprene rubber, butyl rubber (IIR), halogenated butyl rubber, ethylene-propylene rubber (EPR, EPDM), fluororubber, silicone rubber, and polyurethane rubber.
[0187] [filler]
[0188] The rubber composition contains a nitrogen adsorption specific surface area (BET method) of 130 m 2 / g or more and less than 330m 2 The content of the filler in the rubber composition is 40 to 125 parts by mass based on 100 parts by mass of the rubber component.
[0189] When the content of the filler in the rubber composition is less than 40 parts by mass relative to 100 parts by mass of the rubber component, sufficient tire reinforcement cannot be achieved and rolling resistance cannot be reduced. When the content is more than 125 parts by mass, the elastic modulus of the tire becomes too high and the wet grip is not excellent.
[0190] From the viewpoint of further reducing rolling resistance, the content of the filler in the rubber composition is preferably 48 parts by mass or more, more preferably 53 parts by mass or more, even more preferably 58 parts by mass or more, and still more preferably 62 parts by mass or more, relative to 100 parts by mass of the rubber component. In addition, from the viewpoint of improving wet grip, the content of the filler in the rubber composition is preferably 105 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 95 parts by mass or less, still more preferably 90 parts by mass or less, and even more preferably 85 parts by mass or less, relative to 100 parts by mass of the rubber component.
[0191] (Silicon Dioxide)
[0192] The filler contains nitrogen adsorption specific surface area (BET method) of 130m 2 / g or more and less than 330m 2 / g of silica.
[0193] When the nitrogen adsorption specific surface area of silicon dioxide (BET method) is less than 130 m 2 / g, the tire cannot be sufficiently reinforced and the rolling resistance cannot be reduced. In addition, when the nitrogen adsorption specific surface area (BET method) of silica is 330m 2 When the elastic modulus of the tire is greater than 300 / g, the elastic modulus of the tire becomes too high and wet grip performance cannot be obtained.
[0194] From the viewpoint of further reducing rolling resistance and improving tire wear resistance, the nitrogen adsorption specific surface area (BET method) of silica is preferably 150 m 2 / g or more, more preferably 170m 2 / g or more, even more preferably 180m 2 / g or more, still more preferably 190m 2 / g or more, and even more preferably 195m 2 From the viewpoint of further improving wet grip performance, the nitrogen adsorption specific surface area (BET method) of silica is preferably 300 m 2 / g or less, more preferably 280m 2 / g or less, and even more preferably 270m / g 2 / g or less.
[0195] There is no particular limitation on the silica, as long as the nitrogen adsorption specific surface area (BET method) is 130 m 2 / g or more and less than 330m 2 / g, and examples thereof include wet silica (hydrated silicic acid), dry silica (anhydrous silicic acid), calcium silicate and aluminum silicate, and among these, wet silica is preferred. Regarding these silicas, one of them may be used alone, or two or more of them may be used in combination.
[0196] From the viewpoint of improving the mechanical strength of the tire and further reducing the rolling resistance, the content of silica in the rubber composition is preferably 40 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 55 parts by mass or more relative to 100 parts by mass of the rubber component. In addition, from the viewpoint of further improving the wet grip, the content of silica in the rubber composition is preferably 90 parts by mass or less, more preferably 85 parts by mass or less, and even more preferably 80 parts by mass or less relative to 100 parts by mass of the rubber component.
[0197] (Carbon Black)
[0198] It is preferred that the filler further includes carbon black. However, it is preferred that the carbon black is included so that the content of silica in the filler is in the range of 70% by mass or more. When the content of silica in the filler is 70% by mass or more, the mechanical strength of the tire can be improved, and the rolling resistance can be further reduced. More preferably, the content of silica in the filler is 80% by mass or more, more preferably the content of silica in the filler is 85% by mass or more, and even more preferably the content of silica in the filler is 90% by mass or more and less than 100%.
[0199] Carbon black reinforces vulcanized rubber and improves the wear resistance of the vulcanized rubber.
[0200] The carbon black is not particularly limited, and examples include GPF, FEF, HAF, ISAF, and SAF grade carbon blacks. These carbon blacks may be used alone, or two or more thereof may be used in combination.
[0201] From the viewpoint of improving the wear resistance of the vulcanized rubber, the content of carbon black in the rubber composition is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more. In addition, from the viewpoint of the handleability of the rubber composition, the content of carbon black in the rubber composition is preferably 20 parts by mass or less, and more preferably 15 parts by mass or less relative to 100 parts by mass of the rubber component.
[0202] In addition to silica and carbon black, the filler may also include inorganic fillers such as clay, talc, calcium carbonate or aluminum hydroxide.
[0203] [Hydrogenated resin]
[0204] The rubber composition contains a hydrogenated resin having a softening point higher than 110° C. and a weight average molecular weight of 200 to 1200 g / mol in terms of polystyrene. The content of the hydrogenated resin in the rubber composition is 5 to 50 parts by mass per 100 parts by mass of the rubber component.
[0205] When the softening point of the hydrogenated resin is 110° C. or lower, the tire cannot be sufficiently reinforced, and the rolling resistance cannot be reduced. From the viewpoint of further reducing the rolling resistance, the softening point of the hydrogenated resin is preferably 115° C. or higher, more preferably 118° C. or higher, even more preferably 123° C. or higher, and still more preferably 125° C. or higher. Furthermore, from the viewpoint of wet grip performance, the softening point of the hydrogenated resin is preferably 145° C. or lower, more preferably 138° C. or lower, and even more preferably 133° C. or lower.
[0206] When the weight average molecular weight of the hydrogenated resin in terms of polystyrene is less than 200 g / mol, the hydrogenated resin precipitates from the tire and the effect brought by the hydrogenated resin cannot be fully manifested, and when the weight average molecular weight in terms of polystyrene is greater than 1200 g / mol, the hydrogenated resin is incompatible with the rubber component.
[0207] From the viewpoint of suppressing precipitation of the hydrogenated resin from the tire and suppressing deterioration of the tire appearance, the weight average molecular weight of the hydrogenated resin in terms of polystyrene is preferably 500 or more, more preferably 550 or more, even more preferably 620 or more, still more preferably 670 or more, even more preferably 720 or more, still more preferably 750 or more, and even more preferably 780 or more. Furthermore, from the viewpoint of improving the compatibility of the hydrogenated resin with the rubber component and further improving the effect brought about by the hydrogenated resin, the weight average molecular weight of the hydrogenated resin in terms of polystyrene is preferably 1100 or less, more preferably 1050 or less, even more preferably 950 or less, still more preferably 900 or less, and even more preferably 850 or less.
[0208] Softening point of hydrogenated resin (Ts HR ) (unit: °C) relative to the weight average molecular weight (Mw) of the hydrogenated resin in terms of polystyrene HR ) (unit: g / mol) is preferably 0.15 or more [0.15≤(Ts HR / Mw HR )].
[0209] (Ts HR / Mw HR ) is more preferably 0.155 or more, even more preferably 0.158 or more, still more preferably 0.160 or more, and even more preferably 0.162 or more. In addition, (Ts HR / Mw HR ) is preferably 0.2 or less, more preferably 0.185 or less, even more preferably 0.178 or less, still more preferably 0.172 or less, even more preferably 0.168 or less, and still more preferably 0.163 or less.
[0210] When the content of the hydrogenated resin in the rubber composition is less than 5 parts by mass relative to 100 parts by mass of the rubber component, the effect brought by the hydrogenated resin cannot be exhibited, and when the content exceeds 50 parts by mass, the hydrogenated resin precipitates from the tire and the effect brought by the hydrogenated resin cannot be fully exhibited.
[0211] From the viewpoint of further improving the effect brought about by the hydrogenated resin, the content of the hydrogenated resin in the rubber composition is preferably 5 parts by mass or more, more preferably 7 parts by mass or more, and even more preferably 9 parts by mass or more relative to 100 parts by mass of the rubber component. Furthermore, from the viewpoint of suppressing the precipitation of the hydrogenated resin from the tire and suppressing the deterioration of the tire appearance, the content of the hydrogenated resin in the rubber composition is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less relative to 100 parts by mass of the rubber component.
[0212] The hydrogenated resin means a resin obtained by reducing and hydrogenating a resin.
[0213] Examples of resins serving as raw materials for the hydrogenated resin include C5-based resins, C5-C9-based resins, C9-based resins, terpene-based resins, dicyclopentadiene-based resins, and terpene aromatic compound-based resins, and regarding these resins, one of them may be used alone, or two or more of them may be used in combination.
[0214] Examples of the C5-based resin include aliphatic petroleum resins obtained by polymerizing a C5 fraction obtained by thermal cracking of naphtha in the petrochemical industry.
[0215] The C5 fraction generally includes olefin hydrocarbons such as 1-pentene, 2-pentene, 2-methyl-2-butene, 2-methyl-1-butene, and 3-methyl-1-butene; and diolefin hydrocarbons such as 2-methyl-1,3-butadiene, 1,2-pentadiene, 1,3-pentadiene, and 3-methyl-1,2-butadiene. Incidentally, regarding the C5 resin, a commercially available product can be used.
[0216] C5-C9 series resin refers to C5-C9 series synthetic petroleum resin, and as for C5-C9 series resin, for example, C5-C9 series resin derived from petroleum is synthesized by using a Friedel-Crafts catalyst such as AlCl3 and BF3 can be mentioned. 11 More specific examples include copolymers containing styrene, vinyltoluene, α-methylstyrene, and indene as main components.
[0217] Regarding the C5-C9-based resin, a resin having a reduced amount of components of C9 or more is preferred from the viewpoint of compatibility with the rubber component. Here, the phrase "reduced amount of components of C9 or more" means that the proportion of the components of C9 or more in the total amount of the resin is less than 50% by mass, and preferably 40% by mass or less. Regarding the C5-C9-based resin, a commercially available product can be used.
[0218] Furthermore, the resin as a raw material of the hydrogenated resin may include, for example, a resin obtained by copolymerizing a C5 fraction and dicyclopentadiene (DCPD) (C5-DCPD-based resin).
[0219] Here, when the proportion of the component derived from dicyclopentadiene in the total amount of the resin is 50% by mass or more, it should be noted that the C5-DCPD resin is included in the dicyclopentadiene resin. When the proportion of the component derived from dicyclopentadiene in the total amount of the resin is less than 50% by mass, it should be noted that the C5-DCPD resin is included in the C5 resin. The same applies to the case where a small amount of a third component is further included.
[0220] From the viewpoint of increasing the compatibility between the rubber component and the hydrogenated resin, further improving the wet grip and further reducing the rolling resistance, the hydrogenated resin is preferably selected from at least one of the group consisting of hydrogenated C5 resins, hydrogenated C5-C9 resins, and hydrogenated dicyclopentadiene resins (hydrogenated DCPD resins); more preferably selected from at least one of the group consisting of hydrogenated C5 resins and hydrogenated C5-C9 resins; even more preferably hydrogenated C5 resins. In addition, the hydrogenated resin is preferably a resin having at least a hydrogenated DCPD structure or a hydrogenated cyclic structure in the monomer.
[0221] (Silane coupling agent)
[0222] Preferably, the rubber composition further contains a silane coupling agent.
[0223] As for the silane coupling agent, a silane coupling agent commonly used in the rubber industry can be used. In addition, from the viewpoint of rolling resistance and improving wet road performance, it is preferred that the rubber composition includes a silane coupling agent having a mercapto group. Examples of the silane coupling agent having a mercapto group include mercapto-containing silanes such as γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyltriethoxysilane.
[0224] (Other softeners)
[0225] The rubber composition according to the present invention may further include a softener (referred to as other softener) other than the hydrogenated resin of the present invention.
[0226] Examples of other softeners include thermoplastic resins other than the hydrogenated resin of the present invention and oils. The rubber composition does not necessarily need to include oil.
[0227] Here, oil is a general term for filler oil included in the rubber component and liquid oil added as a compounding agent of the rubber composition, and examples thereof include petroleum softeners such as aromatic oil, paraffin oil, and naphthenic oil; and plant softeners such as palm oil, castor oil, cottonseed oil, and soybean oil. Among the above oils, it is preferred that the rubber composition according to the present invention includes an oil that is liquid at normal temperature such as 25°C, for example, a petroleum softener such as aromatic oil, paraffin oil, or naphthenic oil.
[0228] From the standpoint of operability, the preferred ratio of filler oil:mixing agent oil fraction is 1:1 to 10:1 on a volume basis.
[0229] When the rubber component is composed of three components of natural component / modified SBR with a low bound styrene amount / modified SBR with a high bound styrene amount, the preferred total amount of the softener in the rubber composition according to the present invention is 35% by mass or less, and more preferably 30% by mass or less or 25% by mass or less, and even more preferably 5% by mass or more, 8% by mass or more, or 15% by mass or more.
[0230] When the rubber composition according to the present invention includes oil, from the viewpoint of optimizing the softening point and molecular weight of the softener as a whole, the ratio of the thermoplastic resin (a) including the hydrogenated resin in the total amount (a+b) of the softener composed of the thermoplastic resin (a) including the hydrogenated resin and the oil (b) is preferably 50% or more, more preferably 70% or more, and even more preferably 80% or more on a mass basis. In addition, the ratio is preferably 100% or less, and more preferably 95% or less.
[0231] As described above, the rubber composition according to the present invention may further include a thermoplastic resin other than the hydrogenated resin of the present invention. In this case, the content ratio of the hydrogenated resin (c) in the total amount (c+d) of the hydrogenated resin (c) and the thermoplastic resin (d) is more preferably 40% or more, even more preferably 50% or more, still more preferably 55% or more, and even more preferably 60% or more on a mass basis from the viewpoint of optimizing the softening point of the resin as a whole and the molecular weight of the resin.
[0232] In addition, from the viewpoint of further improving wet road performance, the thermoplastic resin other than the hydrogenated resin is preferably at least one selected from C5-based resins, C9-based resins, C5-C9-based resins, terpene-based resins, terpene aromatic compound-based resins, rosin-based resins, dicyclopentadiene-based resins, and alkylphenol-based resins, and among the above, the resin selected from the group consisting of C9-based resins and C5-C9-based resins is particularly preferred.
[0233] (Various components)
[0234] The rubber composition according to the present invention may contain the aforementioned rubber component, filler, and hydrogenated resin, and as needed, various components commonly used in the rubber industry, such as a processability improver, stearic acid, an antioxidant, zinc oxide, a vulcanization accelerator, and a vulcanizing agent, which may be appropriately selected within the range not impairing the purpose of the present invention.
[0235] [Method for producing rubber composition]
[0236] The method for producing the rubber composition according to the present invention is not particularly limited; however, for example, the rubber composition can be produced by mixing various components appropriately selected as needed with the aforementioned rubber component, silica and the hydrogenated resin of the present invention, and kneading, heating, and extruding the mixture.
[0237] <Tires>
[0238] The tire (pneumatic tire) of the present invention is formed by using the rubber composition of the present invention.
[0239] As described above, the tire obtained from the rubber composition according to the present invention has excellent wet grip and low rolling resistance. The rubber composition according to the present invention is suitable for the manufacture of a tire tread portion.
[0240] The tire can be obtained by molding using an unvulcanized rubber composition according to the type and member of the tire to be applied, and then vulcanizing the molded product, or can be obtained by first obtaining a semi-vulcanized rubber from the unvulcanized rubber composition through a pre-vulcanization step, and then molding using the semi-vulcanized rubber, and then further performing main vulcanization. Incidentally, as for the gas filled in the tire, in addition to ordinary air or air with adjusted oxygen partial pressure, an inert gas such as nitrogen, argon, helium, etc. can be used.
[0241] Example
[0242] Hereinafter, the present invention will be described in more detail through examples; however, these examples are for illustrating the present invention and are not intended to limit the present invention.
[0243] <Preparation of Rubber Composition>
[0244] 1. Examples 1 to 5, Comparative Examples 1 to 4, and Comparative Example 6
[0245] The rubber composition was prepared by mixing in the order of the first mixing step and the final mixing step using a common Banbury mixer, according to the mixing formula shown in Table 1 or Table 2. After the first mixing step, the mixture was first taken out of the Banbury mixer, and then the mixture was put into the Banbury mixer again, and the final mixing step was performed. In addition, the maximum temperature of the mixture in the first mixing step was set to 170° C., and the maximum temperature of the rubber composition in the final mixing step was set to 110° C.
[0246] 2. Examples 6 and 7, Comparative Example 5, and Comparative Example 7
[0247] The rubber composition was prepared by mixing in the order of the first mixing step and the final mixing step using a common Banbury mixer, according to the mixing formula shown in Table 1 or Table 2. After the first mixing step, the mixture was first taken out of the Banbury mixer, and then the mixture was put into the Banbury mixer again, and the final mixing step was performed. In addition, the maximum temperature of the mixture in the first mixing step was set to 170° C., and the maximum temperature of the rubber composition in the final mixing step was set to 110° C.
[0248] In Table 1 and Table 2, a blank portion means a number value of 0. Details of the components shown in Table 1 and Table 2 are as follows.
[0249] [Rubber component]
[0250] NR: Natural ingredients
[0251] Modified SBR with low bound styrene content: aminoalkoxysilane-modified styrene-butadiene rubber (bound styrene content 10%) synthesized by the following method and having a bound styrene content of 15% or less
[0252] Modified SBR with high bound styrene content 1: Aminoalkoxysilane-modified styrene-butadiene rubber (bound styrene content 35%) synthesized by the following method and having a bound styrene content of 30% or more
[0253] Modified SBR2 with high bound styrene content: aminoalkoxysilane-modified styrene-butadiene rubber (bound styrene content 41%) synthesized by the following method and having a bound styrene content of 30% or more
[0254] Unmodified SBR with low bound styrene content: Unmodified styrene-butadiene rubber, manufactured by Asahi Kasei Corp., trade name "TUFDENE 2000" (bound styrene content 23.5%)
[0255] Unmodified SBR with high bound styrene content: Unmodified styrene-butadiene rubber (bound styrene content 35% or more)
[0256] [Filler and silane coupling agent]
[0257] Silica 1: manufactured by Tosoh Silica Corp., trade name "Nipsil AQ" (BET specific surface area = 220 m 2 / g)
[0258] Silica 2: BET specific surface area = 110 m 2 / g of silicon dioxide
[0259] Silica 3: BET specific surface area = 245 m 2 / g of silicon dioxide
[0260] Carbon black: N234 grade carbon black
[0261] Silane coupling agent A: manufactured by Degussa AG, trade name "Si75"
[0262] Silane coupling agent B: manufactured by Degussa AG, trade name "Si363"
[0263] Aluminum hydroxide: manufactured by Showa Denko KK, trade name "HIGILITE H-42M"
[0264] Oil component: manufactured by Idemitsu Kosan Co., Ltd., trade name "DIANA processing oil PS-90"
[0265] [Hydrogenated resin]
[0266] Resin 1: Hydrogenated C5 resin, manufactured by Eastman Chemical Company, trade name "Registered Trademark Impera E1780", softening point = 130°C, weight average molecular weight (Mw) = 800
[0267] Resin 2: Hydrogenated C5 / DCPD resin, softening point = 113°C, weight average molecular weight (Mw) = 700
[0268] Resin 3: C5 resin, manufactured by Tonen Chemical Corp., corresponding to the trade name "TrezRA100"
[0269] Resin 4: DCPD resin
[0270] The rubber composition of each of the examples and comparative examples included 5.1 parts by mass of an antioxidant including a trade name "NOCRAC 6C" manufactured by Ouchi Shinko Chemical Industrial Co., Ltd., 0.3 parts by mass of a vulcanization retarder, 1 part by mass of stearic acid, 2.5 parts by mass of zinc oxide, 1.7 parts by mass of sulfur, a total of 2 parts by mass of wax, and 2 parts by mass of a workability improving agent as other components. In addition, the rubber composition of Example 1 included 1 part by mass of thiourea.
[0271] The vulcanization accelerator package includes a sulfenamide-based vulcanization accelerator.
[0272] (Method for synthesizing modified SBR having low bound styrene content)
[0273] Into an 800-mL pressure-resistant glass container that had been dried and purged with nitrogen, a cyclohexane solution of 1,3-butadiene and a cyclohexane solution of styrene were introduced to provide 67.5 g of 1,3-butadiene and 7.5 g of styrene, 0.6 mmol of 2,2-ditetrahydrofuranyl propane was added thereto, 0.8 mmol of n-butyl lithium was added thereto, and then polymerization was performed at 50°C for 1.5 hours. In the polymerization reaction system in which the polymerization conversion rate almost reached 100% at this time, 0.72 mmol of N,N-bis(trimethylsilyl)-3-[diethoxy(methyl)silyl]propylamine as a modifier was added thereto, and the modification reaction was performed at 50°C for 30 minutes. Subsequently, 2 mL of a 5% by mass isopropanol solution of 2,6-di-tert-butyl-p-cresol (BHT) was added thereto to terminate the reaction, and the resultant was dried according to a conventional method to obtain a modified SBR having a low amount of bound styrene. The microstructure of the obtained modified polymer was determined by an infrared method (Morero method), and as a result, the bound styrene amount was 10% by mass.
[0274] (Method for synthesizing modified SBR1 having a high amount of bound styrene)
[0275] A cyclohexane solution of 1,3-butadiene and a cyclohexane solution of styrene were introduced into an 800-mL pressure-resistant glass container that had been dried and purged with nitrogen to provide 67.5 g of 1,3-butadiene and 7.5 g of styrene, 0.6 mmol of 2,2-ditetrahydrofuran propane was added thereto, 0.8 mmol of n-butyl lithium was added thereto, and then polymerization was performed at 50° C. for 1.5 hours. In the polymerization reaction system in which the polymerization conversion rate was almost 100% at this time, 0.72 mmol of N-(1,3-dimethylbutylene)-3-triethoxysilyl-1-propylamine as a modifier was added thereto, and the modification reaction was performed at 50° C. for 30 minutes. Subsequently, 2 mL of a 5% by mass isopropanol solution of 2,6-di-tert-butyl-p-cresol (BHT) was added thereto to terminate the reaction, and the resultant was dried according to a conventional method to obtain a modified SBR1 having a high amount of bound styrene. The microstructure of the obtained modified polymer was determined by an infrared method (Morero method), and as a result, the bound styrene amount was 35% by mass.
[0276] (Method for synthesizing modified SBR2 having a high amount of bound styrene)
[0277] 1. Example of manufacturing a modifier
[0278] Prepare two vacuum-dried 4L stainless steel pressure vessels. 944g of cyclohexane, 161g of the compound represented by the following chemical formula (2-1) and 86g of tetramethylethylenediamine are introduced into the first pressure vessel, and the first reaction solution is manufactured. At the same time, 318g of liquid 20% by mass n-butyl lithium and 874g of cyclohexane are introduced into the second pressure vessel, and the second reaction solution is manufactured. At this time, the molar ratio of the compound represented by the following chemical formula (2-1), n-butyl lithium, and tetramethylethylenediamine is 1:1:1. In a state where the pressure of each pressure vessel is maintained at 7 bar, in a continuous reactor using a mass flow meter, the first reaction solution is injected into the first continuous channel at an injection rate of 1.0g / min, and the second reaction solution is injected into the second continuous channel at an injection rate of 1.0g / min. At this time, the temperature of the continuous reactor was maintained at -10°C, the internal pressure was maintained at 3 bar by using a backpressure regulator, and the residence time in the reactor was adjusted to within 10 minutes. The reaction was completed to obtain a modified initiator.
[0279]
[0280] 2. Production of modified SBR 2 with high bound styrene content
[0281] In the first unit reactor in the continuous reactor having three unit reactors connected in series, a styrene solution in which styrene was dissolved in n-hexane at 60% by mass was injected at a rate of 7.99 kg / h; a 1,3-butadiene solution in which 1,3-butadiene was dissolved in n-hexane at 60% by mass was injected at a rate of 10.55 kg / h; n-hexane was injected at a rate of 47.66 kg / h; a 1,2-butadiene solution in which 1,2-butadiene was dissolved in n-hexane at 2.0% by mass was injected at a rate of 10 g / h; a solution in which 2,2-di(2-(tetrahydrofuryl)propane was dissolved in n-hexane at 10% by mass as a polar additive was injected at a rate of 10.0 g / h; and the modified initiator manufactured in the above manufacturing example was injected at a rate of 292.50 g / h. At this time, the temperature of the first unit reactor was maintained at 50° C., and when the polymerization conversion reached 43%, the polymer product was transported from the first reactor to the second reactor through a transport pipe.
[0282] Subsequently, a 1,3-butadiene solution in which 1,3-butadiene was dissolved in n-hexane at a rate of 0.95 kg / h was injected into the second reactor. At this time, the temperature of the second unit reactor was maintained at 65° C., and when the polymerization conversion rate reached 95% or more, the polymer product was transported from the second reactor to the third reactor through the transport pipe.
[0283] The polymer product was transferred from the second reactor to the third reactor, and a solution of the following formula (1a) dissolved therein as a modifier was introduced into the third reactor (modifier: act.Li=1:1 mol). The temperature of the third reactor was maintained at 65° C. In formula (1a), Me represents a methyl group.
[0284]
[0285] Subsequently, IR1520 (BASF SE) solution in which the compound was dissolved at 30% by mass was injected as an antioxidant into the polymerization solution discharged from the third reactor at a rate of 170 g / h, and the mixture was stirred. As a result, the obtained polymerization product was introduced into hot water heated with steam, the mixture was stirred, and the solvent was removed, thereby obtaining a modified SBR 2 having a high bound styrene content.
[0286] Furthermore, the microstructure of the obtained modified SBR 2 having a high styrene-bonded amount had a styrene content of 41% by mass.
[0287] (Method for producing silicon dioxide 2)
[0288] In a 180-liter jacketed stainless steel reaction tank equipped with a stirrer, 65 liters of water and 1.25 liters of an aqueous sodium silicate solution (SiO2 160 g / liter, SiO2 / NA2O molar ratio 3.3) were introduced, and the mixture was heated to 96° C. The NA2O concentration in the resulting solution was 0.015 mol / liter.
[0289] While the temperature of the solution is maintained at 96°C, a sodium silicate aqueous solution and sulfuric acid (18 mol / liter) similar to the above are simultaneously added thereto, a sodium silicate aqueous solution is added at a flow rate of 750 ml / min, and sulfuric acid is added at a flow rate of 33 ml / min. While adjusting the flow rate, a neutralization reaction is performed while maintaining the NA2O concentration in the reaction solution within the range of 0.005 to 0.035 mol / liter. The reaction solution becomes turbid from the middle of the reaction, the viscosity increases after 30 minutes, and then the reaction solution becomes a gel-like solution. In addition, the addition is continued, and the reaction is terminated at 100 minutes. The silica concentration in the generated solution is 85 g / liter. Subsequently, sulfuric acid similar to the above sulfuric acid is added until the pH of the solution reaches 3, and a silica slurry is obtained. The silica slurry obtained is filtered by a filter press and washed with water to obtain a wet cake. Next, the wet cake is slurried using an emulsifying device, the slurry is dried in a spray dryer, and silica 2 as a wet method hydrated silica is obtained.
[0290] (Method for producing silicon dioxide 3)
[0291] In the same stainless steel reaction tank as used in Production Example 1, 89 liters of water and 1.70 liters of an aqueous sodium silicate solution (SiO2 160 g / liter, SiO2 / NA2O molar ratio 3.3) were introduced, and the mixture was heated to 75° C. The NA2O concentration in the resulting solution was 0.015 mol / liter.
[0292] While the temperature of the solution is maintained at 75°C, a sodium silicate aqueous solution and sulfuric acid (18 mol / liter) similar to the above are simultaneously added thereto, a sodium silicate aqueous solution is added at a flow rate of 520 ml / min, and sulfuric acid is added at a flow rate of 23 ml / min. While adjusting the flow rate, a neutralization reaction is performed while maintaining the NA2O concentration in the reaction solution within the range of 0.005 to 0.035 mol / liter. The reaction solution becomes turbid from the middle of the reaction, the viscosity increases after 46 minutes, and then the reaction solution becomes a gel-like solution. In addition, the addition is continued, and the reaction is terminated at 100 minutes. The silica concentration in the generated solution is 60 g / liter. Subsequently, sulfuric acid similar to the above sulfuric acid is added until the pH of the solution reaches 3, and a silicate slurry is obtained. Thereafter, silica 3 as wet-process hydrated silica is obtained in the same manner as the manufacturing method of silica 2.
[0293] <Vulcanization of Rubber Composition and Evaluation of Vulcanized Rubber>
[0294] [Examples 1 to 5, Comparative Examples 1 to 4, and Comparative Example 6]
[0295] 1. Wet grip
[0296] The vulcanized rubber sample obtained by vulcanizing the rubber composition was subjected to initial strain by a viscoelasticity measuring machine. Subsequently, under the conditions of dynamic strain: 1%, frequency: 52 Hz, and measurement temperature: -5°C, the loss tangent (tan δ) of the vulcanized rubber sample was measured, and the performance in the tire was calculated.
[0297] The resistance value of Example 1 was taken as 100, and the measured values of each Example and Comparative Example were expressed as an index. A larger index indicates a larger resistance value and excellent wet grip. The results are shown in Tables 1 and 2. The allowable range is 95 or more.
[0298] 2. Rolling resistance
[0299] The vulcanized rubber sample obtained by vulcanizing the rubber composition was subjected to initial strain by a viscoelasticity measuring machine. Subsequently, under the conditions of dynamic strain: 1%, frequency: 52 Hz, and measurement temperature: 50° C., the loss tangent (tan δ) of the vulcanized rubber sample was measured, and the performance in the tire was calculated.
[0300] The tan δ of the vulcanized rubber sample of Example 1 was taken as 100, and the measured values of each Example and Comparative Example were expressed as an index. The smaller the index, the smaller and more satisfactory the rolling resistance. The results are shown in Tables 1 and 2. The allowable range is 100 or more.
[0301] 3. Wear resistance
[0302] For the vulcanized rubber obtained by vulcanizing the rubber composition, the wear amount at room temperature when the slip ratio was 100% was measured using a DF tester. The tire performance is shown in the table.
[0303] The wear amount of the vulcanized rubber of Example 1 was taken as 100, and the predictions of each Example and Comparative Example were expressed as an index. A larger index indicates a smaller wear amount and excellent wear resistance. The results are shown in Tables 1 and 2. The allowable range is 99 or more.
[0304] [Examples 6 and 7, Comparative Example 5, and Comparative Example 7]
[0305] 1. Wet grip
[0306] The vulcanized rubber sample obtained by vulcanizing the rubber composition was subjected to initial strain by a viscoelasticity measuring machine. Subsequently, under the conditions of dynamic strain: 1%, frequency: 52 Hz, and measurement temperature: -5°C, the loss tangent (tan δ) of the vulcanized rubber sample was measured, and the performance in the tire was calculated.
[0307] The resistance value of Example 1 was taken as 100, and the measured values of each comparative example were expressed as an index. A larger index indicates a larger resistance value and excellent wet grip. The results are shown in Tables 1 and 2. The allowable range is 95 or more.
[0308] 2. Rolling resistance
[0309] The vulcanized rubber sample obtained by vulcanizing the rubber composition was subjected to initial strain by a viscoelasticity measuring machine. Subsequently, under the conditions of dynamic strain: 1%, frequency: 52 Hz, and measurement temperature: 50° C., the loss tangent (tan δ) of the vulcanized rubber sample was measured, and the performance in the tire was calculated.
[0310] The tan δ of the vulcanized rubber sample of Example 1 was taken as 100, and the measured values of each comparative example were expressed as an index. The smaller the index, the smaller and more satisfactory the rolling resistance. The results are shown in Tables 1 and 2. The allowable range is 100 or more.
[0311] 3. Wear resistance
[0312] For the vulcanized rubber obtained by vulcanizing the rubber composition, the wear amount at a slip ratio of 60% at room temperature was measured using a DF tester. The tire performance is shown in the table.
[0313] The wear amount of the vulcanized rubber of Example 1 was taken as 100, and the prediction of each comparative example was expressed as an index. A larger index indicates a smaller wear amount and excellent wear resistance. The results are shown in Tables 1 and 2.
[0314] The allowable range is 99 or more.
[0315]
[0316] Table 2
[0317]
[0318] It can be understood from the results of Examples shown in Table 1 and Table 2 that a tire having excellent wet grip and low rolling resistance is obtained by using the rubber composition according to the present invention.
[0319] Industrial Applicability
[0320] The rubber composition according to the present invention can be used for tires, particularly tread rubber of tires.
Claims
1. A tire obtained by using a rubber composition, The rubber composition comprises: A rubber component comprising a rubber having an isoprene structure and an aminoalkoxysilane-modified styrene-butadiene rubber having a bound styrene amount of 15% or less; Filler, comprising a nitrogen adsorption specific surface area (BET method) of 130 m 2 / g or more and less than 330m 2 / g of silica, and the amount of the filler is 40 to 125 parts by mass relative to 100 parts by mass of the rubber component; and The hydrogenated resin has a softening point higher than 110° C. and a weight average molecular weight of 200 to 1200 g / mol in terms of polystyrene, and the amount of the hydrogenated resin is 5 to 50 parts by mass based on 100 parts by mass of the rubber component. 2 . The tire according to claim 1 , wherein the content of the modified styrene-butadiene rubber in the rubber component is 10% by mass to 90% by mass. 3 . The tire according to claim 1 , wherein the content of the rubber having an isoprene structure in the rubber component is 10% by mass to 90% by mass. 4 . The tire according to claim 1 , wherein the rubber component further comprises a modified styrene-butadiene rubber having a bound styrene amount of 30% or more. 5 . The tire according to claim 1 , wherein the filler further contains carbon black, and a content of the silica in the filler is 70% by mass or more. 6 . The tire according to claim 1 , wherein the hydrogenated resin is at least one selected from the group consisting of a hydrogenated C5-based resin, a hydrogenated C5-C9-based resin, and a hydrogenated dicyclopentadiene-based resin. 7 . The tire according to claim 1 , wherein the rubber composition further comprises a silane coupling agent having a mercapto group.
Citation Information
Patent Citations
Rubber composition and tire using the same
JP2007217562A
Rubber composition for tire, and pneumatic tire using the same
JP2008184505A
Conjugated diene polymer, process for its production and rubber compositions containing the same
WO2003046020A1
Process for removing acidic compounds from a gaseous effluent with a dihydroxyalkylamine-based absorbent solution
WO2015007970A1
Rubber composition and tire
WO2015079703A1